Methods for recovering rare earth oxides

By using alkali metal or alkaline earth metal borates and oxides of easily oxidizable metals as fluxes, the problems of high flux consumption and large amounts of environmental pollutants in existing technologies are solved, achieving efficient recovery of rare earth oxides and cost reduction.

CN123125352APending Publication Date: 2026-11-17NISSAN MOTOR CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202480091156.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-25
Filing Date
2024-07-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing rare earth oxide recycling methods use a large amount of flux, which increases costs and makes it difficult to reduce the amount of boron, an environmentally controlled substance.

Method used

Using alkali metal or alkaline earth metal borates as fluxes, and adding oxides of easily oxidizable metals during the melting process, a melt of rare earth oxides, borates, and easily oxidizable metals is formed. Rare earth oxides are then recovered through phase separation.

Benefits of technology

It effectively reduces the amount of flux used, lowers recycling costs, improves the recycling efficiency of rare earth oxides, and reduces the use of environmental pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a method for reducing the amount of flux used in a rare earth oxide recovery method that utilizes a boron-containing flux. According to the invention, a rare earth oxide recovery method is provided, which is a method for recovering rare earth oxides from waste containing rare earth elements. The recovery method comprises: a melt preparation step (1) of heating and melting the waste, and at least one borate selected from alkali metal borates and alkaline earth metal borates and / or their precursors to prepare a melt containing at least rare earth oxides, the aforementioned borates, and oxides of easily oxidizable metals; and a separation step (2) of separating a rare earth enriched phase and an Fe-C phase formed by concentrating the rare earth oxides in the aforementioned borates from the melt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for recovering rare earth oxides. More specifically, it relates to a method for recovering rare earth elements in the form of rare earth oxides from waste containing rare earth element-containing materials. Background Technology

[0002] Rare earth elements are used in various products such as phosphors for displays, fluorescent lamps, sensors, permanent magnets, and fuel cells, and are indispensable materials in the manufacture of high-tech equipment such as personal computers, smartphones, and electric vehicles. In recent years, with the widespread adoption of these high-tech devices, the demand for rare earth elements has been increasing. However, the production of rare earth elements is limited, resulting in low output and soaring prices. Therefore, there is a need for the development and improvement of technologies to recover rare earth elements from rare earth-containing materials in discarded high-tech equipment.

[0003] Methods for recovering rare earth elements from rare earth-containing substances include: wet methods, which involve dissolving the target substance in acid or solvent and separating the rare earth elements through solid-liquid separation and solvent extraction; and dry methods, which involve heating and melting the target substance together with a flux to extract rare earth oxides into the flux. Of these methods, wet methods require large quantities of acids and solvents, resulting in the generation of large amounts of waste liquid after treatment. Furthermore, wet methods also suffer from the time-consuming process of dissolving rare earth elements from the target substance into the acid or solvent. On the other hand, dry methods are advantageous because rare earth elements can be easily extracted simply by heating and melting the rare earth-containing substance in the presence of a flux, and the generation of waste liquid can be suppressed.

[0004] Boron compounds such as boron oxide (B₂O₃) and borates are known fluxes used in dry processes. For example, Japanese Patent Application Publication No. 2016-186121 discloses a method for recovering rare earth elements from rare earth-containing substances (a method for recovering rare earth elements in the form of oxides). This method is characterized by adding a melting point depressant, an oxidant, and sodium borate to waste containing rare earth magnets and steel products or semi-finished products, and then melting and separating the rare earth elements into REs. x O y The slag (RE: Nd, Pr, Dy, Tb) and Fe-C phases are recovered together. According to the aforementioned literature, by using sodium borate as a flux, the slag viscosity is reduced compared to existing methods using boron oxide. Therefore, rare earth elements can be recovered more easily and effectively from rare earth-containing materials. Summary of the Invention

[0005] The problem that the invention aims to solve

[0006] However, the recycling methods described in the aforementioned literature have drawbacks: they require a large amount of flux (sodium borate), leading to increased costs (raw material costs and waste disposal costs). Furthermore, boron is an environmentally controlled substance, requiring a reduction in its usage.

[0007] Therefore, the object of the present invention is to provide a method for reducing the amount of flux used in a method for recovering rare earth oxides using a flux containing boron.

[0008] Problem Solving Methods

[0009] The inventors conducted in-depth research to solve the above-mentioned problems. Their findings revealed that by using alkali metal or alkaline earth metal borates as fluxes in the aforementioned dry process and extracting rare earth oxides into the fluxes, the above-mentioned problems can be solved by allowing easily oxidizable metals in the system to coexist in the form of oxides, thus completing this invention.

[0010] That is, one aspect of the rare earth oxide recovery method of the present invention is a method for recovering rare earth oxides from waste containing rare earth element substances. The method comprises: a melt preparation step (1) of heating and melting the waste and at least one borate selected from alkali metal borates and alkaline earth metal borates and / or their precursors to prepare a melt containing at least rare earth oxides, the borates and oxides of easily oxidizable metals; and a separation step (2) of separating the rare earth enriched phase formed by concentrating the rare earth oxides in the borates from the melt and the Fe-C phase. Attached Figure Description

[0011] Figure 1 It is a pseudo-quaternary phase diagram at 1400℃, using Nd2O3 as the rare earth element material, Al2O3 and SiO2 as oxides of easily oxidizable metals, and sodium tetraborate (Na2B4O7) as the borate.

[0012] Figure 2 It is a pseudo-quaternary phase diagram at 1400℃, using RE2O3 (RE: Nd, Pr, Dy, Tb) as the rare earth element-containing material, Al2O3 and SiO2 as oxides of easily oxidizable metals, and sodium tetraborate (Na2B4O7) as the borate. Detailed Implementation

[0013] The embodiments of the present invention will be described below. The technical scope of the present invention should be determined based on the claims, and is not limited to the following. It should be noted that "X~Y" indicating the scope means "X and above and Y and below".

[0014] One aspect of the present invention is a method for recovering rare earth oxides, which is a method for recovering rare earth oxides from waste containing rare earth elements. The recovery method comprises: a melt preparation step (1) of heating and melting the waste, and at least one borate selected from alkali metal borates and alkaline earth metal borates, and / or their precursors, to prepare a melt containing at least rare earth oxides, the aforementioned borates, and oxides of easily oxidizable metals; and a separation step (2) of separating a rare earth-enriched phase, formed by concentrating the rare earth oxides in the aforementioned borates, from the Fe-C phase in the melt. According to this method, the amount of flux used can be reduced in rare earth oxide recovery methods that utilize boron-containing fluxes.

[0015] The following is a detailed explanation of each step in the rare earth oxide recovery method of this approach.

[0016] <Mel preparation process (1)>

[0017] In this step (1), waste containing rare earth elements, and at least one borate selected from alkali metal borates and alkaline earth metal borates, and / or their precursors, are heated and melted. Thus, a melt containing at least rare earth oxides, the aforementioned borates, and oxides of easily oxidizable metals is prepared.

[0018] [Waste]

[0019] Waste containing rare earth elements. Waste can be waste products or semi-finished products containing rare earth elements. As for rare earth element-containing substances, there are no special restrictions as long as they contain one or more of the rare earth elements (i.e., scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium).

[0020] Rare earth element-containing substances can take various forms, including mixtures, compounds, sintered products, alloys, and combinations thereof. Furthermore, rare earth element-containing substances can be included in products that use alloys containing rare earth elements, waste products or semi-finished products, scraps generated during manufacturing processes, defective products, and other waste materials.

[0021] Among rare earth element-containing materials, rare earth magnets rich in rare earth elements are preferred (including sludge generated during their production process). There are no particular restrictions on rare earth magnets as long as they use alloys containing one or more rare earth elements. Specific examples of rare earth magnets include neodymium magnets, samarium-cobalt magnets, praseodymium magnets, and samarium-iron-nitrogen magnets, with neodymium magnets being preferred. Neodymium magnets using rare earth elements (Nd, Pr, Dy, Tb) and other rare metals have been used in the drive systems of electric vehicles (EVs) / hybrid electric vehicles (HEVs) and in electric motors for power generation in environmentally friendly vehicles. Given the supply risk of rare earth elements, and the anticipated increase in demand for environmentally friendly vehicles in countries like Japan and other resource-poor countries, the recycling of rare earth elements from neodymium magnets becomes important. It is preferable to consider aspects that reduce the supply risk of rare earth elements by recycling them from neodymium magnets. Neodymium magnets are generally defined as one of the rare earth magnets with neodymium, iron, and boron as the main components. However, in this specification, neodymium magnets are defined as magnets with R, T, and B as R, T, and B (where R must contain at least one selected from Nd, Pr, Dy, and Tb, T is a transition metal with Fe as an essential component, and B is boron, which can be partially replaced by carbon or nitrogen).

[0022] Regarding products or semi-finished products containing rare-earth magnets, the rare-earth oxide recycling method of the present invention can be applied not only to individual rare-earth magnets but also to forms in which rare-earth magnets are incorporated as components. Examples include electric motors and compressors for air conditioning equipment that incorporate rare-earth magnets as components. Such products or semi-finished products containing rare-earth magnets can retain the original shape of the main parts or be disassembled. Removing rare-earth magnets introduced into electric motors from discarded electric motors is very difficult. In contrast, in the recycling method of this approach, the electric motor itself can be processed without separating the magnets from the discarded motor. Therefore, the recycling of products or semi-finished products containing rare-earth magnets can be easily carried out. Furthermore, it is not necessary to pre-crush the rare-earth magnets. The shape of waste varies depending on the product type. To extract rare-earth magnets, for example, it is necessary to design rare-earth magnet extraction equipment adapted to the shape of the waste, as described in "Neodyne Magnet Recycling in Home Appliance Recycling" (November 29, 2011, China Household Electrical Appliances Association; https: / / www.meti.go.jp / shingikai / sankoshin / sangyo_gijutsu / haikibutsu_recycle / pdf / 016_06_00.pdf). The high cost of this method is one of the main reasons hindering magnet recycling. According to the recycling method described herein, separation and recycling can be achieved by adding at least one borate (flux) selected from alkali metal borates and alkaline earth metal borates to the waste, as well as an easily oxidizable metal (e.g., aluminum, silicon) and / or its oxide, a melting point depressant (e.g., carbon) and / or an oxidant (e.g., iron oxide) as needed, and heating and melting. Therefore, it is not necessary to remove rare earth magnets from the waste, which can be considered a highly economical method.

