Methods for recycling metals

By utilizing cavitation fields and ultrasonic probes to create turbulence in a flow-through reactor, and using weak acid and hydrogen peroxide solutions to accelerate the leaching of transition metals and lithium in the positive electrode of lithium-ion batteries, the environmental risks and low efficiency problems caused by high-temperature and strong acid solution leaching in existing technologies are solved, achieving efficient and safe metal recovery.

CN123125350APending Publication Date: 2026-11-17KING ABDULLAH UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580028185.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-08
Filing Date
2025-03-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode leaching technologies suffer from high environmental risks and low efficiency, especially the soil and water pollution and low recovery rate caused by high-temperature processes and strong inorganic acid solution leaching methods, which make it difficult to achieve commercial application.

Method used

By using cavitation fields and ultrasonic probes to create turbulence in a flow-through reactor, and by using weak acid and hydrogen peroxide solution, the leaching of transition metals and lithium is accelerated through the collapse of cavitation bubbles, avoiding the use of high temperature and strong acid.

Benefits of technology

The process significantly improved the recovery efficiency of transition metals and lithium at ambient temperatures, reduced energy consumption and environmental risks, and achieved an efficient and safe metal recovery process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125350A_ABST
    Figure CN123125350A_ABST
Patent Text Reader

Abstract

This document discloses methods and apparatus for recovering metals. Embodiments of the method include immersing a metal compound in a leaching solution containing leaching aids to form a slurry; and passing the slurry through a cavitation field to dissolve at least a portion of the metal compound.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-references to related applications

[0001] This PCT application claims priority to U.S. Provisional Patent Application No. 63 / 563,121, filed March 8, 2024, the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0002] This invention relates to the field of liquid reactors, and in particular to the recovery of metals from solids by leaching. Background Technology

[0003] A smooth and rapid green transition to net zero requires reducing the use of fossil fuels as an energy source. One of the biggest obstacles to net zero is the cost-effective and scalable storage of renewable energy sources to maintain a continuous and reliable energy supply. Lithium-ion batteries offer the current best practice for storage. However, the high costs associated with mining these elements may hinder or slow further adoption.

[0004] Millions of people worldwide use lithium-ion batteries in their daily lives. The positive electrode of these batteries typically contains transition metals such as cobalt, nickel, and manganese (NMC batteries) and powers smartphones, as well as many household appliances and vehicles. Despite the high environmental and economic costs associated with mining these dwindling resources, only 3-5% of lithium-ion batteries are currently recycled.

[0005] Lithium-ion cathodes have been recovered using high-temperature processes (pyrometallurgical processes) or leaching with strong inorganic acid solutions (hydrometallurgical processes). Hydrometallurgical processes achieve high metal recovery rates and purity; however, the use of these acids is environmentally harmful, posing a high risk of soil and water pollution and resulting in atmospheric emissions of nitrogen oxides and corrosive gases, and has not been commercially adopted to any extent. Cathode leaching typically uses strong inorganic acids such as sulfuric acid or hydrochloric acid with the addition of reducing agents to promote the dissolution of metal ions in the acidic solution. The use of these acids is also environmentally harmful, posing a high risk of soil and water pollution and resulting in atmospheric emissions of nitrogen oxides and corrosive gases, as well as the generation of hazardous or economically unprofitable byproducts (such as sodium sulfate).

[0006] Conventional recycling techniques typically involve pulverizing the battery and then separating lithium and other metals present in the cathode. Recovering these metals requires a complex series of processes, including leaching with chemical solvents to recover lithium, cobalt, and other metals, or separating copper and magnesium using high temperatures.

[0007] Currently, the cathode leaching step is a bottleneck in the hydrometallurgical recovery of waste lithium-ion batteries (LIBs) and requires expensive and hazardous inorganic solvents. Recently, Golmohammadzadeh et al., Waste Management 64 (2017) 244-254, reported the recovery of lithium and cobalt from cathode materials using weak acids such as acetic acid and malic acid at elevated temperatures and in the presence of a reducing agent (e.g., hydrogen peroxide) in a three-necked glass reactor immersed in an ultrasonic bath, employing mechanical agitation. Unfortunately, even at elevated temperatures, the leaching time to achieve 80% recovery of Co and Li is one hour or longer.

[0008] Therefore, there is a need in this field to address one or more of these deficiencies.

[0009] This background information is provided for the purpose of leading the applicant to believe that known information may be relevant to this disclosure. It is not necessarily intended to acknowledge, nor should it be construed, that any of the foregoing information constitutes prior art to this disclosure. Summary of the Invention

[0010] One objective of this disclosure is to achieve the commercially viable recovery of transition metals and lithium from compounds containing one or more transition metals, such as oxides and phosphates.

[0011] Surprisingly, it has been found that transition metals, aluminum, and alkali metals can be rapidly leached (dissolved) from metal compounds (e.g., oxides and phosphates) into the leaching solution by passing a slurry containing metal compounds and a leaching solution through one or more transient cavitation fields, and particularly through the collapse (implosion) of cavitation bubbles. Leaching is thought to be (but not limited to) accelerated by the direct exposure of particles to the implosion of smaller, high-energy bubbles in the cavitation field, which can be facilitated by creating turbulence / vortices at the cavitation bubble formation site using, for example, one or more deflectors or flow restrictors in a flow-through reactor. Such restriction or deflection can be achieved using an ultrasonic probe with a varying diameter along the axis of a flow-through tubular reactor.

[0012] Depending on the microstructure of the metal compound (such as that typically exhibited by cathode particles), cavitation fields with an average bubble size similar to the average particle size of the metal compound (e.g., no greater than 5X, 3X, 2X, or 1.5X) have been found to be particularly useful. This is thought to be (but not limited to) because a sufficient number of cavitation bubbles have a small size to form a jet that can penetrate the pores of the secondary particles and effectively cause the secondary particles to be crushed, resulting in accelerated dissolution of the primary particles (metal) into the acid solution. This method can be carried out without heating except for raising the temperature from ambient (i.e., 20°C to 30°C) to below the boiling point of the acid solution. Ideally, this method is carried out in a flow-through reactor with a cavitation generation device and a fluid deflection device that induces turbulence or eddies within the reactor, resulting in increased exposure time of the particles to the cavitation field within the flowing liquid (especially during the initial cavitation phase).

[0013] A process is shown, comprising: immersing a metal compound in a leaching solution containing a leaching aid to form a slurry; and flowing the slurry through cavitation fields to dissolve at least a portion of the metal compound. Ideally, the slurry flows through a series of cavitation fields, wherein each cavitation field may have the same or similar average bubble size, or may have different average bubble sizes (e.g., the probe vibration frequencies of two or more ultrasonic probes may vary, for example, from 15 kHz to 100 kHz).

[0014] According to one aspect of this disclosure, a method is provided that can be used alone or in combination with any other aspect described herein, the method comprising:

[0015] A metal compound is immersed in a leaching solution containing leaching aids to form a slurry; and

[0016] The slurry is flowed through a cavitation field to dissolve at least a portion of the metal compound.

[0017] In one aspect of this disclosure, the leaching solution contains water.

[0018] In one aspect of this disclosure, the method further includes adding an additional acid during the method.

[0019] In one aspect of this disclosure, the leaching aid includes a weak acid.

[0020] In one aspect of this disclosure, the acid is a carboxylic acid or a peroxyacid of a carboxylic acid.

