Flame-retardant damping compositions, their coatings and applications
By combining vinyl copolymers, acrylic polymers, and other components to form a flame-retardant system, the problem of water-based LASD coatings being unable to simultaneously meet strict fire protection standards and provide sound insulation and waterproofing is solved, achieving excellent flame-retardant and sound insulation effects at high temperatures.
Patent Information
- Application Number
- CN202480090012.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing water-based LASD coatings cannot simultaneously meet the stringent structural fire resistance standard NFPA130 and the European railway fire safety testing standard EN 45545, and lack sound insulation and waterproofing properties, limiting their applicability in outdoor applications.
By employing a composition based on vinyl copolymers, acrylic polymers, expandable graphite, ammonium polyphosphate, melamine, pentaerythritol, and high-purity TiO2, a flame-retardant system is formed through careful selection and combination, achieving excellent flame retardancy, sound insulation, and water resistance.
It provides excellent flame retardancy at high temperatures, meets NFPA130 and EN 45545 standards, and also has good sound insulation and water resistance, making it suitable for outdoor systems.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to flame-retardant damping compositions, their coatings, and uses for motor vehicle applications, and particularly to water-based flame-retardant damping compositions and damping coatings that exhibit excellent flame retardancy, sound insulation and noise reduction, as well as water resistance and solvent resistance. Background Technology
[0002] Sound damping materials play a crucial role in reducing vibration-induced noise in various industrial equipment and vehicles. While traditional methods (e.g., manual bitumen pads) have been used for sound insulation patches, technological advancements have led to the development of sprayable polymer-based sound damping compositions (often referred to as liquid-applied acoustic damping (LASD) materials). These materials are designed to improve the installation and replacement process while providing superior performance.
[0003] Compared to traditional methods, LASD materials offer several advantages. They exhibit higher damping efficiency, reduced odor, and easier application via robotic-controlled coating guns. This method is particularly beneficial for automated, lightweight, and environmentally friendly designs in industrial and automotive applications.
[0004] LASD compositions can be characterized by either water-based or non-water-based systems (e.g., two-component epoxy-based compositions). In particular, water-based systems exhibit several advantages over non-water-based coatings, including easier design implementation, a wider damping range, lower volatile organic compound (VOC) emissions, and cost-effectiveness. However, despite these advantages, current water-based LASD coatings cannot simultaneously meet the stringent structural fire resistance standard NFPA 130 (resistance to burning for at least 90 minutes) and the European railway fire safety testing standard EN 45545 (HL3 level). Furthermore, they typically lack good sound insulation and noise reduction properties and may have limited water resistance or solvent resistance, hindering their suitability for outdoor applications.
[0005] In view of the above, there is still a need for flame-retardant damping compositions that exhibit excellent flame retardancy, sound insulation and noise reduction, as well as good water resistance and salt resistance after curing. Summary of the Invention
[0006] According to a first aspect of the present invention, a flame-retardant damping composition is disclosed herein, the flame-retardant damping composition comprising: (A) Vinyl-based copolymers, (B) Acrylic polymers, (C) Expandable graphite, (D) Ammonium polyphosphate, (E) Melamine, (F) Pentaerythritol, and (G) Titanium dioxide with a TiO2 content greater than 95%; The weight ratio of component (A) to component (B) is 0.9:1 to 5:1, and the total weight of components (D), (E) and (F) is greater than 25.0% by weight, based on the total weight of the damping composition.
[0007] According to a second aspect of the invention, a damping coating is provided herein, the damping coating comprising a cured product of a flame-retardant damping composition according to the invention.
[0008] According to a third aspect of the invention, a panel is provided herein, the panel comprising a substrate and a damping coating disposed on the substrate, wherein the damping coating is a cured product of a flame-retardant damping composition according to the invention.
[0009] According to a fourth aspect of the invention, this document provides the use of the flame-retardant damping composition or the damping coating according to the invention in the manufacture of motor vehicles or building components.
[0010] The invention is characterized by its excellent flame retardancy, simultaneously meeting the stringent structural flame retardancy standard NFPA130 (resistance to burning for at least 90 minutes) and the European railway fire safety testing standard EN 45545 (HL3 level). The invention also achieves satisfactory water and solvent resistance, making the product suitable for use in outdoor systems (e.g., flame-retardant coatings on the underside of high-speed trains). Through careful selection of polymers and the establishment of a flame-retardant system, a damping coefficient loss factor greater than 0.09, preferably greater than 0.14, can be achieved at 20°C, while simultaneously providing good sound insulation and noise reduction at room temperature.
[0011] The following sections elaborate on other features and aspects of this topic. Detailed Implementation
[0012] Those skilled in the art will understand that this invention is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the invention. Unless explicitly stated otherwise, each aspect thus described may be combined with any other one or more aspects. In particular, any feature indicated as preferred or advantageous may be combined with any other one or more features indicated as preferred or advantageous.