[0023] Furthermore, in the prior art, when processing rare earth magnets, demagnetization is performed based on heating or the like (for example, see pages 9-11 of "Recycling of Neodymium Magnets in Household Appliance Recycling" above). According to the recycling method of this approach, products or semi-finished products containing undemagnetized rare earth magnets can also be used.

[0024] Furthermore, depending on the product or semi-finished product, various coatings are sometimes applied to the surface of steel materials such as magnetic steel plates and magnets to improve rust resistance and corrosion resistance. From the perspective of rare earth element recovery, coatings are not preferred because they lead to an increase in impurities, and in existing methods they are removed beforehand by grinding or the like. However, according to the recovery method of this approach, the coating can be directly used for recovery without removing it.

[0025] The waste may contain materials other than those containing rare earth elements. Examples of materials other than those containing rare earth elements include steel and copper. That is, according to a preferred embodiment of the invention, the waste further includes at least one or both of steel and copper.

[0026] Steel materials include, for example, steel plates, screws, product shells, chassis, etc., which are mainly composed of iron and are integrated with the product. There are no particular limitations on the iron content. The steel can be magnetic steel, and its composition can also include various elements such as Ni, Cr, Si, and Co. When rare-earth magnets and steel are included, by appropriately adjusting the carbon content relative to the total iron content, it is possible to separate the steel into two phases: a rare-earth enriched phase and an Fe-C phase. Conversely, when steel is not included, for example, if only rare-earth magnets contain iron, by appropriately adjusting the carbon content relative to the iron content in the rare-earth magnets, it is possible to separate the steel into two phases: a rare-earth enriched phase and an Fe-C phase.

[0027] Furthermore, in this method, when the waste contains copper, it is possible to separate it into three phases: a rare earth enriched phase, an Fe-C phase, and a Cu phase. In the prior art, aluminum and silicon are mixed in the Fe-C phase, making it difficult to recover Cu with good efficiency. However, according to the recovery method of this method, the Cu recovery efficiency can be improved. This will be explained in detail in the separation process (2) section described later.

[0028] [Borates and / or their precursors]

[0029] In this recycling method, at least one borate selected from alkali metal borates and alkaline earth metal borates is used as a flux.

[0030] Examples of alkali metal borates and alkaline earth metal borates include: sodium tetraborate (Na2B4O7), lithium tetraborate (Li2B4O7), potassium tetraborate (K2B4O7), rubidium tetraborate (Rb2B4O7), cesium tetraborate (Cs2B4O7), sodium metaborate (NaBO2), lithium metaborate (LiBO2), potassium metaborate (KBO2), rubidium metaborate (RbBO2), cesium metaborate (CsBO2), barium tetraborate (BaB4O7), magnesium tetraborate (MgB4O7), calcium tetraborate (CaB4O7), strontium tetraborate (SrB4O7), magnesium borate (MgB2O4), calcium borate (CaB2O4), strontium borate (SrB2O4), and barium borate (BaB2O4). Among these, alkali metal borates, such as sodium tetraborate (Na₂B₄O₇), can be suitably used. Sodium tetraborate (Na₂B₄O₇) can be obtained at a lower price than B₂O₃, which is used as a flux in existing dry processes as described in the background art, and calcium borate and magnesium borate, which are specifically used in other existing dry processes, thus greatly contributing to the reduction of rare earth oxide recycling costs. Borates containing alkaline earth metals such as magnesium and calcium can also be used in combination with sodium tetraborate (Na₂B₄O₇) (an alkali metal borate). As alkaline earth metal borates, barium tetraborate (BaB₄O₇) and calcium borate (CaB₂O₄) can be suitably used, for example, to contribute to the reduction of rare earth oxide recycling costs. Among these, barium tetraborate (BaB₄O₇) is more preferred for its ability to significantly reduce the recycling costs of rare earth oxides.

[0031] In this recycling method, borate can be replaced, or a precursor that is heated and melted to produce borate can be added in addition to borate. Examples of such precursors include combinations of boric acid (B₂O₃) with alkali metal oxides (Na₂O, Li₂O, K₂O₇, Rb₂O₇, Cs₂O), combinations of boric acid (B₂O₃) with alkaline earth metal oxides (BaO, MgO, CaO, SrO), combinations of boric acid (B₂O₃) with alkali metal hydroxides (NaOH, LiOH, KOH, RbOH, CsOH), combinations of boric acid (B₂O₃) with alkaline earth metal hydroxides (Ba(OH)₂, Mg(OH)₂, Ca(OH)₂, Sr(OH)₂), combinations of boric acid (B₂O₃) with alkali metal carbonates (Na₂CO₃, Li₂CO₃, K₂CO₃, Rb₂CO₃, Cs₂CO₃), and combinations of boric acid (B₂O₃) with alkaline earth metal carbonates (BaCO₃, MgCO₃, CaCO₃, SrCO₃). The amounts of boron source and alkali metal source or alkaline earth metal source can be adjusted appropriately according to the composition of the target borate.

[0032] The amount of borate or its precursor added is sufficient to form a homogeneous melt (liquid phase region) between the rare earth elements contained in the rare earth-containing substance and the oxides of easily oxidizable metals. In other words, the amount of borate added is above the liquidus line in the phase diagram determined by the mass of rare earth oxides in the rare earth-containing substance and the content of oxides of easily oxidizable metals. Here, in this specification, "mass of rare earth oxides in the rare earth-containing substance" refers to the total mass of rare earth oxides when the rare earth elements (e.g., Nd, Pr, Dy, and Tb) contained in the rare earth-containing substance (e.g., rare earth magnets) are oxidized to rare earth oxides (Nd₂O₃, Pr₂O₃, Dy₂O₃, and Tb₂O₃). Furthermore, the content of oxides of easily oxidizable metals refers to the content of each type. For example, in the case where only Al₂O₃ is contained as an oxide of an easily oxidizable metal, the content of oxides of easily oxidizable metals refers to the content of Al₂O₃. In the case of oxides containing Al2O3 and SiO2 as easily oxidizable metals, the content of the easily oxidizable metal oxides refers to the content of Al2O3 and SiO2 respectively.

[0033] The following refers to "the amount above the liquidus line in the phase diagram determined by the mass of rare earth oxides of rare earth-containing substances and the content of oxides of easily oxidizable metals," please refer to... Figure 1 Please provide an explanation. Figure 1 It is a pseudo-quaternary phase diagram at 1400℃, using Nd2O3 as the rare earth element material, Al2O3 and SiO2 as oxides containing easily oxidizable metals, and sodium tetraborate (Na2B4O7) as the borate. Figure 1 The sides of the regular tetrahedron shown represent the concentrations of the four components. For example, in Figure 1 In the tetrahedron shown, the edges with Nd₂O₃ and Na₂B₄O₇ as vertices are studied. The Nd₂O₃:Na₂B₄O₇ composition ratio (mass ratio) at any point A on this edge corresponds to the "distance from point A to the vertex (Na₂B₄O₇): from point A to the vertex (Nd₂O₃)" (lever law). Here, the sides of the equilateral triangle on the left side of the tetrahedron represent the concentrations of Nd₂O₃, Al₂O₃, and SiO₂. A point on the face of this equilateral triangle (e.g., at...) Figure 1 The point X indicated by the middle arrow represents the composition of the three components mentioned above. More specifically, in... Figure 1In the regular tetrahedron shown, the equilateral triangle with Nd2O3, Al2O3, and SiO2 as vertices is studied. The composition ratio (mass ratio) of Nd2O3:Al2O3:SiO2 at point X on this face is equivalent to "the distance from the line segment connecting Al2O3 and SiO2 to the perpendicular line from point X": "the distance from the line segment connecting Nd2O3 and SiO2 to the perpendicular line from point X": "the distance from the line segment connecting Nd2O3 and Al2O3 to the perpendicular line from point X". The composition of the three components is uniquely determined by the amount of Nd2O3, Al2O3, and SiO2 added in this step (1). The straight line drawn from point X to the vertex (Na2B4O7) represents the concentration of the three components and Na2B4O7 when Na2B4O7 is added relative to the composition of the three components shown at point X. This means that the concentration of Na2B4O7 increases as it approaches the vertex (Na2B4O7). If the concentration of Na₂B₄O₇ is increased relative to the composition of the three components shown at point X, then at a certain concentration, the mixture transitions from a solid / liquid phase region to a liquid phase region (the region where a homogeneous melt is formed). The boundary between the solid / liquid phase region and the liquid phase region is called the "liquidity line." At the liquidity line, the liquid phase typically exists in equilibrium with a portion of the solid phase. It should be noted that... Figure 1 In the pseudo-quaternary phase diagram shown, the boundary between the solid / liquid mixing region and the liquid phase region exists in the form of a surface; therefore, this boundary is sometimes referred to as a "liquid phase surface." However, in this specification, regardless of whether the boundary is a line or a surface, the term "liquid phase line" will be used consistently. The content of borate "amount above the liquid phase line" refers to the concentration corresponding to the liquid phase line or the concentration in the liquid phase region. Figure 1 In the case shown, "amount above the liquidus line" is equivalent to the Na2B4O7 concentration represented by the line segment (excluding the vertex (Na2B4O7)) connecting the intersection of the above straight line and the liquidus line (not shown).

[0034] It should be noted that the above explanation of "the amount above the liquidus line in the phase diagram determined by the mass of rare earth oxides and the content of easily oxidizable metal oxides in the rare earth element-containing substance" used a pseudo-quaternary phase diagram. However, even without constructing a phase diagram, this "amount above the liquidus line" can be determined. That is, if the mass of rare earth oxides and the content of easily oxidizable metal oxides in the rare earth element-containing substance that will exist in the system are determined in advance, the borate concentration corresponding to the liquidus line can be experimentally determined by increasing the borate concentration relative to this composition. Therefore, regardless of the composition of the rare earth elements and easily oxidizable metals (oxides) contained in the rare earth element-containing substance, the composition for forming a homogeneous melt can be determined. Thus, this recycling method can also be applied to waste with various elemental compositions.