[0021] In one aspect of this disclosure, a cavitation field is provided.

[0022] In one aspect of this disclosure, the method includes adding an oxidizing agent to the leaching solution.

[0023] In one aspect of this disclosure, the oxidizing agent is hydrogen peroxide.

[0024] In one aspect of this disclosure, about 0.5% to about 10% vol% of an oxidizing agent is added to the leaching solution.

[0025] In one aspect of this disclosure, the metal compound has an average particle size, and the cavitation field has an average cavitation bubble size, and the ratio of the average cavitation bubble size to the average metal compound particle size is at most 2.

[0026] In one aspect of this disclosure, the slurry is at a temperature below the boiling point of the leaching solution.

[0027] In one aspect of this disclosure, the solid metal oxide comprises lithium and at least one other metal.

[0028] In one aspect of this disclosure, the other metals include one or more of Al and transition metals.

[0029] In one aspect of this disclosure, the transition metal includes one or more of Co, Mn, and Ni.

[0030] In one aspect of this disclosure, the cavitation field is generated by an ultrasonic probe that is at least partially immersed in the slurry.

[0031] In one aspect of this disclosure, an ultrasonic probe is disposed within a tubular reactor having an inlet and an outlet, a first end and a second end positioned to allow slurry to flow through the tubular reactor and through a cavitation field generated by the ultrasonic probe.

[0032] In one aspect of this disclosure, the length of the ultrasonic probe is axially oriented within the length of the tubular reactor.

[0033] In one aspect of this disclosure, the ultrasonic probe has a diameter that varies along the length of the ultrasonic probe, thereby inducing a cavitation field at different points along the length of the ultrasonic probe.

[0034] In one aspect of this disclosure, the tubular reactor includes one or more deflection devices that cause the slurry to be deflected into a cavitation field as it flows through the tubular reactor.

[0035] In one aspect of this disclosure, the one or more deflecting devices are each independently selected from: protrusions, baffles, and deflectors.

[0036] In one aspect of this disclosure, the solid load of the slurry exceeds the solubility limit of the solid in the leaching solution.

[0037] In one aspect of this disclosure, there are at least two or more ultrasound probes.

[0038] In one aspect of this disclosure, the two or more probes vibrate in phase or out of phase.

[0039] In one aspect of this disclosure, the two or more probes have varying diameters along their length, with the diameter of each probe varying asynchronously, synchronously, or in combination along their length.

[0040] In one aspect of this disclosure, the metal compound comprises secondary particles with an average particle size of 2 to 100 micrometers, the secondary particles comprising aggregated primary particles with an average size of up to 2 micrometers.

[0041] In one aspect of this disclosure, the solid loading of the metal compound in the slurry is from 0.1% to 20% by weight.

[0042] In one aspect of this disclosure, the slurry flows sequentially through at least two cavitation fields.

[0043] In one aspect of this disclosure, the slurry flows through two or more tubular reactors connected in series.

[0044] In one aspect of this disclosure, the method further includes separating any undissolved metal oxides.

[0045] In one aspect of this disclosure, the average cavitation bubble size / average metal compound particle size is at most 1.5.

[0046] In one aspect of this disclosure, the metal compound particles comprise open pores having an average pore size, and the average cavitation bubble size is not greater than 10 times the average pore size of the metal compound particles.

[0047] According to another aspect of this disclosure, a process for leaching solid metal oxides is provided, the process being used alone or in combination with any other aspects described herein, the process comprising:

[0048] Exposing solid metal oxides to a leaching solution containing organic acids; and

[0049] Ultrasonic waves are applied to the leaching solution at cavitation frequencies to dissolve solid metal oxides as metal ions into the leaching solution.

[0050] According to another aspect of this disclosure, a process for leaching solid metal oxides is provided, the process being used alone or in combination with any other aspects described herein, the process comprising:

[0051] Exposing solid metal oxides to a leaching solution containing organic acids; and

[0052] Ultrasonic waves are applied to the leaching solution at the cavitation frequency in a cavitation field to dissolve solid metal oxides as metal ions into the leaching solution.

[0053] In one aspect of this disclosure, the organic acid is acetic acid.

[0054] In one aspect of this disclosure, the cavitation frequency is about 20-30 kHz.

[0055] In one aspect of this disclosure, the leaching solution contains an oxidizing agent.

[0056] In one aspect of this disclosure, the oxidizing agent is hydrogen peroxide.

[0057] In one aspect of this disclosure, the leaching solution contains about 0 to about 8 vol% of an oxidizing agent.

[0058] In one aspect of this disclosure, ultrasound is applied for a period of up to about 15 minutes.

[0059] In one aspect of this disclosure, the time period is at most about 8 minutes.

[0060] In one aspect of this disclosure, the solid metal oxide comprises one or more of the following: lithium oxide, cobalt oxide, nickel oxide, manganese oxide, lithium cobalt oxide, lithium manganese oxide, or lithium nickel oxide, and phosphates such as lithium iron phosphate.

[0061] In one aspect of this disclosure, applying ultrasound includes vibrating an acoustic probe that is at least partially immersed in a leaching solution.

[0062] In one aspect of this disclosure, the acoustic probe is connected to a piezoelectric actuator.

[0063] In one aspect of this disclosure, the process further includes:

[0064] Undissolved solid metal oxides and metal phosphates are exposed to a fresh leaching solution containing organic acids; and

[0065] Ultrasonic waves are applied to the fresh leachate at cavitation frequencies.

[0066] In one aspect of this disclosure, the process further includes separating an aqueous solution containing dissolved metal oxide salts from undissolved solid metal oxides after applying ultrasound.

[0067] In one aspect of this disclosure, separation occurs by centrifugation.

[0068] According to another aspect of this disclosure, a reactor is provided for leaching a positive electrode material into a leaching solution, which can be used alone or in combination with any other aspect described herein, the apparatus comprising:

[0069] The reactor wall has a first end and an opposing second end, and the reactor wall defines the internal reactor cavity;

[0070] The inlet, located at or near the first end, is configured to receive a mixture of solid cathode material and aqueous solution into the internal reactor chamber;

[0071] An outlet, located at or near the second end, is configured to at least partially discharge the mixture from the internal reactor cavity; and

[0072] An acoustic probe, at least partially disposed within the internal reactor cavity, is configured to apply ultrasonic waves at a cavitation frequency to the leaching solution to dissolve the solid metal oxide as a metal oxide salt into the leaching solution.

[0073] In one aspect of this disclosure, the inlet defines an inlet axis, the outlet defines an outlet axis, the acoustic probe defines an acoustic probe axis, and the inlet axis and / or the outlet axis are perpendicular to the acoustic probe axis.

[0074] In one aspect of this disclosure, the distance between the outer surface of the acoustic probe and the inner surface of the reactor wall is about 1.05 to about 3.

[0075] According to another aspect of this disclosure, a process for leaching metal compounds such as solid metal oxides is provided, said process being used alone or in combination with any other aspects described herein, said process comprising:

[0076] Expose the metal compound to a leaching solution containing organic acids; and

[0077] Ultrasonic waves are applied to the leaching solution at cavitation frequencies to dissolve the metal compound as metal ions into the leaching solution.

