Negative electrode active material particles, negative electrode for energy storage components and energy storage components
By using natural graphite particles with mixed particle sizes and structures in lithium-ion secondary batteries, the problems of internal resistance and charge-discharge cycle capacity retention were solved, resulting in a negative electrode active material layer with low resistance and high durability.
Patent Information
- Application Number
- CN202580029172.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-25
- Filing Date
- 2025-03-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to reduce the internal resistance of lithium-ion secondary batteries while maintaining capacity retention during charge-discharge cycles, especially when using small-diameter solid natural graphite particles as the negative electrode active material, as durability is easily reduced, leading to a decrease in capacity.
By using a mixture of solid natural graphite particles with an average particle size of 3μm to 8μm and natural graphite particles with a particle size of 10μm to 20μm, and controlling the volume-based content ratio, a negative electrode active material layer is formed, reducing the pressing pressure during manufacturing and maintaining the contact area between particles and appropriate porosity.
It effectively reduces the internal resistance of lithium-ion secondary batteries and suppresses the decrease in capacity retention during charge-discharge cycles, thereby improving the durability of the negative electrode active material.
Smart Images

Figure CN123125697A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to negative electrode active material particles, negative electrodes for energy storage devices, and energy storage devices. Background Technology
[0002] Non-aqueous electrolyte secondary batteries, represented by lithium-ion batteries, are widely used in electronic devices such as personal computers and communication terminals, as well as automobiles, due to their high energy density. Non-aqueous electrolyte secondary batteries typically consist of a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte between the electrodes. They are charged and discharged through the transfer of charge between the two electrodes, such as lithium ions. Besides non-aqueous electrolyte secondary batteries, capacitors such as lithium-ion capacitors and double-layer capacitors are also widely used as energy storage components.
[0003] As an energy storage device, it typically comprises an electrode body consisting of a positive electrode containing a positive active material and a negative electrode containing a negative active material, separated by a separator. This electrode body, along with the electrolyte, is housed in a container to form the energy storage device. Carbon materials, primarily graphite, are used as the negative active material.
[0004] Patent Document 1 describes a method for improving the discharge capacity of energy storage devices by using natural graphite particles as the negative electrode active material. Additionally, Patent Document 1 describes a method for manufacturing a negative electrode by coating a paste containing graphite particles onto a negative electrode substrate, followed by drying and pressing to form a negative electrode active material layer.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: International Publication No. 2021 / 015194 Summary of the Invention
[0008] According to the inventors, reducing the particle size of natural graphite particles can lower the internal resistance of energy storage devices. Furthermore, solidifying the natural graphite particles can suppress capacity reduction during charge-discharge cycles. However, if small-particle-size natural graphite with a solid structure is used as the negative electrode active material, the durability of the negative electrode active material particles is easily reduced due to pressing during negative electrode manufacturing. If the durability of the negative electrode active material particles decreases, cracks and gaps will form in the particles during charge-discharge cycles, making it difficult to fully utilize the capacity reduction suppression effect brought about by solidification. Therefore, for energy storage devices using a negative electrode containing natural graphite particles, it is difficult to simultaneously achieve a reduction in internal resistance and capacity maintenance during charge-discharge cycles.
[0009] The object of the present invention is to provide negative electrode active material particles that can reduce the internal resistance of the energy storage element and suppress the decrease in capacity retention rate during the charge-discharge cycle of the energy storage element, as well as a negative electrode and energy storage element comprising such negative electrode active material particles.
[0010] In one aspect of the present invention, the negative electrode active material particles comprise a first graphite particle and a second graphite particle different from the first graphite particle. The first graphite particle is natural graphite with an average particle size of 3 μm to 8 μm and has a solid structure. The second graphite particle is natural graphite with an average particle size of 10 μm to 20 μm. The ratio of the content of the first graphite particle to the total content of the first graphite particle and the second graphite particle is greater than 0.2 and less than 0.6 on a volume basis.
[0011] In another aspect of the present invention, the negative electrode of the energy storage element comprises a negative electrode active material layer containing negative electrode active material particles from one aspect of the present invention.
[0012] Another aspect of the present invention provides an energy storage element having a negative electrode for an energy storage element according to one aspect of the present invention.
[0013] According to any aspect of the present invention, a negative electrode active material particle capable of reducing the internal resistance of the energy storage element and suppressing the decrease in capacity retention rate during the charge-discharge cycle of the energy storage element, as well as a negative electrode for the energy storage element and the energy storage element comprising such a negative electrode active material particle, can be provided. Attached Figure Description
[0014] Figure 1 This is a perspective view of an energy storage element using negative electrode active material particles according to one embodiment of the present invention.
[0015] Figure 2 It means having multiple Figure 1 A schematic diagram of an energy storage device with energy storage elements. Detailed Implementation
[0016] First, a summary of the negative electrode active material particles, negative electrode for energy storage elements, and energy storage elements disclosed in this specification will be given.
[0017] [1] In one aspect of the present invention, the negative electrode active material particles comprise a first graphite particle and a second graphite particle different from the first graphite particle, wherein the first graphite particle is natural graphite with an average particle size of 3 μm to 8 μm and has a solid structure, and the second graphite particle is natural graphite with an average particle size of 10 μm to 20 μm, and the ratio of the content of the first graphite particle to the total content of the first graphite particle and the second graphite particle is greater than 0.2 and less than 0.6 on a volume basis.
[0018] The negative electrode active material particles described above [1] can reduce the internal resistance of the energy storage element and suppress the decrease in capacity retention rate during charge-discharge cycles. The reason is uncertain, but it is speculated to be as follows. First, if small-particle-size natural graphite particles with a solid structure are used as the negative electrode active material, the internal resistance of the energy storage element decreases. On the other hand, the capacity of the energy storage element is prone to decrease during charge-discharge cycles. The main reason is believed to be the reduced durability of the negative electrode active material particles (natural graphite particles). More specifically, small-particle-size natural graphite particles with the aforementioned solid structure can reduce the internal resistance of the energy storage element. On the other hand, due to their solid structure, they are hard and difficult to deform. In addition, there are many contact points between the particles, resulting in a large frictional force when the particles shift positionally. Therefore, in order to achieve an appropriate porosity (thickness) in the negative electrode active material layer, it is necessary to increase the pressing pressure during the manufacturing of the negative electrode. As a result, the durability of the negative electrode active material particles is prone to decrease. Thus, if the durability of the negative electrode active material particles decreases, cracks and gaps will appear in the negative electrode active material particles during charge-discharge cycles, thereby easily reducing the capacity of the energy storage device. In contrast, the negative electrode active material particles described above [1] contain first graphite particles with a solid structure and small average particle size of natural graphite, and second graphite particles with a large average particle size of natural graphite. Therefore, during negative electrode manufacturing, it is easy to form a negative electrode active material layer in such a way that the first graphite particles enter the gaps in contact with the second graphite particles. As a result, while maintaining the contact area between the negative electrode active material particles in the negative electrode active material layer, it is easy to adjust the negative electrode active material layer to a suitable porosity. That is, it is not necessary to increase the pressing pressure during negative electrode manufacturing, and the durability of the negative electrode active material particles can be maintained. In addition, in the negative electrode active material particles described above [1], the content of the first graphite particles and the content of the second graphite particles are controlled to a suitable ratio. Based on this reasoning, it is speculated that the negative electrode active material particles described above [1] can reduce the internal resistance of the energy storage element and suppress the decrease in capacity retention rate during the charge and discharge cycle of the energy storage element.
[0019] In this invention, "natural graphite" refers to graphite obtained from natural resources that is not artificially generated graphite (man-made graphite). "Graphite" refers to the average lattice spacing (d) of the (002) plane determined by X-ray diffraction before or during charging and discharging. 002The term refers to carbon materials with a wavelength of 0.33 nm or greater and less than 0.34 nm. Here, "discharge state" refers to a state in which lithium ions adsorbed and released from the carbon material, which serves as the negative electrode active material, are fully released during charging and discharging. For example, in a single-electrode battery using a negative electrode containing carbon material as the negative electrode active material as the working electrode and metallic Li as the counter electrode, the open-circuit voltage is 0.7 V or greater. Natural graphite can exhibit four peaks in an X-ray diffraction pattern using CuKα rays measured before charging and discharging or during the discharge state, with a diffraction angle 2θ ranging from 40° to 50°. These four peaks are considered to originate from two hexagonal crystal structures and two rhombohedral crystal structures. In the case of synthetic graphite, it is generally believed that only two peaks originating from the hexagonal crystal structure appear. In the X-ray diffraction pattern using CuKα rays, the ratio of the peak intensity from the (012) crystal plane to the peak intensity from the (100) crystal plane ((012) / (100)) is preferably 0.3 or more, and more preferably 0.4 or more. The aforementioned peak intensity ratio ((012) / (100)) is preferably 0.6 or less. Here, the (100) crystal plane is from a hexagonal crystal system, and the (012) crystal plane is from a rhombohedral crystal system.
