Pyrolysis oils, elastomers, rubber products and resin products
By controlling the specific properties of pyrolysis oil, light olefin-rich pyrolysis oil is prepared, solving the problem that pyrolysis oil is difficult to use as a raw material for chemical products in existing technologies. This enables the reuse of elastomers, rubber products, and resin products, and promotes the recycling of resources such as waste tires.
Patent Information
- Application Number
- CN202580029621.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-23
- Filing Date
- 2025-04-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have failed to effectively study and utilize the components contained in pyrolysis oil, making it difficult to use as a raw material for chemical products and limiting the possibility of reuse.
Pyrolysis oil is prepared by pyrolyzing used tire waste. The distillation temperature is controlled below 400℃ for 90% of the product, the olefin content is above 10% by volume, the density is 0.82g/cm3 to 0.91g/cm3, the density after standing is 0.84g/cm3 to 0.97g/cm3, the iodine value is above 180g I2/100g, the acid value is below 5mg KOH/g, and the aromatic content is below 80% by volume. This oil is used to produce elastomers, rubber products, and resin products.
It provides pyrolysis oil that is easy to use as a raw material for chemical products, promotes the reuse of elastomers, rubber products and resin products, and improves the resource recycling efficiency of waste tires.
Smart Images

Figure CN123125302A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to pyrolysis oils, elastomers, rubber products, and resin products. Background Technology
[0002] In recent years, from the perspective of protecting the global environment, the recycling of used rubber products, including used tires, has been promoted. As a method of such recycling, there are technologies in which waste rubber products are subjected to pyrolysis to recover pyrolysis products, such as oil (pyrolysis oil) and carbon black (carbides). For example, Patent Document 1 discloses a method for recovering a mixture of carbon and hydrocarbons from waste tires or similar polymer materials through pyrolysis treatment.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: JP 2002-523552 A Summary of the Invention
[0006] The problem the invention aims to solve
[0007] As described in Patent Document 1, various studies have been conducted on methods for pyrolyzing used tires, etc., but the components contained in the oil recovered by pyrolysis (pyrolysis oil) have not yet been studied.
[0008] On the other hand, in order to reuse pyrolysis oil recovered from used tires and the like as a raw material for chemical products, it is preferable that the recovered pyrolysis oil has specific properties.
[0009] Therefore, the purpose of this disclosure is to provide pyrolysis oils that are readily used as raw materials for chemical products.
[0010] Another object of this disclosure is to provide elastomer, rubber and resin products that use such pyrolysis oils.
[0011] Solution for solving the problem
[0012] The key features of the pyrolysis oil, elastomer, rubber product, and resin product of this disclosure that solve the above problems are as follows.
[0013] [1] A pyrolysis oil obtained by pyrolysis of waste containing used tires, wherein 90% of the pyrolysis oil is distilled at a temperature below 400°C and has an olefin content of 10% by volume or more as measured by GC×GC-MS.
[0014] [2] The pyrolysis oil according to [1] has an olefin content of 30% or more by volume as measured by GC×GC-MS.
[0015] [3] The pyrolysis oil according to [1] or [2], wherein 10% of the pyrolysis oil is distilled at a temperature of 100°C or higher.
[0016] [4] The pyrolysis oil according to any one of [1] to [3], wherein the density of the pyrolysis oil measured at 40°C within 3 hours after production is 0.82 g / cm³. 3 Up to 0.91 g / cm 3 .
[0017] [5] The pyrolysis oil according to any one of [1] to [4], wherein the density of the pyrolysis oil measured at 40°C after standing for 3 days following production is 0.84 g / cm³. 3 Up to 0.97 g / cm 3 .
[0018] [6] The pyrolysis oil according to any one of [1] to [5], wherein the iodine value of the pyrolysis oil is 180 g I2 / 100 g or more.
[0019] [7] The pyrolysis oil according to any one of [1] to [6], wherein the acid value of the pyrolysis oil is less than 5 mg KOH / g.
[0020] [8] An elastomer obtained using pyrolysis oil according to any one of [1] to [7] as a raw material, either in part or in whole.
[0021] [9] The elastomer according to [8], wherein the elastomer is at least one selected from the group consisting of resin and synthetic rubber.
[0022]
[10] A rubber product obtained by using an elastomer as part or all of the raw material according to [8] or [9].
[0023]
[11] The rubber product according to
[10] , wherein the rubber product is selected from at least one of the group consisting of rubber tires, rubber tracks, rubber hoses, conveyor belts and vibration-damping rubber.
[0024]
[12] A resin product obtained by using the elastomer described in [8] or [9] as part or all of the raw material.
[0025]
[13] The resin product according to
[12] , wherein the resin product is at least one selected from the group consisting of resin tires and resin hoses.
[0026] Beneficial effects
[0027] According to this disclosure, pyrolysis oil that is readily available as a raw material for chemical products can be provided.
[0028] Furthermore, according to this disclosure, such pyrolysis oils can be used to provide elastomers, rubber products, and resin products. Attached Figure Description
[0029] [ Figure 1 [A diagram illustrating the classification of compounds in the pyrolysis oil recovered in the examples and comparative examples.]
[0030] [ Figure 2 [Schematic diagram of the scaling evaluation test apparatus (HLPS) used in the reference embodiment and the reference comparative example.] Detailed Implementation
[0031] In the following text, the pyrolysis oils, elastomers, rubber products and resin products of this disclosure will be described and detailed based on their embodiments.
