Galvanized steel sheets, components and their manufacturing methods

By controlling the steel microstructure and processing technology of galvanized steel sheets, the problem of unstable energy absorption capacity caused by fracture in energy absorption components of high-strength galvanized steel sheets has been solved, achieving high strength and excellent collision characteristics, which is suitable for automotive energy absorption components.

CN123125359APending Publication Date: 2026-11-17JFE STEEL CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580029091.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-25
Filing Date
2025-04-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, high-strength galvanized steel sheets are prone to breakage during collisions in energy absorption components, resulting in an inability to stably perform collision energy absorption. Furthermore, existing evaluation methods cannot effectively assess fracture resistance characteristics during high-speed deformation.

Method used

By controlling the steel microstructure and processing technology of galvanized steel sheets, the proportions of ferrite, bainite, tempered martensite, and retained austenite in the steel sheets are ensured. Furthermore, specific bending processing conditions are applied to improve the tensile strength and impact characteristics of galvanized steel sheets, thus preventing crack formation.

Benefits of technology

Galvanized steel sheets with tensile strength of over 780MPa, yield ratio of over 65%, and crack length of less than 0.5mm have been developed, which are suitable for automotive energy absorption components, improving the collision safety and lightweighting effect of automobiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
Patent Text Reader

Abstract

The object of this invention is to provide galvanized steel sheets, components, and methods for manufacturing them that have excellent tensile and impact properties. A galvanized steel sheet comprises a steel sheet having a defined steel structure and a zinc coating on the surface of the steel sheet. After performing a U-bending process on the galvanized steel sheet at a stroke speed of 1500 mm / min with a bending radius R = 4 mm, a spacer with a thickness of 5 mm is provided on the inner side (compression side) of the bending section of the galvanized steel sheet. The bending process is continued until the two sides of the steel sheet, located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly adhered to the spacer. At this point, no cracks are generated on the outer side (tension side) of the bending section, and the tensile strength is 780 MPa or more and less than 1180 MPa, with a yield ratio of 65% or more and less than 95%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to galvanized steel sheets and components with high strength and excellent impact resistance, and methods for manufacturing the same. The galvanized steel sheets of this invention are primarily suitable for use as automotive steel sheets. Background Technology

[0002] From the perspective of protecting the Earth's environment, reducing CO2 emissions while maintaining the strength of the car body and achieving lightweighting, as well as improving fuel efficiency, has always been an important issue in the automotive industry. To achieve lightweighting while maintaining the strength of the car body, reducing the wall thickness of steel sheets used as raw materials for automotive components by increasing their strength is effective. On the other hand, automotive components made from steel sheets must ensure the safety of the occupants during a collision. Therefore, high-strength galvanized steel sheets used as raw materials for automotive components are required not only to have the desired strength but also to have excellent crash characteristics.

[0003] In recent years, the application of high-strength galvanized steel sheets with a tensile strength (TS) of 780 MPa or higher in automobile bodies has been expanding. From a collision characteristics perspective, automobile components are broadly divided into non-deformable components such as pillars and bumpers, and energy-absorbing components such as longitudinal beams. In the event of a collision during vehicle operation, necessary collision characteristics are required for each to ensure occupant safety. In non-deformable components, the trend towards higher strength is underway, and high-strength galvanized steel sheets with a tensile strength (hereinafter referred to as TS) of 780 MPa or higher have been put into practical use. However, in applications to energy-absorbing components, high-strength galvanized steel sheets with a strength of 780 MPa or higher are prone to fracture during a collision, with the point of origin being the area formed during the initial processing. Therefore, there is a challenge in consistently achieving high collision energy absorption capacity, leading to the primary use of materials with a strength below 590 MPa. Therefore, in the development of energy-absorbing components, there is room for ensuring collision safety by suppressing component fracture during a collision and consistently achieving high energy absorption, while also considering environmental protection through lightweighting. Based on the above, energy absorption components need to use high-strength galvanized steel sheets with excellent impact characteristics and a TS of 780MPa or higher.

[0004] To address such requirements, for example, Patent Document 1 discloses a technology involving high-strength galvanized steel sheets with a maximum tensile strength of 780 MPa or more, which can be used in impact-absorbing components during collisions. Furthermore, Patent Document 2 discloses a patent involving galvanized steel sheets with a tensile strength of 980 MPa or more, good fracture resistance, and excellent impact characteristics with good energy absorption.

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-175061

[0008] Patent Document 2: Japanese Patent Application Publication No. 2022-34015 Summary of the Invention

[0009] The problem that the invention aims to solve

[0010] However, in Patent Document 1, regarding impact characteristics, although crack identification and fracture resistance evaluation are performed on the cap-shaped component through axial crushing tests, the process from crack initiation during crushing to fracture, which is crucial for impact characteristics, cannot be evaluated because crack identification is performed after crushing. The reason is that during crushing, even minor cracks that do not penetrate the plate thickness in the early stages of crack formation may reduce energy absorption, but such minor cracks are difficult to identify after crushing. Furthermore, in the case of cracks initiating later in the crushing process, even large cracks penetrating the plate thickness may have almost no impact on energy absorption. Therefore, it is considered insufficient to evaluate fracture resistance solely based on crack identification after crushing.

[0011] Furthermore, in Patent Document 2, regarding collision characteristics, fracture resistance is evaluated by measuring the void number density in a cross-section within a 0-50 μm region from the surface of the steel plate on the compression side during a 90° bending process at a stroke speed of 20 mm / min, and by measuring the stroke-load curve at the maximum load during a bending-orthogonal bending test at a stroke speed of 20 mm / min. Energy absorption is evaluated through an axial crush test of the cap-shaped component. However, the fracture resistance required for energy-absorbing components in automobiles is fracture resistance under high-speed deformation. Therefore, the evaluation of fracture resistance based on bending tests and bending-orthogonal bending tests at a stroke speed of 20 mm / min is insufficient for evaluating the fracture resistance of materials used in energy-absorbing components of automobiles that deform at high speeds. In other words, the fracture resistance may not be sufficient for use as a material in energy-absorbing components of automobiles.

[0012] Thus, it is hoped that a new technology for galvanized steel sheets with excellent tensile properties, including tensile strength TS, and consequently excellent impact properties, can be established.

[0013] The present invention was made in view of the above circumstances, and its object is to provide galvanized steel sheets, components, and methods for manufacturing them that are suitable for use as energy absorption components in automobiles and have excellent tensile and impact properties.

[0014] Here, excellent tensile properties mean that, after a tensile test according to JIS Z2241 (2011), the tensile strength TS is 780 MPa or more and less than 1180 MPa, and the elongation EL is 11% or more.

[0015] In addition, excellent impact characteristics refer to high load-bearing capacity, good energy absorption capacity, and consequently good fracture resistance.

[0016] High load-bearing capacity means that the yield ratio YR obtained by tensile testing according to JIS Z2241 (2011) is 65% or more and 95% or less.

[0017] Good energy absorption capacity means that, in a tensile test according to JIS Z2241 (2011), the value B (hereinafter, refer to formula (2)) obtained by dividing the area enclosed by the above curve in the range of strain Q from 0 to 4%, the straight line of stress P=0 and strain Q=4 by the tensile strength TS is 3.15% or more.

[0018]

[0019] In the formula, P: stress (MPa), Q: strain (%), TS: tensile strength (MPa).

[0020] Good fracture resistance means that when galvanized steel sheets are subjected to U-bending processing (high-speed U-bending processing) and close bending test (high-speed close bending test) under specific conditions, the length of the crack formed on the outer side (tensile side) of the bent part is less than 0.5 mm.

[0021] Here, the above-mentioned U-bending process is carried out with a bending radius R=4mm and a stroke speed of 1500mm / minute.

[0022] In addition, in the tight bending test, the thickness of the spacer sandwiched between the galvanized steel plates was set to 5 mm, and the test was carried out under the conditions of a stroke speed of 1500 mm / min, a pressing load of 10 tons, and a pressing time of 3 seconds.

[0023] Methods for solving problems

[0024] In order to solve the above-mentioned problems, the inventors have conducted repeated and in-depth research and discovered the following results.

[0025] The galvanized steel sheet comprises a steel sheet and a zinc coating formed on the surface of the steel sheet. The steel sheet has a steel microstructure, by area percentage, of ferrite: less than 30.0% (inclusive), bainite: greater than 40.0% and less than 80.0%, the total of tempered martensite and bainite: greater than 60.0%, retained austenite: more than 1.5% and less than 20%, and fresh martensite: less than 20.0%. Furthermore, in the aforementioned galvanized steel sheet, when the ferrite by area percentage is greater than 0.0%, the area percentage of high-Mn ferrite (HF) with a Mn concentration greater than 0.80 times the Mn concentration of the steel sheet is 30% or more relative to the total area percentage of ferrite, and the area percentage of the hard second phase in contact with bainite is 30% or more relative to the total area percentage of the hard second phase composed of retained austenite and fresh martensite. The galvanized steel sheet is subjected to a stroke speed of 1500 mm / min. After a U-bending process with a bending radius R=4mm, a 5mm thick spacer is placed on the inner side (compression side) of the bending section of the galvanized steel sheet. Bending is then performed at a stroke speed of 1500mm / min, a pressing load of 10 tons, and a pressing time of 3 seconds, until both sides of the galvanized steel sheet, located opposite each other in the thickness direction of the spacer, are tightly adhered to the spacer. At this point, no cracks larger than 0.5mm are generated on the outer side (tension side) of the bending section. Therefore, a steel sheet with excellent tensile and impact properties can be obtained.

[0026] This invention was made based on the following insight, the gist of which is as follows.