[0020] In this invention, "having a solid structure" means that the interior of the graphite particles is completely filled and substantially free of voids. More specifically, "solid" means that, in an SEM image obtained using a scanning electron microscope (SEM), the internal porosity (area ratio) of the particle, relative to the total area of the particle, is less than 3% in the observed cross-section. In a preferred embodiment, the aforementioned internal porosity of the graphite particles having a solid structure may be less than 1%.
[0021] The "internal porosity" of graphite particles refers to the area ratio of the voids within the particle relative to the total area of the particle in a cross-section observed using a scanning electron microscope (SEM). The "internal porosity" of graphite particles is determined through the following steps.
[0022] (1) Preparation of the test sample
[0023] The test object can be graphite particles or a negative electrode containing graphite particles. When the test object is a negative electrode, prepare it according to the following steps. If the negative electrode can be prepared before assembling the storage element, use it directly. When preparing the negative electrode from the assembled storage element, first, discharge the storage element at a constant current of 0.1C to the discharge termination voltage used in normal operation. Disassemble the storage element, remove the negative electrode, wash it thoroughly with dimethyl carbonate, and then dry it under reduced pressure for 24 hours at room temperature. All operations from disassembling the storage element to preparing the negative electrode for testing are carried out in a dry air atmosphere with a dew point below -40°C. Fix multiple graphite particles or negative electrodes used as the test object with a thermosetting resin. For the resin-fixed negative electrode, expose the cross-section by ion milling to prepare the test sample.
[0024] (2) Acquisition of SEM images
[0025] To acquire SEM images, a JSM-7001F (manufactured by Nippon Electron Ltd.) was used as the SEM. The SEM image was set to observe secondary electron images. The accelerating voltage was set to 5kV. The magnification was set to a magnification where at least 3 and no more than 15 graphite particles appeared in a single field of view. The obtained SEM images were saved as image files. Furthermore, various conditions such as spot diameter, working distance, irradiation current, brightness, and focus were appropriately adjusted to make the outlines of the graphite particles clear.
[0026] (3) Shearing of the contours of graphite particles
[0027] Using the image cropping function of Adobe Photoshop Elements (registered trademark) 11, the outlines of graphite particles were cropped from the acquired SEM image. This cropping was done by using the Quick Selection Tool to select the outer edges of the graphite particle outlines and then editing the area outside the graphite particles to a black background. If fewer than three graphite particles were croppable, the SEM image was acquired again, and this process was repeated until at least three croppable graphite particles were found.
[0028] (4) Binarization
[0029] For the image of the first graphite particle in the excised graphite particles, the image analysis software PopImaging (registered trademark) 6.00 was used. The concentration 20% lower than the concentration at maximum intensity was set as the threshold for binarization. The area of the high-concentration side was calculated using the binarization process and used as the "area S1 of the voids within the particle".
[0030] Next, for the image of the first graphite particle, which is the same as before, binarization is performed with a concentration threshold of 10%. The outer edge of the graphite particle is determined by the binarization process, and the area inside the outer edge is calculated as the "area S0 of the particle as a whole".
[0031] By using the calculated S1 and S0, the ratio of S1 to S0 (S1 / S0) is calculated, thereby calculating the "area ratio R1 of the voids within the first graphite particle relative to the total area of the particle".
[0032] For the images of the second and subsequent graphite particles in the cut graphite particles, the above binarization process is also performed to calculate the area S1 and area S0. Based on the calculated area S1 and area S0, the area ratios R2, R3, ... of the voids in each graphite particle are calculated.
[0033] (5) Determination of the area ratio of voids
[0034] By calculating the average value of the area ratios R1, R2, R3, ... of all voids obtained through binarization, the "area ratio of the voids within a particle relative to the total area of the particle (internal porosity)" is determined.
[0035] It should be noted that, instead of the scanning electron microscope used in “acquiring SEM images”, the image editing software used in “cutting out the contours of graphite particles”, and the image analysis software used in “binarization processing”, devices and software capable of performing equivalent measurements, image editing, and image analysis can also be used.
[0036] In this invention, "average particle size" refers to the value of 50% of the cumulative distribution of the volumetric baseline (D50: median particle size) based on the particle size distribution measured by laser diffraction and scattering method for a diluent of particles diluted with solvent, according to JIS-Z-8825 (2013) and calculated according to JIS-Z-8819-2 (2001). It should be noted that the average particle size based on the above measurements is approximately consistent with the average secondary particle size, which is the average particle size of 50 secondary particles measured from the SEM image of the particles, excluding extremely large and extremely small particles. The particle size of each secondary particle measured from this SEM image is calculated as follows: The shortest diameter passing through the center of the smallest circumcircle of each secondary particle is taken as the minor axis, and the diameter passing through the center and orthogonal to the minor axis is taken as the major axis. The average of the major and minor axes is taken as the particle size of each secondary particle. In the case where there are two or more shortest diameters, the longest orthogonal diameter is taken as the minor axis.
[0037] The average particle size of graphite particles, used as the negative electrode active material, is determined by examining the graphite particles before charging and discharging, or by examining the graphite particles contained in the negative electrode of the energy storage element after processing according to the following steps. First, the energy storage element is discharged at a constant current of 0.1C until the discharge termination voltage is reached under normal use. The energy storage element is then disassembled, and the negative electrode is removed. Using the removed negative electrode as the working electrode and lithium metal as the counter electrode, a test battery is assembled. Pure lithium metal is used as the lithium metal electrode. For the test battery, a constant current discharge of 50mA per 1g of negative electrode active material is applied until the closed-circuit voltage reaches 1.5V, adjusting the graphite particles to a fully discharged state. The test battery is then disassembled again, and the negative electrode is removed. The removed negative electrode is washed with dimethyl carbonate. Then, the negative electrode active material layer containing graphite particles is peeled off from the negative electrode substrate, and the negative electrode active material layer is washed with a solvent soluble in the adhesive to remove the adhesive. The washed negative electrode active material layer is immersed in an acid or alkaline solution to remove metals and SEI (solid electrolyte interface) films from the negative electrode substrate. Then, the graphite active material layer is washed with water and dried under reduced pressure at room temperature for 24 hours to obtain graphite particles. Disassembly of the energy storage element and test battery is performed in an argon atmosphere with a dew point below -60°C. "Normal use" refers to using the energy storage element under the recommended or specified charge / discharge conditions, or, if equipment for using the energy storage element is available, using that equipment.
[0038] In determining the average particle size of graphite particles, when two or more types of particles with different average particle sizes are included, a particle size distribution containing multiple peaks (a particle size distribution with the horizontal axis representing particle size and the vertical axis representing the proportion of particles relative to volume) is sometimes obtained. When the particle size distributions of different particles do not overlap, the average particle size is calculated for each particle's respective particle size distribution. When the particle size distributions of different particles overlap, the particle size distributions of each particle are separated to determine the average particle size. The separation of particle size distributions can be performed using known methods. Numerical analysis software can also be used for particle size distribution separation. Examples of numerical analysis software include MATLAB (registered trademark, The MathWorks) and ORIGIN PRO (registered trademark, Originlab Corporation).
[0039] The various graphite particles contained in the negative electrode active material are identified based on their particle size distribution. That is, particles belonging to each particle size distribution in the negative electrode active material are considered to be of the same type. The internal porosity is measured for each type of particle based on the particle size distribution identification. When there are overlapping portions in the particle size distribution, the internal porosity is measured for particles that do not belong to the overlapping portions. From this point of view, the particles included in the internal porosity measurement are preferably those within 20% of the average particle size of each particle size distribution, and more preferably those within 10% of the average particle size.