[0032] <Definition>
[0033] The compounds described in this specification may be derived in whole or in part from fossil resources, from biological resources such as plant resources, or from renewable resources such as used tires. Furthermore, they may be derived from any mixture of two or more of fossil resources, biological resources, and renewable resources.
[0034] <Pyrolysis Oil>
[0035] The pyrolysis oil of this embodiment is obtained by pyrolyzing waste materials including used tires. The pyrolysis oil of this embodiment is characterized by a 90% distillation temperature below 400°C and an olefin content of 10% by volume or more, as measured by GC×GC-MS.
[0036] Because the pyrolysis oil of this embodiment has a 90% distillation temperature below 400°C, it is lightweight and contains a large proportion of components with relatively small molecular weights. Components with relatively small molecular weights can be readily used as chemical products and can also be easily converted into other chemical products through additional processing or reaction. Furthermore, when components with relatively small molecular weights include butadiene and isoprene, these components can be used as raw materials for rubber (especially diene-based rubbers).
[0037] Furthermore, the pyrolysis oil of this embodiment has an olefin content of 10% by volume or more, as measured by GC×GC-MS, and contains many compounds with non-aromatic carbon-carbon double bonds. Compounds with non-aromatic carbon-carbon double bonds can be readily used as chemical products and can also be easily converted into other chemical products through additional processing or reaction. Moreover, when the compounds with non-aromatic carbon-carbon double bonds include butadiene and isoprene, these components can be used as raw materials for rubber (especially diene-based rubbers).
[0038] Therefore, the pyrolysis oil of this embodiment is light and contains a large amount of olefins (i.e., compounds with non-aromatic carbon-carbon double bonds), making it easy to use as a raw material for chemical products.
[0039] (raw materials)
[0040] The pyrolysis oil of this embodiment is obtained by pyrolyzing waste materials containing used tires. By pyrolyzing waste materials containing used tires to obtain pyrolysis oil that is readily usable as a raw material for chemical products, the waste materials containing used tires can be effectively utilized as a resource. Therefore, the pyrolysis oil of this embodiment can contribute to the recycling (resource recovery) of waste materials containing used tires.
[0041] Waste used as raw material for pyrolysis includes used tires, and may further include waste other than used tires. Examples of waste other than used tires include waste from other rubber products besides tires and waste plastics.
[0042] Waste tires and other rubber products (waste rubber) typically contain diene rubbers as a rubber component, and further contain compounding agents such as fillers (e.g., carbon black, silica, calcium carbonate), silane coupling agents, antioxidants, softeners, processing aids, resins, surfactants, organic acids (e.g., stearic acid), zinc oxide (zinc white), vulcanization accelerators, and crosslinking agents (e.g., sulfur, peroxides). Specific examples of diene rubbers include natural rubber (NR), synthetic isoprene rubber (IR), styrene-butadiene rubber (SBR), butadiene rubber (BR), and chloroprene rubber (CR). The rubber component in the pyrolysis waste can primarily yield the aforementioned lightweight pyrolysis oils, which are readily usable as raw materials for chemical products.
[0043] (T90)
[0044] The 90% distillation temperature (T90) of the pyrolysis oil in this embodiment is below 400°C, and preferably below 350°C. When the 90% distillation temperature of the pyrolysis oil is below 400°C, the pyrolysis oil becomes lighter and easier to use as a raw material for chemical products. When the 90% distillation temperature of the pyrolysis oil is below 350°C, the pyrolysis oil is even easier to use as a raw material for chemical products. There is no particular limitation on the lower limit of the 90% distillation temperature, but generally the 90% distillation temperature of the pyrolysis oil is above 250°C. Pyrolysis oil with a 90% distillation temperature above 250°C can be easily obtained, for example, by means of the method described below, through the pyrolysis of waste materials containing used tires.
[0045] Here, in this specification, the 90% distillation temperature of the pyrolysis oil is the value measured using a distillation gas chromatograph (GC) according to ASTM D7169.
[0046] (T10)
[0047] The 10% (by mass) distillation temperature (T10) of the pyrolysis oil in this embodiment is preferably 100°C or higher, and more preferably 110°C or higher. Pyrolysis oil with a 10% distillation temperature of 100°C or higher contains fewer components with excessively small molecular weights and is even easier to use as a raw material for chemical products. There is no particular upper limit to the 10% distillation temperature, but typically the 10% distillation temperature of the pyrolysis oil is below 200°C. Pyrolysis oil with a 10% distillation temperature below 200°C can be readily obtained, for example, by the method described below, through the pyrolysis of waste materials containing used tires.
[0048] Here, in this specification, the 10% distillation temperature of the pyrolysis oil is the value measured using a distillation gas chromatograph (GC) according to ASTM D7169.
[0049] (density)
[0050] The density of the pyrolysis oil in this embodiment, measured at 40°C within 3 hours after production, is preferably 0.82 to 0.91 g / cm³. 3 The density is 0.82 g / cm³. 3 The above-mentioned pyrolysis oils contain fewer components with excessively small molecular weights and are even easier to use as raw materials for chemical products. Density is 0.91 g / cm³. 3 The following pyrolysis oils contain a large proportion of components with appropriately low molecular weights and are even more readily used as raw materials for chemical products. Therefore, their density ranges from 0.82 to 0.91 g / cm³. 3 Pyrolysis oil is even easier to use as a raw material for chemical products. From the viewpoint of ease of use as a raw material for chemical products, the density of pyrolysis oil is more preferably 0.84 g / cm³. 3 The above, and even more preferably less than 0.89 g / cm³ 3 .
