Glass with high elastic modulus

By using common components such as quicklime, alumina, and silica, high elastic modulus glass was prepared, solving the problems of rare glass components and environmental pollution from mining, and realizing the sustainable preparation and strengthening of high stiffness glass.

CN123125178APending Publication Date: 2026-11-17CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580026454.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-08
Filing Date
2025-04-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing glass components are rare and resource-intensive to extract, leading to environmental pollution and making it difficult to obtain high-rigidity glass in a sustainable manner.

Method used

High-elasticity glass is formed by combining common components such as quicklime, alumina, and silicon dioxide in specific proportions. High-rigidity glass is also prepared by combining high amounts of alkaline earth metal oxides such as quicklime and magnesium oxide with sodium oxide.

Benefits of technology

High elastic modulus glass is produced, suitable for protective covers and other applications, with excellent coating properties and scratch resistance, and its strength can be enhanced by ion exchange chemical tempering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125178A_ABST
    Figure CN123125178A_ABST
Patent Text Reader

Abstract

This disclosure provides a glass comprising, in mole percentage (mol%) of oxide components, at least 18 mol% and no more than 42 mol% silica, at least 18 mol% and no more than 40 mol% alumina, at least 5 mol% alkali metal oxide, at least 2 mol% quicklime, and at least 0.1 mol% and no more than 30 mol% magnesium oxide. The total of the quicklime and the magnesium oxide is at least 26 mol% and no more than 40 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This application claims priority to U.S. Application Serial No. 63 / 575,880, filed April 8, 2024, the contents of which are used as a basis and are incorporated herein by reference in their entirety. Background Technology

[0003] Various aspects of this disclosure relate to glass, such as glass that can be used as a housing or cover for electronic devices or for other purposes.

[0004] Glass (such as glass sheets) can provide a protective cover for the displays of electronic devices such as mobile phones and laptops. Glass can be formed into sheets using a melt-forming process or what is known as the float glass process. The glass can then be cut into the desired shape and integrated into electronic components. Furthermore, such glass can be inherently strong and can be strengthened, for example, through ion-exchange chemical tempering. However, the components used to manufacture such glass can be quite rare and may require resource-intensive mining to obtain. Furthermore, such mining can be harmful to the environment.

[0005] There is a need for glass that can be used as a protective cover or in applications where the high stiffness of the glass may benefit, and that is made from components that can be obtained in a fairly sustainable manner. Summary of the Invention

[0006] The glass disclosed herein comprises fairly common components such as quicklime (CaO), alumina (Al2O3), and silicon dioxide (Si2O). The glass may also include sodium oxide (Na2O), magnesium oxide (MgO), and other components. These components are combined in novel and unexpected ways, for example, including more quicklime than silicon dioxide, and as further explained below, the elastic modulus of the glass unexpectedly exceeds 90 GPa, typically exceeding 100 GPa, 110 GPa, or even exceeding 115 GPa. In contrast, the elastic modulus of a “sodium-calcium silicate” glass consisting of about 70 wt% silicon dioxide, 15 wt% sodium oxide, 10 wt% quicklime, and 5 wt% trace amounts of other compounds (such as alumina, potassium oxide (K2O), and magnesium oxide (MgO)) is less than 75 GPa, such as about 70 or 72 GPa. The increased stiffness of the glass disclosed herein gives it unique advantages over glass made from commonly available components in terms of coating performance and scratch resistance, thereby facilitating its use as a protective cover or in other applications such as windows, containers, enclosures, panels, and laboratory equipment.