[0040] In this invention, the "content ratio" of the volume reference for graphite particles is calculated according to JIS-Z-8825 (2013) based on the particle size distribution (the horizontal axis represents particle size, and the vertical axis represents the proportion of the volume reference) obtained by measuring a diluted solution containing particles diluted with solvent using laser diffraction / scattering. When the sample contains two or more types of particles with different average particle sizes, the above method is appropriately used to separate the particle size distributions of each particle, and an integral value is calculated based on the particle size distribution. The "content ratio" of the volume reference is calculated by comparing the above integral values.
[0041] [2] Among the negative electrode active material particles described in [1] above, the second graphite particle may have a solid structure.
[0042] The negative electrode active material particles described in [2] above can further suppress the decrease in capacity retention rate during the charge-discharge cycle of the energy storage element.
[0043] [3] In the negative electrode active material particles described in [1] or [2] above, the sphericity of the first graphite particle and the second graphite particle may be greater than 0.6.
[0044] The sphericity is calculated based on the projected image of the projected graphite particles using the following formula.
[0045] Sphericity = (4π × total area of the particle) / (circumference of the particle) 2
[0046] Sphericity was measured using a particle shape analyzer. Examples of particle shape analyzers include the Sysmex FPIA 3000 manufactured by Malvern. It should be noted that the sphericity was measured using graphite particles that had undergone pretreatment according to the steps described in the determination of graphite particles before charging and discharging or the average particle size.
[0047] In the negative electrode active material particles described above [3], since the frictional force between the particles is small (high fluidity) during the pressing process in the negative electrode manufacturing, the pressing pressure during the negative electrode manufacturing can be suppressed. Therefore, the durability of the particles can be easily maintained. As a result, the decrease in capacity retention rate during the charge-discharge cycle of the energy storage element can be further suppressed. Here, "the sphericity of the first graphite particle and the second graphite particle is greater than 0.6" means that the sphericity of the first graphite particle is greater than 0.6, and the sphericity of the second graphite particle is greater than 0.6.
[0048] [4] In any one of the negative electrode active material particles described in [1] to [3] above, the ratio of the average particle size of the first graphite particle to the average particle size of the second graphite particle may be 0.6 or less.
[0049] If the negative electrode active material particles described in [4] are used, it is easier to adjust the negative electrode active material layer to an appropriate porosity while maintaining the contact area between particles in the negative electrode active material layer. Therefore, it is possible to further reduce the internal resistance of the energy storage element and further suppress the decrease in capacity retention rate during the charge-discharge cycle of the energy storage element.
[0050] [5] The negative electrode of the energy storage element of another aspect of the present invention comprises a negative electrode active material layer comprising any one of the negative electrode active material particles described in [1] to [4] above.
[0051] The negative electrode of the energy storage element described in [5] above has a negative electrode active material layer containing negative electrode active material particles as described in any one of [1] to [4] above, thereby reducing the internal resistance of the energy storage element and suppressing the decrease in capacity retention rate during the charge and discharge cycle of the energy storage element.
[0052] [6] In the negative electrode of the energy storage element described in [5] above, the BET specific surface area of the negative electrode active material layer can be 3.0 m². 2 / g~4.3m 2 / g.
[0053] The “BET specific surface area” is a value obtained by measuring the following steps: 1.00 g of the negative electrode active material layer sample is placed in a sample tube for measurement and dried under reduced pressure at 120°C for 12 hours. Then, using the nitrogen adsorption method with liquid nitrogen, adsorption isotherms are measured in the range of relative pressure P / P0 (P0 = approximately 760 mmHg) from 0 to 0.95. The measuring apparatus used is an autosorb iQ manufactured by Quantachrome. Five points are extracted from the region of P / P0 = 0.05 to 0.3 of the obtained adsorption isotherms, and a BET plot is performed. The BET specific surface area is calculated based on the y-intercept and slope of the line. It should be noted that the BET specific surface area is measured using negative electrode active material layers that have undergone pretreatment as described in the steps for measuring the negative electrode active material layer before charge / discharge or the average particle size.
[0054] The negative electrode of the energy storage element described in [6] above can further reduce the internal resistance of the energy storage element.
[0055] [7] The energy storage element of another aspect of the present invention has a negative electrode for energy storage element as described in [5] or [6] above.
[0056] The energy storage element described in [7] above has a negative electrode for the energy storage element described in [5] or [6] above, therefore its internal resistance is low and its capacity retention rate during charge and discharge cycles is difficult to reduce.
[0057] The following describes in detail one embodiment of the present invention, including negative electrode active material particles, a negative electrode for an energy storage element, an energy storage element, a method for manufacturing the energy storage element, an energy storage device, and other embodiments. It should be noted that the lower and upper limits of the numerical ranges described in the embodiments of the present invention can be arbitrarily combined.
[0058] [Negative electrode active material particles]
[0059] One embodiment of the present invention comprises a negative electrode active material particle containing a first graphite particle and a second graphite particle different from the first graphite particle. The first graphite particle (hereinafter also referred to as "the first particle") is natural graphite with an average particle size of 3 μm to 8 μm and has a solid structure. The second graphite particle (hereinafter also referred to as "the second particle") is natural graphite with an average particle size of 10 μm to 20 μm. The ratio of the content of the first particle to the total content of the first particle and the second particle is greater than 0.2 and less than 0.6 on a volume basis. This negative electrode active material particle is used as the negative electrode of an energy storage device such as a non-aqueous electrolyte secondary battery. In addition, this negative electrode active material particle is usually formed into a negative electrode active material layer in the negative electrode of the energy storage device together with other arbitrary components. The negative electrode active material layer is formed, for example, by coating a paste containing the negative electrode active material particle onto a negative electrode substrate and then pressing it after drying.
[0060] The negative electrode active material particles readily form a negative electrode active material layer by the first particle entering the gap where the second particle contacts. Therefore, while maintaining the contact area between the negative electrode active material particles in the layer, the porosity of the negative electrode active material layer can be easily adjusted. That is, the durability of the negative electrode active material particles can be maintained without increasing the pressing pressure during negative electrode manufacturing. Furthermore, the ratio of the content of the first particle to the content of the second particle is controlled appropriately. Therefore, the negative electrode active material particles effectively reduce the internal resistance of the energy storage element and suppress the decrease in capacity retention rate during charge-discharge cycles of the energy storage element.
[0061] (Particle 1)
[0062] The first particle is a natural graphite particle with a solid structure. Examples of the shape of the first particle include flake-like, block-like (scaly), and earth-like shapes. The first particle can also be a spheroidized natural graphite particle obtained by spheroidizing flake-like natural graphite.
[0063] The lower limit of the sphericity of the first particle is preferably greater than 0.6, more preferably 0.65. By ensuring that the sphericity of the first particle is above the aforementioned lower limit, the durability of the negative electrode active material particle can be easily maintained. The lower limit of the sphericity of the first particle can be 0.7 or 0.8. On the other hand, the upper limit of the sphericity of the first particle is not particularly limited, and from a manufacturing point of view, it can be 0.99, 0.95, or 0.9.
[0064] The lower limit of the average particle size of the first particle is 3 μm, preferably 4 μm, more preferably 5 μm, further preferably 6 μm, and even more preferably 7 μm. On the other hand, the upper limit of the average particle size of the first particle is 8 μm, preferably 7.8 μm, and more preferably 7.6 μm. If the average particle size of the first particle is within the above range, the internal resistance of the energy storage element can be reduced.
[0065] (Particle 2)
[0066] The second particle is a natural graphite particle. The shape of the second particle can be the same as that of the first particle described above. Preferably, the second particle has a solid structure. By having both the first and second particles have solid structures, the decrease in capacity retention during charge-discharge cycles of the energy storage element can be further suppressed.
[0067] The lower limit of the sphericity of the second particle is preferably greater than 0.6, more preferably 0.65. By ensuring that the sphericity of the second particle is above the aforementioned lower limit, the durability of the negative electrode active material particles can be easily maintained. The lower limit of the sphericity of the second particle can be 0.7 or 0.8. On the other hand, the upper limit of the sphericity of the second particle is not particularly limited, and from a manufacturing point of view, it can be 0.99, 0.95, or 0.9.
[0068] The lower limit of the average particle size of the second particle is 10 μm, preferably 11 μm, more preferably 12 μm, and even more preferably 13 μm. On the other hand, the upper limit of the average particle size of the second particle is 20 μm, preferably 18 μm, and more preferably 16 μm. By making the average particle size of the second particle above or above the aforementioned lower limit, the decrease in capacity retention rate during charge-discharge cycles of the energy storage element can be suppressed. In addition, by making the average particle size of the second particle below or below the aforementioned upper limit, the internal resistance of the energy storage element can be reduced.