[0035] [Easily oxidizable metals and / or their oxides]

[0036] In this step (1), in addition to the waste containing rare earth elements and borates and / or their precursors mentioned above, easily oxidizable metals and / or their oxides may also be added. In this specification, "easily oxidizable metal" refers to a metal or half-metal that is more easily oxidized than the oxidizing agents described later (e.g., iron oxide (Fe2O3)). Examples of easily oxidizable metals include aluminum (Al), silicon (Si), titanium (Ti), and zirconium (Zr). Preferably, the easily oxidizable metal is at least one or both of aluminum (Al) and silicon (Si), and more preferably a combination of aluminum (Al) and silicon (Si). Furthermore, these easily oxidizable metals may be added in the form of oxides. Examples of oxides of easily oxidizable metals include aluminum oxide (Al2O3), silicon dioxide (SiO2), titanium oxide (TiO2), and zirconium oxide (ZrO2). Preferably, at least one or both of alumina (Al2O3) and silicon dioxide (SiO2) are used, and more preferably, a combination of alumina (Al2O3) and silicon dioxide (SiO2) is used. It should be noted that if the waste containing rare earth elements contains a sufficient amount of easily oxidizable metals and / or their oxides, no additional addition is necessary. Therefore, according to a preferred embodiment, the waste contains rare earth elements and easily oxidizable metals. According to a more preferred embodiment, the waste contains rare earth elements, aluminum, and silicon.

[0037] Melting point depressant

[0038] Waste materials may contain a large amount of iron. For example, waste electric motors contain a significantly larger amount of iron from the electromagnet steel sheet portion compared to rare-earth magnets. When waste materials contain a large amount of iron, the melting point of iron is as high as 1538°C. Therefore, considering the efficiency of phase separation and the reduction of energy during dissolution, it is preferable to melt the waste in the presence of a melting point depressant. Carbon is preferably used as a melting point depressant. Carbon has the effect of preventing the oxidation of iron and preventing iron from migrating to the rare-earth enriched phase, thus improving separation. Examples of carbon supply sources include using a carbon crucible in a heating furnace (melting furnace); carbon coating the furnace walls; and adding Fe-C alloys such as pig iron, coke, graphite, commercially available carbon-reinforcing materials, plastics, organic matter, etc., as additives to the reaction system. Alternatively, examples include introducing gaseous carbon sources such as carbon dioxide or hydrocarbon gases. Furthermore, as described later, when carbon is used as a melting point depressant, high-purity iron such as electrolytic iron added for the purpose of generating Fe-C alloys is also considered to be a substance included in the melting point depressant. Additionally, as mentioned above, when a heating furnace and its wall are used as a carbon supply source (melting point depressant), carbon material on the surface of the furnace wall dissolves into the melt formed from molten waste, thus becoming an additive in the form of a melting point depressant.

[0039] Additionally, electrolytic iron can be added when melting point depressants are added to waste electromagnetic steel sheets containing rare earth magnets and the sheets are heated to melt. While electrolytic iron is not necessary for melting the electromagnetic steel sheets containing rare earth magnets at temperatures above 1500°C, the addition of carbon as a melting point depressant allows the electrolytic iron to react with the carbon in the melting point depressant to form an Fe-C alloy. Thus, by generating an Fe-C alloy that melts at around 1200°C before the electromagnetic steel sheets are heated to melt, the melting of the electromagnetic steel sheets can be promoted, achieving a molten state in a shorter time and at a lower temperature.

[0040] For the sake of minimizing the melting temperature, the amount of such a melting point depressant added is preferably set near the composition of the eutectic point. When using carbon as a melting point depressant, from the viewpoint of lowering the melting point and anti-oxidation effect, it is preferable to heat and melt in a carbon-saturated state, i.e., a state where no more carbon dissolves into the melt. As a general standard, the amount of melting point depressant added can be set in the range of 5% to 10% by mass relative to the amount of iron in the waste. However, the above range is only the standard when the melting point depressant is added to the reaction system as an additive such as pig iron or Fe-C alloys, coke, graphite, commercially available carbon-reinforcing materials, plastics, organic matter, etc., or when a gaseous carbon source such as carbon dioxide or hydrocarbon gases is introduced. As a melting point depressant, when a carbon crucible or a material obtained by carbon coating the furnace wall is used as a carbon supply source or used in combination, the above range is not limited. However, it should be noted that when a part of these heating furnaces (melting furnaces) is used as a carbon source, the furnace wall needs to be repaired and the crucible replaced regularly, so it is preferable to use other carbon sources.

[0041] [Oxidizing agent]

[0042] In this recycling method, in order to convert the rare earth elements contained in the rare earth element-containing material into rare earth oxides before phase separation, an oxidant for oxidizing the rare earth elements can be added in step (1). Furthermore, in the case of containing easily oxidizable metals (e.g., Al and / or Si), phase separation is performed after converting them into easily oxidizable metal oxides using an oxidant. Here, it is preferable to convert at least 90 mol% or more of the easily oxidizable metals in the system into easily oxidizable metal oxides, more preferably at least 95 mol%, even more preferably at least 99 mol%, and even more preferably at least 100 mol%. By increasing the proportion of oxides, the amount of borate used can be further reduced (in particular, the increase in the amount of borate used, which is described later, can be more effectively suppressed). In addition, the easily oxidizable metals can be recovered with higher efficiency. Oxidants can be added to molten rare earth-containing substances and easily oxidizable metals to provide sufficient oxygen for the oxidation of rare earth elements and easily oxidizable metals. From the viewpoint of improving phase separation and the recovery rate of rare earth oxides, promoting the oxidation of rare earth elements and easily oxidizable metals is preferred.

[0043] Examples of oxidizing agents include oxidizing gases such as air, oxygen, and carbon dioxide, iron oxide, and composite oxides containing iron oxide. Among these, iron oxide is preferred because it not only provides sufficient oxygen for the oxidation of rare earth elements and easily oxidizable metals, but also reduces impurities in the recovered iron.

[0044] Preferably, the amount of iron oxide added is set to a molar ratio of 1.5 to 2.0 times the amount of rare earth elements and easily oxidizable metals in the waste containing rare earth elements (e.g., rare earth magnets). It should be noted that in an inactive atmosphere, without the addition of iron oxide, there is a risk that the added borate may react with the rare earth elements in the magnet and be reduced, thus reducing its function as a flux. Therefore, without the addition of iron oxide, this process (1) is preferably carried out in the presence of oxidizing gases such as air, oxygen, and carbon dioxide.

[0045] In this step (1), as described above, waste containing rare earth elements, and borates and / or their precursors are heated and melted. The preferred heating temperature is 1250°C to 1700°C. If the temperature is above 1250°C, a homogeneous melt (liquid phase region) is easily formed. In addition, from the viewpoint of the durability of the refractory used in the melting furnace for heating and melting, the heating temperature is preferably below 1700°C. Furthermore, from the viewpoint of improving the two-phase separation of the rare earth enriched phase and the Fe-C phase, the heating temperature is more preferably 1400°C to 1600°C. If the temperature is above 1400°C, rare earth element-containing substances (e.g., rare earth magnets) are easily melted. In addition, it is more preferably below 1600°C for the following reasons: the melting point of pure iron is 1535°C; the rare earth enriched phase and the Fe-C phase can be easily separated by density difference through pouring.

[0046] It should be noted that heating to temperatures higher than the aforementioned temperature range is preferable because it would worsen the two-phase separation. However, preheating to a temperature higher than the aforementioned temperature range before maintaining it at that range is effective from the perspective of dissolving rare earth elements mixed into high-melting-point substances such as iron. Therefore, as a temperature change during heating and melting, sometimes the temperature is heated to the aforementioned temperature range suitable for two-phase separation, and then cooled. In addition, in order to form a homogeneous melt, sometimes the temperature is heated to a temperature higher than the aforementioned temperature range more suitable for two-phase separation (e.g., above 1600°C but below 1700°C), then the temperature is lowered and maintained at the aforementioned temperature range more suitable for two-phase separation, and then cooled.

[0047] From the viewpoint of improving phase separation, it is preferable to maintain the melt after heating and melting within the above-mentioned temperature range for 10 minutes or more, and more preferably for 60 minutes or more. However, it should be noted that even if the holding time is too long, it will not produce an effect exceeding the theoretical distribution ratio. Therefore, considering economic factors, it is preferable to set the holding time to 180 minutes or less.

[0048] The preferred heating temperature range is the same as above when the waste further contains copper and is separated into three phases: rare earth enriched phase, Fe-C phase, and Cu phase.

[0049] This process (1) preferably includes the following processes (1a) to (1c) in sequence: Process (1a): The above-mentioned waste containing rare earth elements, aluminum and silicon is heated and melted to obtain melt (1a). Step (1b): The oxidant is brought into contact with the above melt (1a) to obtain melt (1b); Step (1c): The above-mentioned borate and / or its precursor are added to the above melt (1b) to obtain melt (1c).

[0050] Based on these steps (1a) to (1c), melts suitable for phase separation can be prepared with simpler operation.

[0051] The melt obtained in step (1) contains at least rare earth oxides, borates, and oxides of easily oxidizable metals. Here, when the oxides of the easily oxidizable metals are aluminum oxide and silicon dioxide, and the borate is sodium tetraborate (Na₂B₄O₇), the composition of these components is preferably within the following range. That is, according to a preferred embodiment of the invention, relative to the total mass of the rare earth oxides containing rare earth elements, the content of the oxides of easily oxidizable metals, and the content of borates, the proportion of aluminum oxide is 0-31.34% by mass, the proportion of silicon dioxide is 12.71-51.87% by mass, and the proportion of borates is 10.0-70.1% by mass. According to a more preferred embodiment of the invention, relative to the above total, the proportion of aluminum oxide is 0-31.34% by mass, the proportion of silicon dioxide is 17.79-51.87% by mass, and the proportion of borates is 10.0-35.0% by mass. According to a further preferred embodiment of the invention, the proportion of alumina is 0 to 31.34% by mass, the proportion of silicon dioxide is 18.43 to 51.80% by mass, and the proportion of borates is 10.0 to 34.6% by mass, relative to the above total. By adding rare earth element-containing substances, borates or their precursors, and easily oxidizable metals or their oxides in such a manner as to obtain a homogeneous melt, it is easier to obtain.