[0007] Further features and advantages will be set forth in the following detailed description, and some will be apparent to those skilled in the art from the specification or will be recognized by practice of the techniques described in the written description and claims and the accompanying drawings. It should be understood that both the foregoing general description and the following detailed description are merely exemplary and intended to provide an overview or framework for understanding the nature and characteristics of the claims. Attached Figure Description

[0008] The accompanying drawings are provided to provide a further understanding and are incorporated in and constitute a part of this specification. The figures in the drawings illustrate one or more aspects of this disclosure and, together with the detailed description, explain the principles and operation of each aspect. Therefore, this disclosure will be more fully understood from the following detailed description taken in conjunction with the accompanying drawings, in which:

[0009] Figure 1 This is a front view of a glass article formed by drop pressing according to one aspect of this disclosure. Detailed Implementation

[0010] Before referring to the following detailed description and accompanying drawings, which illustrate various aspects of this disclosure in detail, it should be understood that the technology of the invention is not limited to the details or methods set forth in the detailed description or shown in the accompanying drawings. For example, as those skilled in the art will understand, features and attributes shown in the accompanying drawings or described in text related to a particular aspect may be applied to other aspects described elsewhere in the text.

[0011] The applicant has discovered a novel glass with useful properties and made generally of fairly common components. More specifically, the components include relatively large amounts of quicklime, alumina, and silica (all fairly common materials), and may also include sodium oxide (another fairly common material). According to one aspect, the glass may be single-phase, wherein the glass is amorphous rather than glass-ceramic, and the glass has the same physical and chemical properties overall, exhibiting the characteristics of an isotropic, homogeneous material. Therefore, aspects of this disclosure relate to glass, methods of manufacturing and using said glass, articles comprising glass, and methods of manufacturing and using said articles, wherein the concentration of the constituent components in oxide form (e.g., quicklime, silica, alumina, sodium oxide, etc.) is expressed as a molar percentage (mol%) based on oxides unless otherwise specified (e.g., when expressed as a weight percentage). It should be noted that, in addition to the components described above, the glass may also include other alkali metal oxides, such as potassium oxide and possibly lithium oxide (Li₂O), and the glass may include alkaline earth metal oxides other than quicklime, such as magnesium oxide; and / or may include zirconium oxide (ZrO₂) and other components.

[0012] Although many, most, or even all of the components of glass are ubiquitous, at least some of the glasses disclosed herein possess very high moduli of elasticity, such as exceeding 90 GPa, typically exceeding 100 GPa, 110 GPa, and even exceeding 115 GPa. The modulus of elasticity (also known as Young's modulus, as shown in Table 2 below) can be measured by Brillouin spectroscopy (Table 1), resonant ultrasonic spectroscopy (Table 2), or a simple tensile test, and corresponds to the slope of stress (tensile load per unit cross-sectional area) versus strain (length change per unit length) in the elastic region of the glass under standard conditions (e.g., approximately until failure for brittle materials such as the glass described herein). The applicant considers the novel glass with such a high modulus of elasticity, made primarily of ubiquitous components, to be significant and unexpected. Such high-modulus glasses have advanced the technology in the field because they open the door to new combinations of materials, such as glasses reinforced or paired with coatings having a comparable elastic modulus (e.g., within 20 GPa; within 10 GPa; less than the elastic modulus of glass), and thus overcome coating-related challenges such as delamination or interfacial strain caused by elastic modulus mismatch. Furthermore, the applicant believes that the glasses disclosed herein have comparable advantages in hardness and scratch resistance, as compared to soda-lime silicates.

[0013] According to one aspect, the glass may be translucent and / or transparent, such as having an average transmittance of at least 10% for light in the wavelength range of 380 nm to 750 nm at a path length (e.g., thickness) of linear dimensions (e.g., 0.6 mm, 0.8 mm, 1.0 mm, 1.4 mm, 2 mm), such as at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, and / or even more than 90%. The transmittance in the visible spectrum can be measured using a Lambda 950 UV / Vis / NIR spectrophotometer manufactured by PerkinElmer Inc. (Waltham, Massachusetts USA). The Lambda 950 device can be equipped with a 150 mm integrating sphere. An open beam baseline and Spectralon can then be used. ®Data is collected using a reference reflector. For total transmittance, the sample can be fixed at the entrance point of the integrating sphere. As used herein with respect to the visible spectrum, the term "average transmittance" refers to the average of total transmittance measurements obtained over a given wavelength range, where each integer wavelength is weighted equally. As used herein, "average transmittance" for the visible spectrum is reported in the wavelength range of 380 nm to 750 nm (inclusive). Unless otherwise stated, average transmittance is expressed for a 0.6 mm optical path length (e.g., article thickness) through glass of the same composition.