[0013] In the context of this invention, unless otherwise specified, the terminology used will be interpreted according to the following definitions.
[0014] Unless otherwise specified, the terms “a / an” and “the” as used herein include both the singular and plural references.
[0015] As used herein, the term “comprising / comprises” is synonymous with “including / includes” or “containing / contains”, and is inclusive or open-ended, and does not exclude additional undescribed members, elements, or method steps.
[0016] The terms “at least one” or “one or more” used in this document to define components refer to the type of component, not the absolute number of molecules. For example, “one or more polyols” means a type of polyol or a mixture of several different polyols.
[0017] As used in this article, "flame retardant" refers to the use of non-combustible materials to protect the substrate from combustion.
[0018] The term "polymer" as used in this article is consistent with its common usage in chemistry. A polymer is composed of many repeating subunits. The term "polymer" is used to describe the material obtained from a polymerization reaction.
[0019] The term “vinyl-based copolymer” used in this article is consistent with its common usage in chemistry, which includes vinyl monomers in its structure.
[0020] The term "solid content" used in this article is determined according to ISO 3251.
[0021] The term "acrylic acid" refers to either or both of "acrylic acid" and "methacrylic acid".
[0022] The term "acrylate" refers to either or both of "acrylate" and "methacrylate".
[0023] As used herein, the term "room temperature" refers to a temperature of about 20°C to about 25°C, preferably about 25°C.
[0024] The term "emulsion" refers to a fine dispersion of tiny droplets (EVA copolymers) dispersed in water by a surfactant (e.g., soap), and is used to distinguish it from solutions or blends.
[0025] The term "D50 particle size" refers to the median diameter in a volume-based particle size distribution curve obtained by measuring with a laser diffraction particle size analyzer.
[0026] As used herein, the term "curing" refers to the hardening process of a material. This term is intended to encompass drying the material by evaporating water and a co-solvent from it, as well as crosslinking (where applicable) of components within the material that have reactive groups.
[0027] Unless otherwise specified, the definition of numerical endpoints includes all numbers and fractions falling into their respective ranges, as well as the listed endpoints.
[0028] All references cited in this specification are hereby incorporated in their entirety by reference.
[0029] In this context, the glass transition temperature (Tg) or melting point of a specific polymer is determined using DSC according to DIN 53 765.
[0030] Unless otherwise defined, all terms used in this invention (including technical and scientific terms) have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains.
[0031] In one aspect, this disclosure generally relates to flame-retardant damping compositions comprising: (A) Vinyl-based copolymers, (B) Acrylic polymers, (C) Expandable graphite, (D) Ammonium polyphosphate, (E) Melamine, (F) Pentaerythritol, and (G) Titanium dioxide with a TiO2 content greater than 95%; The weight ratio of component (A) to component (B) is 0.9:1 to 5:1, and the total weight of components (D), (E) and (F) is greater than 25.0% by weight, based on the total weight of the damping composition.
[0032] (A) Vinyl-based copolymers According to the present invention, the flame-retardant damping composition comprises a vinyl-based copolymer to provide adhesion to a substrate when exposed to high temperatures (>200°C).
[0033] The vinyl-based copolymers suitable for use in this invention can be aqueous dispersions (emulsions) of vinyl-based copolymers that can adequately bind the flame retardant, thereby allowing it to adhere to the substrate. The aqueous dispersions of vinyl-based copolymers preferably have a resin solids content of 40 to 70% by weight.
[0034] Generally, any type of vinyl-based copolymer can be used in this invention, such as ethylene-vinyl acetate copolymers, vinyl acetate-vinyl versatate copolymers, and vinyl chloride-vinyl acetate copolymers. However, particular advantages have been observed when using aqueous dispersions of ethylene-vinyl acetate copolymers or vinyl acetate-vinyl versatate copolymers. Unlike acrylic resins or other polymers that decompose and disperse like powder when exposed to high temperatures (>200°C), vinyl-based copolymer dispersions provide strong adhesion under such conditions, making them highly suitable for this invention.
[0035] The ethylene-vinyl acetate copolymers suitable for use in this invention comprise, for example, 10 to 95% by weight of vinyl acetate and the remainder being a copolymer of ethylene. Suitable aqueous dispersions of ethylene-vinyl acetate copolymers preferably have a solids content of 40 to 70% by weight, a viscosity of 50 to 9000 cp, and a pH of 2 to 7.
[0036] The vinyl acetate-vinyl tert-carbonate copolymer suitable for use in this invention comprises, for example, the following copolymers: 5 to 30 wt% ethylene; 15 to 70 wt%, or preferably 30 to 70 wt% vinyl acetate; and 25 to 75 wt%, or preferably 25 to 65 wt% vinyl tert-carbonate. Because the vinyl acetate-vinyl tert-carbonate copolymer has -OCO-CH3 groups and also contains a large amount of oxygen, its flame-retardant effect is generally significant when used in combination with ammonium polyphosphate. A suitable aqueous dispersion of the vinyl acetate-vinyl tert-carbonate copolymer preferably has a solids content of 40 to 70 wt%, a viscosity of 1000 to 7000 cp, and a pH of 2 to 7.