[0027] [1] A galvanized steel sheet, comprising a steel sheet and a zinc coating on the surface of the steel sheet, wherein, The steel plate has the following microstructure: based on the area ratio at 1 / 8 to 3 / 8 of the plate thickness, ferrite: less than 30.0% (inclusive), bainite: greater than 40.0% and less than 80.0%, the total of tempered martensite and bainite: greater than 60.0%, retained austenite: more than 1.5% and less than 20%, and fresh martensite: less than 20.0% (inclusive). When the ferrite content is greater than 0.0% by area, the area ratio of high-Mn ferrite, where the Mn concentration is greater than 0.80 times that of the steel plate, is more than 30% relative to the total area ratio of the ferrite. The hard second phase, comprising more than 30% of the perimeter of the hard second phase in contact with bainite, has an area ratio of more than 30% relative to the total area ratio of the hard second phase composed of the retained austenite and the fresh martensite. For the galvanized steel sheet, after performing a U-bending process with a bending radius R=4mm at a stroke speed of 1500mm / min, a 5mm thick spacer is placed on the inner side of the bending section of the galvanized steel sheet. The bending process is then performed at a stroke speed of 1500mm / min, a pressing load of 10 tons, and a pressing time of 3 seconds, until both sides of the galvanized steel sheet, located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly adhered to the spacer. At this point, the crack generated on the outer side of the bending section is less than 0.5mm. The galvanized steel sheet has a tensile strength of 780 MPa or higher and less than 1180 MPa, and a yield ratio of 65% or higher and less than 95%.

[0028] [2] According to the galvanized steel sheet described in [1] above, the steel sheet has a composition in terms of mass% containing C: 0.05 to 0.20%, Si: 0.10 to 2.00%, Mn: 2.0 to 3.5%, P: less than 0.050%, S: less than 0.050%, sol.Al: 0.005 to 2.000%, and N: less than 0.010%, with the balance being Fe and unavoidable impurities.

[0029] [3] According to the galvanized steel sheet described in [2] above, the composition, in mass percentage, further contains the following components: Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less. The following are at least one of the following: Zn: less than 0.0200%, Co: less than 0.0200%, Zr: less than 0.1000%, Ca: less than 0.0200%, Se: less than 0.0200%, Te: less than 0.0200%, Ge: less than 0.0200%, As: less than 0.0500%, Sr: less than 0.0200%, Cs: less than 0.0200%, Hf: less than 0.0200%, Pb: less than 0.0200%, Bi: less than 0.0200%, and REM: less than 0.0200%.

[0030] [4] The galvanized steel sheet according to any one of [1] to [3] above, wherein the zinc coating is an electro-galvanized layer, a hot-dip galvanized layer or an alloyed hot-dip galvanized layer.

[0031] [5] A component, which is formed by forming and welding at least one of the galvanized steel sheet described in any one of [1] to [4] above.

[0032] [6] A method for manufacturing galvanized steel sheet, comprising: The hot rolling process, wherein for a steel billet having the composition described in [2] or [3] above, hot rolling is performed at a finishing temperature of 850 to 950°C and coiling is performed at a coiling temperature of 600°C or below; The cold rolling process, wherein the hot-rolled steel sheet after the hot rolling process is cold-rolled with a reduction rate of more than 20%; The annealing process, wherein the cold-rolled steel sheet after the cold rolling process is heated to an annealing temperature of 750°C or higher under the condition that A as shown in the following formula (1) satisfies 4 or more and 70 or less, and is held at the annealing temperature for 30 seconds or more; In the plating process, after the annealing process, the plate is cooled to a temperature range of 300 to 600°C and held at that temperature range for 10 to 300 seconds before galvanizing the steel plate surface. The quenching and tempering process, wherein after the plating process, the material is cooled to a cooling stop temperature of (Ms-300℃) to (Ms-50℃), and then held at a tempering temperature of 250 to 500℃ for 20 to 500 seconds; and The cooling process involves cooling the material from the tempering temperature to 50°C at an average cooling rate of 20°C / s or higher after the quenching and tempering processes.

[0033] In the formula, T Ac1 Temperature at point Ac1 (°C) T RT Annealing temperature (°C) t RT From the start of the annealing process through heat treatment until the annealing temperature T is reached. RT The time (in seconds) required so far. t Ac1 The temperature T from the start of the heat treatment process in the initial annealing stage until point Ac1 is reached. Ac1 The time (in seconds) required so far. T(t): Temperature (°C) t seconds after the start of the heat treatment process in the annealing step.

[0034] [7] According to the manufacturing method of galvanized steel sheet described in [6] above, the galvanizing treatment is to perform electro-galvanizing, hot-dip galvanizing or alloyed hot-dip galvanizing treatment on the surface of the steel sheet.

[0035] [8] A method for manufacturing a component, wherein the component is made by performing at least one of forming and welding on the galvanized steel sheet described in any one of [1] to [4] above.

[0036] Invention Effects

[0037] According to the present invention, galvanized steel sheets with excellent tensile and impact properties can be obtained. Components obtained by forming, welding, etc., the galvanized steel sheets of the present invention can be used as energy-absorbing components in the automotive field. Detailed Implementation

[0038] The present invention will now be described in detail.

[0039] Galvanized steel sheet

[0040] The galvanized steel sheet of the present invention comprises a steel sheet and a zinc coating on the surface of the steel sheet, wherein the steel sheet has the following steel structure: at a position of 1 / 8 to 3 / 8 of the sheet thickness, in terms of area ratio, ferrite: less than 30.0% (including 0.0%), bainite: greater than 40.0% and less than 80.0%, the total of tempered martensite and bainite: greater than 60.0%, retained austenite: more than 1.5% and less than 20%, fresh martensite: less than 20.0% (including 0.0%), when ferrite in terms of area ratio is greater than 0.0%, the area ratio of high Mn ferrite (HF) with a Mn concentration greater than 0.80 times the Mn concentration of the steel sheet is more than 30% of the total ferrite area ratio, and the area ratio of the hard second phase composed of retained austenite and fresh martensite is more than 30% of the perimeter of the hard second phase. The area ratio of the hard second phase in contact with bainite is more than 30% of the total area ratio of the hard second phase. After performing U-bending processing on the galvanized steel sheet with a bending radius R=4mm at a stroke speed of 1500mm / min, a spacer with a thickness of 5mm is set on the inner side (compression side) of the bending processing section of the galvanized steel sheet. The bending processing of the bending processing section is carried out under the conditions of a stroke speed of 1500mm / min, a pressing load of 10 tons, and a pressing time of 3 seconds, until the two sides of the galvanized steel sheet, which are located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly attached to the spacer. At this time, the crack generated on the outer side (tension side) of the above-mentioned bending processing section is less than 0.5mm, the tensile strength is more than 780MPa and less than 1180MPa, and the yield ratio is more than 65% and less than 95%.

[0041] Ferrite area fraction: less than 30.0% (including 0.0%)

[0042] Ferrite is effective in improving elongation, but it reduces yield strength (YS) and tensile strength (TS). Furthermore, the increased hardness difference between soft ferrite and adjacent structures makes the area more susceptible to fracture during high-speed impact due to void formation and bonding, thus reducing fracture resistance during high-speed impact. Consequently, when the ferrite area fraction is 30.0% or more, it is difficult to satisfy all requirements: a yield ratio (YR) of 65% or more, a TS of 780 MPa or more, and fracture resistance during high-speed impact. Therefore, the ferrite area fraction is less than 30.0%, preferably 20.0% or less, and more preferably less than 10.0%. While there is no particular limitation on the lower limit, the ferrite area fraction is preferably 1.0% or more, and more preferably 3.0% or more.

[0043] Bainite area ratio: greater than 40.0% and less than 80.0%

[0044] Bainite, being an intermediate hardness phase, reduces the hardness difference with adjacent martensite and ferrite by forming an area fraction greater than 40.0%, suppressing the formation of voids during high-speed collisions and improving high-speed collision characteristics. Furthermore, bainite increases elongation. When the area fraction of bainite is less than 40.0%, this effect cannot be fully achieved, making it difficult to satisfy all the requirements for a hardness tolerance (TS) of 780 MPa or higher, an elongation of 11% or higher, and high-speed collision characteristics. Therefore, the area fraction of bainite is greater than 40.0%, preferably greater than 45.0%, and more preferably greater than 50.0%.

[0045] Furthermore, when the area ratio of bainite is greater than 80.0%, it is difficult to obtain the desired tensile strength. Therefore, the area ratio of bainite is 80.0% or less, preferably 70.0% or less, and more preferably 65.0% or less.

[0046] The combined area ratio of tempered martensite and bainite is greater than 60.0%.

[0047] Tempered martensite and bainite are effective in improving high-speed impact characteristics and strength by suppressing component fracture during impact deformation. When the combined area fraction of tempered martensite and bainite is less than 60.0%, this effect is insufficient, making it difficult to meet both the stress resistance (TS) of 780 MPa and high-speed impact characteristics. Therefore, their combined area fraction is greater than 60.0%, preferably greater than 65.0%, and more preferably greater than 82.0%.

[0048] In addition, there is no upper limit to their total area ratio, but considering the balance with other organizations, the total area ratio is preferably below 95.0%.

[0049] The area ratio of retained austenite is: 1.5% or more but less than 20%.

[0050] Retained austenite delays crack formation during impact, effectively improving impact characteristics. The mechanism is not fully understood, but it is believed to be as follows: Retained austenite undergoes work hardening during impact deformation, thereby increasing the radius of curvature during bending deformation and dispersing strain in the bending region. By dispersing strain, stress concentration towards void formation caused by the primary processing is mitigated, resulting in improved impact characteristics. This effect is sometimes not achieved when the area fraction of retained austenite is less than 1.5%. Furthermore, when the area fraction of retained austenite is less than 1.5%, elongation decreases. Therefore, the area fraction of retained austenite is 1.5% or more, preferably 3% or more, and more preferably 5% or more.