[0051] Here, in this specification, the density of the pyrolysis oil is the value measured at 40°C according to ASTM D4052, and samples were taken immediately after pyrolysis.
[0052] Furthermore, the density of the pyrolysis oil in this embodiment, measured at 40°C after standing for 3 days following production, is preferably 0.84 to 0.97 g / cm³. 3 This is because when pyrolysis oil is left to stand for an extended period, the low-boiling-point components volatilize and the density changes. The density measured at 40°C after standing for 3 days post-production was 0.84 to 0.97 g / cm³. 3Pyrolysis oil is also more readily used as a raw material for chemical products.
[0053] (Olefin content)
[0054] The pyrolysis oil of this embodiment has an olefin content (olefin content) of 10% by volume or more, preferably 30% by volume or more, and more preferably 35% by volume or more, as measured by GC×GC-MS (two-dimensional gas chromatography-mass spectrometry). When the olefin content of the pyrolysis oil is 10% by volume or more, the pyrolysis oil is easily used as a raw material for chemical products. Pyrolysis oil with an olefin content of 30% by volume or more is even easier to use as a raw material for chemical products. There is no particular upper limit to the olefin content of the pyrolysis oil, but generally the olefin content of the pyrolysis oil is 60% by volume or less. Pyrolysis oil with an olefin content of 60% by volume or less can be easily obtained, for example, by pyrolysis of waste containing used tires, etc., using the method described below.
[0055] In this specification, "olefin" refers to a hydrocarbon having one or more carbon-carbon double bonds and lacking heteroatoms, aromatic rings, or carbon-carbon triple bonds, and it can be in chain or cyclic form. Examples of olefins include butadiene, isoprene, pentene, hexene, cyclopentene, cyclohexene, cyclopentadiene, dicyclopentadiene, and limonene. Butadiene and isoprene can be used as raw materials for rubber (especially diene-based rubbers).
[0056] Furthermore, in this specification, the olefin content (olefin content) of the pyrolysis oil is a value measured using GC×GC-MS (two-dimensional gas chromatography-mass spectrometry) by the method described in the examples.
[0057] (Iodine value)
[0058] The iodine value of the pyrolysis oil in this embodiment is preferably 180 g I2 / 100 g or higher. Pyrolysis oil with an iodine value of 180 g I2 / 100 g or higher contains a large amount of olefins and is even more readily used as a raw material for chemical products. From the viewpoint of ease of use as a raw material for chemical products, the iodine value of the pyrolysis oil is more preferably 200 g I2 / 100 g or higher. There is no particular upper limit to the iodine value of the pyrolysis oil, but generally the iodine value of the pyrolysis oil is 400 g I2 / 100 g or lower. Pyrolysis oil with an iodine value of 400 g I2 / 100 g or lower can be easily obtained, for example, by pyrolysis of waste containing used tires, etc., using the method described below.
[0059] Here, in this specification, the iodine value of the pyrolysis oil is the value measured according to JIS K0070.
[0060] (Acid value)
[0061] The acid value of the pyrolysis oil in this embodiment is preferably below 5 mg KOH / g. When the acid value of the pyrolysis oil is below 5 mg KOH / g, precipitation is unlikely to occur when the pyrolysis oil is processed into raw materials for chemical products, making it easy to process and obtain high-quality chemical product raw materials.
[0062] Furthermore, it is preferable that benzoic acid and its chloride are not present in the pyrolysis oil of this embodiment. When benzoic acid and its chloride are not present in the pyrolysis oil, precipitation is less likely to occur when the pyrolysis oil is processed into raw materials for chemical products, making it easier to process and obtain high-quality chemical product raw materials.
[0063] Here, in this specification, the acid value of the pyrolysis oil is the value measured according to JIS K2501.
[0064] (Aromatic content)
[0065] The aromatic content (content of aromatic compounds) of the pyrolysis oil in this embodiment, as measured by GC×GC-MS (two-dimensional gas chromatography-mass spectrometry), is preferably 80% by volume or less, more preferably 60% by volume or less, and even more preferably 40% by volume or less. Aromatic compounds are generally chemically stable and therefore difficult to convert into other compounds, making them unsuitable for use as chemical products. Therefore, when the aromatic content of the pyrolysis oil is 80% by volume or less, the pyrolysis oil is even more readily used as a raw material for chemical products other than benzene, toluene, and xylene. There is no particular limitation on the lower limit of the aromatic content of the pyrolysis oil, but typically the aromatic content is 10% by volume or more. Pyrolysis oil with an aromatic content of 10% by volume or more can be readily obtained, for example, by the method described below, through the pyrolysis of waste containing used tires.
[0066] Here, in this specification, the aromatic content (content of aromatic compounds) of the pyrolysis oil is a value measured using GC×GC-MS (two-dimensional gas chromatography-mass spectrometry) by the method described in the examples.