[0037] Typically, the vinyl-based copolymers used in this invention have a glass transition temperature (Tg) ranging from about -40°C to about 40°C. In one embodiment of the invention, a combination of vinyl-based polymers is used, wherein the two vinyl-based polymers have different Tgs (both above 0°C).
[0038] Commercially available vinyl-based copolymers (in emulsion form) suitable for use in this invention may be obtained from Synthomer as EMULTEX™ FR 797 and EMULTEX™ FR 728; from Wacker as EAF 68 and EP 724; and from Celanese as Vinamul 8482 and Celvolit 1496.
[0039] Particularly preferably, the amount of vinyl-based copolymer (A) may be from 6.0% to 30.0% by weight, preferably from 7.0% to 26.0% by weight, based on the total weight of the damping composition. It is worth noting that, when using a polymer dispersion, the weight ratios herein refer to the weight of the polymer excluding the water content.
[0040] (B) Acrylic polymers According to the present invention, the flame-retardant damping composition includes an acrylic polymer as a second essential component to provide the damping composition with good sound insulation, water resistance and solvent resistance properties.
[0041] The acrylic polymers applicable to this invention are in dispersed (emulsified) form and can be selected from any acrylic polymer material conventionally used in aqueous compositions capable of forming a damping coating on a substrate surface.
[0042] Preferred acrylic polymers include dispersions of acrylate polymers and copolymers (sometimes referred to in the art as acrylic resins), for example, copolymers of lower alkyl esters of (meth)acrylate (e.g., n-butyl acrylate) with comonomers (e.g., styrene and / or acrylonitrile) are also preferred. Mixtures of the above polymers can be used, and are preferred to obtain a desired combination of properties in the final cured coating. For example, different polymers with different glass transition temperature characteristics can be used in combination.
[0043] Typically, the acrylic polymers used in this invention have a glass transition temperature ranging from about -10°C to about 40°C, preferably from 0°C to 20°C. In one embodiment of the invention, the acrylic polymer used has a Tg above 0°C (e.g., 3°C).
[0044] Commercially available acrylic polymers (in emulsion form) suitable for this invention may be obtained from Wanhua: Antamp™ 0658, Tekspro5117, Antamp™ 0656, and Antamp™ 0655; from BASF: Acronal 3612 and Acronal 4569; from DOW: AV-1220, SD-65, and AV-2240; from Trinseo: 3612; and from Synthomer: B500 and 31Y40.
[0045] According to the present invention, the aqueous dispersion of the acrylic polymer is typically obtained with a solids content of more than 45% by weight, preferably more than 50% by weight.
[0046] Particularly preferably, the amount of acrylic polymer (B) is greater than 2.5% by weight and less than 10.0% by weight, preferably 3.0% by weight and 8.0% by weight, based on the total weight of the damping composition. It is worth noting that, when using a polymer dispersion, the weight ratios mentioned herein refer to the weight of the polymer excluding the water content.
[0047] According to the present invention, the weight ratio of component (A) to component (B) is critical, ranging from 0.9:1 to 5:1, preferably from 1:1 to 4:1, and more preferably from 1:1 to 3:1. This range is essential for achieving a balance of performance in terms of flame retardancy, water resistance, and sound insulation. As mentioned above, component (A) contributes to adhesion at high temperatures, while component (B) imparts excellent sound insulation, water resistance, and solvent resistance to the damping composition. If the weight ratio of component (A) to component (B) is less than 0.9:1 (indicating insufficient vinyl-based copolymer according to the present invention), the damping composition may not meet the flame retardancy criteria specified in the context. Conversely, if the weight ratio of component (A) to component (B) exceeds 5:1 (indicating insufficient acrylic polymer content according to the present invention), the sound insulation and water resistance of the damping composition will be unsatisfactory.
[0048] (C) Expandable graphite According to the present invention, the flame-retardant damping composition comprises expandable graphite as a first flame retardant, which exhibits rapid expansion upon exposure to temperatures ranging from 160 to 200°C, thereby forming an initial expanded carbon layer. This expanded layer effectively prevents the spread of combustion.
[0049] Typically, expandable graphite (also known as exfoliated graphite) can be produced from naturally occurring mineral graphite. The layered structure of graphite allows molecules to insert between the graphite layers. If expandable graphite is heated, the graphite sheet will expand to several times its initial volume.