[0051] On the other hand, when the area ratio of retained austenite is greater than 20%, the fresh martensite generated by processing-induced phase transformation sometimes reduces the fracture resistance during impact. Therefore, the area ratio of retained austenite is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less.

[0052] Fresh martensite: less than 20.0% (including 0.0%)

[0053] Fresh martensite is effective for increasing strength. However, voids tend to form at grain boundaries with the soft phase, and when the area fraction of fresh martensite is greater than 20.0%, the collision properties may sometimes be reduced. Therefore, the area fraction of fresh martensite is preferably 20.0% or less (including 0.0%), more preferably 15.0% or less, and even more preferably 10.0% or less.

[0054] High-Mn ferrite (HF) with a Mn concentration greater than 0.80 times that of the steel plate: 30% or more (including 100.0%) of the total ferrite area fraction.

[0055] Low-Mn ferrite (LF), with a Mn concentration less than 0.80 times that of the steel plate, has a lower dislocation density and is relatively softer compared to high-Mn ferrite (HF), with a Mn concentration greater than 0.80 times that of the steel plate. To suppress fracture during high-speed collisions, it is necessary to reduce the amount and hardness difference of regions with high hardness differences. When the area fraction of relatively soft low-Mn ferrite (LF) in the total ferrite area is 70% or less, i.e., when the area fraction of high-Mn ferrite (HF) is 30% or more, a stress resistance (TS) of 780 MPa or higher and high high-speed collision characteristics can be obtained. Therefore, when the ferrite content is greater than 0.0% in terms of area fraction, the area fraction of high-Mn ferrite (LF) is set to 30% or more (including 100.0%) of the total ferrite area fraction. Preferably, the area fraction of high-Mn ferrite is 50% or more of the total ferrite area fraction, more preferably 70% or more.

[0056] The area fraction of low-Mn ferrite (LF) is set to be 70% or less (including 0.0%) of the area fraction of all ferrite. The area fraction of low-Mn ferrite relative to the area fraction of all ferrite is preferably 50% or less, more preferably 30% or less.

[0057] Here, low-Mn ferrite (LF) includes recrystallized ferrite (RF) formed during the heating of heat treatment, or may be composed of this recrystallized ferrite.

[0058] In addition, high-Mn ferrite (HF) includes, or can be composed of, cooling-generated ferrite (TF) formed during cooling.

[0059] The area fraction of hard second phase in contact with bainite exceeding 30% of the perimeter: exceeding 30% of the total area fraction of hard second phase.

[0060] In the island-like regions constituting the hard second phase composed of retained austenite and fresh martensite, the island-like regions where more than 30% of the perimeter is in contact with bainite have a high concentration of dissolved carbon and high stability of retained austenite. Therefore, the island-like regions where more than 30% of the perimeter is in contact with bainite play an important role in ensuring good work hardening ability and ductility.

[0061] That is, during cooling after annealing, when bainite is formed under appropriate conditions, dissolved carbon diffuses from the bainite to the surrounding untransformed austenite, resulting in a locally high concentration of dissolved carbon only in the region of the untransformed austenite adjacent to the bainite. Then, under appropriate conditions, reheating is performed in this state, thereby forming a hard second phase with a high concentration of dissolved carbon around or inside the bainite. Therefore, the stability of the retained austenite contained in the hard second phase with a high concentration of dissolved carbon around or inside the bainite is increased, playing an important role in ensuring good work hardening ability and ductility. It should be noted that ensuring ductility in this invention refers to an elongation (E1) of 11% or more.

[0062] In summary, the total area of ​​the hard second phase that is in contact with bainite at a perimeter of 30% or more is 30% or more of the total area of ​​all hard second phases, preferably 40% or more, and more preferably 60% or more. It should be noted that there is no particular upper limit, and it can be 100%.

[0063] The area ratio of each microstructure refers to the proportion of the area of ​​each phase in the observed area. The area ratio of each microstructure is determined as follows: After grinding the thickness section of a steel plate cut at a right angle relative to the rolling direction, it is etched with a 3% (v / v) nitric acid ethanol solution. Three fields of view are captured at 1500x magnification at the 1 / 4 position of the plate thickness using a SEM (scanning electron microscope), with a field of view range of 85 μm × 64 μm. The area ratio of each microstructure is calculated using Image-Pro from Media Cybernetics based on the obtained image data. The average of the area ratios of the three fields of view is taken as the area ratio of each microstructure of the present invention. In the image data, ferrite, bainite, retained austenite, fresh martensite, and tempered martensite are distinguished as follows.

[0064] Ferrite: A black region within the grain containing neither retained austenite nor fresh martensite with an aspect ratio greater than 2.0; Bainite: A black region within the grain containing one or more of retained austenite and fresh martensite with an aspect ratio greater than 2.0; Tempered martensite: A light gray region containing one or more of retained austenite and fresh martensite with an aspect ratio greater than 2.0 and containing carbides; Retained austenite and fresh martensite: White regions, thus distinguished by these characteristics.

[0065] Here, fresh martensite and retained austenite are difficult to distinguish in SEM images. Therefore, the area ratio of fresh martensite is obtained by subtracting the area ratio of retained austenite obtained by the method described later from the total area ratio of fresh martensite and retained austenite.

[0066] Regarding the area ratio of retained austenite, in this invention, the volume ratio of retained austenite is determined by measuring the X-ray diffraction intensity, and this volume ratio is regarded as the area ratio of retained austenite. The volume ratio of retained austenite is determined by the ratio of the X-ray diffraction integral intensity of the (200), (220), and (311) planes of fcc iron in the 1 / 4 thickness plane to the X-ray diffraction integral intensity of the (200), (211), and (220) planes of bcc iron.

[0067] In this invention, the average Mn concentration of the steel plate is calculated based on the numerical data of Mn concentration obtained by mapping analysis using FE-EPMA, and the area ratio of Mn concentration less than 0.80 times the average Mn concentration of the steel plate is calculated, thereby determining the area ratio of low Mn ferrite.

[0068] In addition, the area fraction of high-Mn ferrite is obtained by subtracting the area fraction of low-Mn ferrite from the total area fraction of ferrite.

[0069] It should be noted that the low-Mn ferrite region is generated by the distribution of Mn from ferrite to austenite during the annealing process (heating process and annealing holding process). During the subsequent cooling process, the Mn concentration of bainite, martensite, tempered martensite and austenite formed from austenite must be greater than 0.80 times the Mn concentration of the base material.

[0070] Cracks generated on the outer side (tensile side) of the bending section after the high-speed U-bending + high-speed close-fitting bending test: less than 0.5 mm.

[0071] In the galvanized steel sheet of the present invention, after performing a U-bending process (high-speed U-bending process) with a bending radius R=4mm at a stroke speed of 1500mm / min, a close-fitting bending test (high-speed close-fitting bending test) is conducted. A spacer with a thickness of 5mm is provided on the inner side (compression side) of the bending section of the galvanized steel sheet, and bending processing of the bending section is performed (stroke speed: 1500mm / min, pressing load: 10 tons, pressing time: 3 seconds) until the two sides of the galvanized steel sheet, which are located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly attached to the spacer. At this point, no cracks of 0.5mm or more are generated on the outer side (tension side) of the bending section. As a result, high impact characteristics can be obtained. In the case of cracks of 0.5mm or more, the fracture resistance is insufficient, and therefore the impact characteristics are insufficient due to the generation and propagation of cracks during impact.

[0072] Here, the U-bending process is ended and the spacer is placed inside the bending section of the galvanized steel sheet, which can be set such that the angle formed on the opposing steel sheet surfaces is 0 to 20° (=10±10°).

[0073] Alternatively, stroke speed can be determined, for example, by actually measuring the stroke at regular intervals using a ruler and converting it into the amount of movement per 60 seconds.

[0074] The amount of movement can be defined as the relative movement of one end of the bent steel plate relative to the other end when viewed in a U-shape. It should be noted that the stroke measurement can be performed at any position within the bending testing machine, as long as it is a part of the bending testing machine that moves as part of the pressing fitting that presses against the steel plate.

[0075] The time can be adjusted within a range that can be measured normally; for example, a 5-second stroke can also be measured.

[0076] Tensile strength: ≥780MPa and <1180MPa

[0077] Yield ratio: 65% or higher and 95% or lower

[0078] The galvanized steel sheet of this invention has a tensile strength of 780 MPa or higher and less than 1180 MPa, and a yield ratio of 65% or higher and less than 95%, exhibiting high load-bearing capacity. When the yield ratio is greater than 95%, the fracture resistance decreases.

[0079] It should be noted that by controlling the heating rate and temperature before annealing and the cooling rate after annealing, as described later, and then performing plating treatment before the quenching and tempering processes, the desired impact characteristics can be obtained. By controlling the heating rate and temperature before annealing, the amount of low-Mn ferrite (LF), high-Mn ferrite (HF), and bainite formed during the pre-quenching holding process can be controlled. Thus, by forming high-Mn ferrite (HF), which is relatively hard compared to low-Mn ferrite (LF), and by generating bainite during the pre-quenching holding process and softening it during the plating and tempering processes, the hardness difference between ferrite and bainite is reduced, suppressing the formation of voids at the ferrite-bainite interface. As a result, the crack length can be suppressed to less than 0.5 mm (including 0 μm).