[0067] (Olefin content / Aromatic content)
[0068] The volume ratio (olefin content / aromatic content) of the pyrolysis oil in this embodiment, measured by GC×GC-MS (two-dimensional gas chromatography-mass spectrometry), is preferably 0.1 or more, more preferably 0.2 or more, and even more preferably 0.5 or more. Olefins are compounds having non-aromatic carbon-carbon double bonds and are readily used as chemical products, or can be easily converted into other chemical products through additional processing or reaction. On the other hand, as mentioned above, aromatic compounds are chemically stable and therefore difficult to convert into other compounds. Therefore, pyrolysis oil with a volume ratio (olefin content / aromatic content) of 0.1 or more contains many compounds having non-aromatic carbon-carbon double bonds that are readily used as chemical products, and contains fewer aromatic compounds that are difficult to use as chemical products, making it even easier to use as a raw material for chemical products. There is no particular upper limit to the volume ratio (olefin content / aromatic content), but typically the volume ratio (olefin content / aromatic content) of the pyrolysis oil is 10 or less. Pyrolysis oil with a volume ratio (olefin content / aromatic content) of less than 10 can be readily obtained, for example, by pyrolysis of waste containing used tires, by the method described below.
[0069] (Other components)
[0070] In addition to the olefins and aromatic compounds mentioned above, the pyrolysis oil of this embodiment may contain alkanes, alkynes and heterocyclic compounds, and may further contain nitrogen compounds, sulfur compounds and chlorine compounds.
[0071] <Production Methods of Pyrolysis Oil>
[0072] The method for producing pyrolysis oil described in this embodiment is not particularly limited. For example, the pyrolysis oil of this embodiment can be produced by a process including the steps of pyrolyzing waste materials containing used tires in a pyrolysis furnace to obtain pyrolysis gas, and cooling the pyrolysis gas to obtain pyrolysis oil. A preferred embodiment of the method for producing pyrolysis oil will be described below.
[0073] A preferred embodiment of the method for producing pyrolysis oil includes a step (pyrolysis step) of pyrolyzing waste materials containing used tires in a pyrolysis furnace to obtain pyrolysis gas and solids containing carbides, and a step (cooling step) of cooling the pyrolysis gas to obtain pyrolysis oil, wherein the pyrolysis temperature is 300°C to 500°C, and the pyrolysis reaction time is preferably 0.6 minutes or more. Here, in the case of a sealed pyrolysis furnace, the pyrolysis reaction time refers to the time from when the furnace temperature reaches the reaction temperature to release the furnace gas, while in the case of an open or continuous pyrolysis furnace, it refers to a value calculated based on the following equation.
[0074] [Mathematical Expression 1]
[0075]
[0076] When the pyrolysis temperature is above 300°C and the pyrolysis reaction time is above 0.6 minutes, the pyrolysis of waste materials, including used tires, can be sufficiently promoted. Furthermore, when the pyrolysis temperature is below 500°C, the aromatization of the pyrolysis gas can be suppressed, and by cooling the obtained pyrolysis gas, a light pyrolysis oil rich in olefins can be obtained. Therefore, according to the preferred embodiment of the pyrolysis oil production method, a light pyrolysis oil rich in olefins can be effectively obtained.
[0077] (Pyrolysis step)
[0078] In the pyrolysis step, waste materials containing used tires are pyrolyzed in a pyrolysis furnace to obtain pyrolysis gases and solids containing carbides. By pyrolyzing waste materials containing used tires to obtain pyrolysis gases and further cooling them to obtain light pyrolysis oil rich in olefins, waste materials containing used tires can be effectively utilized as a resource. During the pyrolysis step, portions or components of the waste materials that do not become raw materials for pyrolysis gases remain as residue in the pyrolysis furnace. Examples of residue include carbides, such as carbon black.
[0079] -Raw materials-
[0080] Waste materials used as raw materials for pyrolysis include used tires. Used tires can be pre-grouped by tire type (e.g., for passenger cars, for trucks and buses, for large vehicles such as off-road vehicles, for aircraft, for agricultural vehicles, etc.), and each group can be pyrolyzed. Alternatively, used tires can be pre-grouped by tire components (e.g., tread rubber, sidewall rubber, bead rubber, steel cord coated rubber, organic fiber cord coated rubber, pad rubber, cushion rubber, etc.), and each group can be pyrolyzed. Furthermore, both grouping by tire type and grouping by tire component can be performed, and each group can be pyrolyzed. When each group is pyrolyzed in this way, pyrolysis oil with more uniform physical properties can be obtained.
[0081] Used tires may contain metal reinforcement materials, such as steel cords and bead cores. When used tires contain metal reinforcement materials, these materials may be removed beforehand from the used tires, or they may not be removed. If the metal reinforcement materials are not removed from the used tires, they remain as residue in the pyrolysis furnace. Used tires may also be pre-cut or shredded.
[0082] There are no particular limitations on the methods for removing metal reinforcement from used tires or their crushed products, and examples include methods using magnets and sieves.
[0083] Used tires may contain organic fiber reinforcement materials, such as organic fiber cords. When used tires contain organic fiber reinforcement materials, these materials may be removed from the used tires beforehand, or they may not be removed. If the organic fiber reinforcement materials are not removed from the waste tires, they are retained in the pyrolysis furnace as residue or evaporated and discharged as gas. Used tires may also be pre-cut or shredded.