[0050] Various expandable graphite materials with different densities, shapes, particle sizes, and expansion rates can be used in this invention. The density of expandable graphite can range from 1.5 to 2.1 g / cm³. 3 Within the range (by weight). The expandable graphite suitable for use in this invention is typically in flake form, such as 50-mesh flakes, typically about 0.5 mm in length and width, with the largest particles typically about 0.9 mm and a typical thickness of about 0.08 mm; or 80-mesh flakes, typically about 0.4 mm in length and width, with a typical thickness of about 0.07 mm. The expansion rate of the preferred expandable graphite used in this invention can be greater than 50 ml / g, more preferably from 90 ml / g to 400 ml / g. Expansion rate refers to the increase in volume of graphite when exposed to heat or high temperatures.
[0051] The commercially available expandable graphite suitable for use in this invention can be obtained from Hebei ADT Trading CO., LTD, namely ADT 95, ADT 1002, ADT 802, ADT 249, ADT 251 and ADT 351.
[0052] Particularly preferably, the amount of expandable graphite (C) present can be from 1.0 wt% to 35.0 wt%, preferably from 5.0 wt% to 30.0 wt%, based on the total weight of the damping composition.
[0053] (D) Ammonium polyphosphate According to the present invention, the flame-retardant damping composition comprises ammonium polyphosphate (D).
[0054] Ammonium polyphosphates suitable for use in this invention include, for example, ammonium polyphosphate and amide polyphosphate. However, any compound with equivalent properties may be used if desired. By using microencapsulated ammonium polyphosphate compounds, the viscosity increase of the aqueous dispersion can generally be reduced when the ammonium polyphosphate compound is incorporated into the aqueous dispersion resin. The ammonium polyphosphate compound can be made relatively insoluble in water and can be stabilized by microencapsulation. The ammonium polyphosphate preferably has a phosphorus content of 15 to 35%. Due to the insufficient water resistance of ammonium polyphosphate, it is preferable to use ammonium polyphosphate with a degree of polymerization greater than 1000.
[0055] Commercially available ammonium polyphosphate suitable for this invention can be obtained from Hangzhou JLS FlameRetardants Chemical Co., LTD. (JLS-104 MF).
[0056] Particularly preferably, based on the total weight of the damping composition, the amount of ammonium polyphosphate (D) may be greater than 10.0% by weight to 40.0% by weight, preferably 15.0% by weight to 35.0% by weight.
[0057] (E) Melamine According to the present invention, the flame-retardant damping composition comprises melamine (E).
[0058] Melamine can have the following chemical structure. Because it contains 66% nitrogen by mass, melamine is flame-retardant by releasing nitrogen gas when burned or charred.
[0059] Commercially available melamine suitable for use in this invention is obtained from BASF.
[0060] Particularly preferably, based on the total weight of the damping composition, the amount of melamine (E) present is greater than 5.0% to 15.0% by weight, preferably 5.0% to 12.0% by weight.
[0061] (F) Pentaerythritol According to the present invention, the flame-retardant damping composition comprises pentaerythritol (F).
[0062] Pentaerythritol (F) can be represented by the formula C(CH2OH)4.
[0063] The commercially available melamine suitable for this invention can be obtained from Hangzhou JLS FlameRetardants Chemical Co., LTD. (JLS-PENTA).
[0064] Particularly preferably, the amount of pentaerythritol (F) present is greater than 5.0% to 10.0% by weight, preferably 5.0% to 9.0% by weight, based on the total weight of the damping composition.
[0065] Components (D), (E), and (F) described herein together form a flame-retardant system. When exposed to temperatures ranging from 200 to 230°C, ammonium polyphosphate (D) decomposes during combustion, producing nitrogen gas that suppresses oxygen and phosphoric acid. A reaction occurs by blending melamine (E) and pentaerythritol (F) described herein, wherein pentaerythritol undergoes intramolecular dehydration and esterification under acid catalysis, resulting in the formation of a second carbon layer. Melamine decomposes, releasing volatile substances that cause the second carbon layer to expand, thereby enhancing flame retardancy.
[0066] When the amount of the mixture of components (D), (E), and (F) based on the total weight of the damping composition is greater than 25% to 60%, the damping composition preferably exhibits flame retardancy and salt resistance. Furthermore, the weight ratio of components (D), (E), and (F) is preferably in the range of 1:1:1 to 3:1:1.
[0067] (G) Titanium dioxide According to the present invention, the flame-retardant damping composition comprises titanium dioxide with a TiO2 content greater than 95%, which acts as a third flame retardant.
[0068] When the temperature exceeds 300℃, the second expanded carbon layer formed will continue to form a more heat-resistant titanium pyrophosphate carbon layer with high-purity titanium dioxide, thereby further improving the flame retardant effect.