[0078] According to another aspect of this disclosure, a process for leaching metal compounds such as solid metal oxides is provided, said process being used alone or in combination with any other aspects described herein, said process comprising:

[0079] Expose the metal compound to a leaching solution containing organic acids; and

[0080] Ultrasonic waves are applied to the leaching solution at a cavitation frequency in a cavitation field to dissolve the metal compound as metal ions into the leaching solution.

[0081] In one aspect of this disclosure, the organic acid is acetic acid.

[0082] In one aspect of this disclosure, the cavitation frequency is about 20-30 kHz.

[0083] In one aspect of this disclosure, the leaching solution contains an oxidizing agent.

[0084] In one aspect of this disclosure, the oxidizing agent is hydrogen peroxide.

[0085] In one aspect of this disclosure, the leaching solution contains about 0 to about 8% by volume of an oxidizing agent.

[0086] In one aspect of this disclosure, ultrasound is applied for a period of up to about 15 minutes.

[0087] In one aspect of this disclosure, the time period is at most about 8 minutes.

[0088] In one aspect of this disclosure, the metal compound comprises one or more of the following: lithium oxide, cobalt oxide, nickel oxide, manganese oxide, lithium cobalt oxide, lithium manganese oxide, or lithium nickel oxide, and phosphates such as lithium iron phosphate.

[0089] In one aspect of this disclosure, applying ultrasound includes vibrating an acoustic probe that is at least partially immersed in a leaching solution.

[0090] In one aspect of this disclosure, the acoustic probe is connected to a piezoelectric actuator.

[0091] In one aspect of this disclosure, the process further includes:

[0092] Exposing undissolved metal compounds to a fresh leaching solution containing organic acids; and

[0093] Ultrasonic waves are applied to the fresh leachate at cavitation frequencies.

[0094] In one aspect of this disclosure, the process further includes separating an aqueous solution containing dissolved metal compounds, such as metal oxide salts, from undissolved metal compounds, such as solid metal oxides, after applying ultrasound.

[0095] In one aspect of this disclosure, separation occurs by centrifugation.

[0096] According to another aspect of this disclosure, a reactor is provided for leaching a positive electrode material into a leaching solution, which can be used alone or in combination with any other aspect described herein, the apparatus comprising:

[0097] The reactor wall has a first end and an opposing second end, and the reactor wall defines the internal reactor cavity;

[0098] The inlet, located at or near the first end, is configured to receive a mixture of solid cathode material and aqueous solution into the internal reactor chamber;

[0099] An outlet, located at or near the second end, is configured to at least partially discharge the mixture from the internal reactor cavity; and

[0100] An acoustic probe, at least partially disposed within the internal reactor cavity, is configured to apply ultrasonic waves at a cavitation frequency to the leaching solution to dissolve the solid metal oxide as a metal oxide salt into the leaching solution.

[0101] In one aspect of this disclosure, the inlet defines an inlet axis, the outlet defines an outlet axis, the acoustic probe defines an acoustic probe axis, and the inlet axis and / or the outlet axis are perpendicular to the acoustic probe axis.

[0102] In one aspect of this disclosure, the distance between the outer surface of the acoustic probe and the inner surface of the reactor wall is about 1.05 to about 3.

[0103] Other aspects and features of this disclosure will become clear to those skilled in the art upon review of the following description of specific embodiments of this disclosure. Attached Figure Description

[0104] Figure 1 It is a scanning electron micrograph (SEM) of the original metal compound particles.

[0105] Figure 2 This is a SEM of metal compound particles subjected to transient cavitation treatment in water under conditions without acid or reducing agent.

[0106] Figure 3 This is a SEM image of metal compound particles after acid treatment for 8 minutes using the method described in this paper.

[0107] Figure 4 This is a graph comparing the leaching efficiency of one of the methods described in this paper with existing technologies.

[0108] Figure 5 It is a schematic diagram of an apparatus that can be used to perform one or more methods as described herein.

[0109] Figure 6 A diagram of a reactor that can be used to perform the methods described herein is shown.

[0110] Figure 7 This is a three-dimensional view of the reactor that can be used in this method.

[0111] Figure 8 yes Figure 6 and Figure 7 The image depicts a model of cavitation in a reactor.

[0112] Figure 9 It can be used Figure 6-8 The diagram depicts a cross-sectional view of the reactor in a flow-through tubular reactor.

[0113] Figure 10 It can be used Figure 6-8 The radial and three-dimensional views of the acoustic probe in the flow-through tubular reactor are depicted.

[0114] Figure 11 This is a comparison image of dissolved black mass. Detailed Implementation

[0115] One or more illustrative embodiments have been described by way of examples. This document describes processes, apparatus, and methods for leaching, dissolving, and recovering one or more metal compounds. It will be understood that the embodiments and examples are provided for illustrative purposes to those skilled in the art and are not intended to be limiting in any way. All references to embodiments, examples, aspects, formulations, solutions, etc., are intended to be illustrative and non-limiting.

[0116] It has been found that the reaction (e.g., dissolution) of solid particles in a liquid (slurry) can be surprisingly accelerated by passing the particles in the slurry through a cavitation field, in which the initiation and collapse of cavitation bubbles occur. It has also been surprisingly found that the dissolution rate of electrode metal compounds is not proportional to the power (amplitude) input to the slurry, with higher dissolution rates occurring at a combination of power (W / L) and frequency input to the slurry volume.

[0117] This process can be carried out at near-ambient temperatures and pressures, reducing the energy consumption, thermal management complexity, cost, and risks associated with heating battery components.

[0118] The term "reactor" refers to the reactor described herein. Such reactors may include flow-through cavitation fields. The terms "acoustic processor," "acoustic amplitude transformer," and "ultrasonic probe" are interchangeable and used to describe devices for inducing transient cavitation induced by ultrasonic vibrations.

[0119] The term "cavitation field" refers to the region where transient cavitation is induced by appropriate means. A suitable cavitation field involves the nucleation, growth, oscillation, and collapse of bubbles. Cavitation fields can be generated by ultrasonic agitation.

[0120] The term "acoustic probe" refers to the internal portion of an ultrasonic probe in a reactor (as described herein). An acoustic probe (e.g., an ultrasonic probe) is a vibrating component that causes changes in the pressure field of the flowing liquid, resulting in transient cavitation.

[0121] "Black powder" is a term used to describe intermediate waste (electronic waste) that contains valuable metallic components obtained from spent batteries during mechanical processing such as crushing, grinding, heat treatment, and density separation to produce powdered materials. Black powder can be a mixture of positive electrode materials (such as the secondary particles described herein) and other components used to manufacture the positive electrode (such as electrolytes containing salts (e.g., LiPF6, LiBF4, LiCF3SO3) and organic solvents (e.g., 1,3-dioxane, propylene carbonate-DMF)). It is often difficult to provide a definitive composition of black powder because it can be highly dependent on the source of the battery and the mechanical dismantling process. Lithium metal oxides (LiMeOx) or phosphates are commonly used as positive electrodes covered with metal foils such as aluminum (Al) foil, and negative electrodes are typically composed of copper (Cu) foil coated with a negative electrode material (such as graphite), but may contain other materials such as lithium metal or its alloys, lithium metal oxides (e.g., lithium titanate), and silicon, silicon alloys, and silicon oxides.