[0052] Furthermore, the composition is preferably within the following ranges. Specifically, according to a preferred embodiment of the invention, relative to the total mass of rare earth oxides containing rare earth elements, oxides of easily oxidizable metals, and borates, the proportion of aluminum oxide is 4.1 to 10.8% by mass, the proportion of silicon dioxide is 13.2 to 34.5% by mass, and the proportion of borates is 21.5 to 70% by mass. According to a more preferred embodiment of the invention, relative to the above total, the proportion of aluminum oxide is 4.1 to 10.7% by mass, the proportion of silicon dioxide is 13.2 to 34.1% by mass, and the proportion of borates is 22.5 to 70% by mass. According to a further preferred embodiment of the invention, relative to the above total, the proportion of aluminum oxide is 8.4 to 10.7% by mass, the proportion of silicon dioxide is 26.9 to 34.1% by mass, and the proportion of borates is 22.5 to 38.7% by mass. By adding substances containing rare earth elements, borates or their precursors, and easily oxidizable metals or their oxides in a manner that results in such a composition, it is easier to obtain a homogeneous melt.

[0053] Furthermore, according to a preferred embodiment of the present invention, the proportion of alumina content is 5.4 to 14.0% by mass, the proportion of silicon dioxide content is 17.4 to 45.0% by mass, and the proportion of borate content is 22.5 to 70% by mass, relative to the total mass of the rare earth oxide containing rare earth elements, the content of oxides of easily oxidizable metals, and the content of borate. According to a more preferred embodiment of the present invention, the proportion of alumina content is 5.4 to 13.5% by mass, the proportion of silicon dioxide content is 17.4 to 43.5% by mass, and the proportion of borate content is 25.0 to 70% by mass, relative to the total mass of the above-mentioned materials. According to a further preferred embodiment of the present invention, the proportion of alumina content is 13.2 to 13.5% by mass, the proportion of silicon dioxide content is 42.7 to 43.5% by mass, and the proportion of borate content is 25.0 to 26.4% by mass, relative to the total mass of the above-mentioned materials. By adding rare earth elements, borates or their precursors, and easily oxidizable metals or their oxides in such a composition, a homogeneous melt is more easily obtained.

[0054] <Separation Process (2)>

[0055] In this step (2), the rare earth enriched phase, formed by concentrating rare earth elements in borate, and the Fe-C phase are separated from the melt obtained in step (1). In the melt state, the Fe-C phase with a relatively higher density separates to the lower layer, and the rare earth enriched phase with a relatively lower density separates to the upper layer. Here, in addition to the rare earth oxides extracted using borate, the rare earth enriched phase may also contain oxides of easily oxidizable metals (e.g., Al2O3 and / or SiO2). In the recovery method described in the above-mentioned literature, it is stated that "the amount of sodium borate added is such that it reaches 0.5 to 10 times the mass of the rare earth magnet...". If the amount of sodium borate added is expressed as a ratio relative to the "mass of rare earth oxides containing rare earth elements" in this specification, it is stated that "the amount of sodium borate added is such that it reaches 60% by mass of the sum of the amount of sodium borate added and the mass of rare earth oxides containing rare earth elements...". According to the recycling method of this invention, by coexisting the oxides of easily oxidizable metals when extracting rare earth oxides into the flux (borate), a homogeneous melt can be obtained even with a reduced amount of flux compared to existing technologies. It is known that in the composition of Reference Example 7 described later, the content of borate can be reduced to at least 41% by mass relative to the total mass of borate and rare earth oxides containing rare earth elements. Furthermore, it is known that in the composition of Reference Example 16 described later, the content of borate can be reduced to at least 54.7% by mass relative to the total mass of borate and rare earth oxides containing rare earth elements. In addition, the inventors have found through research that, depending on the type of waste, sometimes a larger amount of borate is needed than the amount of borate expected to be required to obtain a homogeneous melt based on the mass of rare earth oxides. This phenomenon can be attributed to the following reason: when the waste contains easily oxidizable metals, the borate is reduced by the easily oxidizable metals, thus reducing its function as a flux. According to the recycling method described herein, by converting easily oxidizable metals into oxide forms, the functional degradation caused by the reduction of borates can be suppressed, thus reducing the amount of borates used. Therefore, in these respects, the recycling method described herein has advantages over existing technologies.

[0056] By separating the rare earth enriched phase and the Fe-C phase during their liquid phase state after their formation, the phases can be separated and recovered. According to this recovery method, by using borate as a flux, the rare earth enriched phase becomes low in viscosity, thus allowing it to be easily separated by pouring it from the top of the furnace.

[0057] Another method for separating the liquids is to discharge them sequentially from the bottom of the furnace starting with the densest phase. Alternatively, the melt can be cooled and solidified, then cut along the phase boundaries using a cutting machine or similar device. During cooling, to improve separability, slow cooling until solidification is preferred, but rapid cooling to solidify is also possible.

[0058] When the waste contains copper, the melt is separated into three phases: a rare earth enriched phase, an Fe-C phase, and a Cu phase. Specifically, according to a preferred embodiment of the invention, the waste further contains copper, and in the separation step (2), the rare earth enriched phase, the Fe-C phase, and the Cu phase, formed by concentrating rare earth elements in borate, are separated from the melt. When the melt contains copper, it is separated into a rare earth enriched phase (upper layer), an Fe-C phase (middle layer), and a Cu phase (lower layer) in order of increasing density. Similar to two-phase separation, these phases can be removed by any of the following methods: pouring, draining from the bottom of the furnace, or solidifying and cutting. In the case where aluminum and silicon are not converted into oxides as in the prior art, the Fe-C phase contains aluminum and silicon, thus sometimes making the separation of the Fe-C phase and the Cu phase difficult. According to the recycling method of this embodiment, by converting easily oxidizable metals into oxides, the rare earth enriched phase contains oxides of easily oxidizable metals. As a result, the Fe-C phase contains almost no easily oxidizable metals, thus achieving good phase separation between the Fe-C and Cu phases, enabling efficient Cu recovery. Therefore, this recovery method offers advantages over existing technologies.

[0059] The rare earth enriched phase (rare earth enrichment) separated in separation step (2) comprises rare earth oxides, oxides of easily oxidizable metals, and borates. That is, according to another aspect of the invention, a rare earth enrichment is provided that comprises rare earth oxides, oxides of easily oxidizable metals, and at least one borate selected from alkali metal borates and alkaline earth metal borates. According to the rare earth oxide recovery method of the invention, by allowing the easily oxidizable metals in the system to coexist in the form of oxides when the rare earth oxides are extracted into the flux (borate), the amount of flux (borate) used can be reduced. Therefore, the rare earth enrichment obtained by the recovery method of the invention, compared with the rare earth enrichment obtained by conventional recovery methods, has the characteristics of containing oxides of easily oxidizable metals and a reduced borate content. By reducing the borate content in the rare earth enrichment, boron in the waste liquid discharged when recovering rare earth element oxides from the rare earth enrichment can be reduced in the following steps (3a) to (3c). The proportions (mass %) of rare earth oxides, oxides of easily oxidizable metals, and borates contained in the rare earth concentrate can be substantially the same (within ±10%) as the respective proportions (mass %) of these components in the melt during melt preparation step (1). That is, according to a preferred embodiment of the present invention, relative to the sum of the contents of rare earth oxides, oxides of easily oxidizable metals, and borates in the rare earth concentrate, the proportion of alumina is 0-31.34% by mass, the proportion of silicon dioxide is 12.71-51.87% by mass, and the proportion of borates is 10.0-70.1% by mass. According to a more preferred embodiment of the present invention, relative to the above sum, the proportion of alumina is 0-31.34% by mass, the proportion of silicon dioxide is 17.79-51.87% by mass, and the proportion of borates is 10.0-35.0% by mass. According to a further preferred embodiment of the present invention, the proportion of alumina content is 0 to 31.34% by mass, the proportion of silicon dioxide content is 18.43 to 51.80% by mass, and the proportion of borate content is 10.0 to 34.6% by mass, relative to the above total.

[0060] <Processes (3a)~(3c)>

[0061] In this recovery method, after the separation step (2) described above, there may be further steps (3a) to (3c) for recovering rare earth oxides from the rare earth enriched phase. That is, according to a preferred embodiment of the present invention, after the separation step (2) described above, the following steps (3a) to (3c) are performed sequentially: Step (3a): The rare earth enriched phase obtained in step (2) is leached with acid to obtain a rare earth element leachate; Step (3b): The rare earth elements in the above rare earth element leachate are precipitated in the form of salt to obtain a precipitate; Step (3c): The above precipitate is heated to recover rare earth elements in the form of oxides.

[0062] Examples of acids used in the leaching process of step (3a) include oxalic acid, hydrochloric acid, and sulfuric acid. After the rare earth elements are dissolved by acid leaching in step (3a), an alkali (e.g., ammonium hydroxide, ammonium sulfate, sodium hydroxide) is added in step (3b) to adjust the pH (e.g., pH 2), thereby causing the precipitate (salts of rare earth elements) to precipitate. At this time, the components derived from borate remain dissolved in the leachate, and therefore, the precipitate (salts of rare earth elements) can be recovered by solid-liquid separation. Then, in step (3c), the precipitate (salts of rare earth elements) is calcined at 600°C to 1000°C for 30 to 90 minutes, thereby recovering it in the form of rare earth oxides.

[0063] In addition, in the recycling method of this method, the obtained rare earth oxides can also be recycled by using known methods such as molten salt electrolysis (molten salt reduction method) and Ca reduction method (calcium reduction method), which are existing methods for reducing oxides to metals, after steps (3a) to (3c), to reduce the rare earth oxides to elemental rare earth elements.