[0069] The component (G) suitable for use in this invention can have a concentration of 2 to 15 g / cm³. 3The density is determined by DIN ENISO 787-10. Titanium dioxide may or may not have surface treatment. Preferred titanium dioxide (G) has a sieve residue of not more than 40.0% (greater than 40 µm) after dispersion in water, and a sieve residue of not more than 0.5% (greater than 200 µm) after dispersion in water.
[0070] Compared to conventional metal hydroxides (e.g., aluminum hydroxide, magnesium hydroxide) or ordinary titanium dioxide with a TiO2 content of about 95% or less, the flame-retardant damping composition with component (G) exhibits better flame-retardant properties. The TiO2 content in the titanium dioxide used in this article was determined according to DIN EN ISO 591.
[0071] Suitable titanium dioxide with a TiO2 content greater than 95% can be produced by the sulfate process, or it can be commercially obtained from Omya using KRONOS3025.
[0072] Particularly preferably, the amount of component (G) present can be from 1 wt% to 20.0 wt%, preferably from 1 wt% to 10 wt%, based on the total weight of the damping composition.
[0073] Optional components The compositions according to the invention may also contain additives known to those skilled in the art and typically present in polymer compositions, provided that they do not substantially impair the invention, particularly defoamers, pigments, thickeners, drying control agents, surfactants (e.g., sodium hexametaphosphate, sodium tripolyphosphate), polymer surfactants, foaming agents, nucleating agents, softeners, heat stabilizers, etc. Other substances that promote flame retardancy may also be optionally added, such as char-forming substances (e.g., polyphenylene ethers and polycarbonates), and substances that regulate dripping behavior (e.g., fluoropolymers, such as polytetrafluoroethylene). In particular, the damping composition contains a defoamer. Commercially available defoamers are available from BASF at Foamaster MO NXZ.
[0074] Based on the total composition, the total amount of optional additives in the composition is preferably up to 10.0% by weight, more preferably from 0.1% to 10% by weight or from 0.1% to 7.5% by weight. The desired viscosity of the composition will generally determine the total amount of optional additives added.
[0075] Damping Composition In a particularly preferred embodiment, based on the total weight of the flame-retardant damping composition, the flame-retardant damping composition according to any one of the preceding claims comprises: 6.0% to 30.0% by weight of vinyl-based copolymers, Acrylic copolymers comprising more than 2.5% by weight and less than 10.0% by weight. Expandable graphite ranging from 1.0 wt% to 35.0 wt%. A mixture comprising more than 25.0% to 60.0% by weight of ammonium polyphosphate, melamine, and pentaerythritol. Titanium dioxide with a TiO2 content greater than 95% and a content ranging from 0.1% to 20.0% by weight.
[0076] It is not intended to particularly limit the amount of water contained in the aqueous composition, but it is preferred that the composition contains 5.0 to 30.0% by weight of water as the liquid phase.
[0077] Preparation method of damping composition The flame-retardant damping composition is formulated by simply mixing the components.
[0078] The equipment used for these mixing, stirring, and dispersing processes is not particularly limited. Automatic mortars, Henschel mixers, three-roll mills, ball mills, planetary mixers, bead mills, etc., equipped with stirrers and heaters can be used. Furthermore, appropriate combinations of these devices can be used. The preparation method of the flame-retardant damping composition is not particularly limited, as long as a composition in which the above components are uniformly mixed is obtained.
[0079] According to the broadest aspect of the invention, the above composition is applied to a substrate and then cured in situ.
[0080] According to a second aspect of the invention, a damping coating is provided herein, the damping coating comprising a cured product of a flame-retardant damping composition according to the invention.
[0081] According to a third aspect of the invention, a panel is provided herein, the panel comprising a substrate and a damping coating disposed on the substrate, wherein the damping coating is a cured product of a flame-retardant damping composition according to the invention.
[0082] The invention is not intended to limit the substrates to which the compositions can be applied. In applications to vehicle panels, exemplary substrates may be metallic, polymeric, or combinations thereof. However, specific references may be made to: ferrous metals, such as iron, steel, and their alloys; non-ferrous metals, such as aluminum, zinc, and their alloys; and combinations thereof. In illustrative embodiments, the substrate may be formed of: cold-rolled steel; electro-galvanized steel, such as hot-dip galvanized steel or electro-galvanized iron-zinc steel; or aluminum.
[0083] The composition can be applied to the substrate by any convenient means known in the art, such as by coating (by brushing or spraying).
[0084] Pretreatment of the relevant surfaces to remove foreign matter is generally recommended before applying the composition; if applicable, this step can promote the subsequent adhesion of the composition to them. Such treatments are known in the art and can be performed in a single-stage or multi-stage manner, for example, by immersion in an aqueous alkaline degreasing bath; treatment with an aqueous cleaning emulsion; treatment with a cleaning solvent (e.g., carbon tetrachloride or trichloroethylene); and rinsing with water, preferably with deionized or demineralized water. In those instances where an aqueous alkaline degreasing bath is used, any degreasing agent remaining on the surface should be expected to be removed by rinsing the substrate surface with deionized or demineralized water.