[0122] Polymer binders such as polyvinylidene fluoride (PVDF) can be used to bond cathode particles together and adhere them to the foil. PVDF binders can appear on the surface of the black powder particles and hinder their recycling. Typically, LIBs from different types of cathode materials (e.g., NMC) are processed by dry mechanical processing, which consists of two stages of crushing, screening, and magnetic separation. Commercially valuable elements found in black powder are typically transition metals such as Co, Ni, Mn, copper, and iron, as well as Al and Li. Active cathode materials greatly facilitate the economic feasibility of LIB recycling processes and are recovered into so-called black powder in a second stage of recycling after dismantling. Depending on the dismantling and processing steps of the recycling process, black powder may also contain graphite, organic binders, and electrode components.

[0123] In one embodiment, the method includes immersing a metal compound in a leaching solution to form a slurry. The metal compound may be any metal found in the black powder, such as the metal of interest for extraction. The metal compound may be one or more elements found in an electrode (such as a positive or negative electrode). Examples of suitable positive electrode materials may include phosphates, fluorophosphates, fluorosulfates, fluorosilicates, spinels, lithium-rich layered oxides, and composite layered oxides. Further examples of suitable positive electrode materials may include spinel-structured lithium metal oxides, layered lithium metal oxides, lithium-rich layered lithium metal oxides, lithium metal silicates, lithium metal phosphates, metal fluorides, metal oxides, sulfur, metal sulfides, disordered rock salt structures, or any combination thereof. Examples of suitable negative electrode materials may include lithium titanate, graphite, silicon components, and others.

[0124] This method has been found to be particularly suitable for dissolving secondary particles that comprise primary particles that are at least partially sintered together and exhibit some open porosity (common in battery electrode materials). However, this method can also be used for primary particles, and for particles of 5 mm, 2 mm, 1 mm, or 0.5 mm, which can be either primary or secondary particles. Illustratively, this method is particularly suitable for dissolving and extracting from metal compound particles. In one embodiment, the average primary particle size is typically less than 2 micrometers, 1 micrometer, 0.5 micrometers to 5 or 10 nanometers. Typically, the primary particles are substantially less than 500 nm (an average of less than 500 nanometers by volume or number, or an equivalent sphere diameter of less than 500 nanometers with a D90 of less than 500 nanometers). Typically, the average primary particle size is at most 20 micrometers, but typically the average primary particle size is at most about 2 micrometers to 0.1 micrometers. Primary particles can aggregate to form aggregates. Aggregates can be secondary particles, such as those produced by spray drying and already at least partially sintered. Pores typically have the same size range as primary particles, and include open pores, which also contain pores within the same size range as described for primary particles.

[0125] Suitable primary particle diameters can be in the range of 0.01-20 μm or any value therein (optionally rounded to the nearest 0.001), or any subrange such as 0.05-2 μm spanning any two of these values. For example, consider 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045, 0.05, 0.055, 0.06, 0.065, 0.07, 0.075, 0.08, 0.085, 0.09, 0.095, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.2 4, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.7, 0. 71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.8, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1. 18, 1.19, 1.2, 1.21, 1.22, 1.23, 1.24, 1.25, 1.26, 1.27, 1.28, 1.29, 1.3, 1.31, 1.32, 1.33, 1.34, 1.35, 1.36, 1.37, 1.38, 1.39, 1.4, 1.41, 1.42, 1.43, 1.44, 1.45, 1.46, 1.47, 1.48, 1.49, 1.5, 1.51, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.58, 1.59, 1.6, 1.61, 1.62, 1.63, 1.64, 1.Diameters of 65, 1.66, 1.67, 1.68, 1.69, 1.7, 1.71, 1.72, 1.73, 1.74, 1.75, 1.76, 1.77, 1.78, 1.79, 1.8, 1.81, 1.82, 1.83, 1.84, 1.85, 1.86, 1.87, 1.88, 1.89, 1.9, 1.91, 1.92, 1.93, 1.94, 1.95, 1.96, 1.97, 1.98, 1.99, 2 μm, and other values.

[0126] The particle size of the secondary particles can have an average or median particle size (D50) of about 1 micrometer (μm), 2 μm, 5 μm, 10 μm or 20 μm to 150 μm, 100 μm, 75 μm or 50 μm by volume. D50 refers to the particle size (equivalent sphere diameter) in the particle size distribution, in which at least 50% of the particles by volume are smaller than this size.

[0127] Suitable secondary particle diameters can be in the range of 0.1–200 μm or any value between these values ​​(optionally rounded to the nearest 0.001), or span any subrange between any two of these values, such as 0.05–2 μm. For example, consider the following numbers: 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 6 0, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 1 Diameters of 57, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 186, 187, 188, 189, 190, 191, 192, 193, 194, 195, 196, 197, 198, 199, 200 μm, and other values.

[0128] Particle size can be determined by any suitable method, such as those known in the art, including, for example, laser diffraction or image analysis of microscopic images of a sufficient number of particles (about 100 to about 200 particles). A representative laser diffractometer is the Microtrac S3500. Porosity can be determined by any suitable method, such as those known in the art, including, for example, gas adsorption techniques, Archimedes' method, and / or mercury porosimetry.

[0129] Illustratively, the electrode material may be a composite oxide of lithium and at least one metal selected from cobalt (Co), nickel (Ni), and combinations thereof, and more particularly, may be a compound represented by at least one of the following formulas: Li a A 1-b B b D2 (where 0.90≤a<1.8 and 0≤b≤0.5), LiaE 1-b B b O 2-c D c (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05), LiE 2- b B b O 4-c D c (Where, 0≤b≤0.5, 0≤c≤0.05), Li a Ni 1-b-c Co b B c D α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2), Li a Ni l-b-c Co b B c O 2-a F 𝛼 (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2), Li a Ni 1-b-c Co b B c O 2-α F α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2), Li a Ni 1-b-c Mn b B c D α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2), Li a Ni 1-b- c Mn b B c O 2-α F α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2), Li a Ni b E c G dO2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1), Li a Ni b Co c Mn d GeO2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5), Li a NiG b O2 (where 0.90≤a≤1.8, 0.001≤a≤1.8, 0.001≤a≤1.8, 0.90 ... b ≤0.1), Li a CoG b O2 (where 0.90≤a≤1.8, 0.001≤b≤0.1), Li a MnG b O2 (where 0.90≤a≤1.8, 0.001≤b≤0.1), Li a Mn2G b O4 (where 0.90≤a≤1.8, 0.001≤b≤0.1), QO2, QS2, LiQS2, V2O5, LiV2O2, LiIO2, LiNiVO4, Li (3-f) J2(PO4)3 (where 0≤f≤2), Li (3-f) Fe2(PO4)3 (where 0≤f≤2) and LiFePO4.

[0130] In the above formula, A is Ni, Co, manganese (Mn), or a combination thereof; B is aluminum (Al), Ni, Co, Mn, chromium (Cr), iron (Fe), strontium (Sr), vanadium (V), or a combination thereof; D is oxygen (O), fluorine (F), sulfur (S), phosphorus (P), or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, magnesium (Mg), lanthanum (La), cerium (Ce), Sr, V, or a combination thereof; Q is titanium (Ti), molybdenum (Mo), Mn, or a combination thereof; I is Cr, V, Fe, scandium (Sc), yttrium (Y), or a combination thereof; J is V, Cr, Mn, Co, Ni, copper (Cu), or a combination thereof.