[0080] It should be noted that in the absence of ferrite, the formation of voids caused by the hardness difference of the microstructure is suppressed, and the collision characteristics are improved, so ferrite may not be present.

[0081] Furthermore, for the bainite generated during the tempering process, the softening caused by tempering during cooling is suppressed by accelerating the cooling rate after tempering. Then, the softening caused by tempering during plating is suppressed by performing a plating treatment before the tempering process, thereby suppressing the formation of voids at the interface with the hard, fresh martensite. As a result, the crack length can be suppressed to less than 0.5 mm (including 0 μm).

[0082] The crack length mentioned in this invention refers to the length of the crack generated on the outer side (tension side) of the bending section after performing a U-bending process with a bending radius R=4mm at a stroke speed of 1500mm / min, setting a 5mm thick spacer on the inner side (compression side) of the bending section of the galvanized steel sheet, and performing bending processing on the bending section until the two sides of the galvanized steel sheet, which are located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly attached to the spacer.

[0083] The method for determining the crack length is as follows. For galvanized steel sheet, as a high-speed U-bending process, a U-bending process with a bending radius R=4mm is performed at a stroke speed of 1500mm / min. As a close-fitting bending test (high-speed close-fitting bending test), a spacer with a thickness of 5mm is placed on the inner side (compression side) of the bending section of the galvanized steel sheet. The bending process is performed under the conditions of a stroke speed of 1500mm / min, a pressing load of 10 tons, and a pressing time of 3 seconds until the two sides of the steel sheet, which are located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly attached to the spacer. At this time, the length of the crack generated on the outer side (tension side) of the bending section is determined by visual observation.

[0084] The galvanized steel sheet of the present invention has a zinc coating on its surface. The zinc coating may be, for example, an electroplated zinc coating, a hot-dip galvanized coating, or an alloyed hot-dip galvanized coating.

[0085] The galvanized steel sheet of this invention has excellent tensile properties. In this invention, "excellent tensile properties" refers to high strength and excellent ductility.

[0086] The galvanized steel sheet of the present invention has a tensile strength TS of 780 MPa or higher and less than 1180 MPa. In this invention, "high strength" refers to a tensile strength TS of 780 MPa or higher and less than 1180 MPa.

[0087] In this invention, "excellent ductility" refers to an elongation of E1 of 11% or more.

[0088] It should be noted that the methods for determining tensile strength TS and elongation E1 are as described in the examples.

[0089] From the viewpoint of effectively obtaining the effects of the present invention, the thickness of the galvanized steel sheet of the present invention is preferably 0.2 mm or more and 3.2 mm or less.

[0090] The galvanized steel sheet of this invention exhibits excellent impact characteristics. Excellent impact characteristics, as described in this invention, refer to high load-bearing capacity, good fracture resistance, and good energy absorption. High load-bearing capacity, as described in this invention, refers to a yield ratio YR of 65% or higher and 95% or lower. The method for determining the yield ratio YR is as described in the examples.

[0091] In this invention, "good fracture resistance" means that the crack length during the U-bending + tight bending described in the embodiments is less than 0.5 mm. In this invention, "good impact resistance" means that, in the tensile test described in the embodiments, the value B obtained by dividing the area enclosed by the above-mentioned curves within the strain Q range of 0 to 4%, the straight line with stress P=0, and strain Q=4 by the tensile strength (TS) during the tensile test is 3.15% or higher.

[0092] (Composition of steel plates)

[0093] Next, the preferred composition of the steel sheet constituting the galvanized steel sheet will be explained. It should be noted that, unless otherwise specified, the "%" indicating the content of the constituent elements refers to "mass %".

[0094] C: 0.05~0.20%

[0095] C readily forms phases other than ferrite and also forms alloying compounds with Nb, Ti, etc., thus it is an element required to improve strength. When the C content is less than 0.05%, even with optimized manufacturing conditions, the desired strength cannot always be guaranteed. Therefore, the C content is preferably 0.05% or more, and more preferably 0.07% or more.

[0096] On the other hand, when the C content is greater than 0.20%, the strength of the martensite increases excessively, and even with optimized manufacturing conditions, the impact characteristics of the present invention are sometimes not obtained. Therefore, the C content is preferably 0.20% or less, and more preferably 0.18% or less.

[0097] Si: 0.10~2.00%

[0098] Si inhibits carbide formation, thus contributing to the stabilization of retained austenite. Furthermore, Si is a solid solution strengthening element, contributing to an improved balance between strength and ductility. To achieve this effect, the Si content is preferably 0.10% or more, more preferably 0.50% or more.

[0099] On the other hand, when the Si content is greater than 2.00%, the tempering of martensite is suppressed, thereby increasing the hardness difference between tempered martensite and ferrite. Even if the microstructure meets the requirements of the present invention, the desired yield strength ratio may not be obtained. Therefore, the Si content is preferably 2.00% or less, and more preferably 1.50% or less.

[0100] Mn: 2.0~3.5%

[0101] Mn is a martensite-forming element and also a solid solution strengthening element. Furthermore, Mn helps stabilize retained austenite. To achieve these effects, the Mn content is preferably 2.0% or more. More preferably, the Mn content is 2.5% or more.

[0102] On the other hand, when the Mn content is greater than 3.5%, the residual austenite fraction increases excessively, and the impact characteristics sometimes decrease. Therefore, the Mn content is preferably 3.5% or less, and more preferably 3.3% or less.

[0103] P: below 0.050%

[0104] Polymer (P) is an effective strengthening element for steel. However, when the P content is greater than 0.050%, it can sometimes significantly delay the alloying rate. Furthermore, when P is present in excess (greater than 0.050%), embrittlement occurs due to grain boundary segregation, sometimes deteriorating the fracture resistance upon impact even in steels that meet the requirements of this invention. Therefore, the P content is preferably 0.050% or less, more preferably 0.010% or less.

[0105] There is no specific lower limit for phosphorus content, but the currently feasible lower limit in industry is around 0.002%, which is actually higher than that.

[0106] S: Below 0.050%

[0107] S forms inclusions such as MnS, which contribute to cracks that cause metal flow along the weld. Even if the steel structure meets the requirements of this invention, its impact characteristics may sometimes be reduced. Therefore, the amount of S is preferably as low as possible, but from a manufacturing cost perspective, the S content is preferably 0.050% or less. The S content is more preferably 0.010% or less. There is no particular lower limit for the S content, but the currently industrially feasible lower limit is around 0.0002%, which is practically higher.

[0108] sol.Al: 0.005~2.000%

[0109] Al acts as a deoxidizer and is also a solid solution strengthening element. When the sol.Al content is less than 0.005%, these effects are sometimes not achieved, and even steel structures meeting the requirements of this invention may sometimes experience reduced strength. Therefore, the sol.Al content is preferably 0.005% or more.

[0110] On the other hand, when the sol.Al content is greater than 2.000%, the quality of the slab deteriorates during steelmaking. Furthermore, even if the steel microstructure meets the requirements of this invention, the fracture resistance may sometimes decrease when the sol.Al content is greater than 2.000%. Therefore, the sol.Al content is preferably 2.000% or less, and more preferably 1.000% or less.

[0111] N: below 0.010%

[0112] Nitrogen forms coarse nitrides, thus becoming the starting point for void formation during collision deformation, sometimes reducing collision properties. Therefore, the amount of nitrogen should be as low as possible, but from a manufacturing cost perspective, the nitrogen content is preferably below 0.010%, more preferably below 0.006%. It should be noted that there is no particular lower limit for the nitrogen content, but currently, the industrially feasible lower limit is around 0.0003%, which is practically higher.

[0113] The steel plate of the present invention preferably contains the above-mentioned constituent elements as basic components, with the balance consisting of iron (Fe) and unavoidable impurities.

[0114] The steel plate of the present invention may contain, depending on the desired properties, the following components (optional elements).

[0115] Nb: below 0.200%

[0116] Nb increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling and annealing. To achieve this effect, it is preferable that the Nb content is 0.001% or more. More preferably, the Nb content is 0.005% or more.

[0117] On the other hand, when the Nb content is greater than 0.200%, large amounts of coarse precipitates and inclusions are sometimes formed. In such cases, these coarse precipitates and inclusions become the starting point for voids and cracks during high-speed bending tests, which may result in poor fracture resistance. Therefore, when Nb is present, the Nb content is preferably 0.200% or less. More preferably, the Nb content is 0.060% or less.

[0118] Ti: below 0.200%

[0119] Similar to Nb, Ti increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling and annealing. To achieve this effect, it is preferable to set the Ti content to 0.001% or more. More preferably, the Ti content is 0.005% or more.

[0120] On the other hand, when the Ti content is greater than 0.200%, large amounts of coarse precipitates and inclusions are sometimes formed. In such cases, these coarse precipitates and inclusions become the starting point for voids and cracks during high-speed bending tests, which may result in poor fracture resistance. Therefore, when Ti is present, the Ti content is preferably 0.200% or less. More preferably, the Ti content is 0.060% or less.

[0121] V: Below 0.200%

[0122] Similar to Nb and Ti, V increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling and annealing. To achieve this effect, it is preferable to set the V content to 0.001% or more. More preferably, the V content is 0.003% or more. Even more preferably, the V content is 0.005% or more.

[0123] On the other hand, when the V content is greater than 0.200%, large amounts of coarse precipitates and inclusions are sometimes generated. In such cases, these coarse precipitates and inclusions become the starting point for voids and cracks during high-speed bending tests, which may prevent the achievement of good fracture resistance. Therefore, when V is present, the V content is preferably 0.200% or less. More preferably, the V content is 0.060% or less.