[0064] It should be noted that the following embodiments are also included within the scope of the present invention: the recycling method of claim 1 having the features of claim 2; the recycling method of claim 1 or 2 having the features of claim 3; the recycling method of any one of claims 1 to 3 having the features of claim 4; the recycling method of any one of claims 1 to 4 having the features of claim 5; the recycling method of any one of claims 1 to 5 having the features of claim 6; the recycling method of any one of claims 1 to 6 having the features of claim 7; the recycling method of claim 4 having the features of claim 8; the recycling method of claim 8 having the features of claim 9; the recycling method of claim 9 having the features of claim 10; the recycling method of any one of claims 1 to 10 having the features of claim 11; the recycling method of any one of claims 1 to 11 having the features of claim 12; and the rare earth enrichment of claim 13 having the features of claim 14.

[0065] Example

[0066] The present invention will now be described in more detail through embodiments. However, the scope of the present invention is not limited to the following embodiments.

[0067] <Confirmation of the liquidus line>

[0068] [Reference Example 1]

[0069] A mixture of 0.127 g of Nd₂O₃ (99.9% by mass), 0.7 g of Na₂B₄O₇, 0.041 g of Al₂O₃, and 0.132 g of SiO₂ was used as the sample for this reference example. It should be noted that the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ was Nd₂O₃:Al₂O₃:SiO₂ = 42.3:13.7:44.0. The sample was inserted into an iron crucible with an inner diameter of 8 mm, a thickness of 1 mm, and a height of 50 mm, and heated in a Kanthal furnace at 1400 °C in air for 24 hours. The sample was then quenched by water cooling after the given time. The quenched sample was subjected to microstructural observation using optical microscopy and scanning electron microscopy (SEM), and phase identification using X-ray diffraction (XRD). Based on these results, the solubility of Nd₂O₃ by the Na₂B₄O₇ flux was investigated. As a result, in the sample after quenching, only the homogeneous melt that had been cooled and vitrified was observed, thus confirming that the sample of this reference example generated a homogeneous melt at high temperature.

[0070] [Reference Example 10]

[0071] A mixture of 0.072 g of Nd₂O₃ (99.9% by mass), 0.7 g of Na₂B₄O₇, 0.054 g of Al₂O₃, and 0.174 g of SiO₂ was used as the sample for this reference example. It should be noted that the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ was Nd₂O₃:Al₂O₃:SiO₂ = 24.0:18.0:58.0. The sample was inserted into an iron crucible with an inner diameter of 8 mm, a thickness of 1 mm, and a height of 50 mm, and heated in a Kanthal furnace at 1400 °C in air for 24 hours. The sample was then quenched by water cooling after the given holding time. The quenched sample was subjected to microstructural observation using optical microscopy and scanning electron microscopy (SEM), and phase identification using X-ray diffraction (XRD). Based on these results, the solubility of Nd₂O₃ by the Na₂B₄O₇ flux was investigated. As a result, in the sample after quenching, only the homogeneous melt that had been cooled and vitrified was observed, thus confirming that the sample of this reference example generated a homogeneous melt at high temperature.

[0072] [Refer to Examples 2-9, 11-16, and compare with Examples 1-7]

[0073] Nd₂O₃, Na₂B₄O₇, Al₂O₃, and SiO₂ with a purity of 99.9% by mass were weighed and mixed as samples for each example, as shown in Table 1 below. It should be noted that in Reference Examples 2-9 and Comparative Reference Examples 1-5, the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ was approximately the same as that in Reference Example 1 (error ±0.1% by mass). Furthermore, in Reference Examples 11-16 and Comparative Reference Example 7, the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ was approximately the same as that in Reference Example 10 (error ±0.1% by mass). The sample was inserted into an iron crucible with an inner diameter of 8 mm, a thickness of 1 mm, and a height of 50 mm, and heated in an air atmosphere at 1350°C or 1400°C (refer to Table 1) for 24 hours using a Kanthal furnace. The sample was then quenched by water cooling after the given holding time. For the quenched samples, microstructure observation was performed using optical microscopy and SEM, and phase identification was performed using XRD. Based on these results, the solubility of Nd2O3 by the Na2B4O7 flux was investigated. Furthermore, based on whether only a homogeneous melt was observed to have vitrified upon cooling in the quenched samples, it was determined whether a homogeneous melt was formed at high temperature or a mixture of liquid and solid phases was achieved.

[0074] The results are shown in Table 1 below. In Table 1, "L" indicates that a homogeneous melt was formed, and "L+S" indicates that the liquid and solid phases were mixed.

[0075]

[0076] According to the results shown in Table 1, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 42.3:13.7:44.0, and the melt temperature is 1400°C, a liquidus exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 20.0% by mass and less than 22.5% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 22.5% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 41% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 1-7 and Comparative Reference Examples 1-5 are equivalent to... Figure 1 The composition of the line segment connecting point X and vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0077] Furthermore, according to the results shown in Table 1, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 24.0:18.0:58.0, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 20.0% by mass and less than 22.5% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 22.5% by mass (the mass ratio of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 54.7% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 10-16 and Comparative Reference Example 7 are equivalent to... Figure 1 The composition of the line segment connecting point Y and vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0078] [Refer to Examples 17-69, and compare with Examples 8-15]

[0079] Nd₂O₃, Na₂B₄O₇, Al₂O₃, and SiO₂ with a purity of 99.9% by mass were weighed and mixed as samples for each example, as shown in Tables 2-9 below. The samples were inserted into an iron crucible with an inner diameter of 8 mm, a thickness of 1 mm, and a height of 50 mm, and heated in a Kanthal furnace at 1400 °C in air for 24 hours. The samples were then quenched by water cooling after the given time. The quenched samples were subjected to microstructural observation using optical microscopy and SEM, and phase identification using XRD. Based on these results, the solubility of Nd₂O₃ by the Na₂B₄O₇ flux was investigated. Furthermore, based on whether a homogeneous melt was observed to have vitrified upon cooling in the quenched samples, it was determined whether a homogeneous melt was formed at high temperature or a mixture of liquid and solid phases was achieved.

[0080] The results are shown in Tables 2-9 below. In Tables 2-9, "L" indicates that a homogeneous melt was formed, and "L+S" indicates that the liquid and solid phases were mixed.

[0081]

[0082] According to the results shown in Table 2, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 22.7:18.4:58.9 (error ±0.1) and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 20.0% by mass and less than 22.5% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 22.5% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 56.1% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 17-24 and Comparative Reference Example 8 are equivalent to... Figure 2 The composition of the line segment connecting the node Z and the vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0083]

[0084] According to the results shown in Table 3, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 31.4:43.2:25.4, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 26.00% by mass and less than 27.50% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 27.50% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 54.7% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 25-28 and Comparative Reference Example 9 are equivalent to... Figure 2 The composition of the line segment connecting the node V and the vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0085]

[0086] According to the results shown in Table 4, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 20.6:36.6:42.8, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 17.50% by mass and less than 20.00% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 20.00% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 54.8% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 29-34 and Comparative Reference Example 10 are equivalent to... Figure 2 The composition of the line segment connecting the node W and the vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0087]

[0088] According to the results shown in Table 5, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 50.0:0.0:50.0, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 10.00% by mass and less than 12.50% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 12.50% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 22.22% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 35-38 and Comparative Reference Example 11 are equivalent to... Figure 2 The composition of the line segment connecting point Q and vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0089]

[0090] According to the results shown in Table 6, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 37.2:28.8:34.0, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 10.00% by mass and less than 12.50% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 12.50% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 27.8% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 39-47 and Comparative Reference Example 12 are equivalent to... Figure 2 The composition of the line segment connecting the node R and the vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0091]

[0092] According to the results shown in Table 7, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 22.8:26.0:51.2, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 12.50% by mass and less than 15.00% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 15.00% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 43.6% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 48-52 and Comparative Reference Example 13 are equivalent to... Figure 2 The composition of the line segment connecting point S and vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0093]

[0094] According to the results shown in Table 8, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 46.7:11.1:42.2, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 10.00% by mass and less than 12.50% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 12.50% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 23.4% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 53-60 and Comparative Reference Example 14 are equivalent to... Figure 2 The composition of the line segment connecting the node T and the vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0095]

[0096] According to the results shown in Table 9, when the mass ratio of Nd₂O₃, Al₂O₃, and SiO₂ is Nd₂O₃:Al₂O₃:SiO₂ = 26.8:15.5:57.6, and the melt temperature is 1400°C, a liquidus line exists in the range where the proportion of Na₂B₄O₇ relative to the total mass of Na₂B₄O₇, Nd₂O₃, Al₂O₃, and SiO₂ is greater than 7.50% by mass and less than 10.00% by mass. This confirms that if the proportion of Na₂B₄O₇ in this composition is at least 10.00% by mass (the mass of Na₂B₄O₇ relative to the total mass of Nd₂O₃ and Na₂B₄O₇ is at least 29.3% by mass), a homogeneous melt is generated. It should be noted that the compositions in Reference Examples 61-69 and Comparative Reference Example 15 are equivalent to... Figure 2 The composition of the line segment connecting point U and vertex (Na2B4O7) in the pseudo-quaternary phase diagram shown.

[0097] <Recovery of Rare Earth Oxides>

[0098] [Example 1-1]

[0099] A 15.1 kg rotor containing waste materials including rare earth elements and steel, along with 2000 g of pig iron (as a melting point lowering agent) and 920 g of carbon-reducing material, was added to a graphite silicon carbide crucible (Phenix) manufactured by Nippon Crucible Co., Ltd. (model: CD 100HP, maximum throughput per batch: 100 kg). The mixture was then heated using a high-frequency induction furnace. It should be noted that 1771 g of neodymium magnets (magnet 1), containing rare earth elements, were inserted into the rotor. The composition of neodymium magnets was Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 1.0 wt%, and Fe: 70.2 wt%. Additionally, the rotor contained 290 g of silicon and 103 g of aluminum. After heating to 1440℃ to melt it, 1980g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 746g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0100] After holding for 30 minutes, RE, which serves as the rare earth enriched phase, is removed from the crucible by pouring. x O y The Na2B4O7 slag (RE: Nd, Pr, Dy, and Tb) and molten Fe-C phase were naturally cooled. It should be noted that the composition of the neodymium magnet (magnet 1) was determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). The amounts of rare earth oxides (considered as the total mass of Nd2O3, Pr2O3, Dy2O3, and Tb2O3 contained in magnet 1 when oxidized to Nd2O3, Pr2O3, Dy2O3, and Tb2O3), oxides of easily oxidizable metals (SiO2 and Al2O3), and borate (Na2B4O7) in this embodiment are shown in Table 10 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 1-7 and Comparative Reference Examples 1-5, with a rare earth oxide mass: Al2O3: SiO2 ratio of 42.2:13.8:44.0. The content of borates relative to the total mass of borates and rare earth oxides is 55.6% by mass.