[0069] The upper limit of the ratio of the average particle size of the first particle to the average particle size of the second particle can be 0.7, preferably 0.6, and more preferably 0.55. By making the above ratio below the above upper limit, the first particle can more easily enter the gap contacted by the second particle, and the above-mentioned effects of the present invention can be easily enjoyed. The lower limit of the ratio of the average particle size of the first particle to the average particle size of the second particle is not particularly limited, and can be 0.1 or 0.2.
[0070] The lower limit of the volume ratio of the content of the first particle to the total content of the first and second particles is greater than 0.2, preferably 0.25. On the other hand, the upper limit of the above ratio is 0.6, preferably 0.55. By making the above ratio above the lower limit, the internal resistance of the energy storage element can be reduced. In addition, by making the above ratio below the upper limit, the decrease in the capacity retention rate of the energy storage element during charge and discharge cycles can be suppressed.
[0071] The negative electrode active material particles can include other negative electrode active materials besides the first and second particles. Examples of other negative electrode active materials include metallic lithium; metals or quasi-metals such as silicon and tin; metal oxides or quasi-metal oxides such as silicon oxide, titanium oxide, and tin oxide; and Li₄Ti₅O. 12 Titanium oxides such as LiTiO2 and TiNb2O7; polyphosphate compounds; silicon carbide; carbon materials such as artificial graphite and non-graphitic carbon.
[0072] "Non-graphitic carbon" refers to the average lattice spacing (d) of the (002) crystal plane determined by X-ray diffraction before or during charging and discharging. 002Carbon materials with a wavelength of 0.34 nm to 0.42 nm are used. As non-graphitic carbon, examples include difficult-to-graphitize carbon and easily-graphitize carbon. "Difficult-to-graphitize carbon" refers to the aforementioned d... 002 Carbon materials with a wavelength of 0.36 nm to 0.42 nm. "Easily graphitizable carbon" refers to the aforementioned d... 002 It is a carbon material with a wavelength greater than 0.34 nm and less than 0.36 nm.
[0073] The total content of the first and second particles in the negative electrode active material particles is preferably 90% by mass or more, more preferably 99% by mass or more, and may also be substantially 100% by mass. That is, the negative electrode active material particles may be substantially composed of the first and second particles.
[0074] [Negative terminal for energy storage components]
[0075] A negative electrode (hereinafter also simply referred to as "negative electrode") for an energy storage element according to one embodiment of the present invention has a negative electrode substrate and a negative electrode active material layer laminated directly or through an intermediate layer onto the negative electrode substrate. The negative electrode active material layer contains negative electrode active material particles according to one embodiment of the present invention. Typically, the negative electrode has a portion of the negative electrode substrate exposed. This exposed portion of the negative electrode substrate is typically connected to a negative electrode lead. The negative electrode may, for example, have a sheet, plate, or strip shape.
[0076] The negative electrode contains the aforementioned negative electrode active material particles, thus achieving the effect of reducing the internal resistance of the energy storage element and suppressing the decrease in capacity retention rate during the charge and discharge cycles of the energy storage element.
[0077] The negative electrode substrate is conductive. In this specification, "conductive" means that the volume resistivity is 10⁻⁶. -2 Below Ω·cm. The volume resistivity is a value measured according to JIS-H-0505 (1975). On the other hand, in this specification, "non-conductive" or "(electrically) insulating" means that the above-mentioned volume resistivity is 10 Ω·cm or less. 7 The anode material can be Ω·cm or higher. Examples of materials that can be used as the negative electrode substrate include metals such as copper, nickel, iron, their alloys (stainless steel, etc.), and carbon materials. Copper or copper alloys are preferred.
[0078] The negative electrode substrate may have shapes such as sheet, plate, or strip. Examples of negative electrode substrate forms include foil, vapor-deposited film, mesh, and porous materials, with foil being preferred. For example, the negative electrode substrate may be copper foil or copper alloy foil.
[0079] The average thickness of the negative electrode substrate can be, for example, 2 μm to 35 μm. The lower limit of the average thickness of the negative electrode substrate can be 3 μm, 4 μm, or 5 μm. The upper limit of the average thickness of the negative electrode substrate can be 30 μm or 20 μm. In this specification, "average thickness" refers to the average value of the thickness measured at any 5 locations.
[0080] The intermediate layer is a layer disposed between the negative electrode substrate and the negative electrode active material layer. The intermediate layer may contain, for example, a conductive agent and a binder. When the intermediate layer contains a conductive agent, the contact resistance between the negative electrode substrate and the negative electrode active material layer can be reduced. Examples of conductive agents and binders used in the intermediate layer are the same as those used in the negative electrode active material layer, which will be described later.
[0081] In addition to the aforementioned negative electrode active material particles, the negative electrode active material layer may also contain any components such as conductive agents, binders, thickeners, and fillers, as needed. The negative electrode active material layer can be formed from a negative electrode compound containing negative electrode active materials and other arbitrary components. For example, the negative electrode active material layer may be disposed only on one side of the negative electrode substrate with a sheet-like or similar shape, or it may be disposed on both sides.
[0082] The content of the aforementioned negative electrode active material particles in the negative electrode active material layer is preferably 60% to 99% by mass, more preferably 90% to 98% by mass. By setting the content of the aforementioned negative electrode active material particles within the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved. Furthermore, the aforementioned effects of the present invention are readily available.
[0083] Conductive agents are typically composed of materials with conductive properties. When the volume resistivity of a conductive agent cannot be directly measured, it is determined by a volume resistivity of 10⁻⁶. -2 Materials composed of known materials with a content below Ω·cm are also considered conductive agents. Examples of conductive agents include carbon materials, metals, and conductive ceramics. Carbon materials refer to materials whose main constituent element is carbon. The main constituent element is the element with the highest content by mass. For example, the carbon content in a carbon material can be 80% by mass or more, 90% by mass or more, or 95% by mass, 99% by mass, or 99.9% by mass or more. Preferably, carbon materials are carbon materials other than uncarbonized polymer compounds. Examples of carbon materials include non-graphitic carbon and graphene-based carbon. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, and carbon black. Examples of carbon black include furnace black, acetylene black, and Ketjen black. Examples of graphene-based carbon include graphene, carbon nanotubes (CNTs), and fullerenes. Examples of conductive agent forms include powder and fibrous forms. One or more conductive agents can be used. These materials can be used as conductive agents by combining them. For example, a material made by combining carbon black with CNTs can also be used.
[0084] When the negative electrode active material layer contains a conductive agent, the content of the conductive agent in the negative electrode active material layer is preferably 1% to 10% by mass, more preferably 3% to 9% by mass. The content of the conductive agent in the negative electrode active material layer can be 5% by mass or less, or 2% by mass or less. The technology disclosed herein can also be implemented in a manner where the negative electrode active material layer does not contain a conductive agent.
[0085] The lower limit of the BET specific surface area of the negative electrode active material layer is preferably 3.0 m². 2 / g, more preferably 3.5m 2 / g, further preferably 4.0m 2 / g. On the other hand, the upper limit of the BET specific surface area of the negative electrode active material layer can be 5.0m². 2 / g, preferably 4.3m 2 / g. If the BET specific surface area of the negative electrode active material layer is within the above range, the internal resistance of the energy storage element can be reduced. Furthermore, by setting the BET specific surface area below the upper limit, the decrease in capacity retention during charge-discharge cycles of the energy storage element can be further suppressed. The BET specific surface area of the negative electrode active material layer can be adjusted, for example, by selecting the type and content ratio of the first and second particles of the negative electrode active material to achieve the desired BET specific surface area.
[0086] Examples of adhesives include water-based adhesives and organic solvent-based adhesives.
[0087] Aqueous adhesives are adhesives that dissolve or disperse in water. Aqueous adhesives can be adhesives that dissolve or disperse more than 1 part by mass relative to 100 parts by mass of water at 20°C. Aqueous adhesives (water-soluble or water-dispersible polymer materials) can be used when forming a negative electrode active material layer using a negative electrode paste in which water or a mixed solvent with water as the main component is used as the dispersion medium. Examples of aqueous adhesives include polyethylene oxide, polypropylene oxide, polyvinyl alcohol, polyacrylic acid, polymethacrylic acid, polytetrafluoroethylene, styrene-butadiene rubber, polyethylene, polypropylene, nitrile rubber, and cellulose.