[0014] For “silicate glasses,” silica is typically the major or largest component (in mol%), and / or usually the major glass-forming component. However, for at least some of the glasses disclosed herein, alumina is the major glass-forming component; and at least some of the glasses disclosed herein contain comparable amounts of silica and alumina, as further explained herein, such that they differ from each other by less than 20 mol%, less than 15 mol%, and less than 10 mol%. In even some of the glasses disclosed herein, alumina is the largest single component (in mol%). Alumina can contribute to achieving the particularly high modulus of elasticity found for the glasses disclosed herein.

[0015] According to one aspect of this disclosure, the glass comprises at least some silica and / or at least some alumina, such as at least 10 mol% of either or both of silica and alumina, such as at least 15 mol% of either or both of silica and alumina, such as at least 18 mol% of either or both of silica and alumina, such as at least 20 mol% of either or both of silica and alumina. According to one aspect of this disclosure, the glass comprises at least 25 mol% of either silica or alumina. Excessive silica (such as exceeding 50 mol%, exceeding 45 mol%, or exceeding 42% according to some aspects of this disclosure) may reduce the elastic modulus or, when combined with other components disclosed herein, produce a material that is not a single-phase glass. Similarly, excessive alumina (such as exceeding 50 mol%, exceeding 45 mol%, or exceeding 42% according to some aspects of this disclosure) may, when combined with other components disclosed herein, produce a material that is not a single-phase glass.

[0016] According to one aspect, as alumina increases, silica decreases, and vice versa, resulting in a total alumina and silica content between 41 mol% and 61 mol%, such as between 45 mol% and 55 mol%. Those skilled in the art will consider the amount of such network-forming components to be unexpectedly low. According to another aspect, the alumina in the glass is in the range of 18 mol% to 40 mol%, where it combines with silica in a similar range of 18 mol% to 42 mol%. This unexpectedly low amount of silica and alumina network formation is subsequently compensated for by an unexpectedly high amount of alkaline earth metal oxides.

[0017] According to one aspect of this disclosure, the glass contains unexpectedly high amounts of alkaline earth metal oxides, such as quicklime and magnesium oxide. Such amounts would not be expected by those skilled in the art to form a glass. The applicant has found that the high amounts of alkaline earth metal oxides, combined with the aforementioned network forgings, produce a glass with a high elastic modulus, as disclosed herein. According to one aspect, the glass contains at least 20 mol% of alkaline earth metal oxides, such as at least 22 mol%, at least 25 mol%, at least 26 mol%, and such amounts may be expressed solely as the sum of quicklime and magnesium oxide, such as where the sum of the mol% of quicklime and the mol% of magnesium oxide is at least 26 mol%. According to one aspect, the glass contains non-zero amounts of both quicklime and magnesium oxide, such as at least 0.08 mol% each, such as at least 0.1 mol% each, for example, at least 0.08 mol% of magnesium oxide and at least 2 mol% of quicklime combined with alumina in the range of 18 mol% to 40 mol% and silica in the range of 18 mol% to 42 mol%. Even so, excessive alkaline earth metal oxides (such as more than 30 mol% magnesium oxide or more than 40 mol% quicklime) can disrupt glass formation. For example, the total amount of magnesium oxide and quicklime can be less than 50 mol%, such as less than 45 mol%, such as less than 40 mol%, such as at least a non-zero amount of both, such as at least 0.08 mol% magnesium oxide and at least 2 mol% quicklime combined with silica and alumina as just described. Surprisingly, quicklime may be the largest oxide component in glass, as shown in some examples provided herein.