[0101]

[0102] The compositional analysis results of the recovered Fe-C phase are shown in Table 11 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.03% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0103]

[0104] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 12 below. The total amount of rare earth oxides in the powder relative to the total mass of the powder was 98.5% by mass. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0105]

[0106] [Examples 1-2]

[0107] A 15.1 kg rotor containing waste materials including rare earth elements and steel, along with 811.9 g of carbon-adding material, was added to a graphite silicon carbide crucible (Phenix) manufactured by Nippon Crucible Co., Ltd. (model: CD 100HP, maximum throughput per batch: 100 kg). Heating was performed using a high-frequency induction furnace. It should be noted that 1771 g of neodymium magnets (magnet 1), containing rare earth elements, were inserted into the rotor. The composition of neodymium magnets was Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 0.95 wt%, and Fe: 70.15 wt%. Additionally, the rotor contained 290.1 ​​g of silicon and 102.9 g of aluminum. After heating to 1400℃ to melt it, 1810g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 470.5g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0108] After holding for 30 minutes, RE, which serves as the rare earth enriched phase, is removed from the crucible by pouring. x O y -Na2B4O7 slag (RE: Nd, Pr, Dy, and Tb) and molten Fe-C phase were naturally cooled. It should be noted that the composition of the neodymium magnet (magnet 1) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The amounts of rare earth oxides (considered as the total mass of Nd2O3, Pr2O3, Dy2O3, and Tb2O3 contained in magnet 1 when oxidized to Nd2O3, Pr2O3, Dy2O3, and Tb2O3), oxides of easily oxidizable metals (SiO2 and Al2O3), and borate (Na2B4O7) in this embodiment are shown in Table 13 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 1-7 and Comparative Reference Examples 1-5, with a rare earth oxide mass:Al2O3:SiO2 ratio of 42.3:13.8:44. The content of borates relative to the total mass of borates and rare earth oxides is 40.7% by mass.

[0109]

[0110] The compositional analysis results of the recovered Fe-C phase are shown in Table 14 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0111]

[0112] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 15 below. The total amount of rare earth oxides in the powder relative to the total mass of the powder was 97.9% by mass. The composition of the powder was determined by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry).

[0113]

[0114] [Example 2]

[0115] A graphite crucible (model: NO.8, maximum throughput per batch: 8 kg) manufactured by Nippon Crucible Co., Ltd. was filled with 945.8 g of rotor and 1219.5 g of stator, which consisted of waste materials containing rare earth elements, steel, and copper; 93.6 g of carbon-reinforcing material as a melting point lowering agent; and 1248.2 g of copper to promote phase separation. The crucible was then heated using a high-frequency induction furnace. It should be noted that 110.7 g of neodymium magnet (magnet 1), which contained rare earth elements, was inserted into the rotor. Its composition was Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 0.95 wt%, and Fe: 70.15 wt%. Furthermore, the rotor and stator together contained 42.0 g of silicon, 14.9 g of aluminum, and 323.8 g of copper. After heating to 1400℃ to melt it, 229g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 45.1g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0116] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y-Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb), Fe-C phase, and Cu phase. It should be noted that the composition of the neodymium magnet (magnet 1) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 1 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3), and the amount of borate (Na2B4O7) are shown in Table 16 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 10-16 and Comparative Reference Example 7, with a rare earth oxide mass:Al2O3:SiO2 ratio of 24:18.1:57.9. The content of borates relative to the total mass of borates and rare earth oxides is 54.7% by mass.

[0117]

[0118] The compositional analysis results of the recovered Fe-C phase are shown in Table 17 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0119]

[0120] The compositional analysis results of the recovered Cu phase are shown in Table 18 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Cu phase was 0% by mass relative to the total mass of the Cu phase. Since the Cu phase contains almost no rare earth elements, it can be considered that the rare earth components in the neodymium magnet were transferred to the slag phase (rare earth enriched phase). The composition of the Cu phase was determined by ICP-AES.

[0121]

[0122] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 19 below. The total amount of rare earth oxides in the powder was 98.8% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0123]

[0124] [Example 3]

[0125] A graphite crucible (model: NO.8, maximum throughput per batch: 8 kg) manufactured by Nippon Crucible Co., Ltd. was filled with 945.8 g of a rotor containing rare earth elements, steel, and copper, 50.7 g of carbonizing material as a melting point lowering agent, and 676.7 g of copper to promote phase separation. The crucible was then heated using a high-frequency induction furnace. It should be noted that 110.7 g of neodymium magnet (magnet 1), containing rare earth elements, was inserted into the rotor. Its composition is: Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 0.95 wt%, Fe: 70.15 wt%. Furthermore, the rotor and stator together contain 18.1 g of silicon, 6.4 g of aluminum, and 0.0 g of copper. After heating to 1400℃ to melt it, 113g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 25.6g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0126] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y-Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb), Fe-C phase, and Cu phase. It should be noted that the composition of the neodymium magnet (magnet 1) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 1 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3), and the amount of borate (Na2B4O7) are shown in Table 20 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 1-7 and Comparative Reference Examples 1-5, with a rare earth oxide mass:Al2O3:SiO2 ratio of 42.3:13.8:44. The content of borates relative to the total mass of borates and rare earth oxides is 40.7% by mass.

[0127]

[0128] The compositional analysis results of the recovered Fe-C phase are shown in Table 21 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase was 0% by mass relative to the total mass of the Fe-C phase. Since the Fe-C phase contains almost no rare earth elements, it can be considered that the rare earth components in the neodymium magnet were transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0129]

[0130] The compositional analysis results of the recovered Cu phase are shown in Table 22 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Cu phase was 0% by mass relative to the total mass of the Cu phase. Since the Cu phase contains almost no rare earth elements, it can be considered that the rare earth components in the neodymium magnet were transferred to the slag phase (rare earth enriched phase). The composition of the Cu phase was determined by ICP-AES.

[0131]

[0132] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 23 below. The total amount of rare earth oxides in the powder was 99.3% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry).

[0133]

[0134] [Example 4]

[0135] A graphite crucible (model: NO.8, maximum throughput per batch: 8 kg) manufactured by Nippon Crucible Co., Ltd. was filled with 945.8 g of rotor and 1219.5 g of stator, which consisted of waste materials containing rare earth elements, steel, and copper; 99.3 g of carbonizing material as a melting point lowering agent; and 1324.6 g of copper to promote phase separation. The crucible was then heated using a high-frequency induction furnace. It should be noted that 110.7 g of neodymium magnet (magnet 1), which contained rare earth elements, was inserted into the rotor. Its composition was Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 0.95 wt%, and Fe: 70.15 wt%. Furthermore, the rotor and stator together contained 45.2 g of silicon, 16.0 g of aluminum, and 323.8 g of copper. After heating to 1400℃ to melt it, 244g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 47.7g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0136] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y-Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb), Fe-C phase, and Cu phase. It should be noted that the composition of the neodymium magnet (magnet 1) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 1 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3), and the amount of borate (Na2B4O7) are shown in Table 24 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 17-24 and Comparative Reference Example 8, with the rare earth oxide mass: Al2O3: SiO2 ratio being 22.7:18.4:58.9. The content of borates relative to the total mass of borates and rare earth oxides is 56.1% by mass.

[0137]

[0138] The compositional analysis results of the recovered Fe-C phase are shown in Table 25 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.02% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0139]

[0140] The compositional analysis results of the recovered Cu phase are shown in Table 26 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Cu phase relative to the total mass of the Cu phase is 0.05% by mass. The Cu phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Cu phase was determined by ICP-AES.

[0141]

[0142] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 27 below. The total amount of rare earth oxides in the powder was 98.9% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry).

[0143]

[0144] [Example 5]

[0145] A 12kg rotor containing waste materials including rare earth elements and steel, along with 623.1g of carbon-adding material, was added to a graphite silicon carbide crucible (Phenix) manufactured by Nippon Crucible Co., Ltd. (model: CD 100HP, maximum throughput per batch: 100kg). Heating was performed using a high-frequency induction furnace. It should be noted that 1645g of neodymium magnets (magnet 2), containing rare earth elements, were inserted into the rotor. The composition of neodymium magnets was Nd: 29.2 wt%, Pr: 0.0 wt%, Dy: 1.6 wt%, Tb: 0.5 wt%, B: 0.95 wt%, and Fe: 67.75 wt%. Additionally, the rotor contained 227.4g of silicon and 80.7g of aluminum. After heating to 1400℃ to melt it, 1499g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 725.7g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0146] After holding for 30 minutes, RE, which serves as the rare earth enriched phase, is removed from the crucible by pouring. x O yThe Na2B4O7 slag (RE: Nd, Pr, Dy, and Tb) and molten Fe-C phase were naturally cooled. It should be noted that the composition of the neodymium magnet (magnet 2) was determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). The amounts of rare earth oxides (considered as the total mass of Nd2O3, Pr2O3, Dy2O3, and Tb2O3 contained in magnet 2 when oxidized to Nd2O3, Pr2O3, Dy2O3, and Tb2O3), oxides of easily oxidizable metals (SiO2 and Al2O3), and borate (Na2B4O7) in this embodiment are shown in Table 28 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 25-28 and Comparative Reference Example 9, with a rare earth oxide mass: Al2O3: SiO2 ratio of 31.4:43.2:25.4. The content of borates relative to the total mass of borates and rare earth oxides is 54.7% by mass.