[0131] Leaching aids can be any suitable compound used to dissolve or react with metal compounds, such as strong or weak acids, oxidizing agents, or caustic compounds. The use of weak acids in subsequent separation steps has been found to have advantages in separating specific metals. For example, when using a base (such as ammonia or hydroxides) to precipitate the anions of a weak acid instead of a stronger acid (such as acetic acid versus sulfuric acid), more economically valuable compounds (such as sodium acetate versus sodium sulfate) can be recovered. In some cases, basic compounds can be used when dissolving certain compounds (such as those containing silicon). Suitable basic compounds include any compound with a pH above 7.0, such as ammonium, alkali metal, and alkaline earth metal hydroxides.

[0132] A weak acid can be any compound exhibiting a pKa of about 1, 1.5, 2, 2.5, or 3 to 7, 6.5, or 6. For example, a weak acid can have a pKa of about 4.76. It will be understood that pKa is the logarithm of the dissociation constant of an acid in water or a mixture of such compounds. It should also be understood that in some cases, when the polymer contains multiple carboxylic acid groups, the pKa may be difficult to determine, but these are considered herein. A weak acid can be polyfunctional (i.e., with two or more acid groups), but generally includes monofunctional acids. A weak acid can be saturated or unsaturated. A weak acid can be any carboxylic acid, such as naturally occurring carboxylic acids. For example, carboxylic acids can be abietic acid, alginic acid, gallic acid, azelaic acid, caffeic acid, malic acid, pyruvic acid, nicotinic acid, citric acid, biotin, abietic acid, cholic acid resin, pectin, alginic acid, rosin (a mixture of naturally occurring acids), or combinations thereof. Fatty acids can be any fatty acid derived from any animal fat or vegetable oil and can be saturated or unsaturated. Exemplary oils include linseed oil, palm oil, coconut oil, olive oil, tung oil, soybean oil, peanut oil, sunflower oil, cottonseed oil, rapeseed oil, or combinations thereof. Any fatty acid derived from the above oils and fats (e.g., isostearic acid) may be used. In one embodiment, the fatty acid is dimerized to form a dimer acid, trimer acid, or a more advanced polymeric acid. Typically, readily available dimer acids contain small amounts of monomeric acid, trimer acid, and more advanced polymeric acid.

[0133] The weak acid can be any carboxylic acid such as a monocarboxylic acid, a dicarboxylic acid, or a higher (e.g., tri or tetra)carboxylic acid (e.g., ascorbic acid and ethylenediaminetetraacetic acid). Illustratively, the carboxylic acid can have a linear or branched alkane chain having 1, 2, or 5 to 30, 20, or 15 carbons, or mixtures thereof. Examples may include formic acid, acetic acid, butyric acid, valeric acid, hexanoic acid, adipic acid, heptanoic acid, pimelic acid, octanoic acid, octanoic acid, nonanoic acid, azelaic acid, decanoic acid, sebacic acid, 2,3-dimethylbutyric acid, 2,3-dimethylbutanoic acid, 2,3-dimethylsuccinic acid, 2,2-dimethylbutyric acid, 2,2-dimethylsuccinic acid, 3-methylheptanoic acid, 3-methylpimelic acid, or mixtures thereof.

[0134] The weak acid can be a sterically hindered carboxylic acid with a short and highly branched alkyl chemical structure, such as 2,2,3,5-tetramethylhexanoic acid, 2,4-dimethyl-2-isopropylvaleric acid, 2,5-dimethyl-2-ethylhexanoic acid, 2,2-dimethyloctanoic acid, or 2,2-diethylhexanoic acid.

[0135] Weak acids can also be carboxyl-containing compounds such as: polyethers, polyesters, polyether esters, polyamides, conjugated diene polymers or conjugated diene copolymers, polyurethanes, polystyrene, polyolefins, polysiloxanes, or combinations thereof. Weak acids can also be polysaccharides, polypeptides, proteins, phosphoric acid, nitrous acid, sulfurous acid, oxalic acid, chromic acid, hydrofluoric acid, hydrogen sulfide, or combinations of these weak acids or any of the foregoing weak acids.

[0136] The acid can be used undiluted, or preferably in the form of an aqueous solution or a water-polar solvent solution (e.g., an alcohol-water solution). The concentration of the acid in the solution can be any useful concentration sufficient to dissolve the target metal (up to its solubility limit). Illustratively, the acid / water volume ratio can be from 0.1, 0.5, or 1 to 3, 4, 5, or 10.

[0137] In some cases, an acid / water volume ratio of approximately 0.01-20 or any value in between (optionally rounded to the nearest 0.01) or any subrange (such as 1-3) spanning any two of these values ​​can be used. For example, consider the following values: 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5 1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10, and the ratios of other values.

[0138] The solution preferably contains an oxidizing agent such as a peroxide, which may include those formed by mixing a peroxide with a weak acid (described herein) or its corresponding anhydride (e.g., hydrogen peroxide and acetic acid to form peracetic acid). The concentration may be any suitable concentration, such as 1% or 2% to 6%, 8% or 10% by volume.

[0139] In some cases, solutions of approximately 0.01-20% by volume, or any value in between (optionally rounded to the nearest 0.1), or any subrange (e.g., 2-6%) between any two of these values, may be used. For example, consider solutions of 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5, 20%, and other values ​​by volume.

[0140] The slurry contains metal compound particles immersed in the leaching solution. Any commercially viable metal compound particle with a useful solids load can be used. It has been found that dissolution occurs more rapidly when the solids load of the metal compound exceeds the solubility limit of that metal compound in a given leaching solution. Typically, the solids load (grams of solid metal compound per volume of leaching solution (g / L)) can be substantially the same as the solubility limit of the metal compound (g / L), or can be a solids load (g / L) / solubility limit (g / L) ratio of 0.1, 0.25, 0.5, 0.75 to 1.25, 1.5, 1.75, 2, 3, or 5. Illustratively, the solids load can be 0.1%, 1%, 2%, or 5% by volume or weight to any feasible value such as 50%, 33%, 25%, or 20%. Any undissolved metal compound particles can be separated and reintroduced, either alone or with fresh metal compound, to be dissolved with fresh leaching solution (e.g., water, acid, and oxidizing agent).

[0141] In some cases, solid loads of approximately 0.1% to 50% by volume or weight, or any value between these values ​​(optionally rounded to the nearest 0.1), or any subrange (e.g., approximately 0.1% to 20%), can be used. For example, consider solid loads of 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5. 19, 19.5, 20, 20.5, 21, 21.5, 22, 22.5, 23, 23.5, 24, 24.5, 25, 25.5, 26, 26.5, 27, 27.5, 28, 28.5, 29, 29.5, 30, 30.5, 31, 31.5, 32, 32.5, 33, 33.5, 34, 34.5, 35, 35.5 36, 36.5, 37, 37.5, 38, 38.5, 39, 39.5, 40, 40.5, 41, 41.5, 42, 42.5, 43, 43.5, 44, 44.5, 45, 45.5, 46, 46.5, 47, 47.5, 48, 48.5, 49, 49.5, 50, 51, 52, 53, 54, 55, 56, 57 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100%, and other values.

[0142] In this method, as described above, the slurry flows through the cavitation zone as it collapses. The flow is preferably turbulent or includes eddies, such that the metal compound particles can flow through a single cavitation field and / or a series of cavitation fields caused by turbulence / eddies in the flowing slurry more than once. The flow can occur, for example, by any suitable means using any suitable method to allow liquid to flow into the cavitation field. In one embodiment, as described for Example A below, the flow can be caused by the cavitation field itself, wherein a sufficient amount of cavitation causes slurry flow, and the walls of the sealed container are close enough to cause the slurry to flow repeatedly through the cavitation field. Alternatively, as described herein, the flow can be provided by a radial or axial stirring impeller combined with cavitation provided by an ultrasonic probe or other cavitation device immersed in the slurry.