[0018] According to one aspect of this disclosure, the glass contains a non-zero amount of alkali metal oxides, such as sodium oxide, lithium oxide, and / or potassium oxide (e.g., at least 5 mol%), such as at least 5 mol% sodium oxide. Alkali metal oxides can promote glass strengthening (e.g., through ion exchange). Further, the applicant believes that, at relatively low contents, alkali metal oxides can be replaced by alkaline earth metal oxides, particularly quicklime, without significantly reducing the elastic modulus of the resulting glass. Therefore, the sum of alkali metal oxides and alkaline earth metal oxides (e.g., quicklime + magnesium oxide + sodium oxide + lithium oxide in mol%) can be greater than 35 mol%, such as greater than 40 mol%, such as greater than 41 mol%. Unexpectedly, the sum of alkali metal oxides and alkaline earth metal oxides in mol% can be greater than silicon dioxide, greater than aluminum oxide in mol%, and / or greater than the sum of network formations (e.g., the sum of silicon dioxide and aluminum oxide). This result, the formation of a glass with a high modulus, is unexpected, because quicklime and magnesium oxide are generally considered modifiers, and such glasses may contain excessive amounts of modifiers, which could increase non-bridging oxygen and thus potentially reduce the elastic modulus. However, the findings disclosed in this paper indicate that this is not the case.

[0019] Sodium oxide is a preferred alkali metal oxide because, unlike lithium oxide, it is a fairly common material, and sodium, being a relatively small atom, is useful during ion-exchange chemical tempering, where sodium near the surface of such glass articles can be replaced by larger atoms (such as potassium), thereby imparting compressive stress. However, another envisioned aspect could have high amounts of lithium oxide, such as at least 5 mol%, at least 9 mol%, at least 10 mol%, at least 11 mol%, and / or not exceeding 25 mol%. Such glasses can benefit from high modulus and relatively strong chemical tempering.

[0020] As shown in Tables 1 and 2 below, in addition to the components disclosed above, the glasses disclosed herein may also contain, for example, phosphorus pentoxide (P₂O₅), boron oxide (B₂O₃), yttrium oxide (Y₂O₃), and zirconium oxide (ZrO₂). Further, the glass may include, for example, some tin dioxide (SnO₂) or other clarifying agents as a clarifying agent. For example, the glass may include at least 0.01 mol% of phosphorus pentoxide. The glass may optionally contain boron oxide, such as zero in some glasses, and at least 1 mol% and / or no more than 26 mol% in other glasses disclosed herein. Boron oxide can improve scratch resistance. The glass may optionally contain yttrium oxide, such as zero in some glasses, and at least 1 mol% and / or no more than 7 mol% in other glasses disclosed herein. Yttrium oxide can improve stiffness, but it may be a relatively rare material compared to other materials disclosed herein. The glass may optionally contain zirconium oxide, such as zero in some glasses and at least 1 mol% and / or no more than 5 mol% in others disclosed herein.

[0021] Many of the glasses disclosed herein have particularly high strain points, as illustrated in the examples, such as above 600°C, above 625°C, above 650°C, and in some cases even above 675°C. Therefore, the applicant believes that the glasses can be chemically tempered in a high-temperature molten salt bath, such as in a bath at temperatures exceeding 500°C, above 525°C, or above 550°C, to improve chemical tempering. The applicant has found that, for effective use of salts at such temperatures, a combination of nitrogen-based and sulfur-based salts can be used, wherein the weight percentage of the sulfur-based salt is increased at higher bath temperatures. Further, when the glass comprises sodium oxide or other alkali metal oxides as disclosed above, the bath can comprise potassium- and sodium-containing salts. Therefore, according to one aspect, the glass can be ion-exchanged in a salt bath containing a molten mixture of sodium nitrate, sodium sulfate, potassium nitrate, and / or potassium sulfate salts at temperatures exceeding 500°C to achieve surface or peak compressive stress (e.g., at least 50 MPa, at least 100 MPa) and central tension (e.g., at least 10 MPa). In a salt bath, the wt% of sodium nitrate may be greater than that of sodium sulfate, the wt% of potassium nitrate may be greater than that of potassium sulfate, and / or the wt% of sodium-containing salts may be greater than that of potassium-containing salts. Compared to chemical tempering, for example, in salt baths at temperatures below 400°C and in all nitrate baths, hotter salt baths can increase the depth of compression (e.g., at least 5 µm, at least 10 µm, at least 30 µm) (the depth at which compressive stress in a glass article transitions to tensile stress), can reduce the amount of time required to immerse the glass in such a bath, and can increase surface or peak compressive stress. The applicant hereby incorporates, in its entirety, U.S. Application No. 63 / 600,790, filed November 20, 2023, by reference.