[0147]

[0148] The compositional analysis results of the recovered Fe-C phase are shown in Table 29 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.02% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0149]

[0150] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and kept at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 30 below. The total amount of rare earth oxides in the powder relative to the total mass of the powder was 99.1% by mass. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0151]

[0152] [Example 6]

[0153] A graphite crucible (model: NO.8, maximum throughput per batch: 8 kg) manufactured by Nippon Crucible Co., Ltd. was filled with 751.6 g of rotor and 1029.9 g of stator, which consisted of waste materials containing rare earth elements, steel, and copper; 78.8 g of carbonizing material as a melting point lowering agent; and 1051.1 g of copper to promote phase separation. The crucible was then heated using a high-frequency induction furnace. It should be noted that 102.8 g of neodymium magnet (magnet 2), which contained rare earth elements, was inserted into the rotor. Its composition was Nd: 29.2 wt%, Pr: 0.0 wt%, Dy: 1.6 wt%, Tb: 0.5 wt%, B: 0.95 wt%, and Fe: 67.75 wt%. Furthermore, the rotor and stator together contained 36.4 g of silicon, 12.9 g of aluminum, and 288.1 g of copper. After heating to 1400℃ to melt it, 201g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 45.5g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0154] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y -Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb), Fe-C phase, and Cu phase. It should be noted that the composition of the neodymium magnet (magnet 2) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 2 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3), and the amount of borate (Na2B4O7) are shown in Table 31 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 29-34 and Comparative Reference Example 10, with a rare earth oxide mass:Al2O3:SiO2 ratio of 20.6:36.6:42.8. The content of borates relative to the total mass of borates and rare earth oxides is 54.8% by mass.

[0155]

[0156] The compositional analysis results of the recovered Fe-C phase are shown in Table 32 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0157]

[0158] The compositional analysis results of the recovered Cu phase are shown in Table 33 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Cu phase was 0% by mass relative to the total mass of the Cu phase. Since the Cu phase contains almost no rare earth elements, it can be considered that the rare earth components in the neodymium magnet were transferred to the slag phase (rare earth enriched phase). The composition of the Cu phase was determined by ICP-AES.

[0159]

[0160] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 34 below. The total amount of rare earth oxides in the powder was 98.9% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0161]

[0162] [Example 7]

[0163] The following were added to a graphite crucible (model: NO.8, maximum throughput per batch: 8 kg) manufactured by Nippon Crucible Co., Ltd.: 110.7 g of neodymium magnet (magnet 1), simulating the composition of a rotor and stator containing rare earth elements and steel; 807.3 g of electrolytic iron powder; 37.3 g of SiO2, simulating the oxidation (SiO2ization) of all silicon contained in the rotor and stator; and 47.5 g of carbonizing material, a melting point lowering agent. The crucible was then heated using a high-frequency induction furnace. It should be noted that the neodymium magnet (magnet 1) has the following composition: Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 0.95 wt%, Fe: 70.15 wt%. After heating to 1400℃ to melt it, 25g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components using the iron oxide and oxygen in the air. Then, 10.6g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0164] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y -Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb) and Fe-C phase. It should be noted that the composition of the neodymium magnet (magnet 1) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 1 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3) and the amount of borate (Na2B4O7) are shown in Table 35 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 35-38 and Comparative Reference Example 11, with the rare earth oxide mass:Al2O3:SiO2 ratio being 50.0:0.0:50.0. The content of borates relative to the total mass of borates and rare earth oxides is 22.2% by mass.

[0165]

[0166] The compositional analysis results of the recovered Fe-C phase are shown in Table 36 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.04% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0167]

[0168] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 37 below. The total amount of rare earth oxides in the powder was 99.3% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0169]

[0170] [Example 8]

[0171] A 15.067 kg rotor containing waste materials including rare earth elements and steel, and 812.9 g of carbon-adding material were added to a graphite silicon carbide crucible (Phenix) manufactured by Nippon Crucible Co., Ltd. (model: CD 100HP, maximum throughput per batch: 100 kg). The crucible was then heated using a high-frequency induction furnace. It should be noted that 1761 g of neodymium magnets (magnet 3), containing rare earth elements, were inserted into the rotor. The composition of neodymium magnets was Nd: 26.1 wt%, Pr: 0.0 wt%, Dy: 4.277 wt%, Tb: 0.221 wt%, B: 0.89 wt%, and Fe: 68.485 wt%. Additionally, the rotor contained 267.6 g of silicon and 257.4 g of aluminum. After heating to 1400℃ to melt it, 2185g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 240.9g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0172] After holding for 30 minutes, RE, which serves as the rare earth enriched phase, is removed from the crucible by pouring. x O y The Na2B4O7 slag (RE: Nd, Pr, Dy, and Tb) and molten Fe-C phase were naturally cooled. It should be noted that the composition of the neodymium magnet (magnet 3) was determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). The amounts of rare earth oxides (considered as the total mass of Nd2O3, Pr2O3, Dy2O3, and Tb2O3 contained in magnet 3 when oxidized to Nd2O3, Pr2O3, Dy2O3, and Tb2O3), oxides of easily oxidizable metals (SiO2 and Al2O3), and borate (Na2B4O7) in this embodiment are shown in Table 38 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 39-47 and Comparative Reference Example 12, with a rare earth oxide mass: Al2O3: SiO2 ratio of 37.22:28.84:33.94. The content of borates relative to the total mass of borates and rare earth oxides is 27.7% by mass.

[0173]

[0174] The compositional analysis results of the recovered Fe-C phase are shown in Table 39 below. The total residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0175]

[0176] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 40 below. The total amount of rare earth oxides in the powder relative to the total mass of the powder was 99.2% by mass. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0177]

[0178] [Example 9]

[0179] A graphite crucible (model: NO.8, maximum throughput per batch: 8 kg) manufactured by Nippon Crucible Co., Ltd. was filled with 941.7 g of rotor and 1203.9 g of stator, which consisted of waste materials containing rare earth elements, steel, and copper; 100.4 g of carbonizing material as a melting point lowering agent; and 1338.8 g of copper to promote phase separation. The crucible was then heated using a high-frequency induction furnace. It should be noted that 110.1 g of neodymium magnet (magnet 3), which contained rare earth elements, was inserted into the rotor. Its composition was Nd: 26.1 wt%, Pr: 0.0 wt%, Dy: 4.277 wt%, Tb: 0.221 wt%, B: 0.89 wt%, and Fe: 68.485 wt%. Furthermore, the rotor and stator together contained 40.9 g of silicon, 23.6 g of aluminum, and 293.8 g of copper. After heating to 1400℃ to melt it, 251g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 30.2g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0180] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y-Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb), Fe-C phase, and Cu phase. It should be noted that the composition of the neodymium magnet (magnet 3) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 3 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3), and the amount of borate (Na2B4O7) are shown in Table 41 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 48-52 and Comparative Reference Example 13, with a rare earth oxide mass:Al2O3:SiO2 ratio of 22.9:26:51.1. The content of borates relative to the total mass of borates and rare earth oxides is 43.5% by mass.

[0181]

[0182] The compositional analysis results of the recovered Fe-C phase are shown in Table 42 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0183]

[0184] The compositional analysis results of the recovered Cu phase are shown in Table 43 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Cu phase was 0% by mass relative to the total mass of the Cu phase. Since the Cu phase contains almost no rare earth elements, it can be considered that the rare earth components in the neodymium magnet were transferred to the slag phase (rare earth enriched phase). The composition of the Cu phase was determined by ICP-AES.

[0185]

[0186] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a rare earth oxalate precipitate. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 44 below. The total amount of rare earth oxides in the powder relative to the total mass of the powder was 98.4% by mass. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0187]

[0188] [Example 10]

[0189] A 16.461 kg rotor containing waste materials including rare earth elements and steel, and 820.6 g of carbon-adding material were added to a graphite silicon carbide crucible (Phenix) manufactured by Nippon Crucible Co., Ltd. (model: CD 100HP, maximum throughput per batch: 100 kg). The crucible was then heated using a high-frequency induction furnace. It should be noted that 1908 g of neodymium magnets (magnet 4), containing rare earth elements, were inserted into the rotor. The composition of neodymium magnets was Nd: 23.3 wt%, Pr: 0.0 wt%, Dy: 7.808 wt%, Tb: 0.0 wt%, B: 0.4 wt%, and Fe: 68.485 wt%. Additionally, the rotor contained 290.7 g of silicon and 87.1 g of aluminum. After heating to 1400℃ to melt it, 1735g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 210.9g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0190] After holding for 30 minutes, RE, which serves as the rare earth enriched phase, is removed from the crucible by pouring. x O yThe Na2B4O7 slag (RE: Nd, Pr, Dy, and Tb) and molten Fe-C phase were naturally cooled. It should be noted that the composition of the neodymium magnet (magnet 4) was determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). The amounts of rare earth oxides (considered as the total mass of Nd2O3, Pr2O3, Dy2O3, and Tb2O3 contained in magnet 4 when oxidized to Nd2O3, Pr2O3, Dy2O3, and Tb2O3), oxides of easily oxidizable metals (SiO2 and Al2O3), and borate (Na2B4O7) in this embodiment are shown in Table 45 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 53-60 and Comparative Reference Example 14, with the rare earth oxide mass: Al2O3: SiO2 ratio being 46.72:11.15:42.13. The content of borates relative to the total mass of borates and rare earth oxides is 23.4% by mass.

[0191]

[0192] The compositional analysis results of the recovered Fe-C phase are shown in Table 46 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase was 0% by mass relative to the total mass of the Fe-C phase. Since the Fe-C phase contains almost no rare earth elements, it can be considered that the rare earth components in the neodymium magnet were transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0193]

[0194] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 47 below. The total amount of rare earth oxides in the powder was 98.9% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry).

[0195]

[0196] [Example 11]

[0197] 1028.8g of rotor and 1249.5g of stator (containing waste materials including rare earth elements, steel, and copper), 104.9g of carbonizing material (as a melting point lowering agent), and 1048.6g of copper (to promote phase separation) were added to a graphite crucible (model: NO.8, maximum throughput per batch: 8kg) manufactured by Nippon Crucible Co., Ltd., and heated using a high-frequency induction furnace. It should be noted that 119.3g of neodymium magnet (magnet 4), containing rare earth elements, was inserted into the rotor. Its composition is: Nd: 23.3 wt%, Pr: 0.0 wt%, Dy: 7.808 wt%, Tb: 0.0 wt%, B: 0.89 wt%, Fe: 67.995 wt%. Furthermore, the rotor and stator together contain 43.1g of silicon, 13.2g of aluminum, and 306.3g of copper. After heating to 1400℃ to melt it, 230g of iron oxide (Fe2O3) as an oxidant was added, and the molten metal was further stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 17.8g of sodium tetraborate (Na2B4O7) as a borate was added, and the molten metal was stirred with a carbon rod.