[0124] B: Below 0.0100%

[0125] Boron (B) is an element that improves hardenability by segregating at austenite grain boundaries. Furthermore, B is an element that controls ferrite formation and grain growth during cooling after annealing. To achieve this effect, it is preferable that the B content is 0.0001% or more. More preferably, the B content is 0.0002% or more. Even more preferably, the B content is 0.0003% or more.

[0126] On the other hand, when the boron content is greater than 0.0100%, cracks may form inside the steel sheet during hot rolling. Furthermore, during high-speed bending tests, the formation of voids and the propagation of cracks originating from the martensite may result in suboptimal fracture resistance. Therefore, when boron is present, the boron content is preferably 0.0100% or less. More preferably, the boron content is 0.0050% or less.

[0127] Cr: less than 1.000%

[0128] Cr is an element that improves hardenability; therefore, the addition of Cr generates an appropriate amount of martensite, thereby increasing TS and YS. To achieve this effect, the Cr content is preferably set to 0.0005% or more. Furthermore, the Cr content is more preferably 0.0010% or more. The Cr content is even more preferably 0.010% or more.

[0129] On the other hand, when the Cr content is greater than 1.000%, the martensite area ratio increases. During high-speed bending tests, voids are generated and cracks propagate starting from the martensite, which may prevent the attainment of the desired fracture resistance. Therefore, when Cr is present, the Cr content is preferably 1.000% or less. Furthermore, the Cr content is more preferably 0.250% or less, and even more preferably 0.100% or less.

[0130] Ni: below 1.000%

[0131] Ni is an element that improves hardenability; therefore, the addition of Ni leads to the formation of a large amount of tempered martensite, thus increasing TS and YS. To achieve this effect, it is preferable that the Ni content is 0.005% or more. More preferably, the Ni content is 0.010% or more. Even more preferably, the Ni content is 0.020% or more.

[0132] On the other hand, when the Ni content is greater than 1.000%, the martensite area ratio increases. During high-speed bending tests, voids and crack propagation originating from this martensite may occur, potentially resulting in unsatisfactory fracture resistance properties. Therefore, when Ni is present, the Ni content is preferably 1.000% or less. More preferably, the Ni content is 0.800% or less.

[0133] Mo: 1.000% or less

[0134] Mo is an element that improves hardenability, and therefore, the addition of Mo leads to the formation of a large amount of tempered martensite, thus increasing TS and YS. To achieve this effect, it is preferable that the Mo content is 0.010% or more. More preferably, the Mo content is 0.030% or more.

[0135] On the other hand, when the Mo content is greater than 1.000%, the martensite area ratio increases. During high-speed bending tests, voids may form and cracks may propagate starting from this martensite, potentially resulting in poor fracture resistance. Therefore, when Mo is present, the Mo content is preferably 1.000% or less. More preferably, the Mo content is 0.500% or less, even more preferably 0.450% or less, and still more preferably 0.400% or less.

[0136] Sb: below 0.200%

[0137] From the viewpoint of suppressing nitriding, oxidation, and decarburization in the vicinity of the steel plate surface, Sb can be added as needed. By suppressing such nitriding and oxidation, it has the effect of preventing a reduction in the amount of martensite formed on the steel plate surface and improving impact characteristics. However, when Sb is greater than 0.200%, impact characteristics may sometimes decrease due to grain boundary embrittlement. Therefore, when Sb is present, the Sb content is preferably 0.200% or less. Even a low Sb content can achieve the effects of the present invention, so the lower limit of each content is not particularly limited. To more effectively obtain the effect of improving impact characteristics, the Sb content is preferably 0.003% or more. The Sb content is more preferably 0.005% or more.

[0138] Sn: below 0.200%

[0139] Similar to Sb, Sn can be added as needed from the viewpoint of suppressing nitriding, oxidation, and decarburization in the vicinity of the steel plate surface. By suppressing such nitriding and oxidation, it has the effect of preventing a reduction in the amount of martensite formed on the steel plate surface and improving impact characteristics. However, when Sn is greater than 0.200%, impact characteristics may sometimes decrease due to grain boundary embrittlement. Therefore, when Sn is present, the Sn content is preferably 0.200% or less. The effects of the present invention can be obtained even with a low Sn content, so the lower limit of each content is not particularly limited. To more effectively obtain the effect of improving impact characteristics, the Sn content is preferably 0.003% or more. The Sn content is more preferably 0.005% or more.

[0140] Cu: below 1.000%

[0141] Cu is an element that improves hardenability; therefore, the addition of Cu leads to the formation of a large amount of martensite, thus increasing TS and YS. To achieve this effect, it is preferable that the Cu content is 0.005% or more. More preferably, the Cu content is 0.010% or more. Even more preferably, the Cu content is 0.020% or more.

[0142] On the other hand, when the Cu content is greater than 1.000%, the martensite area ratio sometimes increases excessively. Additionally, large amounts of coarse precipitates and inclusions may be formed. In such cases, the excessively formed martensite and coarse precipitates and inclusions can lead to the formation of voids and the propagation of cracks starting from the aforementioned martensite during high-speed bending tests, potentially resulting in poor fracture resistance. Therefore, when Cu is present, the Cu content is preferably set to 1.000% or less. More preferably, the Cu content is 0.200% or less.

[0143] Ta: Below 0.100%

[0144] Similar to Ti, Nb, and V, Ta increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling and annealing. Furthermore, Ta partially dissolves in Nb carbides and Nb carbonitrides, forming composite precipitates such as (Nb,Ta)(C,N). This suppresses the coarsening of precipitates and stabilizes precipitation strengthening. To achieve this effect, it is preferable to set the Ta content to 0.001% or more. The Ta content is more preferably 0.002% or more.

[0145] On the other hand, when the Ta content is greater than 0.100%, large amounts of coarse precipitates and inclusions are sometimes formed. In such cases, during high-speed bending tests, the formation of voids and the propagation of cracks originating from the aforementioned martensite may result in poor fracture resistance. Therefore, when Ta is present, the Ta content is preferably 0.100% or less.

[0146] W: Below 0.500%

[0147] W is an element that improves hardenability, and therefore, the addition of W leads to the formation of a large amount of martensite, thus increasing TS and YS. To achieve this effect, it is preferable to set the W content to 0.001% or more. More preferably, the W content is 0.010% or more. Even more preferably, the W content is 0.030% or more.

[0148] On the other hand, when the W content is greater than 0.500%, the martensite area ratio increases. During high-speed bending tests, voids and crack propagation originating from this martensite may occur, potentially resulting in poor fracture resistance. Therefore, when W is present, the W content is preferably 0.500% or less. More preferably, the W content is 0.450% or less, and even more preferably 0.400% or less.

[0149] Mg: below 0.0200%

[0150] Mg is an effective element used to spheroidize inclusions such as sulfides and oxides, thereby increasing the fracture resistance of steel plates. To achieve this effect, it is preferable to set the Mg content to 0.0001% or more. More preferably, the Mg content is 0.0002% or more.

[0151] On the other hand, when the Mg content is greater than 0.0200%, large amounts of coarse precipitates and inclusions are sometimes formed. In such cases, excessively coarse precipitates and inclusions may lead to the formation of voids and the propagation of cracks starting from the martensite during high-speed bending tests, potentially resulting in poor fracture resistance. Therefore, when Mg is present, the Mg content is preferably set to 0.0200% or less.

[0152] Zn: below 0.0200%

[0153] Zinc (Zn) is an effective element used to spherize inclusions and increase the fracture resistance of steel plates. To achieve this effect, the Zn content is preferably 0.0005% or more. More preferably, the Zn content is 0.0010% or more.

[0154] On the other hand, when the Zn content is greater than 0.0200%, large amounts of coarse precipitates and inclusions are sometimes formed. In such cases, these excessively coarse precipitates and inclusions may lead to the formation of voids and the propagation of cracks starting from the martensite during high-speed bending tests, potentially resulting in poor fracture resistance. Therefore, when Zn is present, the Zn content is preferably set to 0.0200% or less.

[0155] Co: below 0.0200%

[0156] Like Zn, Co is an effective element used to spherize inclusions and increase the fracture resistance of steel plates. To achieve this effect, the Co content is preferably set to 0.0010% or higher.

[0157] On the other hand, when the Co content is greater than 0.0200%, large amounts of coarse precipitates and inclusions are sometimes formed. In such cases, excessively coarse precipitates and inclusions may lead to the formation of voids and the propagation of cracks starting from the martensite during high-speed bending tests, potentially resulting in poor fracture resistance. Therefore, when Co is present, the Co content is preferably set to 0.0200% or less.

[0158] Zr: below 0.1000%

[0159] Like Zn and Co, Zr is an effective element used to spherize inclusions and increase the fracture resistance of steel plates. To achieve this effect, the Zr content is preferably 0.0005% or more. The Zr content is further preferably 0.0010% or more.

[0160] On the other hand, when the Zr content is greater than 0.1000%, the excessively large precipitates and inclusions may lead to the formation of voids and the propagation of cracks starting from the martensite during high-speed bending tests, potentially resulting in poor fracture resistance. Therefore, when Zr is present, the Zr content is preferably set to 0.1000% or less.

[0161] Ca: below 0.0200%

[0162] Ca exists in steel as inclusions. When the Ca content is greater than 0.0200%, large, coarse inclusions are sometimes formed. In such cases, these excessively coarse precipitates and inclusions may lead to the formation of voids and the propagation of cracks starting from the martensite during high-speed bending tests, potentially resulting in poor fracture resistance. Therefore, when Ca is present, the Ca content is preferably set to 0.0200% or less. The Ca content is preferably 0.0020% or less.