[0022] Table 1 below provides examples of glasses manufactured and found to have the properties disclosed herein. Examples are presented in mol% of the analysis. The physical properties of the glasses were measured by Brillouin scattering and may include a certain error range or tolerance, such as + / - 10%. The liquidus was measured by gradient boat method and may also include a certain error range or tolerance, such as + / - 5%.

[0023] Table 1:

[0024]

[0025] Table 1 (continued):

[0026]

[0027] Table 2 below provides examples of glass samples manufactured and found to have the properties disclosed herein. Examples are provided in mol% of the analysis. The abbreviation RUS stands for Resonance Ultrasonic Spectroscopy, BBV for Beam Flexural Viscosity, and PPV for Parallel Plate Viscosity, and the measurement method may include a certain error range or tolerance, such as + / - 10%; see also ASTM C829-81 and ASTM C1351M. The liquidus is measured by the gradient boat method and may also include a certain error range or tolerance, such as + / - 5%; see also ASTM C829-81. Some common properties described herein are measured by different techniques (e.g., Brillouin scattering and Resonance Ultrasonic Spectroscopy), therefore, unless otherwise specified in the claims, values ​​refer to values ​​measurable by the techniques in Table 2, such as having reasonable error tolerances as disclosed or known in the art.

[0028] Table 2:

[0029]

[0030] Table 2 (continued)

[0031]

[0032] Table 2 (continued)

[0033]

[0034] According to one aspect and as shown in the example, the density of the glass can be at least 2.5 g / cm³. 3 For example, at least 2.6g / cm 3 For example, at least 2.612 g / cm³ 3 and / or not exceeding 3.1 g / cm 3 If not exceeding 3.011 g / cm 3 The density can be, for example, 2.6 g / cm³. 3 With 3 g / cm 3 between.

[0035] According to one aspect and as exemplified, when using Brillouin scattering, the refractive index of the glass at 589.3 nm can be at least 1.5 (dimensionless), such as at least 1.55, such as at least 1.567, and / or not more than 1.7, such as not more than 1.65, such as not more than 1.63, such as not more than 1.628. The refractive index can be, for example, between 1.55 and 1.65.

[0036] According to one aspect and as exemplified, such as by Brillouin scattering or by resonance ultrasonic spectroscopy, the Young's modulus (also known as the elastic modulus) of the glass may be at least 80 GPa, such as at least 90 GPa, such as at least 95 GPa, such as at least 96.5 GPa, and / or not exceeding 140 GPa, such as not exceeding 125 GPa, such as not exceeding 115 GPa, such as not exceeding 110.7 GPa. The Young's modulus may, for example, be between 90 GPa and 140 GPa, such as between 100 GPa and 130 GPa, such as between 110 GPa and 125 GPa.

[0037] According to one aspect and as exemplified, such as by Brillouin scattering or by resonance ultrasonic spectroscopy, the shear modulus of the glass may be at least 30 GPa, such as at least 35 GPa, such as at least 38 GPa, such as at least 38.2 GPa, and / or not more than 55 GPa, such as not more than 50 GPa, such as not more than 45 GPa, such as not more than 43.6 GPa. The shear modulus may, for example, be between 35 GPa and 50 GPa.

[0038] According to one aspect and as exemplified, such as by Brillouin scattering or by resonance ultrasonic spectroscopy, the Poisson's ratio of the glass may be at least 0.25 (dimensionless), such as 0.26, such as 0.262, and / or not exceeding 0.29, such as not exceeding 0.28, such as not exceeding 0.273. The Poisson's ratio may, for example, be between 0.25 and 0.29.