[0085] The composition is then applied to a preferably pretreated, optionally primer-coated surface of a substrate by conventional application methods such as brushing; roller coating; doctor blade application; printing; and spraying, including but not limited to air atomization spraying, air-assisted spraying, airless spraying, and high-volume low-pressure spraying.
[0086] The thickness of the coating applied in this invention can be adjusted to ensure that the final cured coating effectively provides flame retardancy and noise suppression to the desired degree. In many cases, the composition is applied as a wet film thickness of 1 to 5 mm. Applying thinner layers within this range is more economical and offers the potential for a reduction in harmful thick cured areas. However, strict control must be exercised when applying thinner coatings or layers to avoid the formation of discontinuous cured films.
[0087] The curing of the compositions of the present invention is typically carried out at room temperature for 24 to 48 hours, or in the range of 20°C to 60°C. The appropriate temperature depends on the specific compound present and the desired curing rate, and can be determined by those skilled in the art in each case using simple preliminary tests (if necessary).
[0088] According to a fourth aspect of the invention, this document provides the use of the flame-retardant damping composition or the damping coating according to the invention in the manufacture of motor vehicles or building components.
[0089] The suitable motor vehicles include, but are not limited to: automobiles, trucks, buses, motorcycles, delivery vehicles, bicycles, and special-purpose vehicles such as electric scooters, golf carts, and engineering vehicles such as high-speed trains, underground trains, shuttle buses, subways, public transportation, recreational activities, and other industrial operations or public transport.
[0090] The building components include, but are not limited to: walls, roofs, floors; and structural frames in building complexes, apartments, museums, stadiums, infrastructure, and other building groups.
[0091] Example The following examples are intended to help those skilled in the art better understand and practice the present invention. The scope of the invention is not limited by the examples, but is defined by the appended claims. Unless otherwise stated, all parts and percentages are based on weight.
[0092] raw material: EMULTEX™ FR 797 is a vinyl acetate-vinyl tert-carbonate copolymer dispersion with a solids content of 55%, a viscosity of 1100 mPa·s at 23°C, and a Tg of 13°C. It is available from a Synthomer.
[0093] EMULTEX™ FR 728 is a vinyl acetate-vinyl tert-carbonate copolymer dispersion with a solids content of 50%, a viscosity of 2250 mPa·s at 23°C, and a Tg of 23°C. It is available from a Synthomer.
[0094] Antamp™ 0658 is an aqueous acrylic copolymer emulsion with a solids content of 50% as determined by WHPU / T 011-571-2017 and a Tg of 3°C. It is available from Wanhua.
[0095] JLS-104 MF is ammonium polyphosphate, available from Hangzhou JLS Flame Retardants Chemical Co., LTD.
[0096] Melamine can be obtained from BASF.
[0097] JLS-PENTA is pentaerythritol, which is available from Hangzhou JLS Flame Retardants Chemical Co., Ltd.
[0098] ADT 351 is expanded graphite with an expansion rate greater than 350 ml / g, available from Hebei ADT Trading CO.,LTD.
[0099] KRONOS 3025 is a high-purity titanium dioxide with a TiO2 content >99% as determined by DIN EN ISO 591, and is available from Omya.
[0100] Ti-Pure™ R-902+ is titanium dioxide with a TiO2 content of 93% as determined by DIN EN ISO 591, and is available from DuPont.
[0101] Aluminum hydroxide powder is available from Chinalco.
[0102] Foamaster MO NXZ is an antifoaming agent available from BASF.
[0103] Preparation method Preparation of damping compositions of Examples 1-3 and Comparative Examples 1-9 (Ex. 1 to Ex. 3 and CE1 to CE9) The compositions of Examples 1-3 and Comparative Examples 1-9 comprise the following raw materials in the indicated amounts. The compositions were obtained by first adding the liquid material to a container and mixing it at a temperature below 30°C. Then, powdered filler material was added, and mixing continued until a well-mixed, homogeneous paste was obtained. Rheology modifiers and water were then added during mixing to adjust the desired viscosity. Vacuum was preferably used during mixing to reduce trapped air bubbles.
[0104] <Cure of the Damping Composition> The composition is applied to the substrate by manual brushing. The thickness is controlled from about 1 mm to about 4 mm. After application to the substrate, the composition is typically dried at room temperature for 24 hours to no more than 48 hours.
[0105] Test methods Damping Coefficient Test Damping tests were performed on the damping coatings prepared in the examples and comparative examples using a TWS Michael Schulthes obster testing system. The specific damping test method was performed according to GB / T 18258-2000. The stainless steel plate dimensions were 220 mm × 3 mm × 1 mm. The damping coating dimensions were 220 mm × 3 mm × 2.0 mm, and it was cured in an oven at 50°C for 6 hours. Before testing, the samples were placed at room temperature for at least 48 hours. Damping coefficient tests were performed at a temperature range of -40°C to 60°C, and measurements were taken every 2.5°C when the temperature stabilized. The composite loss factor was recorded at a frequency of 200 Hz and measured using 3 kg / cm². 3 The surface density is normalized. Table 1 shows the measurement results of the damping coefficient.