[0084] There are no particular limitations on the methods for removing organic fiber reinforcement from used tires or their crushed products, and examples include methods using centrifugal force and sieving.
[0085] Furthermore, there are no particular restrictions on the methods used to crush tires, and examples include mechanical crushing using single-shaft or twin-shaft crushers, water jet crushing, cryogenic crushing, and laser crushing.
[0086] Waste materials can include waste materials other than used tires. Examples of waste materials other than used tires include waste materials from other rubber products besides tires and waste plastics. As mentioned above, waste materials such as used tires and waste materials from other rubber products (waste rubber) typically contain diene rubber as a rubber component, and primarily, by subjecting the rubber component to pyrolysis, the aforementioned lightweight pyrolysis oil rich in olefins can be obtained.
[0087] -Pyrolysis temperature-
[0088] The preferred pyrolysis temperature is 300°C to 500°C. When the pyrolysis temperature is above 300°C, the pyrolysis of waste materials, including used tires, can be promoted. Furthermore, when the pyrolysis temperature is below 500°C, the aromatization of the generated pyrolysis gases can be suppressed, resulting in a light pyrolysis oil rich in olefins. From the viewpoint of promoting the pyrolysis of waste materials, the preferred pyrolysis temperature is 350°C or higher, and from the viewpoint of suppressing the aromatization of the generated pyrolysis gases, the preferred pyrolysis temperature is 450°C or lower.
[0089] There are no particular limitations on the method of controlling the temperature of pyrolysis, and for example, a method in which a heating device is attached to the pyrolysis furnace and the pyrolysis furnace is heated by the heating device, or a method in which the pyrolysis furnace is introduced into an electric furnace heated to a predetermined temperature, or a method in which high-temperature gas heated to a predetermined temperature is introduced into the pyrolysis furnace, or other methods may be used.
[0090] -Pyrolysis Furnace-
[0091] There are no particular restrictions on pyrolysis furnaces, and examples include batch pyrolysis furnaces, fluidized bed pyrolysis furnaces, and kiln pyrolysis furnaces.
[0092] In one embodiment, the pyrolysis furnace includes an inlet flow path for introducing inert gas and an outlet flow path for discharging inert gas and generated pyrolysis gas. Furthermore, it is preferred that a flow regulating device is attached to the inlet flow path, and the amount of inert gas introduced can be adjusted by the flow regulating device. There are no particular limitations on the flow regulating device installed in the inlet flow path, and examples include mass flow controllers, etc. Furthermore, it is preferred that the flow regulating device is also attached to the outlet flow path, and the amount of the mixture of discharged inert gas and generated pyrolysis gas can be adjusted by the flow regulating device. There are no particular limitations on the flow regulating device installed in the outlet flow path, and examples include back pressure valves, etc. Note that compared to a flow regulating device installed in the outlet flow path, a flow regulating device installed in the inlet flow path makes it easier to control the residence time of the pyrolysis gas in the pyrolysis furnace and to control the pyrolysis reaction time.
[0093] -Reaction Time-
[0094] The pyrolysis reaction time is preferably 0.6 minutes or more, and more preferably 1.0 minute or more. When the pyrolysis reaction time is 0.6 minutes or more, the pyrolysis of waste materials, including used tires, is fully carried out, and when it is 1.0 minute or more, the pyrolysis of the waste materials is further carried out.
[0095] Furthermore, the pyrolysis reaction time is preferably 10.0 minutes or less. If the pyrolysis reaction time exceeds 10.0 minutes, waste gas from the pyrolysis gases will form, the yield of the pyrolysis oil will decrease, and the aromatization of the pyrolysis gases will occur, resulting in an even lower yield of the light pyrolysis oil rich in olefins.
[0096] -atmosphere-
[0097] Pyrolysis is preferably carried out in an atmosphere of gases produced by pyrolysis, or in an atmosphere of a mixture of gases produced by pyrolysis and inert gases. By carrying out pyrolysis in an atmosphere of gases produced by pyrolysis or in an atmosphere of a mixture of gases produced by pyrolysis and inert gases, oxidation of the waste materials used as feedstock and the generated pyrolysis gases can be suppressed, thereby obtaining pyrolysis gases containing a higher olefin content, and through the cooling step described later, obtaining pyrolysis oil containing a higher olefin content. Examples of inert gases here include nitrogen, carbon dioxide, argon, and helium. Furthermore, the atmosphere of gases produced by pyrolysis, or the atmosphere of a mixture of gases produced by pyrolysis and inert gases, may contain less than 1% by volume of oxygen.
[0098] Pyrolysis is preferably carried out while the gas produced by pyrolysis, or a mixture of the gas produced by pyrolysis and an inert gas, is flowing through the pyrolysis furnace. By conducting pyrolysis while the gas produced by pyrolysis, or a mixture of the gas produced by pyrolysis and an inert gas, is flowing through the pyrolysis furnace, oxidation of the waste material used as feedstock and the generated pyrolysis gas can be suppressed, thereby obtaining pyrolysis gas containing a higher olefin content. Furthermore, by adjusting the flow rate of the inert gas, it becomes easy to precisely control the residence time of the pyrolysis gas in the pyrolysis furnace, i.e., the pyrolysis reaction time, and through the cooling step described later, a light pyrolysis oil containing a higher olefin content can be obtained.