[0143] Preferably, the flow includes allowing slurry to flow into a flow-through reactor, the flow-through reactor including one or more cavitation fields and one or more means for deflecting the slurry into the cavitation fields, wherein the slurry preferably flows sequentially through 2, 3, 4, 5, or 10 or more, up to any feasible number of cavitation fields. Illustratively, the reactor may include: a tube having walls defining an inner diameter, length, and first and second ends, an inlet and an outlet positioned along the length of the tube for allowing fluid to flow through at least a portion of the tube; a cavitation generating means for generating the cavitation fields within the tube; and at least one fluid deflecting means for deflecting the fluid into the cavitation fields. Such a reactor may be referred to as a "tubular reactor".

[0144] In a particular implementation (see, for example, an applicable illustration), Figure 6-10 The cavitation field is provided by an ultrasonic probe, see also, for example, WO2022 / 234502, which is incorporated herein by reference. In these embodiments, fluid deflection is provided at least in part by the diameter of the ultrasonic probe, which varies along its axial length within the reactor tube, wherein the slurry flow is deflected by a contraction between the ultrasonic probe and the reactor wall, resulting in flow deflection into one or more modeled cavitation fields (see...). Figure 6 and Figure 10 The ultrasonic probe is designed to generate a cavitation field with nanoscale bubble formation and collapse.

[0145] In other embodiments, more than one ultrasonic probe with varying diameters may be axially inserted into the cavity of the flow reactor. These multiple ultrasonic probes may vibrate in phase or out of phase. The multiple ultrasonic probes may have varying lengths, with the diameter of each probe varying asynchronously, synchronously (maximum diameter aligned, or out of phase by 180 degrees, with probes meshing together being an example), or in combination thereof along their lengths.

[0146] The at least one deflection device may include a baffle, a protrusion, or other insert into the cavity of the flow-through reactor to cause slurry flow to increase the residence time of particles over the cavitation field. In another embodiment, the cavitation field may be generated by one or more ultrasonic probes perpendicular to the length of the reactor, and one or more protrusions or inserts within the reactor cavity that project radially inward from the inner diameter of the reactor deflect the flow to the wall that generates the cavitation field.

[0147] Any apparatus suitable for imparting cavitation in a slurry can be used, such as those known in the art. However, cavitation must include transient (also known as “inertial”) cavitation. In transient cavitation, nanoscale bubbles form and collapse under varying pressure levels experienced in the slurry. Non-inertial cavitation, such as that occurring in an ultrasonic bath, is insufficient. In non-inertial cavitation, bubbles fluctuate only in size or shape, as in an ultrasonic bath. Ideally, all cavitation is transient. The average cavitation size can be any size suitable for accelerating the leaching of the metal compound, but preferably, the size (equivalent sphere diameter) is within 5, 3, 2, or 1 times the average or maximum bubble size of the cavitation field, which can be determined by any known method, such as that described in Ultrasonics Sonochemistry 108 (2024) 106957. Illustratively, the average cavitation bubble size is within 50% of the average particle size of the metal compound.

[0148] Cavitation can be transient cavitation imparted by ultrasound. A suitable method, preferably using a vibrating probe in direct contact with the slurry, is to ultrasonically form cavitation. The frequency can be any useful frequency, such as from 15 kHz to 100 kHz, and can vary depending on the size of the metal particles. Multiple frequencies can be used in the same reactor, and this method is particularly suitable for metal compounds with different sizes or properties, such as reintroducing metal compound particles previously subjected to one or more cavitation fields into a slurry containing fresh (untreated) metal compound particles.

[0149] In a particular embodiment, electrode metal compound particles that typically have the characteristics described above (e.g., average secondary particle size of 10 to 50 micrometers) are ideally employed with a frequency cavitation field generated at frequencies of 20 kHz, 22 kHz, or 23 kHz to 30 kHz.

[0150] In some cases, frequencies of approximately 20-30 kHz or any value in between (optionally rounded to the nearest 0.1) or any subrange spanning any two of these values ​​(such as 23-30 kHz) can be used. For example, consider frequencies of 20, 20.5, 21, 21.5, 22, 22.5, 23, 23.5, 24, 24.5, 25, 25.5, 26, 26.5, 27, 27.5, 28, 28.5, 29, 29.5, and 30 kHz.

[0151] Surprisingly, the dissolution rate is not proportional to the power input per unit volume of slurry. Even though the bubble collapse intensity increases with increasing power (amplitude), the dissolution rate has shown to be relatively slow. In other words, it has been surprisingly found that the dissolution of metallic compound electrode materials, even when using weak acids, is more efficient at lower power. The power input per unit volume of reactor (W / L) can be any useful power input, but ideally any power input sufficient to accelerate the dissolution rate, and preferably up to 5000 W / L, 2000 W / L, 1000 W / L, or 500 W / L to any feasible value to initiate and sustain transient cavitation; in many cases, 100 W / L is sufficient.

[0152] In some cases, power inputs of approximately 100-5000 W / L or any value in between (optionally rounded to the nearest 0.1) or spanning any subrange between any two of these values ​​can be used. For example, consider power inputs of 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, and 147. 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 178, 179, 180, 181, 182, 183, 184, 185, 186, 187, 188, 189, 190, 191, 192, 193, 194, 195, 196 197, 198, 199, 200, 205, 210, 215, 220, 225, 230, 235, 240, 245, 250, 255, 260, 265, 270, 275, 280, 285, 290, 295, 300, 310, 320, 330, 340, 350, 360, 370, 380, 390, 400, 420, 440, 460, 480, 500, 550, 600, 650, 700, 800, 850, 900, 950, 1000, 11 Power input values ​​of 00, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800, 3900, 4000, 4100, 4200, 4300, 4400, 4500, 4600, 4700, 4800, 4900, 5000 W / L, and other values.

[0153] In one embodiment of a recycling facility employing this method, the leaching unit may begin in a mixing tank that receives black powder and chemicals from an oxidant tank and an acid tank. The slurry obtained from the combination of black powder (solid) and chemicals (liquid) can then be transferred from the mixing tank to a series of ultrasonic devices, such as… Figures 6 to 10 The reactor and ultrasonic probe are depicted in the diagram. After the metal is dissolved, the leachate can then be fed into a centrifuge. The centrifuge may have the capacity to remove the final undissolved solids, i.e., undissolved black powder, graphite, or impurities (which are disposed of or ultimately recycled to a mixing tank for a second (or more) pass through the flow-through reactor). Additional acids, acid solutions, and reducing agents may be added during the process, such as when separating and recovering undissolved metal compounds for further dissolution. In some cases, different solutions may be used in a sequential reactor to selectively dissolve and separate different metals / elements (e.g., preferentially dissolving Li from LFP).

[0154] The distance between the acoustic probe and the inner surface of the reactor wall can be varied, for example, to generate the desired flow in a flow-through reactor and expose the particles to the cavitation field. Ideally, as... Figure 9 As shown, the W / D (wall distance / module depth) ratio is from 0.1 to 15, and preferably from 1 to 15, or from 2 to 15. The distance between the acoustic probe and the slurry inlet can be any useful distance, but is typically at least about 0.1 cm to 50 cm.