[0088] Organic solvent-based adhesives are adhesives that are dissolved or dispersed in an organic solvent (e.g., N-methylpyrrolidone). Organic solvent-based adhesives can be adhesives that dissolve or disperse more than 1 part by mass relative to 100 parts by mass of an organic solvent (e.g., N-methylpyrrolidone) at 20°C. Organic solvent-based adhesives (for polymeric materials that are soluble or dispersible in organic solvents) can be used when forming a negative electrode active material layer using a negative electrode paste in which the dispersion medium is an organic solvent or a mixed solvent with an organic solvent as the main component. Examples of organic solvent-based adhesives include, for instance, polyvinylidene fluoride, copolymers of polyvinylidene fluoride and hexafluoropropylene, copolymers of ethylene and vinyl alcohol, polyacrylonitrile, polyphosphazene, polysiloxane, polyvinyl acetate, polymethyl methacrylate, polystyrene, polycarbonate, polyamide, polyimide, polyamide-imide, cross-linked polymers of cellulose and chitosan pyrrolidone carboxylate, and derivatives of chitosan.
[0089] Adhesives can be fluoropolymers (polytetrafluoroethylene, polyvinylidene fluoride, etc.), polyolefins (polyethylene, polypropylene, etc.), elastomers (ethylene propylene diene rubber, styrene-butadiene rubber, fluororubber, etc.), polysaccharide polymers (cellulose, chitosan derivatives, etc.). One or more types of adhesives can be used.
[0090] When the negative electrode active material layer includes a binder, the content of the binder in the negative electrode active material layer is preferably 0.1% to 5% by mass, more preferably 0.4% to 3% by mass. The content of the binder in the negative electrode active material layer can be 5% by mass or less, or 2% by mass or less. The technology disclosed herein can also be implemented in a manner where the negative electrode active material layer does not contain a binder.
[0091] Examples of thickeners include polysaccharide polymers such as carboxymethyl cellulose and methyl cellulose. When a thickener has functional groups that react with lithium, these functional groups can be deactivated beforehand through methylation or similar methods. Thickeners can also function as adhesives. One or more thickeners can be used.
[0092] When the negative electrode active material layer contains a thickener, the content of the thickener in the negative electrode active material layer is preferably 0.1% to 5% by mass, more preferably 0.4% to 3% by mass. The content of the thickener in the negative electrode active material layer can be less than 5% by mass or less than 2% by mass. The technology disclosed herein can also be implemented in a manner where the negative electrode active material layer does not contain a thickener.
[0093] There are no particular limitations on the filler. The filler can be any component other than the aforementioned negative electrode active material particles, conductive agents, binders, and thickeners, and is intentionally included. The filler can be included as a component to fill the gaps in the negative electrode active material layer, or it can be included for other purposes. The filler can be organic materials such as polyolefins, or inorganic materials such as inorganic oxides, hydroxides, and carbonates. One or more fillers can be used.
[0094] When the negative electrode active material layer includes filler, the filler content in the negative electrode active material layer can be set to 0.1% to 8% by mass, typically preferably 5% by mass or less, and more preferably 2% by mass or less. The technology disclosed herein can also be implemented with the negative electrode active material layer not containing filler.
[0095] The negative electrode active material layer may further contain other components besides the aforementioned negative electrode active material particles, conductive agent, binder, thickener, and filler. These other components also include those unintentionally generated in the negative electrode active material layer. Furthermore, as such other components, the negative electrode active material layer may also contain unintentionally present impurities, provided that the effects of this invention are achieved. The maximum content of the aforementioned other components in the negative electrode active material layer can be 10% by mass, or 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass. The maximum content of unintentionally generated components in the negative electrode active material layer can be 10% by mass, or 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass. The maximum content of unintentionally present impurities in the negative electrode active material layer can be 10% by mass, or 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass.
[0096] The average thickness of the first layer of the negative electrode active material can be, for example, 3 μm to 1000 μm. The lower limit of the average thickness of the first layer of the negative electrode active material can be 5 μm, 10 μm, or 20 μm. The upper limit of the average thickness of the first layer of the negative electrode active material can be 800 μm, 500 μm, 200 μm, 100 μm, 80 μm, or 60 μm.
[0097] The porosity of the negative electrode active material layer can be, for example, 20% to 70%. The lower limit of the porosity of the negative electrode active material layer can be 25% or 30%. The upper limit of the porosity of the negative electrode active material layer can be 60% or 50%. The "porosity (%)" of the negative electrode active material layer and the positive electrode active material layer (described later) is calculated using the formula (1 - V2 / V1) × 100, where the apparent volume (including the volume of voids) of the negative (positive) electrode active material layer is set as V1, and the sum of the actual volumes of the materials constituting the negative (positive) electrode active material layer is set as V2. The sum of the actual volumes V2 of the materials constituting the negative (positive) electrode active material layer can be calculated based on the content and true density of each material in the negative (positive) electrode active material layer.
[0098] (Method for manufacturing the negative electrode)
[0099] The negative electrode can be manufactured using known methods. For example, it can be manufactured by coating a paste-like negative electrode agent (negative electrode agent paste) directly or through an intermediate layer onto a negative electrode substrate and then drying it to form a negative electrode active material layer. The negative electrode agent paste typically contains the aforementioned negative electrode active material particles, other arbitrary components, and a dispersion medium. After drying, the negative electrode active material layer can be pressed, etc.
[0100] [Electronic storage components]
[0101] An energy storage element according to one embodiment of the present invention includes a positive electrode, a negative electrode according to another embodiment of the present invention, an electrolyte, and a container for housing them. The energy storage element may also further include an insulating member sandwiched between the positive electrode and the negative electrode to electrically insulate the positive electrode from the negative electrode. The positive electrode, the negative electrode, and any insulating member typically constitute an electrode body. At least a portion of the electrolyte is typically present immersed in the electrode body. The energy storage element according to one embodiment of the present invention may further include other components.
[0102] Because this energy storage element has a negative electrode containing negative electrode active material particles according to one embodiment of the present invention, it has the effect of low internal resistance and the ability to suppress the decrease in capacity retention during charge and discharge cycles.
[0103] For example, one embodiment of the present invention Figure 1 The energy storage element 1 shown has an electrode body 2, an electrolyte (not shown), and a cuboid container 3 for housing them. Figure 1 The energy storage element 1 also includes a positive lead 4, a positive external terminal 5, a negative lead 6, and a negative external terminal 7. The positive lead 4 and negative lead 6 are housed together with the electrode body 2 within the container 3. The positive external terminal 5 and negative external terminal 7 are located outside the container 3. The positive electrode constituting the electrode body 2 is electrically connected to the positive external terminal 5 via the positive lead 4. The negative electrode constituting the electrode body 2 is electrically connected to the negative external terminal 7 via the negative lead 6.
[0104] The energy storage element of the present invention can be a non-aqueous electrolyte secondary battery. Hereinafter, the main components of the energy storage element constituting one embodiment of the present invention will be described in detail, focusing on the case where the energy storage element is a non-aqueous electrolyte secondary battery (especially a lithium-ion secondary battery), but this is not intended to limit the scope of the present invention.
[0105] (positive electrode)
[0106] The positive electrode has a positive electrode substrate and a layer of positive electrode active material stacked directly on or separated from the positive electrode substrate by an intermediate layer. Typically, the positive electrode has an exposed portion of the positive electrode substrate. This exposed portion of the positive electrode substrate is usually connected to the aforementioned positive electrode lead. The positive electrode can, for example, have a sheet, plate, or strip shape.
[0107] The positive electrode substrate is conductive. Materials that can be used as the positive electrode substrate include, for example, metals such as aluminum, titanium, iron, and their alloys (stainless steel, etc.). Among these, aluminum or aluminum alloys are preferred from the viewpoints of high potential resistance, high electronic conductivity, and cost.
[0108] The positive electrode substrate may have shapes such as sheet, plate, or strip. Examples of positive electrode substrate forms include foil, vapor-deposited film, mesh, and porous materials, with foil being preferred. For example, the positive electrode substrate may be aluminum foil or aluminum alloy foil.
[0109] The average thickness of the positive electrode substrate can be, for example, 3 μm to 50 μm. The lower limit of the average thickness of the positive electrode substrate can be 5 μm, 8 μm, or 10 μm. The upper limit of the average thickness of the positive electrode substrate can be 40 μm, 30 μm, or 25 μm.