[0099] -other-
[0100] The pyrolysis step can be carried out at any pressure, including under reduced pressure, atmospheric pressure, or pressurized pressure. Note that by carrying out pyrolysis under reduced pressure or atmospheric pressure, the polymerization (repolymerization) of olefins in the pyrolysis gas can be suppressed. The pressure in the pyrolysis furnace is preferably below 0.1 kPaG, and more preferably below 0 kPaG. When the pressure in the pyrolysis furnace is below 0.1 kPaG, the polymerization (repolymerization) of olefins in the pyrolysis gas can be further suppressed, and when the pressure in the pyrolysis furnace is below 0 kPaG, the polymerization (repolymerization) of olefins in the pyrolysis gas can be suppressed even more. When the pressure in the pyrolysis furnace is below 0 kPaG, this includes a reduced pressure state.
[0101] The pyrolysis step can be carried out with or without a catalyst, but it is preferred to do so without a catalyst. By not using a catalyst in the pyrolysis step, the cost of the pyrolysis step can be reduced. When a catalyst is used, any catalyst that promotes the pyrolysis reaction of waste materials containing used tires can be used, and examples of such catalysts include acidic catalysts such as zeolites, activated clays, acidic clays, and bentonite, as well as basic catalysts such as sodium carbonate.
[0102] (Cooling Step)
[0103] In the cooling step, the pyrolysis gas is cooled to obtain pyrolysis oil. By cooling the pyrolysis gas, it is separated into waste gas that remains in a gaseous state and liquefied pyrolysis oil, and a light pyrolysis oil rich in olefins can be obtained.
[0104] The composition of the exhaust gas depends on the cooling temperature; however, for example, at atmospheric pressure and 20°C, the gaseous components include hydrogen and hydrocarbons with 1 to 4 carbon atoms. The exhaust gas can be used as a feedstock for chemical products or as fuel for a pyrolysis furnace.
[0105] There are no particular limitations on the cooling method for the pyrolysis gas, and the gas can be actively cooled using a condenser or cooling tower, or it can be cooled naturally by releasing heat. There are no particular limitations on the cooling temperature of the pyrolysis gas, but it is preferably from -20°C to 100°C, and more preferably from 0°C to 50°C. When a medium is used to cool the pyrolysis gas, there are no particular limitations on the medium, and examples include water, etc.
[0106] The yield of pyrolysis oil based on the mass of waste is preferably 30% or more, and more preferably 35% or more. When the yield of pyrolysis oil based on the mass of waste is 30% or more, a large amount of light pyrolysis oil rich in olefins can be effectively obtained, thereby improving economic efficiency and facilitating the recycling of waste including used tires.
[0107] In one embodiment, it is preferable to recover more than 55% by mass of the pyrolysis gas as pyrolysis oil. When more than 55% by mass of the pyrolysis gas is recovered as pyrolysis oil, a large amount of light pyrolysis oil rich in olefins can be effectively obtained, thereby further improving economics and further contributing to the recycling of waste materials including used tires.
[0108] (Other steps)
[0109] The above-described method for producing pyrolysis oil may include steps other than the pyrolysis and cooling steps described above. Examples of other steps include a raw material pretreatment step, a carbide treatment step to obtain carbon black by treating carbides, and a purification step for the resulting pyrolysis oil.
[0110] Carbide processing steps may include, for example, steps to remove substances other than carbon black, pulverization steps, and carbon black granulation steps. There are no particular limitations on the methods used in carbide processing steps, and commonly known processing methods can be used.
[0111] However, it is preferable that the method for producing pyrolysis oil does not include a distillation step for the pyrolysis oil obtained in the cooling step. By omitting the distillation step for the pyrolysis oil obtained after cooling the pyrolysis gases, the yield of pyrolysis oil based on the quality of the rubber component in the waste used as raw material is improved, and the entire process is simplified, thereby improving economic efficiency.
[0112] <Elastomers>
[0113] The elastomer of this embodiment is characterized in that the aforementioned pyrolysis oil is used as part or all of the raw material. Because the elastomer of this embodiment uses the aforementioned pyrolysis oil as part or all of the raw material, it can help promote the recycling of waste materials including used tires.
[0114] Preferably, the elastomer is at least one selected from the group consisting of resins and synthetic rubbers. Elastomers selected from the group consisting of resins and synthetic rubbers are readily used as rubber or resin products and are in high demand, thus they can further contribute to promoting the recycling of waste materials including used tires.
[0115] Examples of resins here include thermoplastic elastomers, such as polyester thermoplastic elastomers (TPC), polyamide thermoplastic elastomers (TPA), polyolefin thermoplastic elastomers (TPO), and polystyrene thermoplastic elastomers (TPS). Examples of synthetic rubbers include diene rubbers, such as synthetic isoprene rubber (IR), styrene-butadiene rubber (SBR), butadiene rubber (BR), and chloroprene rubber (CR).
[0116] Rubber Products
[0117] The rubber product of this embodiment is characterized in that the aforementioned elastomer is used as part or all of the raw material. Because the rubber product of this embodiment uses the aforementioned elastomer as part or all of the raw material, it can help promote the recycling of waste materials including used tires.