[0155] In some cases, W / D ratios of approximately 0.1–20 or any value in between (optionally rounded to the nearest 0.1) or spanning any subrange between any two of these values ​​(such as approximately 2–15) can be used. For example, consider ratios of 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5, 20, and other values.

[0156] In some cases, the distance between the acoustic probe and the slurry inlet can be approximately 0.1 cm to 50 cm or any value in between (optionally rounded to the nearest 0.1) or spans any subrange (such as approximately 2-15) between any two of these values. For example, consider 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5, 20, 20.5, 21, 21.5, 22, 22.5, 23, 23.5, 24, 24.5, 25, 25.5, 2 The distances to 6, 26.5, 27, 27.5, 28, 28.5, 29, 29.5, 30, 30.5, 31, 31.5, 32, 32.5, 33, 33.5, 34, 34.5, 35, 35.5, 36, 36.5, 37, 37.5, 38, 38.5, 39, 39.5, 40, 40.5, 41, 41.5, 42, 42.5, 43, 43.5, 44, 44.5, 45, 45.5, 46, 46.5, 47, 47.5, 48, 48.5, 49, 49.5, 50 cm, and other values.

[0157] The black powder can be introduced into the reactor as a slurry through an inlet that is perpendicularly aligned with one or more modules. In some cases, the slurry travels perpendicular to the module and parallel to the ultrasonic probe.

[0158] Slurries containing metal compounds can be kept at suitable temperatures during dissolution. For example, the slurry can be kept at a temperature below the boiling point of the leaching solution. The slurry can also be kept at ambient temperature.

[0159] Example

[0160] Example A:

[0161] Table 1 shows the metal compounds (NMC-Li) used in the examples. 1.05 Co 0.33 Ni 0.33 Mn 0.33Secondary particle sizes of O2; LCO-LiCoO2 and LFP LiFePO4. The metal compounds were obtained from MSE Supplies™. Particle sizes were specified by the company and also confirmed by scanning electron microscopy (SEM). The porosity of each material is also shown in Table 1, which is the porosity reported by the supplier. Table 2 shows the leaching parameters and results for leaching lithium cobalt oxide (LCO), and Table 3 shows the leaching parameters and results for leaching NMC in Example A, with the amount dissolved determined by gravimetric analysis. Table 4 shows the leaching parameters and results for leaching NMC, where the dissolution was determined by ICP-OES of the leachate. The data obtained in Tables 2 and 3 were determined by gravimetric analysis of the residual solids filtered from the leachate. Table 4 shows the results of leaching NMC using the same method, where the amount of black powder leached was determined by analysis of the leachate.

[0162] Table 1: Secondary particle size and porosity of the metal compounds used in the examples

[0163]

[0164] As shown in Table 2-4, an acoustic amplitude transducer consisting of a piezoelectric generator and an ultrasonic probe (acoustic probe) was used in the presence of an oxidizing agent (hydrogen peroxide 30% v / v, VWR Chemicals) and acetic acid (glacial acetic acid diluted with Milli-Q™ water as described) in an acidic solution (approximately 200 ml, containing black powder (NMC-Li) suspended therein). 1.05 Co 0.33 Ni 0.33 Mn 0.33 Ultrasonication was performed at 20 kHz in a 400 ml borosilicate beaker containing O2 or LCO-LiCoO2 (slurry). The resulting cavitation field engulfed the entire slurry volume and caused significant agitation within the beaker, resulting in repeated flow of the slurry through the cavitation field due to deflection from the beaker wall caused by the small size of the beaker. The average size of the secondary NMC cathode particles prior to any treatment was... Figure 1 The sample is shown to be approximately 10 micrometers in size, with an average primary particle size about an order of magnitude smaller, and at least a portion of the open pores at the surface having a size similar to that of the primary particles. The probe input energy is approximately 2000 W / L. Figure 2 Corresponding to the positive electrode particles after treatment in water (without acid or hydrogen peroxide), reflecting the original particle microstructure and morphology. Figure 1 and Figure 2This has been reproduced from Canciani et al., “On the effect of cavitation on particles in leaching processes: implications to battery recycling.” Environmental Advances 17 (2024): 100570 (which is incorporated herein by reference).

[0165] Figure 3 The particles after treatment according to Run 3 in Table 4 are shown. Characterization techniques may include any suitable techniques known in the art, such as scanning electron microscopy (SEM), energy-dispersive X-ray spectroscopy (EDX), inductively coupled plasma optical emission spectroscopy (ICP-OES), mercury porosimetry, and microscopic image analysis techniques.

[0166] Table 2: Example A (LCO solubility determined by gravimetric analysis):

[0167]

[0168] Table 3: Example A (NMC solubility determined by gravimetric analysis)

[0169]

[0170] Table 4. Example A (LCO solubility determination by ICP-OES)

[0171]

[0172] Figure 4 The leaching efficiency at a solid load of 40 g / L NMC black powder is shown. The efficiency curve shows that the solubility limit of the metal is reached at approximately 35 g / L within about 8 minutes (due to the transient enhancement of ultrasonic-induced cavitation), while similar reports of conventional leaching with acoustic bath assistance at similar black powder, acid, and hydrogen peroxide loads show results below 20% even after 15 or 20 minutes. Figure 4 The “reference” mentioned refers to Xiao et al., Green Chem. 2021, 23, 8519, DOI: 10.1039 / d1gc02693c, which is incorporated herein by reference. Without limitation in any way, the improvement is considered to be attributable to the injection of the leaching solution into the pores of the particles due to: direct exposure to microjets resulting from the implosion of finer cavitation bubbles (transient cavitation) during cavitation initiation and re-exposure caused by agitation from direct insertion of the probe into the slurry, and the particle morphology of the cathode particles (including secondary particles comprising sintered primary oxide particles and pores between primary particles).

[0173] LFP was dissolved for 10 minutes at 100% amplitude, approximately 24 g / L solid load (5.2 g LFP), and 8.6 g / g water / acid for the same manner as described above (A). This method selectively dissolves the more desired Li while dissolving LFP. The dissolution efficiency of Li is greater than 94%, Fe less than 0.5%, and P less than 2.5%, which is desirable in recovering Li and retaining ferric phosphate (which can be directly recycled to form new LFP).

[0174] Example B:

[0175] Pilot-scale ultrasonic flow-through reactor Figures 5 to 10 As shown, the experiment was set up in Figure 5 As shown in the figure, Figure 5 The flow loop through the reservoir and reactor is shown, and the residence time is calculated as the actual treatment time multiplied by the ratio of the treatment volume to the reactor volume. LCO, NMC, and LFP (LiFePO4) electrode metal compounds were tested. Figure 8 The results of computational fluid dynamics simulations of cavitation bubble distribution in a flow-through reactor are also shown. Any suitable software, such as those commercially available and described by P. Guida et al., Chemical Engineering Journal Advances, Vol. 12, November 15, 2022, 100362 (which is incorporated herein by reference), can be used. Operating parameters are shown in Table 5.

[0176] Table 5: Operating parameters of reactor in Example B.