[0110] The composition of the intermediate layer for the positive electrode is not particularly limited; for example, it can be selected from the composition exemplified for the intermediate layer of the negative electrode.
[0111] The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer may, as needed, contain any components such as conductive agents, binders, thickeners, and fillers. These components can be selected from the materials exemplified in the negative electrode description above. The positive electrode active material layer may be formed from a positive electrode compound containing the positive electrode active material and other arbitrary components. For example, relative to a positive electrode substrate having a sheet-like shape, the positive electrode active material layer may be disposed on only one side or on both sides.
[0112] The positive electrode active material can be any known positive electrode active material. Positive electrode active materials used in lithium-ion secondary batteries typically employ materials capable of both attracting and releasing lithium ions. Examples of positive electrode active materials include lithium transition metal composite oxides, polyanionic compounds, chalcogenide compounds, chalcogenide materials, and lithium oxide. One or more positive electrode active materials can be used.
[0113] Examples of transition metal elements contained in lithium transition metal composite oxides include nickel, cobalt, and manganese. Typical lithium transition metal composite oxides may also contain aluminum. Examples of lithium transition metal composite oxides include those with an α-NaFeO2 crystal structure and those with a spinel crystal structure.
[0114] As lithium transition metal composite oxides with an α-NaFeO2-type crystal structure, examples include those made from Li 1+α Ma 1-α O2 (Ma is a substance containing one or more transition metal elements, excluding lithium, where 0 ≤ α < 1). Ma preferably contains one or more of Ni, Co, and Mn. The total content of Ni, Co, and Mn relative to Ma ((Ni + Co + Mn) / Ma) is preferably 90 mol% or more, more preferably 98 mol% or more.
[0115] Examples of lithium transition metal composite oxides with a spinel-type crystal structure include those composed of Li β Mb₂O₄ (where Mb is a metallic element other than lithium that contains one or more transition metal elements, and 0 < β ≤ 1.2) is a substance. Mb preferably contains Mn. The content of Mn relative to Mb (Mn / Mb) is preferably 50 mol% or more, more preferably 80 mol% or more.
[0116] Polyanionic compounds are compounds composed of polyanions (i.e., polyvalent oxyacid anions) and cations. Preferably, polyanionic compounds contain lithium cations and transition metal cations. Examples of polyanionic compounds include LiFePO4, LiMnPO4, and LiMn... x Fe 1-x Examples of polyanionic compounds include PO4 (0 < x < 1), LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, and Li2CoPO4F. The surface of polyanionic compound particles can also be coated with other materials (such as carbon materials).
[0117] Examples of chalcogenide compounds include titanium disulfide, molybdenum disulfide, and molybdenum dioxide.
[0118] Examples of sulfur-based materials include elemental sulfur, metal sulfides such as lithium sulfide, organic disulfide compounds, and organic sulfur compounds such as carbon-sulfur compounds.
[0119] In these materials used as positive electrode active materials, some of the atoms or polyanions can be replaced by atoms or anions composed of other elements. The surface of these materials can also be coated with other materials.
[0120] The positive electrode active material is typically in particulate form. The average particle size of the positive electrode active material is preferably, for example, 0.1 μm to 20 μm. By setting the average particle size of the positive electrode active material to the lower limit or above, the manufacture or handling of the positive electrode active material becomes easier. By setting the average particle size of the positive electrode active material to the upper limit or below, the electronic conductivity of the positive electrode active material layer is improved. It should be noted that when using a composite of the positive electrode active material and other materials, the average particle size of the composite is used as the average particle size of the positive electrode active material.
[0121] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% to 99% by mass, more preferably 70% to 98% by mass, and may also be 80% to 95% by mass. By setting the content of the positive electrode active material within the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.
[0122] When the positive electrode active material layer contains a conductive agent, the content of the conductive agent in the positive electrode active material layer is preferably 0.1% to 10% by mass, more preferably 1% to 9% by mass, and even more preferably 3% to 8% by mass. The upper limit of the above-mentioned conductive agent content can be 5% by mass, 4% by mass, or 3% by mass. By making the content of the conductive agent within the above range, the energy density of the energy storage element can be improved.
[0123] When the positive electrode active material layer includes a binder, the content of the binder in the positive electrode active material layer is preferably 0.1% to 10% by mass, more preferably 1% to 9% by mass, and even more preferably 3% to 8% by mass. The upper limit of the above-mentioned binder content can be 5% by mass, 4% by mass, or 3% by mass. By keeping the binder content within the above range, the positive electrode active material, etc., can be stably maintained. The technology disclosed herein can also be implemented in a manner where the positive electrode active material layer does not contain a binder.
[0124] When the positive electrode active material layer contains a thickener, the content of the thickener in the positive electrode active material layer is preferably 0.1% to 8% by mass, more preferably 5% by mass or less, and even more preferably 2% by mass or less. The technology disclosed herein can also be implemented in a manner where the positive electrode active material layer does not contain a thickener.
[0125] When the positive electrode active material layer includes filler, the filler content in the positive electrode active material layer can be set to 0.1% to 8% by mass, typically preferably 5% by mass or less, and more preferably 2% by mass or less. The technology disclosed herein can also be implemented with the positive electrode active material layer not containing filler.
[0126] The positive electrode active material layer may further contain other components besides the positive electrode active material, conductive agent, binder, thickener, and filler. These other components also include those unintentionally generated in the positive electrode active material layer. Furthermore, the positive electrode active material layer may also contain unintentionally present impurities as part of these other components, provided that the effects of this invention are achieved. The maximum content of the other components in the positive electrode active material layer can be 10% by mass, or 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass. The maximum content of unintentionally generated components in the positive electrode active material layer can be 10% by mass, or 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass. The maximum content of unintentionally present impurities in the positive electrode active material layer can be 10% by mass, or 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass.
[0127] The thickness of the positive electrode active material layer is appropriately set according to the type of positive electrode active material and the application of the energy storage device. The average thickness of the first positive electrode active material layer can be, for example, 5 μm to 1000 μm. The lower limit of the average thickness of the first positive electrode active material layer can be 10 μm or 20 μm. The upper limit of the average thickness of the first positive electrode active material layer can be 800 μm, 500 μm, 200 μm, or 100 μm.
[0128] The porosity of the positive electrode active material layer can be, for example, 20% to 50%. The lower limit of the porosity of the positive electrode active material layer can be 25%. The upper limit of the porosity of the positive electrode active material layer can be 45%.
[0129] (The manufacturing method of the positive electrode)
[0130] The positive electrode can be manufactured using known methods. For example, the positive electrode can be manufactured by coating a paste-like positive electrode agent (positive electrode agent paste) directly or through an intermediate layer onto a positive electrode substrate and then drying it to form a positive electrode active material layer. The positive electrode agent paste typically contains a positive electrode active material, as well as other arbitrary components and a dispersion medium. After drying, the positive electrode active material layer can be pressed, etc.
[0131] (Isolation component)
[0132] The spacer can be a known spacer. For example, a spacer consisting only of a substrate layer or a spacer having an inorganic layer containing inorganic particles and an adhesive formed on one or both sides of the substrate layer can be used.
[0133] Examples of substrate layers for the insulating element include woven fabrics, nonwoven fabrics, and porous resin membranes. Among these, porous resin membranes are preferred from the viewpoint of strength, while nonwoven fabrics are preferred from the viewpoint of retaining non-aqueous electrolytes. The material used for the substrate layer of the insulating element is not particularly limited as long as it is an insulating material; resins such as polyolefins (polyethylene, polypropylene, etc.), polyimides, and aromatic polyamides are preferred.
[0134] Examples of inorganic compounds constituting inorganic particles include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, and magnesium oxide; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon; and substances derived from mineral resources or their derivatives such as talc, zeolite, kaolin, bentonite, and mica. One or more types of inorganic particles may be used. The average particle size of the inorganic particles is preferably, for example, 0.5 μm to 10 μm. The content of inorganic particles in the inorganic layer is preferably 50% to 99% by mass, more preferably 80% to 98% by mass.
[0135] As a binder used in the inorganic layer, the same binder exemplified in the positive electrode active material layer can be cited.
[0136] The porosity of the separator can be, for example, 20% to 80%. From the viewpoint of discharge performance, the lower limit of the porosity of the separator can be 30%, 40%, or 50%. From the viewpoint of strength, the upper limit of the porosity of the separator can be 70%, 60%, or 50%. In this specification, "porosity" refers to a volume-based value, which is the value measured using a mercury porosimeter.