[0118] Here, rubber products can be produced, for example, by pre-preparing a rubber composition containing synthetic rubber and a vulcanizing agent such as sulfur, shaping the rubber composition into a desired shape, and then subjecting it to a vulcanization step by heating. The rubber composition may further contain compounding agents, such as fillers (carbon black, silica, calcium carbonate, etc.), silane coupling agents, antioxidants, softeners, processing aids, resins, surfactants, organic acids (e.g., stearic acid), zinc oxide (zinc white), and vulcanization accelerators, etc.
[0119] Preferably, the rubber product is at least one selected from the group consisting of rubber tires, rubber tracks, rubber hoses, conveyor belts, and vibration-damping rubber. Rubber products selected from the group consisting of rubber tires, rubber tracks, rubber hoses, conveyor belts, and vibration-damping rubber are widely used and produced in large quantities, thus they can further contribute to promoting the recycling of waste materials, including used tires.
[0120] <Resin Products>
[0121] The resin product of this embodiment is characterized in that the aforementioned elastomer is used as part or all of the raw material. Because the resin product of this embodiment uses the aforementioned elastomer as part or all of the raw material, it can help promote the recycling of waste materials including used tires.
[0122] Here, the resin product can be produced, for example, by molding the resin into a desired shape. Alternatively, for example, a resin composition comprising the resin and desired additives can be prepared in advance, and the resin composition can be molded into the desired shape to produce the resin product. Examples of additives added to the resin composition include weather-resistant antioxidants, heat-resistant antioxidants, moisture-resistant additives, antistatic agents, lubricants, crystallizing nucleating agents, tackifiers, antifogging agents, release agents, plasticizers, fillers, dyes, fragrances, and flame retardants, etc.
[0123] Preferably, the resin product is at least one selected from the group consisting of resin tires and resin hoses. Resin products selected from the group consisting of resin tires and resin hoses have a high resin content, and therefore can further contribute to promoting the recycling of waste materials including used tires.
[0124] Example
[0125] The present invention will now be described in more detail with reference to embodiments, but the present invention is not limited in any way to the following embodiments.
[0126] <Sample Preparation>
[0127] As samples of used tires, tire pads were prepared from actual used truck and bus (TBR) tires and used passenger car (PSR) tires, respectively.
[0128] Production of Pyrolysis Oil
[0129] Prepare a pyrolysis furnace with a capacity of 34L, equipped with an inlet flow path for introducing inert gas and an outlet flow path for discharging inert gas and generating pyrolysis gas. Attach a mass flow controller to the inlet flow path to allow adjustment of the amount of inert gas introduced. Attach a back pressure valve to the outlet flow path to allow adjustment of the amount of inert gas discharged and the amount of pyrolysis gas generated.
[0130] After placing the vulcanized rubber sample (tire sheet) prepared as described above in the pyrolysis furnace, the pyrolysis furnace containing the vulcanized rubber sample was placed in an electric furnace adjusted to the temperature shown in Table 1, and the pyrolysis of the vulcanized rubber sample was started. In Examples 3 and Comparative Examples 1-4 and 6, nitrogen gas was introduced from the inlet flow path of the pyrolysis furnace, and a mixture of nitrogen gas and generated pyrolysis gas was taken out from the outlet flow path. The amount of nitrogen gas introduced and the amount of the mixture of nitrogen gas and pyrolysis gas discharged were adjusted so that the pyrolysis reaction time is as shown in Table 1. Based on the amount of nitrogen gas introduced, the amount of pyrolysis gas generated, the average molecular weight of the pyrolysis gas, the temperature of the pyrolysis gas, and the capacity of the pyrolysis furnace, the pyrolysis reaction time was calculated according to the following formula:
[0131] [Mathematical Expression 2]
[0132]
[0133] Next, the gas obtained from the discharge flow path is cooled to 0°C by a condenser, separated into pyrolysis oil and waste gas, and the pyrolysis oil is recovered.
[0134] In addition, the recovered pyrolysis oil is subjected to GC×GC-MS analysis by the following method to measure the content of each component. The distillation properties, iodine value and density of the recovered pyrolysis oil are measured by the following methods.
[0135] Furthermore, the measurement of the acid value of the pyrolysis oil and the evaluation of heat exchanger fouling caused by the pyrolysis oil are carried out by the following methods.
[0136] <GC×GC-MS Analysis>
[0137] The component composition of the recovered pyrolysis oil was analyzed using a two-dimensional gas chromatograph mass spectrometer (GC×GC-MS, manufactured by JEOL, product name "JEOL JMS-T2000GC") equipped with "DB-1" from Agilent Technology (length 60 m, inner diameter 0.25 mm, film thickness 0.1 μm) as the first dimension and "DB-17" from Agilent Technology (length 2 m, inner diameter 0.25 mm, film thickness 0.1 μm) as the second dimension. Qualitative analysis was performed on the detected peaks, and as Figure 1 shown, classification was performed based on the structures. Specifically, first, the compounds are classified according to whether they contain heteroatoms (S, N, O), and the compounds containing heteroatoms are classified as "heterocompounds". Next, the compounds containing no heteroatoms are classified according to whether they contain aromatic rings. The compounds containing aromatic rings are further classified into "monocyclic aromatics" for compounds having one aromatic ring, "dicyclic aromatics" for compounds having two aromatic rings, and "tricyclic or higher aromatics" for compounds having three or more aromatic rings. The compounds containing no aromatic rings are classified as "paraffins" for compounds having only single bonds, "alkynes" for compounds having triple bonds, and "olefins" for compounds having double bonds but no triple bonds.