[0039] The viscosity of glass can be measured according to ASTM C829-81. The "softening point" refers to the viscosity of the glass at 1 × 10⁻⁶. 7.6 The softening point can be measured using the parallel plate viscosity method, similar to ASTM C1351M, which measures the glass at 10°C. 7 Up to 10 9 Viscosity varies with temperature within the Poisson range. The "annealing point" can refer to a glass with a viscosity of 1 × 10⁻⁶. 13.18 The temperature at which the glass is held. The "strain point" can refer to the point where the glass viscosity is 1 × 10⁻⁶. 14.68 The liquidus temperature. "Liquidline viscosity" can refer to the viscosity of the glass at the onset of devitrification, i.e., the viscosity at which crystallization first occurs, or it can refer to the viscosity at the liquidus temperature as determined by the gradient furnace method according to ASTM C829-81. Therefore, "liquidline temperature" can refer to the temperature at which the glass composition begins to devitrify, as determined by the gradient furnace method according to ASTM C829-81.

[0040] According to one aspect and as exemplified, such as by measurement using the gradient boat method, the liquidus temperature of the glass can be at least 1150°C, such as at least 1200°C, and / or not higher than 1600°C, such as not higher than 1500°C. The liquidus temperature can, for example, be between 1200°C and 1500°C.

[0041] According to one aspect and as exemplified, such as by measurement via beam flexural viscosity, the strain point of the glass can be at least 450°C, such as at least 460°C, such as at least 500°C, and / or not higher than 800°C, such as not higher than 750°C, such as not higher than 700°C. The strain point can, for example, be between 450°C and 750°C.

[0042] According to one aspect and as exemplified, such as by measurement via beam flexural viscosity, the annealing point of the glass can be at least 470°C, such as at least 490°C, such as at least 491°C, such as at least 520°C, and / or not higher than 820°C, such as not higher than 770°C, such as not higher than 750°C, such as not higher than 739°C. The annealing point can, for example, be between 490°C and 750°C.

[0043] According to one aspect and as exemplified, such as by measuring the viscosity of a parallel plate, the softening point of the glass can be at least 470°C, such as at least 600°C, such as at least 620°C, such as at least 628°C, and / or not higher than 950°C, such as not higher than 910°C, such as not higher than 904°C. The softening point can be, for example, between 620°C and 910°C.

[0044] According to one aspect and as shown in the example, the glass may have: HTV A (dimensionless) ranging from -8.4 (e.g., -8.423) to 1.5 (e.g., 1.478); HTV B ranging from 140°C (e.g., 148.4°C) to 14500°C (e.g., 14371.6°C); and HTV T0 ranging from -550°C (e.g., -499.7°C) to 1250°C (e.g., 1124.1°C).

[0045] According to one aspect and as illustrated by example, the liquidus viscosity of the glass can be less than 1000 poise, such as less than 500 poise, such as less than 200 poise, such as not greater than 168.5 poise, and / or at least 1 poise, such as at least 5 poise, such as at least 7.4 poise. Those skilled in the art may find that glass with such low liquidus viscosity is difficult to form into articles, such as by melt-forming or float-forming methods. According to one aspect, a method of manufacturing an article having the glass disclosed herein includes droplet pressing of the glass, such as dropping a droplet of molten glass into a mold and rapidly pressing the molten glass into a desired shape, wherein the droplet is a discrete and relatively small volume of molten glass (e.g., less than, for example, 0.5 L). “Pre-forming” the droplet (e.g., elongating the droplet) before positioning it in the mold can, for example, allow for thinner articles, where the thicker portions are further away from the center of the mold. U.S. Patent Application No. 63 / 525,060, filed July 5, 2023, is hereby incorporated herein by reference in its entirety. In addition, pressing the glass more than once can improve the dimensional control of the pressing process, thereby reducing the need for finishing.

[0046] Figure 1 This includes an image representing a glass article 110 (e.g., a part blank) formed by drop pressing of the glass disclosed herein. This article can be cut into glass parts and finished, such as by computer numerical control grinding and polishing, to form articles suitable for use in electronic devices (such as the housings or covers disclosed above) or for other applications. Similarly, the glass disclosed herein can be molded into other articles, such as flat or curved sheets, containers, housings, panels, fibers, substrates (e.g., for memory disks, circuits, encapsulation), windows, covers, etc.