[0177]

[0178] A slurry containing metal compounds (NMC, LCO, or LFP-LiFePO4), as well as acid and hydrogen peroxide, is tangentially inserted, and water is further inserted axially to protect the probe. After passing through the reactor and then through multiple cavitation fields, the slurry is discharged at the top, and the flow is disturbed by an ultrasonic probe, which is thought to (but not limited to) induce eddies, prolonging the exposure time to the initial stage of cavitation bubbles.

[0179] As shown in Table 6, for Example B, the dissolution of LCO and NMC was close to the solubility within a residence time of less than 10 minutes.

[0180] Table 6: Dissolution of LCO, NMC and LFP

[0181]

[0182] Comparative Example 1 and Comparative Example 2

[0183] Comparative Example 1: NMC was leached in a 400 ml beaker using only a magnetic stir bar, with acetic acid concentration of 25% v / v in water and H2O2 concentration of 3% v / v in water, at a loading of approximately 40 g / L. The leaching curve is shown in [the figure]. Figure 11 The image shows a comparison with the leaching of Example AB. Figure 11 Examples A and B in the illustrations all used the same leaching solution and solid load, except that Example B used 30 g / L.

[0184] Comparative Example 2: LFP leaching was carried out in the same manner as described above for Example A, with stirring only using a magnetic stir bar (silent treatment), for 24 hours at a solid load of approximately 24 g / L (5.2 g LFP) and a water / acid ratio of 8.6 g / g. This method also selectively dissolves the more desired Li, but takes more than two orders of magnitude longer.

[0185] Figure 11 The graphs illustrate the leaching efficiencies of different methods. Leaching caused by direct ultrasonic agitation (where the slurry flows through the cavitation field initiation zone) is particularly effective, achieving substantially complete dissolution to the solubility limit of the leachable metal in less than 8 minutes and significantly faster than reported using reactors immersed in an ultrasonic bath. Similarly, it is noted that the power of Example B is substantially less than that of Example A; however, it is surprising that the leaching efficiency was significantly improved by using the reactor of Example B, which is believed (but not limited to) at least in part to be due to the creation of turbulence or eddies within the flow reactor, which causes the slurry particles to be exposed to multiple cavitation fields during the initial bubble generation stage.

[0186] Examples AB dissolve metal oxides much faster, resulting in leaching efficiencies reaching 100% of the solubility limits of weak acid and hydrogen peroxide solutions after only 2 or 8 minutes. This is at least an order of magnitude faster than similar cathode materials reported in the literature (e.g., Xiao et al., Green Chemistry 2021, 23(21), 8519-8532). This much slower rate is likely due to the lack of acoustic cavitation generated by ultrasound or the lack of exposure to the cavitation field at the onset of cavitation.

[0187] The leaching of various metal compounds, particularly electrode metal compounds such as LCO, LFP (lithium iron phosphate), and NMC, has been achieved at a dissolution rate more than an order of magnitude faster than reported in existing technologies. This reduced leaching time leads to several advantages compared to conventional leaching techniques: modularity: the capacity of the recovery system can be expanded by increasing the number of modules rather than developing larger equipment; flexibility: the recovery system has a very limited start-up time, allowing it to operate intermittently based on the amount of metal compound available at a given time; smaller footprint: the system is continuous, requires shorter residence times, and occupies at least 10 times less space than the dissolution rates reported in existing technologies; and lower environmental impact: the process uses mild organic acids, while competitors rely on more hazardous media such as sulfuric acid. Surprisingly, the process is more energy efficient at certain lower power inputs, resulting in cost advantages related to waste treatment and energy management.

[0188] The description provided is merely an illustration of the application of the principles of this disclosure. However, it will be apparent to those skilled in the art that many variations and modifications can be made without departing from the scope of the following claims.

Claims

1. A method comprising: The metal compound is immersed in a leaching solution containing leaching aids to form a slurry; as well as The slurry is flowed through a cavitation field to dissolve at least a portion of the metal compound.

2. The method according to claim 1, wherein, The leachate contains water.

3. The method of claim 1, further comprising adding an additional acid during the method.

4. The method according to claim 1, wherein, Leaching aids include weak acids.

5. The method according to claim 1, wherein, An acid is a carboxylic acid or a peroxyacid of a carboxylic acid.

6. The method according to claim 1, wherein, Provides cavitation field.

7. The method according to claim 1, wherein, The method includes adding an oxidizing agent to the leaching solution.

8. The method according to claim 7, wherein, The oxidizing agent is hydrogen peroxide.

9. The method according to claim 7, wherein, Add approximately 0.5% to approximately 10% vol% of an oxidizing agent to the leaching solution.

10. The method according to claim 1, wherein, The metal compound has an average particle size, the cavitation field has an average cavitation bubble size, and the ratio of the average cavitation bubble size to the average particle size of the metal compound is at most 2.

11. The method according to claim 1, wherein, The slurry is at a temperature below the boiling point of the leaching solution.

12. The method according to claim 1, wherein, Solid metal oxides contain lithium and at least one other metal.

13. The method according to claim 12, wherein, The other metals include one or more of Al and transition metals.

14. The method according to claim 13, wherein, Transition metals include one or more of Co, Mn, and Ni.

15. The method according to claim 1, wherein, The cavitation field is generated by an ultrasonic probe that is at least partially immersed in the slurry.

16. The method according to claim 15, wherein, An ultrasonic probe is installed inside a tubular reactor, which has an inlet and an outlet, a first end and a second end positioned to allow the slurry to flow through the tubular reactor and through the cavitation field generated by the ultrasonic probe.

17. The method according to claim 15, wherein, The length of the ultrasonic probe is axially oriented within the length of the tubular reactor.

18. The method according to claim 15, wherein, An ultrasonic probe has a diameter that varies along its length, thereby inducing a cavitation field at different points along the length of the ultrasonic probe.

19. The method of claim 16, wherein, A tubular reactor includes one or more deflection devices that cause the slurry to be deflected into a cavitation field as it flows through the tubular reactor.

20. The method according to claim 19, wherein, The one or more deflection devices are each independently selected from: protrusions, baffles, and deflectors.

21. The method according to claim 1, wherein, The slurry has a solid load exceeding the solubility limit of the solid in the leaching solution.

22. The method according to claim 15, wherein, There are at least two or more ultrasound probes.

23. The method according to claim 22, wherein, The two or more probes may vibrate in phase or out of phase.

24. The method according to claim 22, wherein, The two or more probes have varying diameters along their length, with the diameter of each probe varying asynchronously, synchronously, or in combination along their length.

25. The method according to claim 1, wherein, The metal compound contains secondary particles with an average particle size of 2 to 100 micrometers, which in turn contain aggregated primary particles with an average size of up to 2 micrometers.

26. The method according to claim 1, wherein, The solid loading of the metal compound in the slurry is 0.1% to 20% by weight.

27. The method according to claim 1, wherein, The slurry flows sequentially through at least two cavitation fields.

28. The method according to claim 16, wherein, The slurry flows through two or more tubular reactors connected in series.

29. The method of claim 1, further comprising separating any undissolved metal oxides.

30. The method according to claim 10, wherein, The average cavitation bubble size / average particle size of the metal compound is at most 1.

5.

31. The method according to claim 1, wherein, The metal compound particles contain open pores with an average pore size, and the average cavitation bubble size is no more than 10 times the average pore size of the metal compound particles.

Citation Information

Patent Citations

  • Reactor configuration for ultrasonically induced cavitation with optimal bubbles distribution

    WO2022234502A1