[0163] It should be noted that there is no specific lower limit for the Ca content, but the Ca content is preferably 0.0005% or higher. Furthermore, due to limitations in production technology, the Ca content is more preferably 0.0010% or higher.

[0164] Se: less than 0.0200%, Te: less than 0.0200%, Ge: less than 0.0200%, As: less than 0.0500%, Sr: less than 0.0200%, Cs: less than 0.0200%, Hf: less than 0.0200%, Pb: less than 0.0200%, Bi: less than 0.0200%, and REM: less than 0.0200%.

[0165] Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM are all effective elements used to enhance the fracture resistance of steel plates. To achieve this effect, the contents of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM are preferably set to 0.0001% or more. On the other hand, when the contents of Se, Te, Ge, Sr, Cs, Hf, Pb, Bi, and REM are greater than 0.0200%, or the content of As is greater than 0.0500%, large amounts of coarse precipitates and inclusions may be generated. In such cases, these excessively coarse precipitates and inclusions may lead to the formation of voids and the propagation of cracks starting from the aforementioned martensite during high-speed bending tests, potentially resulting in suboptimal fracture resistance. Therefore, when the product contains at least one of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi and REM, it is preferable that the contents of Se, Te, Ge, Sr, Cs, Hf, Pb, Bi and REM are set to 0.0200% or less, and the content of As is set to 0.0500% or less.

[0166] The Se content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0167] The Se content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0168] The Te content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0169] The Te content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0170] The Ge content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0171] The Ge content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0172] The As content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0173] The As content is more preferably 0.0490% or less, and even more preferably 0.0480% or less.

[0174] The Sr content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0175] The Sr content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0176] The Cs content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0177] The Cs content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0178] The Hf content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0179] The Hf content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0180] The Pb content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0181] The Pb content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0182] The Bi content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0183] The Bi content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0184] The REM content is more preferably 0.0002% or more, and even more preferably 0.0003% or more.

[0185] The REM content is more preferably 0.0190% or less, and even more preferably 0.0180% or less.

[0186] It should be noted that, in this invention, REM refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and the lanthanides from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM content in this invention refers to the total content of one or more elements selected from the above-mentioned REMs. There is no particular limitation on REMs, but La and / or Ce are preferred.

[0187] The aforementioned unavoidable impurities are those that inevitably mix in from raw materials, manufacturing processes, or manufacturing equipment, and are permitted to be included to a extent that does not impair the purpose of this invention. Examples of raw materials include iron ore, reduced iron, and waste. Examples of impurities include, for example, H and O.

[0188] <Manufacturing Method of Galvanized Steel Sheet>

[0189] The following is a detailed description of one embodiment of the method for manufacturing the galvanized steel sheet of the present invention. It should be noted that, unless otherwise specified, the temperatures used for heating or cooling steel billets (steel raw materials), steel sheets, etc., as shown below refer to the surface temperatures of the steel billets (steel raw materials), steel sheets, etc.

[0190] The method for manufacturing galvanized steel sheet of the present invention includes: a hot rolling process, wherein a steel billet having the above-mentioned composition is hot rolled at a finishing rolling temperature of 850 to 950°C and coiled at a coiling temperature of 600°C or lower; a cold rolling process, wherein the hot-rolled steel sheet after the hot rolling process is cold-rolled at a reduction rate of more than 20%; an annealing process, wherein the cold-rolled steel sheet after the cold rolling process is heated to an annealing temperature of 750°C or higher under the condition that A as shown in the following formula (1) satisfies 4 or more and 70 or less, and held at the annealing temperature for 30 seconds or more; and a coating process. The process includes: after annealing, cooling to a temperature range of 300–600°C and holding it within this temperature range for 10–300 seconds, followed by galvanizing the steel plate surface; quenching and tempering processes, after plating, cooling to a cooling stop temperature of (Ms-300°C)–(Ms-50°C) and then holding it at a tempering temperature of 250–500°C for 20–500 seconds; and a cooling process, after quenching and tempering, cooling from the tempering temperature to 50°C at an average cooling rate of 20°C / s or higher.

[0191] In the formula, T Ac1 Temperature at point Ac1 (°C), T RT Annealing temperature (°C), t RT From the start of the annealing process through heat treatment until the annealing temperature T is reached. RT The time (in seconds) required up to this point, t Ac1 The temperature T from the start of the heat treatment process in the initial annealing stage until point Ac1 is reached. Ac1 The time (in seconds) required up to this point, T(t): the temperature (°C) t seconds after the start of the heat treatment in the annealing process.

[0192] (Hot rolling process)

[0193] First, the conditions for the hot rolling process will be explained.

[0194] Finishing rolling temperature: 850~950℃

[0195] When the finishing rolling temperature is below 850°C, a ferrite phase transformation occurs during rolling, resulting in a decrease in local strength. Therefore, even if the microstructure meets the requirements of this invention, the required strength may not be achieved. Thus, the finishing rolling temperature is 850°C or higher, preferably 880°C or higher.

[0196] On the other hand, when the finishing rolling temperature is above 950°C, the grains coarsen, and even if the microstructure meets the requirements of the present invention, the strength may not be obtained. Therefore, the finishing rolling temperature is 950°C or below, preferably 930°C or below.

[0197] Winding temperature: below 600℃

[0198] When the coiling temperature exceeds 600°C, the carbides in the hot-rolled steel sheet coarsen. These coarsened carbides do not completely melt during the homogenization process in annealing, thus sometimes failing to achieve the desired impact characteristics. Therefore, a coiling temperature of 600°C or below is preferred, preferably 580°C or below. While there is no particular limitation on the lower limit of the coiling temperature, from the viewpoint of minimizing shape defects in the steel sheet and preventing excessive hardening, a coiling temperature of 400°C or above is preferable.

[0199] (Cold rolling process)

[0200] Hot-rolled steel sheets obtained through the hot rolling process are pretreated by pickling, degreasing, etc., using commonly known methods, and then cold-rolled. The conditions for the cold rolling process are explained.

[0201] Cold rolling reduction rate: greater than 20%

[0202] When the cold rolling reduction rate (cumulative reduction rate) is below 20%, it cannot promote the recrystallization of ferrite. Unrecrystallized ferrite remains, and in cases where the steel structure of the present invention cannot be obtained, coarsening and inhomogenization of the steel structure are likely to occur during the annealing process. In the final product, TS and bendability may be reduced.

[0203] In addition, when the reduction rate of cold rolling is below 20%, the fracture resistance may sometimes decrease.

[0204] Therefore, the reduction rate of cold rolling is greater than 20%, preferably more than 30%.

[0205] There is no specific upper limit, but the reduction rate of cold rolling is preferably below 95%.

[0206] (Annealing process)

[0207] Next, the conditions for the annealing process when annealing cold-rolled steel sheets obtained through the cold rolling process will be explained.

[0208] Heat to the annealing temperature under the condition that A, as expressed by equation (1), is greater than 4 and less than 70.

[0209]

[0210] In the formula, T Ac1 Temperature at point Ac1 (°C), T RT Annealing temperature (°C), t RTFrom the start of the annealing process through heat treatment until the annealing temperature T is reached. RT The time (in seconds) required up to this point, t Ac1 The temperature T from the start of the heat treatment process in the initial annealing stage until point Ac1 is reached. Ac1 The time (in seconds) required up to this point, T(t): the temperature (°C) t seconds after the start of the heat treatment in the annealing process.

[0211] As for the heating conditions up to the annealing temperature, when A, as specified in formula (1), is less than 4, the formation of austenite becomes insufficient, and excess ferrite is formed, resulting in a steel structure that cannot be obtained according to the present invention. Therefore, the fracture resistance characteristics under high-speed bending are reduced. Therefore, A is set to 4 or more, preferably 5 or more, and more preferably 8 or more.

[0212] On the other hand, as the heating condition up to the annealing temperature, when A, as specified in formula (1), is greater than 70, element diffusion occurs, and the elements in the austenite during annealing are uniformly distributed. Therefore, the formation of bainite in the subsequent holding process before quenching and the tempering process is suppressed, and the steel structure of the present invention cannot be obtained. As a result, the fracture resistance during high-speed bending is reduced. Therefore, A is set to 70 or less, preferably 65 or less, and more preferably 60 or less.

[0213] It should be noted that T Ac1 It can be obtained using the following formula (3).

[0214] T Ac1 =723+29×[Si%]-21×[Mn%]-17×[Ni%]+17×[Cr%]…Equation (3)

[0215] In equation (3), [element symbol %] is the content (mass %) of each element contained in the steel plate, and elements that are not contained are set to 0 (zero).

[0216] Annealing temperature: above 750℃, holding time: above 30 seconds

[0217] When the annealing temperature is below 750°C, the formation of austenite becomes insufficient, resulting in the formation of excess ferrite, and the steel microstructure of the present invention cannot be obtained. Therefore, the annealing temperature is 750°C or higher.

[0218] On the other hand, there is no particular upper limit to the annealing temperature, but from a manufacturing point of view, it is preferable to be below 900°C.

[0219] Furthermore, when the holding time at the annealing temperature is less than 30 seconds, the formation of austenite becomes insufficient, resulting in the formation of excess ferrite, and the steel microstructure of the present invention cannot be obtained. Therefore, the holding time at the annealing temperature is 30 seconds or more, preferably 60 seconds or more. There is no particular upper limit to the holding time, but in order not to impair productivity, it is preferable to set the holding time to 600 seconds or less.

[0220] (Plating process)

[0221] Next, the conditions for the plating process will be explained. In the plating process, after the annealing process, the plate is cooled to a temperature range of 300 to 600°C, held at this temperature range for 10 to 300 seconds, and then galvanized.