[0198] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y -Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb), Fe-C phase, and Cu phase. It should be noted that the composition of the neodymium magnet (magnet 4) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 4 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3), and the amount of borate (Na2B4O7) are shown in Table 48 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 61-69 and Comparative Reference Example 15, with a rare earth oxide mass:Al2O3:SiO2 ratio of 26.9:15.6:57.6. The content of borates relative to the total mass of borates and rare earth oxides is 29.2% by mass.

[0199]

[0200] The compositional analysis results of the recovered Fe-C phase are shown in Table 49 below. The total residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0201]

[0202] The compositional analysis results of the recovered Cu phase are shown in Table 50 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Cu phase relative to the total mass of the Cu phase is 0.03% by mass. The Cu phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Cu phase was determined by ICP-AES.

[0203]

[0204] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 51 below. The total amount of rare earth oxides in the powder was 98.3% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (inductively coupled plasma atomic emission spectrometry).

[0205]

[0206] [Example 12]

[0207] A rotor containing waste materials including rare earth elements and steel, and 50.7g of carbon-reducing material as a melting point lowering agent were added to a graphite crucible (model: NO.8, maximum throughput per batch: 8kg) manufactured by Nippon Crucible Co., Ltd., and heated using a high-frequency induction furnace. It should be noted that 110.7g of neodymium magnet (magnet 1), containing rare earth elements, was inserted into the rotor. Its composition is: Nd: 21.0 wt%, Pr: 5.0 wt%, Dy: 2.5 wt%, Tb: 0.4 wt%, B: 0.95 wt%, Fe: 70.15 wt%. Furthermore, the rotor and stator together contain 18.1g of silicon and 6.4g of aluminum. After heating to 1400℃ to melt it, 113g of iron oxide (Fe2O3) as an oxidant was added. The molten metal was then stirred in the atmosphere with a carbon rod to fully oxidize the rare earth components, silicon, and aluminum using the iron oxide and oxygen in the air. Then, 20.3g of boric acid (B2O3) and 15.5g of sodium carbonate (Na2CO3) were added, and the molten metal was stirred with a carbon rod.

[0208] After holding for 30 minutes and allowing it to cool naturally, the REs, which are the rare earth enriched phases, were removed from the crucible by cutting. x O y -Na2B4O7 series slag (RE: Nd, Pr, Dy and Tb) and Fe-C phase. It should be noted that the composition of the neodymium magnet (magnet 1) was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). The mass of rare earth oxides containing rare earth elements in this embodiment (considered as the total mass of Nd2O3, Pr2O3, Dy2O3 and Tb2O3 when Nd, Pr, Dy and Tb contained in magnet 1 are oxidized to Nd2O3, Pr2O3, Dy2O3 and Tb2O3), the amount of oxides of easily oxidizable metals (SiO2 and Al2O3) and the amount of borate (Na2B4O7) are shown in Table 52 below. It should be noted that the mass ratios of rare earth oxides, Al2O3, and SiO2 are approximately the same as those in Reference Examples 1-7 and Comparative Reference Examples 1-5, with a rare earth oxide mass:Al2O3:SiO2 ratio of 42.3:13.8:44. The content of borates relative to the total mass of borates and rare earth oxides is 44.1% by mass.

[0209]

[0210] The compositional analysis results of the recovered Fe-C phase are shown in Table 53 below. The residual RE (RE: Nd, Pr, Dy, and Tb) content in the Fe-C phase relative to the total mass of the Fe-C phase is 0.01% by mass. The Fe-C phase contains almost no rare earth elements, suggesting that the rare earth components in the neodymium magnet have been transferred to the slag phase (rare earth enriched phase). The composition of the Fe-C phase was determined by ICP-AES.

[0211]

[0212] The recovered rare earth enriched phase (RE) was treated with 200 ml of 6 mol / L hydrochloric acid. x O y 10g of Na₂B₄O₇ slag was acid-leached, and the filtrate was obtained by filtration. 100ml of 1mol / L oxalic acid aqueous solution and ammonia were added to the filtrate to adjust the pH to 2. The pH-adjusted solution was stirred and maintained at 40°C for 1-2 hours to obtain a precipitate of rare earth oxalates. The rare earth oxalates were separated by filtration and calcined in a muffle furnace at 900°C for 60 minutes to obtain a powder containing rare earth oxides. The analytical results of this powder are shown in Table 54 below. The total amount of rare earth oxides in the powder was 98.9% by mass relative to the total mass of the powder. The composition of the powder was determined by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry).

[0213]

[0214] This example uses borate precursors (boric acid (B₂O₃) and sodium carbonate (Na₂CO₃)) as flux, confirming that a rare earth enriched phase (RE) was obtained in the same manner as in Examples 1-1, 1-2, and 3, which used borate (sodium tetraborate (Na₂B₄O₇)) as flux. x O y -Na2B4O7 series slag). It was also confirmed that the composition of the recovered rare earth oxides was identical to that in Examples 1-1, 1-2, and 3. It should be noted that carbon dioxide gas was generated during the melt preparation process due to the decomposition of sodium carbonate (Na2CO3), but the rare earth-enriched phase was successfully separated from the Fe-C phase without any problems during the separation process.

[0215] As can be seen from the reference examples, comparative reference examples and embodiments shown above, the recycling method of this manner can reduce the amount of flux used in the recycling method of rare earth oxides that uses a flux containing boron.

[0216] This application is based on Japanese Patent Application No. 2024-071472, filed on April 25, 2024, the disclosure of which is incorporated herein by reference in its entirety.

Claims

1. A method for recovering rare earth oxides, comprising recovering rare earth oxides from waste containing rare earth element substances, the method comprising: Melt preparation step (1): The waste, and at least one borate selected from alkali metal borates and alkaline earth metal borates and / or their precursors are heated and melted to prepare a melt containing at least a rare earth oxide, the borate, and an oxide of an easily oxidizable metal; and Separation process (2): Separating the rare earth enriched phase and the Fe-C phase from the melt, wherein the rare earth enriched phase is formed by concentrating rare earth elements in the borates.

2. The method for recovering rare earth oxides according to claim 1, wherein, The content of the borate is the amount above the liquidus line in the phase diagram, determined by the mass of the rare earth oxides of the rare earth element-containing substance and the content of the oxides of the easily oxidizable metal.

3. The method for recovering rare earth oxides according to claim 1, wherein, The waste further contains copper. In the separation process (2), the rare earth enriched phase, Fe-C phase and Cu phase are separated from the melt. The rare earth enriched phase is formed by concentrating rare earth elements in the borates.

4. The method for recovering rare earth oxides according to claim 1, wherein, The oxides of the easily oxidizable metals are aluminum oxide and / or silicon dioxide.

5. The method for recovering rare earth oxides according to claim 4, wherein, The oxides of the easily oxidizable metals are aluminum oxide and silicon dioxide.

6. The method for recovering rare earth oxides according to claim 5, wherein, The borate is sodium tetraborate (Na2B4O7).

7. The method for recovering rare earth oxides according to claim 1, wherein, The rare earth element-containing material includes neodymium magnets.

8. The method for recovering rare earth oxides according to claim 4, wherein, Relative to the total mass of the rare earth oxides of the rare earth element-containing substances, the content of the oxides of the easily oxidizable metals, and the content of the borates, the proportion of the alumina content is 0~31.34% by mass, the proportion of the silicon dioxide content is 12.71~51.87% by mass, and the proportion of the borates content is 10.0~70.1% by mass.

9. The method for recovering rare earth oxides according to claim 8, wherein, Relative to the total mass of the rare earth oxides of the rare earth element-containing substances, the content of the oxides of the easily oxidizable metals, and the content of the borates, the proportion of the alumina content is 0~31.34% by mass, the proportion of the silicon dioxide content is 17.79~51.87% by mass, and the proportion of the borates content is 10.0~35.0% by mass.

10. The method for recovering rare earth oxides according to claim 9, wherein, Relative to the total mass of the rare earth oxides of the rare earth element-containing substances, the content of the oxides of the easily oxidizable metals, and the content of the borates, the proportion of the alumina content is 0~31.34% by mass, the proportion of the silicon dioxide content is 18.43~51.80% by mass, and the proportion of the borates content is 10.0~34.6% by mass.

11. The method for recovering rare earth oxides according to claim 1, wherein, The melt preparation process (1) sequentially includes the following processes (1a) to (1c): Step (1a): The waste containing rare earth elements, aluminum and silicon is heated and melted to obtain melt (1a). Step (1b): The oxidant is brought into contact with the melt (1a) to obtain melt (1b); Step (1c): The borate and / or its precursor are added to the melt (1b) to obtain melt (1c).

12. The method for recovering rare earth oxides according to claim 1, wherein, Following the separation process (2), the following processes (3a) to (3c) are performed sequentially: Step (3a): The rare earth enriched phase obtained in step (2) is leached with acid to obtain a rare earth element leachate; Step (3b): The rare earth elements in the rare earth element leachate are precipitated in the form of salt to obtain a precipitate; Step (3c): The precipitate is heated to recover rare earth elements in the form of oxides.

13. A rare earth enrichment comprising: Rare earth oxides, Oxides of easily oxidized metals, and At least one borate selected from alkali metal borates and alkaline earth metal borates.

14. The rare earth enrichment according to claim 13, wherein, The proportion of alumina content is 0-31.34% by mass, the proportion of silicon dioxide content is 12.71-51.87% by mass, and the proportion of borate content is 10.0-70.1% by mass, relative to the total content of the rare earth oxides, the oxides of the easily oxidizable metals, and the borates.

Citation Information

Patent Citations

  • Method for recovering rare earth element from rare earth element-containing product