[0106] A loss factor greater than 0.09 at 20°C can be considered an acceptable damping coefficient. A preferred loss factor is equal to or greater than 0.14.
[0107] <Structural Flame Resistance Test> Structural flame retardancy tests were performed on the damping coatings prepared in all examples and comparative examples according to standard NFPA 130. The substrate, Q235 steel, was prepared by rust removal and application of prescribed rust-preventive measures. A 2 mm coating was applied to the surface of a 300*300*2 mm substrate and dried at room temperature for 48 hours to form a test plate. Vertical burning tests were conducted using a flame impact tester (PJKJ-SS-1500). The nozzle was positioned 50 mm from the coating on the test plate to generate an external flame temperature of 1000±50°C. A timer starting at 000000 was placed at the top, while nine thermocouples were positioned on the back plate of the substrate (the uncoated side) to measure the temperature rise.
[0108] Each test panel was subjected to combustion. The combustion time that each sample could withstand is recorded in Table 1. If a hole was burned into the test panel during the combustion process, the duration of combustion was recorded by a timer. Test panels that remained structurally intact after 90 minutes of combustion were considered to have excellent flame retardancy due to the damping coating. Longer combustion times indicate better flame retardancy.
[0109] <European Railway Fire Safety Testing Standards EN45545 R1 R2 R17> The European railway fire safety testing standard EN45545 R1 R2 R17 includes the following three separate test items:
[0110] All tests were conducted by DEATAK.
[0111] The cone calorimeter test was conducted according to the following procedure: • Before testing, condition the sample at 23±2℃ / 50±5% humidity for at least 24 hours to achieve constant weight. Maintain these conditions until the test begins.
[0112] • Turn on the instrument and preheat it for 40-60 minutes.
[0113] • Prepare the sample and start the gas required for the test (CH4, N2, CO / CO2).
[0114] • Open the testing software, click “RUN A TEST” to enter the relevant information, heat the sample to the specified temperature (833℃), and start the test.
[0115] • The test is complete, and the raw data of MAEHE is recorded.
[0116] The smoke density test was conducted according to the following procedure: • Before testing, condition the sample at 23±2℃ / 50±5% humidity for at least 24 hours to achieve constant weight, and maintain these conditions until testing.
[0117] • Turn on the instrument switches, software, and gas valves.
[0118] • Click the Optic lamp, Chamber Heater, and Optic Heater buttons on the panel to preheat the instrument for a period of time.
[0119] • Turn on the heater furnace button and heat to the corresponding temperature of 700°C (50 kW / m²). 2 ).
[0120] • Click “Enter Test Data” in the software, enter the test information, and start the test.
[0121] • The test is complete, and the raw data for Ds4 and VOF4 are recorded.
[0122] The lateral flame spread test is conducted according to the following procedure: • Before testing, condition the sample at 23±2℃ / 50±5% humidity for at least 24 hours to achieve constant weight, and maintain these conditions until ready for testing.
[0123] • Turn on the instrument switches, software, and gas valves.
[0124] • Click the Optic lamp, Chamber Heater, and Optic Heater buttons on the panel to preheat the instrument for a period of time.
[0125] • Turn on the heater furnace button and heat the instrument to the corresponding temperature of 700°C (50 kW / m²). 2 ).
[0126] • Click “Enter Test Data” in the software to input test information and start the test.
[0127] • The test is complete, and the CFE (kW / m²) at the maximum combustion distance of 350 mm is recorded. 2 ) Original data.
[0128] A damping composition is classified as reaching the highest level, denoted as HL3, and marked "Pass" only if it meets all of the following criteria; otherwise, it will be marked "Fail":
[0129] Waterproofing Test The standard tinplate substrates used to test the damping coatings (with a coating thickness of 4 mm) prepared in the examples and comparative examples were completely immersed in water at room temperature for 24 hours at 23±2°C.
[0130] The waterproofing test results are recorded in Table 1 and graded according to the following criteria: - Failed: Cracks, blistering, peeling, or softening occurred. - Passed: No cracking, no blistering, no peeling, no softening <Soluble Resistance Test> Water resistance was measured according to ISO 2812-1974. A standard steel substrate measuring 70*120*0.2 mm, used for testing the damping coating (with a coating thickness of 4 mm) prepared in the examples and comparative examples, was completely immersed in 3% NaCl at room temperature for 24 hours at 23±2°C.