[0222] Holding time within a temperature range of 300–600℃: 10–300 seconds

[0223] Cooling to a temperature range of 300–600°C after annealing and holding it within that range for 10–300 seconds is effective for obtaining bainite. Furthermore, through bainite formation, carbon is enriched in the untransformed austenite, resulting in a large amount of retained austenite. Sometimes, these effects cannot be achieved when the holding time within the 300–600°C range is less than 10 seconds. Additionally, sometimes the desired yield strength ratio is not obtained when the holding time within the 300–600°C range is less than 10 seconds. Therefore, a holding time of 10 seconds or more is necessary.

[0224] On the other hand, when the holding time is greater than 300 seconds in the temperature range of 300 to 600 °C, bainite is excessively generated, C is excessively enriched in the untransformed austenite, pearlite is generated, and sometimes the desired amount of residual austenite is not obtained.

[0225] Therefore, the holding time should be less than 300 seconds, preferably less than 100 seconds.

[0226] In addition, after the above-mentioned holding, the steel sheet is subjected to galvanizing treatment. Galvanizing treatment includes, for example, electro-galvanizing, hot-dip galvanizing, or alloyed hot-dip galvanizing of the steel sheet surface. When hot-dip galvanizing the steel sheet surface, it is preferable to immerse the steel sheet obtained above in a galvanizing bath at a temperature of 440°C or higher and 500°C or lower to form a hot-dip galvanized layer on the steel sheet surface. Here, it is preferable to adjust the coating adhesion by gas wiping or the like after the coating treatment. Alloying can also be performed on the hot-dip galvanized steel sheet. When alloying the hot-dip galvanized layer, it is preferable to hold the alloying at a temperature range of 450°C or higher and 580°C for 1 second or more and 60 seconds or less. It should be noted that when electro-galvanizing the steel sheet surface, the processing conditions for electro-galvanizing are not particularly limited, and conventional methods can be used.

[0227] (Quenching and tempering process)

[0228] Next, the conditions for the quenching and tempering processes performed after the plating process will be explained.

[0229] Cooling stop temperature: (Ms-300℃)~(Ms-50℃)

[0230] When the cooling stop temperature exceeds (Ms-50°C), there are cases where the formation of tempered martensite becomes insufficient or excessive fresh martensite is formed, making it impossible to obtain the steel microstructure of the present invention.

[0231] On the other hand, when the cooling stop temperature is below (Ms-300°C), tempered martensite becomes excessive, and the formation of retained austenite sometimes becomes insufficient. Therefore, the cooling stop temperature is (Ms-300°C) to (Ms-50°C). The cooling stop temperature is preferably (Ms-280°C) or higher. Furthermore, the cooling stop temperature is preferably (Ms-100°C) or lower. It should be noted that in this invention, the cooling rate up to the cooling stop temperature is not limited.

[0232] It should be noted that Ms is the martensitic phase transformation start temperature, which can be obtained by the following equation (4).

[0233] Ms(℃)=550-361×[C%]-39×[Mn%]-10×[Cu%]-17×[Ni%]-20×[Cr%]-5×[Mo%]-35×[V%]+30×[Al%]-5×[W%]+15×[Co%]…Equation (4)

[0234] In equation (4), [element symbol %] represents the content (mass %) of each element contained in the steel plate, and elements that are not contained are set to 0.

[0235] Tempering temperature: 250–500℃, holding time: 20–500 seconds

[0236] It is believed that when the tempering temperature is below 250℃, the tempering of martensite becomes insufficient, and voids are easily generated at the interface between tempered martensite and ferrite during a single processing, reducing the collision characteristics. Therefore, the tempering temperature is 250℃ or higher, preferably 300℃ or higher.

[0237] On the other hand, it is believed that when the tempering temperature is above 500°C, the tempering of martensite and bainite becomes excessive, and voids are easily generated at the interface between fresh martensite and tempered martensite and bainite during a single processing, reducing the collision characteristics. Therefore, the tempering temperature is below 500°C, preferably below 450°C.

[0238] Furthermore, when the holding time at the tempering temperature is less than 20 seconds, the tempering of martensite is considered insufficient, and the impact characteristics decrease. Therefore, the holding time at the tempering temperature is 20 seconds or more, preferably 30 seconds or more. Additionally, when the holding time at the tempering temperature is greater than 500 seconds, the proportion of retained austenite sometimes decreases. Therefore, the upper limit of the holding time at the tempering temperature is 500 seconds or less, preferably 450 seconds or less.

[0239] (Cooling process)

[0240] The conditions for the cooling process following the quenching and tempering processes are described.

[0241] Average cooling rate from the above tempering temperature to 50°C: 20°C / s or higher

[0242] When the average cooling rate from the above tempering temperature to 50°C is less than 20°C / s, the collision characteristics of the present invention cannot be obtained. The reason for this is not yet clear, but it is believed to be as follows: In order to suppress the formation of voids in the primary processing section and improve the collision characteristics, it is necessary to reduce the hardness difference between the soft phase (ferrite) and the hard phase (fresh martensite) using an intermediate hardness phase (tempered martensite, bainite). The hardness difference between the soft phase and the intermediate hardness phase is reduced by softening the bainite formed before plating and the martensite formed during quenching in the tempering process, thereby suppressing the formation of voids. The hardness difference between the hard phase and the intermediate hardness phase is reduced by generating relatively hard bainite in the tempering process, thereby suppressing the formation of voids. When the bainite formed during the tempering process softens, the hardness difference between it and the hard phase increases. Therefore, a high-temperature plating treatment is performed before the tempering process to expose the bainite to heat, thereby accelerating the cooling rate after the tempering process to suppress the tempering of the bainite during cooling. This reduces the hardness difference with the soft phase and suppresses the formation of voids. It is therefore considered that when the average cooling rate from the tempering process to room temperature is less than 20°C / s, the bainite is tempered during cooling, increasing the hardness difference with the hard phase. This makes it easier for voids to form at the interface during a single machining operation, reducing collision characteristics. The average cooling rate is preferably 25°C / s or higher. There is no particular upper limit to the average cooling rate, but from the perspective of energy saving of the cooling equipment, it is preferably 70°C / s or lower.

[0243] The average cooling rate (°C / s) mentioned above is calculated by "(tempering temperature (°C) - 50) / cooling time (s) from tempering temperature to 50°C".

[0244] For purposes such as shape correction and surface roughness adjustment, the galvanized steel sheet of the present invention can be subjected to leveling rolling. However, when the leveling reduction rate of leveling rolling is greater than 0.5%, the bending performance may deteriorate due to surface solidification. Therefore, it is preferable to keep the leveling reduction rate at 0.5% or less. More preferably, it is 0.3% or less. In addition, various coating treatments such as resin or grease coating can also be performed.

[0245] There are no particular limitations on the conditions for other manufacturing methods, but the following conditions are preferred.

[0246] To prevent macroscopic segregation, slabs are preferably manufactured using continuous casting, but ingot casting or thin slab casting methods are also acceptable. For hot rolling, the slab can be temporarily cooled to room temperature and then reheated for hot rolling. Alternatively, the slab can be loaded into a furnace for hot rolling without cooling to room temperature. An energy-saving process involving hot rolling immediately after a short period of holding can also be used. When heating the slab, to prevent increased rolling load and carbide melting, heating to 1100°C or higher is preferred. Furthermore, to prevent increased oxide scale loss, the slab heating temperature is preferably set below 1300°C.

[0247] When hot rolling slabs, from the viewpoint of preventing rolling defects by reducing the heating temperature of the slab, the rough-rolled bars can also be heated. Alternatively, a so-called continuous rolling process can be used, in which the rough bars are joined together and continuously finished rolled. Furthermore, to reduce rolling load and homogenize shape and material, lubricated rolling with a friction coefficient of 0.10 to 0.25 is preferably performed in all or some of the finishing rolling passes.

[0248] The rolled steel sheet can have its oxide scale removed by pickling. After pickling, it is then subjected to cold rolling, annealing, and galvanizing under the conditions described above.

[0249] <Components and their manufacturing methods>

[0250] Next, the components of the present invention and their manufacturing method will be described.

[0251] The component of the present invention is formed by performing at least one of forming and welding on the galvanized steel sheet of the present invention. Furthermore, the manufacturing method of the component of the present invention includes the steps of performing at least one of forming and welding on the galvanized steel sheet manufactured by the manufacturing method of the galvanized steel sheet of the present invention.

[0252] The galvanized steel sheet of the present invention exhibits excellent tensile and impact properties. Therefore, components obtained using the galvanized steel sheet of the present invention also possess excellent tensile and impact properties, and are less prone to fracture upon impact deformation. Consequently, the components of the present invention are suitable for use as energy-absorbing components in automotive parts.

[0253] Forming can be performed using general processing methods such as stamping without restriction. Similarly, welding can be performed using general welding methods such as spot welding and arc welding without restriction.

[0254] Example

[0255] The present invention will be specifically described with reference to the embodiments. The scope of the present invention is not limited to the following embodiments.

[0256] Steels with the compositions shown in Table 1 are melted in a vacuum melting furnace and then rolled into billets. These billets are then heated and subjected to hot rolling, cold rolling, annealing, plating, quenching, tempering, and cooling under the conditions shown in Table 2 to produce galvanized steel sheets. In the plating process, an electro-galvanized layer (EG), a hot-dip galvanized layer (GI), or an alloyed hot-dip galvanized layer (GA) is formed on the surface of the steel sheet. In the electro-galvanizing process, the steel sheet is immersed in a zinc solution and electrolyzed to form a coating with an adhesion weight of 10–100 g / m². 2 The electroplated zinc layer (EG). Alternatively, in hot-dip galvanizing, the steel sheet is immersed in a plating bath, forming a coating with an adhesion weight of 10–100 g / m². 2 The hot-dip galvanized layer (GI) is formed on the steel sheet. Alternatively, in alloyed hot-dip galvanizing, after the hot-dip galvanized layer is formed, alloying treatment is performed to form an alloyed hot-dip galvanized layer (GA). It should be noted that the final thickness of each galvanized steel sheet is 1.2 mm.