[0137] The average thickness of the separator can be, for example, 10μm to 40μm or 15μm to 30μm.
[0138] As a separator, a polymer gel composed of a polymer and a non-aqueous electrolyte can be used. Alternatively, a porous resin membrane, nonwoven fabric, etc., as described above, and the polymer gel can be used together as a separator.
[0139] (Electrode)
[0140] As an electrode body, known structures such as wound electrode bodies and stacked electrode bodies can be used.
[0141] A wound electrode has a structure in which the positive and negative electrodes are wound together in an insulated manner. The wound electrode can be cylindrical or flat. Figure 1 The electrode body 2 of the energy storage element 1 is a flat, wound electrode body. The wound electrode body can be manufactured, for example, by the following steps: First, a positive electrode, an insulating member, and a negative electrode, each formed as a strip, are sequentially overlapped to obtain a laminate. The wound electrode body is obtained by winding this laminate.
[0142] A stacked electrode has a structure in which one or more positive electrodes and one or more negative electrodes are stacked in an insulated manner. For example, a stacked electrode is obtained by sequentially stacking a positive electrode, an insulator, and a negative electrode, which are formed into rectangles, respectively.
[0143] In addition to the above, an electrode body may also be used, for example, an electrode body having a structure in which at least one of the positive and negative electrodes is folded into a corrugated shape and stacked.
[0144] (Non-aqueous electrolyte)
[0145] Non-aqueous electrolytes can be used. A non-aqueous electrolyte is a medium that facilitates the transport of charge-carrying ions (such as lithium ions) between the positive and negative electrodes; it is a substance that does not substantially contain water. Examples of non-aqueous electrolytes include non-aqueous electrolyte solutions and solid electrolytes. Non-aqueous electrolyte solutions and solid electrolytes can also be used in combination.
[0146] (Non-aqueous electrolyte)
[0147] Non-aqueous electrolytes contain a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.
[0148] Known non-aqueous solvents can be used as non-aqueous solvents. Examples of non-aqueous solvents include carbonates, esters, ethers, amides, and nitriles. Examples of carbonates include cyclic carbonates and chain carbonates. Examples of esters include carboxylic acid esters, phosphate esters, and sulfonates. Non-aqueous solvents in which some of the hydrogen atoms in these compounds are replaced by halogen atoms can also be used as non-aqueous solvents. One or more non-aqueous solvents can be used.
[0149] Cyclic carbonates refer to carbonates with a cyclic structure containing a carbonate group (-OC (=O)-O-). Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, butyl carbonate, vinylene carbonate, ethylene ethylene carbonate, chloroethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, styrene carbonate, 1-phenylethylene carbonate, and 1,2-diphenylethylene carbonate. Cyclic carbonates can be saturated cyclic carbonates such as ethylene carbonate, or unsaturated cyclic carbonates such as vinylene carbonate. "Saturated" means that it does not have carbon-carbon unsaturated bonds (carbon-carbon double bonds and carbon-carbon triple bonds). "Unsaturated" means that it has carbon-carbon unsaturated bonds. Saturated cyclic carbonates are preferred, and ethylene carbonate is more preferred.
[0150] Chain carbonates refer to carbonates that do not have a ring structure and contain a carbonate group. Examples of chain carbonates include diethyl carbonate, dimethyl carbonate, methyl ethyl carbonate, diphenyl carbonate, trifluoroethyl methyl carbonate, and bis(trifluoroethyl) carbonate. Chain carbonates can be saturated chain carbonates such as dimethyl carbonate, or unsaturated chain carbonates such as diphenyl carbonate. Saturated chain carbonates are preferred, and methyl ethyl carbonate is more preferred.
[0151] The non-aqueous solvent preferably contains carbonates, more preferably cyclic carbonates and chain carbonates. The carbonate content in the non-aqueous solvent is preferably 80% to 100% by volume, but can be 99% to 100% by volume, or 100% by volume. Using cyclic carbonates promotes the dissociation of electrolyte salts, thereby increasing the ionic conductivity of the non-aqueous electrolyte. Using chain carbonates helps to reduce the viscosity of the non-aqueous electrolyte. When cyclic and chain carbonates are used together, the volume ratio of cyclic carbonate to chain carbonate (cyclic carbonate: chain carbonate) is preferably in the range of 5:95 to 50:50.
[0152] Electrolyte salts can be well-known electrolyte salts. Examples of electrolyte salts include lithium salts, sodium salts, potassium salts, and magnesium salts. Salts, etc. Among them, lithium salts are preferred. One or more electrolyte salts can be used.
[0153] Examples of lithium salts include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, and LiClO4; imide salts such as LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, and LiN(SO2CF3)(SO2C4F9); and lithium oxalate salts such as LiB(C2O4)2, LiBF2(C2O4), and LiPF2(C2O4)2. LiN(SO2F)2 is also equivalent to an inorganic lithium salt. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred. Additionally, imide salts are sometimes preferred.
[0154] The electrolyte salt content in the non-aqueous electrolyte is preferably 0.1 mol / dm³ at 20°C and 1 atmosphere. 3 ~2.5mol / dm 3 More preferably 0.3 mol / dm 3 ~2.0 mol / dm 3 Further preferably 0.5 mol / dm 3 ~1.7mol / dm 3 The preferred value is 0.7 mol / dm³. 3 ~1.5mol / dm 3 By maintaining the electrolyte salt content within the aforementioned range, the ionic conductivity of the non-aqueous electrolyte can be improved.
[0155] In addition to the non-aqueous solvent and electrolyte salt, the non-aqueous electrolyte may also contain additives. One or more additives may be used. When additives are used in the non-aqueous electrolyte, the content of the additive in the non-aqueous electrolyte is preferably 0.01% to 10% by mass, more preferably 0.1% to 7% by mass, even more preferably 0.2% to 5% by mass, and particularly preferably 0.3% to 3% by mass.
[0156] (Solid electrolyte)
[0157] As a solid electrolyte, any material with ionic conductivity, such as lithium, sodium, and calcium, can be selected and is solid at room temperature (e.g., 20°C). Examples of solid electrolytes include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, and polymer solid electrolytes. One or more types of solid electrolytes can be used.
[0158] (container)
[0159] The container houses the electrodes and non-aqueous electrolyte within its internal space. Materials used for the container include metals such as aluminum and stainless steel, as well as resins; from a strength perspective, metals are preferred. Composite materials combining metals and resins can also be used.
[0160] The shape of the container is not particularly limited and can be cylindrical, cuboid (square), disc-shaped, etc. The container can also be a sheet-like shape formed from a metal-resin composite film.
[0161] (The shape, purpose, etc. of energy storage components)
[0162] The shape of the energy storage element in one embodiment of the present invention is not particularly limited. The energy storage element may be, for example, a cylindrical battery, a prismatic battery, a flat battery, a coin-shaped battery, a button battery, etc.
[0163] The application of the energy storage element according to one embodiment of the present invention is not particularly limited. For example, it can be used as a power supply for automobiles such as electric vehicles, hybrid vehicles, and plug-in hybrid vehicles; a power supply for electronic devices such as personal computers and communication terminals; and a power supply for energy storage.
[0164] The energy storage element of the present invention can be used singly or in combination. When the required output and required voltage are relatively low, the energy storage element can be used alone. Alternatively, when at least one of the required output and required voltage is high, the energy storage element can be used as an energy storage device combined with other energy storage elements. In an energy storage device that combines multiple energy storage elements, at least one energy storage element included in the energy storage device need only be an energy storage element according to one embodiment of the present invention. The energy storage device will be described in detail later.
[0165] In one embodiment of the present invention, the energy storage element may be constrained to maintain a certain thickness of the container, or such constraining may not be applied. Alternatively, constraining may be applied to apply a certain load to the container. When the container is constrained, expansion of the container during charge-discharge cycles is sometimes suppressed, and a decrease in charge-discharge performance is suppressed. When the container is constrained, a load may be applied to the electrode body inside the container, or no load may be applied. For example, a constraining component for such constraining may be provided in the energy storage element or energy storage device.
[0166] [Manufacturing method of energy storage components]
[0167] An energy storage element according to one embodiment of the present invention can be manufactured by a known method. The manufacturing method of this energy storage element includes, for example, steps such as: preparing a positive electrode, preparing a negative electrode, preparing an electrolyte, and housing the positive electrode, negative electrode, and electrolyte in a container. The manufacturing method may also include steps such as: preparing an insulating element, and manufacturing an electrode body using the positive electrode, negative electrode, and insulating element. Housing the positive electrode, negative electrode, and electrolyte in the container may involve housing the electrode body and electrolyte in the container.