[0047] As shown in the various aspects, the construction and arrangement of the compositions, components, and structures are illustrative only. Although only a few examples of many aspects are described in detail in this disclosure, many modifications are possible (e.g., variations in the size, dimensions, structure, shape and proportion, parameter values, mounting arrangements, use of materials, color, orientation, etc.) without substantially departing from the novel teachings and advantages of the subject matter described herein. For example, although the glass and corresponding articles of manufacture are translucent and / or transparent as disclosed above, the glass and corresponding articles of manufacture may be colored, and each of U.S. Application No. 63 / 537,466, filed September 8, 2023, and International Application No. PCT / US23 / 82806, filed December 7, 2023, is incorporated herein by reference in its entirety. The order or sequence of any process, logical algorithm, or method steps may be changed or reordered according to alternative embodiments. Other substitutions, modifications, alterations, and omissions may also be made to the design, operating conditions, and arrangements of the various aspects without departing from the scope of the invention.

Claims

1. A glass, comprising, based on the mole percentage (mol%) of the oxide-based components: At least 18 mol% and not more than 42 mol% silicon dioxide; Alumina of at least 18 mol% and not exceeding 40 mol%; At least 5 mol% alkali metal oxides; Alkaline earth metal oxides, wherein the alkaline earth metal oxides cause the glass to comprise: At least 2 mol% quicklime; and At least 0.1 mol% and not more than 30 mol% magnesium oxide; and The total amount of the alkaline earth metal oxides is at least 26 mol% and not more than 40 mol%.

2. The glass according to claim 1, wherein, in mol%, the sum of the quicklime and the magnesium oxide is greater than the silicon dioxide.

3. The glass according to claim 2, wherein the quicklime is greater than the magnesium oxide in mol%.

4. The glass according to any one of claims 1 to 3, wherein the alkali metal oxide comprises sodium oxide, such that the glass comprises at least 5 mol% sodium oxide.

5. The glass according to claim 4, wherein the alkali metal oxide further comprises a non-zero amount of lithium oxide.

6. The glass of claim 1, wherein the alkali metal oxide comprises a non-zero amount of lithium oxide.

7. The glass according to claim 1, wherein the glass is a single-phase glass.

8. The glass of claim 1, wherein the glass has an average transmittance of at least 10% for light in the wavelength range of 380 nm to 750 nm at a thickness of 0.6 mm.

9. A type of glass comprising: The composition comprises sodium oxide, quicklime, and silicon dioxide, wherein the sum of the sodium oxide, quicklime, and silicon dioxide, based on the molar percentage (mol%) of the oxide components, is greater than half of the glass, and wherein the silicon dioxide is less than 40 mol% of the glass. The glass mentioned therein is a single-phase glass; The glass, with a thickness of 0.6 mm, has an average transmittance of at least 60% for light in the wavelength range of 380 nm to 750 nm; and The elastic modulus of the glass is greater than 90 GPa.

10. The glass according to claim 9, wherein the glass comprises at least 30 mol% alkaline earth metal oxide, wherein the alkaline earth metal oxide includes the quicklime.

11. The glass according to claim 10, wherein the alkaline earth metal oxide further comprises at least 0.1 mol% magnesium oxide.

12. The glass according to claim 10, wherein the mol% of the alkaline earth metal oxide in the glass is greater than the mol% of the silicon dioxide.

13. A method of manufacturing a glass article, the method comprising pressing a drop of glass according to any one of the preceding claims to at least partially shape the article.

14. A method for manufacturing glass articles, the method comprising tempering the glass according to any one of the preceding claims in a salt bath at a temperature greater than 500°C.

15. The method of claim 14, wherein the salt bath comprises sodium sulfate and sodium nitrate, wherein the amount of sodium nitrate is greater than the amount of sodium sulfate by weight percentage relative to the salt bath.

16. A method of manufacturing a glass article, the method comprising coating a glass according to any one of the preceding claims with a coating having an elastic modulus that is not more than 40 GPa higher than the elastic modulus of the glass.