[0138] <Distillation GC Analysis>
[0139] The distillation properties of the recovered pyrolysis oil are analyzed using a distillation gas chromatograph (GC) in accordance with ASTM D7169.
[0140] <Measurement of Iodine Value>
[0141] The iodine value of the recovered pyrolysis oil is measured in accordance with JIS K0070.
[0142] <Measurement of Density>
[0143] The density of pyrolysis oil at 40°C was measured according to ASTM D4052.
[0144] [Table 1]
[0145]
[0146] As can be seen from Table 1, the pyrolysis oil according to embodiments of the present invention is light and has a high olefin content, making it easy to use as a raw material for chemical products.
[0147] <Measurement of Acid Value>
[0148] The acid value of pyrolysis oil was measured according to JIS K2501.
[0149] Evaluation of heat exchanger scaling caused by pyrolysis oil
[0150] Due to scale adhering to Figure 2 The temperature drop width (°C) caused by the test piece 11 of the scale evaluation test apparatus (HLPS) 10 shown is measured in the following order.
[0151] 1. Allow the pyrolysis oil at 25℃ to... Figure 2 The scale evaluation test apparatus (HLPS) 10 shown in the diagram has a fixed flow period (200 minutes) at the bottom left side (inlet 12).
[0152] 2. While maintaining the temperature of test piece 11 at a constant 300℃, scaling and adhesion were observed on the surface of test piece 11. When scaling adhered to test piece 11, the heat transfer between the pyrolysis oil and test piece 11 decreased.
[0153] 3. Measure the temperature of the pyrolysis oil discharged from the upper right side (outlet 13) of the scaling evaluation test apparatus (HLPS) 10. Define the difference between the initial measured temperature at outlet 13 and the measured temperature after a fixed time period as "the width of the temperature drop due to reduced heat transfer caused by scaling".
[0154] Here, the "Scale Evaluation of Heat Exchangers" is conducted according to the following criteria.
[0155] (Evaluation Criteria)
[0156] Acceptable: Temperature drop width is less than 2℃ / h, and it is determined that scaling of the heat exchanger is suppressed.
[0157] Unacceptable: Temperature drop width is greater than 2℃ / h, and significant scaling of the heat exchanger is confirmed.
[0158] [Table 2]
[0159]
[0160] As can be understood from Table 2, when the acid value of the pyrolysis oil is below 5 mg KOH / g, scaling of the heat exchanger is unlikely to occur.
[0161] Industrial availability
[0162] The pyrolysis oil disclosed herein can be used as a raw material for chemical products. Furthermore, the pyrolysis oil disclosed herein facilitates the recycling of waste materials including used tires.
[0163] Furthermore, the elastomers disclosed herein can be used in rubber products such as rubber tires, rubber tracks, rubber hoses, conveyor belts, and vibration-damping rubber, as well as resin products such as resin tires and resin hoses.
[0164] Explanation of reference numerals in the attached figures
[0165] 10: Scale Evaluation Test Equipment (HLPS)
[0166] 11: Test piece
[0167] 12: Entrance
[0168] 13: Exports
Claims
1. A pyrolysis oil obtained by pyrolysis of waste materials including used tires, wherein 90% of the pyrolysis oil is distilled at a temperature below 400°C and has an olefin content of 10% by volume or more as measured by GC×GC-MS.
2. The pyrolysis oil according to claim 1, wherein the olefin content measured by GC×GC-MS is 30% by volume or more.
3. The pyrolysis oil according to claim 1, wherein 10% of the pyrolysis oil is distilled at a temperature of 100°C or higher.
4. The pyrolysis oil according to claim 1, wherein the density of the pyrolysis oil measured at 40°C within 3 hours after production is 0.82 g / cm³. 3 Up to 0.91 g / cm 3 .
5. The pyrolysis oil according to claim 1, wherein the density of the pyrolysis oil measured at 40°C after standing for 3 days following production is 0.84 g / cm³. 3 Up to 0.97 g / cm 3 .
6. The pyrolysis oil according to claim 1, wherein the iodine value of the pyrolysis oil is 180g I2 / 100g or higher.
7. The pyrolysis oil according to claim 1, wherein the acid value of the pyrolysis oil is below 5 mg KOH / g.
8. An elastomer obtained using part or all of the pyrolysis oil according to claim 1 as a raw material.
9. The elastomer according to claim 8, wherein the elastomer is at least one selected from the group consisting of resin and synthetic rubber.
10. A rubber product obtained by using the elastomer according to claim 8 as part or all of the raw material.
11. The rubber product according to claim 10, wherein the rubber product is at least one selected from the group consisting of rubber tires, rubber tracks, rubber hoses, conveyor belts, and vibration-damping rubber.
12. A resin product obtained by using the elastomer according to claim 8 as part or all of the raw material.
13. The resin product of claim 12, wherein the resin product is at least one selected from the group consisting of resin tires and resin hoses.
Citation Information
Patent Citations
Process for the recovery of carbon and hydrocarbon mixtures from polymer, preferably in the form of waste tires, by pyrolysis in a pyrolysis reactor
JP2002523552A