[0131] The solvent resistance test results are recorded in Table 1 and graded according to the following criteria: - Failed: Cracks, blistering, peeling, or softening occurred. - Passed: No cracking, no blistering, no peeling, no softening Table 1
[0132] As shown in Table 1, the comparison between CE1 to CE3 and Ex. 1 indicates that the absence of component (G), or its replacement with other inorganic fillers, or titanium dioxide with a TiO2 content lower than the required protection range, results in the damping composition failing to meet the structural flame retardancy standard NFPA 130 (resistance to burning for at least 90 minutes). Similarly, the absence of expandable graphite (C) also fails to achieve the desired flame retardancy (CE5). And the absence of acrylic polymers (B) fails to achieve the desired sound insulation, water resistance, and solvent resistance (CE4).
[0133] Furthermore, when the weight ratio of component (A) to (B) deviates from the specified range (e.g., in CE6 (0.575:1), CE7 (0.875:1) and CE8 (5.36:1)), the damping composition cannot withstand combustion for at least 90 minutes (structural flame retardancy standard NFPA130).
[0134] Furthermore, when the total weight of components (D), (E) and (F) exceeds the range specified according to the present invention, the resulting damping coating lacks satisfactory sound insulation and solvent resistance (CE9).
[0135] Conversely, the damping compositions of Ex.1 to Ex.3 exhibit the desired performance characteristics in terms of flame retardancy, sound insulation, water resistance, and solvent resistance.
[0136] Although some preferred embodiments have been described, many modifications and variations can be made to them in accordance with the foregoing teachings. Therefore, it should be understood that the invention can be practiced in ways different from those specifically described without departing from the scope of the appended claims.
Claims
1. A flame-retardant damping composition, wherein the flame-retardant damping composition comprises: (A) Vinyl-based copolymers, (B) Acrylic polymers, (C) Expandable graphite, (D) Ammonium polyphosphate, (E) Melamine, (F) Pentaerythritol, and (G) Titanium dioxide with a TiO2 content greater than 95%; The weight ratio of component (A) to component (B) is 0.9:1 to 5:1, and the total weight of components (D), (E) and (F) is greater than 25.0% by weight, based on the total weight of the damping composition.
2. The flame-retardant damping composition according to claim 1, wherein the vinyl-based copolymer (A) is an aqueous dispersion of the vinyl-based copolymer, and the resin solids content of the aqueous dispersion is from 40% to 70% by weight.
3. The flame-retardant damping composition according to claim 1 or 2, wherein the vinyl-based copolymer (A) is an aqueous dispersion of ethylene-vinyl acetate copolymer and / or an aqueous dispersion of vinyl acetate-vinyl tert-carbonate copolymer.
4. The flame-retardant damping composition according to any one of the preceding claims, wherein the acrylic polymer (B) is an aqueous dispersion of the acrylic polymer, and the resin solids content of the aqueous dispersion is greater than 45% by weight, preferably greater than 50% by weight.
5. The flame-retardant damping composition according to any one of the preceding claims, wherein the weight ratio of component (A) to component (B) is 1:1 to 4:1, preferably 1:1 to 3:
1.
6. The flame-retardant damping composition according to any one of the preceding claims, wherein, Based on the total weight of the damping composition, the total weight of components (D), (E) and (F) is greater than 25.0% to 60.0%.
7. The flame-retardant damping composition according to any one of the preceding claims, wherein the weight ratio of components (D), (E) and (F) ranges from 1:1:1 to 3:1:
1.
8. The flame-retardant damping composition according to any one of the preceding claims, wherein, based on the total weight of the flame-retardant damping composition, the flame-retardant damping composition comprises: 6.0% to 30.0% by weight of vinyl-based copolymers, Acrylic copolymers comprising more than 2.5% by weight and less than 10.0% by weight. Expandable graphite ranging from 1.0 wt% to 35.0 wt%. A mixture comprising more than 25.0% to 60.0% by weight of ammonium polyphosphate, melamine, and pentaerythritol. Titanium dioxide with a TiO2 content greater than 95% and a content ranging from 1% to 20.0% by weight.
9. The flame-retardant damping composition according to any one of the preceding claims, wherein the flame-retardant damping composition comprises 5.0 to 30.0% by weight of water as a liquid phase.
10. The flame-retardant damping composition according to any one of the preceding claims, wherein the flame-retardant damping composition further comprises an optional component selected from defoamers, pigments, thickeners, drying control agents, surfactants, polymeric surfactants, foaming agents, nucleating agents, softeners, and heat stabilizers.
11. A damping coating comprising a cured product of the flame-retardant damping composition according to claims 1-10.
12. A panel comprising a substrate and a damping coating disposed on the substrate, wherein the damping coating is a cured product of the flame-retardant damping composition according to claims 1-10.
13. Use of the flame-retardant damping composition according to any one of claims 1-10 or the damping coating according to claim 11 in the manufacture of motor vehicles or building components.