[0257] In Table 2, A is represented by the following formula (1).

[0258]

[0259] In the formula, T Ac1 Temperature at point Ac1 (°C), T RT Annealing temperature (°C), t RT From the start of the annealing process through heat treatment until the annealing temperature T is reached. RT The time (in seconds) required up to this point, t Ac1 The temperature T from the start of the heat treatment process in the initial annealing stage until point Ac1 is reached. Ac1 The time (in seconds) required up to this point, T(t): the temperature (°C) t seconds after the start of the heat treatment in the annealing process.

[0260]

[0261] After the obtained galvanized steel sheet is subjected to leveling rolling with a reduction rate of 0.2%, the area ratios of ferrite (F), bainite (B), tempered martensite (TM), fresh martensite (FM), and retained austenite (RA) are calculated according to the above method.

[0262] In addition, following the above method, the area ratios of low-Mn ferrite (LF) and high-Mn ferrite (HF) relative to all ferrite, the area ratios of hard second phases with a perimeter of more than 30% relative to the total area ratio of hard second phases composed of retained austenite and fresh martensite, and the area ratios of hard second phases in contact with bainite are calculated.

[0263] In addition, the tensile properties (tensile strength TS, elongation E1) and impact properties (load resistance (yield ratio YR), fracture resistance, and energy absorption capacity (B)) are evaluated according to the following test methods.

[0264] Tensile Test

[0265] JIS No. 5 tensile test pieces (JIS Z2201) were cut from each galvanized steel sheet at a direction perpendicular to the rolling direction, and subjected to strain rates of 10... -3 The tensile test according to JIS Z2241 (2011) is used to determine the tensile strength (TS), the yield ratio (YR) obtained by dividing the yield strength by the tensile strength, the elongation (E1), and the value B obtained by dividing the area enclosed by the above curve in the stress P (MPa)-strain Q (%) curve within the range of strain Q from 0 to 4%, the straight line with stress P=0, and strain Q=4 by the tensile strength (TS) (hereinafter, refer to Equation (2)). It should be noted that when TS is 780 MPa or more and less than 1180 MPa and E1 is 11% or more, the tensile properties are evaluated as good; when YR is 65% or more and less than 95%, the load-bearing capacity is evaluated as high; and when B is 3.15% or more, the energy absorption capacity is evaluated as good.

[0266]

[0267] In the formula, P: stress (MPa), Q: strain (%), TS: tensile strength (MPa).

[0268] <High-speed U-bend + High-speed close-fitting bend test>

[0269] Using the obtained galvanized steel sheet, a test piece with a thickness of 1.2mm × width of 60mm × length of 30mm was prepared by grinding the two width-measured end faces. This piece was used for U-bending processing (high-speed U-bending processing). A hydraulic bending testing machine was used to perform the processing with a punch bending radius of R=4mm, a stroke speed of 1500mm / min, and bending in the length direction (bending edge length: 30mmL).

[0270] Next, as a tight-fitting bending test (high-speed tight-fitting bending test), a hydraulic bending testing machine was used. The thickness of the spacer sandwiched between the galvanized steel sheets was set to 5 mm. The test was conducted at a stroke speed of 1500 mm / min (high speed), a pressing load of 10 tons, and a pressing time of 3 seconds. Furthermore, if no cracks larger than 0.5 mm appeared on the outer side (tensile side) of the bent section, the fracture resistance was evaluated as good. In the table, cases with good fracture resistance are indicated by ○, and cases with poor fracture resistance are indicated by ×.

[0271]

[0272] The galvanized steel sheet of the invention exhibits excellent tensile and impact properties. On the other hand, the galvanized steel sheet of the comparative example has poor tensile and impact properties at least once.

[0273] Industrial availability

[0274] According to the present invention, galvanized steel sheets with excellent tensile and impact properties can be obtained. When components obtained from the galvanized steel sheets of the present invention are used as automotive parts, they can contribute to the weight reduction of automobiles and greatly contribute to the high performance of automobile bodies.

Claims

1. A galvanized steel sheet, comprising a steel sheet and a zinc coating on the surface of the steel sheet, wherein, The steel plate has the following microstructure: Based on the area ratio at 1 / 8 to 3 / 8 of the plate thickness, ferrite: less than 30.0% (inclusive), bainite: greater than 40.0% and less than 80.0%, the total of tempered martensite and bainite: greater than 60.0%, retained austenite: more than 1.5% and less than 20%, and fresh martensite: less than 20.0% (inclusive). When the ferrite content is greater than 0.0% by area, the area ratio of high-Mn ferrite, where the Mn concentration is greater than 0.80 times that of the steel plate relative to the total area ratio of the ferrite, is 30% or more. The hard second phase, comprising more than 30% of the perimeter of the hard second phase in contact with bainite, has an area ratio of more than 30% relative to the total area ratio of the hard second phase composed of the retained austenite and the fresh martensite. For the galvanized steel sheet, after performing a U-bending process with a bending radius R=4mm at a stroke speed of 1500mm / min, a 5mm thick spacer is placed on the inner side of the bending section of the galvanized steel sheet. The bending process is then performed at a stroke speed of 1500mm / min, a pressing load of 10 tons, and a pressing time of 3 seconds, until both sides of the galvanized steel sheet, located at positions opposite to the upper and lower surfaces in the thickness direction of the spacer, are tightly adhered to the spacer. At this point, the crack generated on the outer side of the bending section is less than 0.5mm. The galvanized steel sheet has a tensile strength of 780 MPa or higher and less than 1180 MPa, and a yield ratio of 65% or higher and less than 95%.

2. The galvanized steel sheet according to claim 1, wherein, The steel plate has a composition, by mass%, of C: 0.05-0.20%, Si: 0.10-2.00%, Mn: 2.0-3.5%, P: less than 0.050%, S: less than 0.050%, sol.Al: 0.005-2.000%, and N: less than 0.010%, with the balance consisting of Fe and unavoidable impurities.

3. The galvanized steel sheet according to claim 2, wherein, The composition, by mass%, further comprises elements selected from the following: Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less. At least one of the following: Co: 0.0200%, Zr: 0.1000%, Ca: 0.0200%, Se: 0.0200%, Te: 0.0200%, Ge: 0.0200%, As: 0.0500%, Sr: 0.0200%, Cs: 0.0200%, Hf: 0.0200%, Pb: 0.0200%, Bi: 0.0200%, and REM: 0.0200%.

4. The galvanized steel sheet according to any one of claims 1 to 3, wherein, The zinc coating is an electroplated zinc coating, a hot-dip galvanized coating, or an alloyed hot-dip galvanized coating.

5. A component formed by forming and welding at least one of the galvanized steel sheet as described in any one of claims 1 to 4.

6. A method for manufacturing a galvanized steel sheet, comprising: The hot rolling process, wherein for a steel billet having the composition described in claim 2 or 3, hot rolling is performed at a finishing temperature of 850 to 950°C and coiling is performed at a coiling temperature of 600°C or below. The cold rolling process, wherein the hot-rolled steel sheet after the hot rolling process is cold-rolled with a reduction rate of more than 20%; The annealing process, wherein the cold-rolled steel sheet after the cold rolling process is heated to an annealing temperature of 750°C or higher under the condition that A as shown in the following formula (1) satisfies 4 or more and 70 or less, and is held at the annealing temperature for 30 seconds or more; In the plating process, after the annealing process, the plate is cooled to a temperature range of 300 to 600°C and held at that temperature range for 10 to 300 seconds before galvanizing the steel plate surface. The quenching and tempering process, wherein after the plating process, the material is cooled to a cooling stop temperature of (Ms-300℃) to (Ms-50℃), and then held at a tempering temperature of 250 to 500℃ for 20 to 500 seconds; and The cooling process involves, after the quenching and tempering processes, cooling from the tempering temperature to 50°C at an average cooling rate of 20°C / s or higher. In the formula, T Ac1 Temperature at point Ac1 (°C) T RT Annealing temperature (°C) t RT From the start of the annealing process through heat treatment until the annealing temperature T is reached. RT The time (in seconds) required up to this point. t Ac1 The temperature T from the start of the heat treatment process in the initial annealing stage until point Ac1 is reached. Ac1 The time (in seconds) required up to this point. T(t): Temperature (°C) t seconds after the start of the heat treatment process in the annealing step.

7. The method for manufacturing galvanized steel sheet according to claim 6, wherein, The galvanizing process refers to the treatment of the steel plate surface by electro-galvanizing, hot-dip galvanizing, or alloyed hot-dip galvanizing.

8. A method for manufacturing a component, wherein, A component is made by performing at least one of forming and welding on the galvanized steel sheet according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • HIGH STRENGTH STEEL SHEET, HIGH STRENGTH HOT-DIP GALVANIZED STEEL SHEET, AND HIGH STRENGTH HOT-DIP GALVANNEALED STEEL SHEET EACH HAVING MAXIMUM TENSILE STRENGTH OF 780 MPa AND EXCELLENT IN COLLISION CHARACTERISTIC, AND PRODUCTION METHODS OF THEM

    JP2015175061A

  • Galvanized steel sheets, components, and their manufacturing methods

    JP2022034015A