[0168] The step of preparing the positive electrode can be the same as the step of manufacturing the positive electrode. The positive electrode can be manufactured using the methods described above. Similarly, the step of preparing the negative electrode can be the same as the step of manufacturing the negative electrode. The negative electrode can also be manufactured using the methods described above. The step of preparing the electrolyte can be the same as the step of preparing the electrolyte. The electrolyte can be prepared, for example, by dissolving an electrolyte salt in a non-aqueous solvent. The positive electrode, negative electrode, separator, and electrolyte can also be prepared by purchasing them.
[0169] The electrodes (or positive and negative electrodes) and electrolyte can be housed in a container using known methods. When the electrolyte is a non-aqueous electrolyte, for example, this can be done by first housing the electrodes (or positive and negative electrodes) in the container, and then injecting the non-aqueous electrolyte through an inlet provided in the container. The inlet is sealed after the non-aqueous electrolyte is injected. This method of manufacturing a non-aqueous electrolyte energy storage element can further include a step of initially charging and discharging the assembled, uncharged energy storage element.
[0170] The energy storage element of one embodiment of the present invention can also be manufactured by other methods. For example, in the case where the energy storage element of one embodiment of the present invention is an all-solid-state battery, it can also be manufactured by pressing the materials forming the positive electrode, the separator, and the negative electrode separately or together.
[0171] [Electronic storage device]
[0172] Figure 2 The energy storage device 30 includes multiple energy storage units 20. Each energy storage unit 20 includes multiple energy storage elements 1 electrically connected to it. The energy storage device 30 may also include a bus (not shown) electrically connecting multiple energy storage elements 1, a bus (not shown) electrically connecting multiple energy storage units 20, etc. The energy storage unit 20 or the energy storage device 30 may also include a status monitoring device (not shown) for monitoring the status of one or more energy storage elements 1.
[0173] [Other Implementation Methods]
[0174] The energy storage element of the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the spirit of the invention. For example, the configuration of other embodiments can be added to the configuration of a certain embodiment; additionally, a part of the configuration of a certain embodiment can be replaced with the configuration of other embodiments or known technology. Furthermore, a part of the configuration of a certain embodiment can be deleted. Furthermore, known technology can be added to the configuration of a certain embodiment.
[0175] In the above embodiments, the case where the energy storage element is used as a rechargeable non-aqueous electrolyte secondary battery has been described, but the type, shape, size, capacity, etc., of the energy storage element are arbitrary. This invention can also be applied to various secondary batteries, double-layer capacitors, or lithium-ion capacitors, etc.
[0176] In the above embodiments, an electrode body with a separator sandwiched between the positive and negative electrodes has been described; however, the electrode body may also lack a separator. For example, the positive and negative electrodes may be in direct contact with each other while a non-conductive layer is formed on the active material layer of either the positive or negative electrode. In this case, the positive and negative electrodes may further have layers other than the substrate, intermediate layer, and active material layer. Alternatively, the positive and negative electrodes may not have a layered structure.
[0177] Example
[0178] The present invention will be described in more detail below through embodiments, but the present invention is not limited to the following embodiments.
[0179] [Example 1]
[0180] (Making the negative electrode)
[0181] As the negative electrode active material particles, a mixture of natural graphite particles (i.e., first graphite particles) with a solid structure, an average particle size of 7.4 μm, and a sphericity of 0.67, and natural graphite particles (i.e., second graphite particles) with a solid structure, an average particle size of 14.2 μm, and a sphericity of 0.68, was used. Both the first and second graphite particles were spheroidized natural graphite particles obtained by spheroidizing flake-like natural graphite. The ratio of the content of the first graphite particles to the total content of the first and second graphite particles was 0.5 on a volume basis. The above-mentioned negative electrode active material particles, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium were mixed to prepare a negative electrode paste. The mass ratio of the above-mentioned negative electrode active material particles, SBR, and CMC, converted from solid components, was 96:3.3:0.7. The negative electrode paste was coated onto both sides of a copper foil serving as the negative electrode substrate, then dried and rolled to form the negative electrode active material layer, thus obtaining the negative electrode. The BET specific surface area of the negative electrode active material layer is 4.2 m². 2 / g.
[0182] (The production of the positive electrode)
[0183] Lithium iron phosphate, which has an olivine-type crystal structure and is represented by LiFePO4, is used as the positive electrode active material.
[0184] The above-mentioned positive electrode active material, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium are mixed to prepare a positive electrode paste. The mass ratio of the above-mentioned positive electrode active material, AB, and PVDF, converted from solid components, is 93.0:4.0:3.0. The positive electrode paste is coated on both sides of an aluminum foil serving as the positive electrode substrate, dried, and rolled to form a positive electrode active material layer, thereby obtaining the positive electrode.
[0185] (Non-aqueous electrolyte)
[0186] In a solvent in which ethylene carbonate (EC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 30:35:35, at a concentration of 1.1 mol / dm³ 3 LiPF6 was dissolved at a concentration that yielded a non-aqueous electrolyte.
[0187] (Isolation component)
[0188] The separator uses a polyethylene microporous membrane.
[0189] (Assembly of energy storage components)
[0190] The positive electrode, negative electrode, and separator are stacked to form an electrode body. The resulting electrode body is placed in a container, and then the non-aqueous electrolyte is injected into the container and sealed to obtain the energy storage element of Example 1.
[0191] [Example 2, Comparative Examples 1-16]
[0192] The types (natural or artificial), structures (solid or hollow), average particle sizes, volume ratios (content ratios) of the first and second graphite particles are set as shown in Table 1. Otherwise, the energy storage elements of Examples 2 and Comparative Examples 1-16 were obtained following the same steps as in Example 1. The pressing during the formation of the negative electrode active material layer was adjusted so that the mass per unit area and porosity of the negative electrode active material layer in Examples 2 and Comparative Examples 1-16 were consistent with those in Example 1. It should be noted that in Table 1, "hollow" means without a solid structure, "small" in particle size classification means an average particle size of 3 μm to 8 μm, "large" in particle size classification means an average particle size of 10 μm to 20 μm, and "-" indicates the absence of the second graphite particles.
[0193] [evaluate]
[0194] (Determination of initial discharge capacity)
[0195] For each energy storage element in the embodiments and comparative examples, the initial discharge capacity was determined by the following method. The following test was conducted in a constant temperature bath at 25°C. A charging current of 1 mA / cm² was applied at an upper limit voltage of 3.5V. 2 After constant current charging, constant voltage charging is performed at 3.5V. The charging termination condition is set to 5 hours from the start of charging. After a 10-minute rest period, discharge at a current of 1mA / cm at the lower limit voltage of 2.0V. 2 A constant current discharge is performed, and the amount of electricity discharged at that time is taken as the initial discharge capacity.
[0196] (Determination of initial DC resistance)
[0197] For each energy storage element, the initial DC resistance is determined using the following method.
[0198] The current capable of charging the initial discharge capacity measured in the "Initial Discharge Capacity Measurement" section above within 1 hour was set as 1C. Starting from the discharge state, a constant current charging was performed at 25°C with a charging current of 0.5C and a charging time of 1 hour to adjust the SOC (State of Charge) to 50%. Then, at 25°C, constant current discharges were performed for 10 seconds each with discharge currents of 0.2C, 0.5C, and 1.0C. After each discharge, a constant current charging was performed at 0.5C to replenish the discharged charge and prevent the SOC from deviating from 50%. The voltage at the first second under each current was plotted to obtain a straight line. The slope of this line was taken as the initial DC resistance (initial DCR). The results are shown in Table 1. It should be noted that the values shown in Table 1 are relative to the initial DCR of Comparative Example 6, which was set to 100.0.
[0199] (Charge-discharge cycle test)
[0200] For each energy storage element that has undergone the above-mentioned "initial discharge capacity measurement", charge-discharge cycle test shall be performed according to the following guidelines.
[0201] Constant current and constant voltage charging was performed with a charging current of 0.1C and a charging termination voltage of 3.5V. The charging termination condition was set at a total charging time of 15 hours. Next, constant current discharging was performed with a discharging current of 0.1C and a discharging termination voltage of 2.0V. A 10-minute rest period was set after discharging and after charging. Discharging, charging, and resting were all performed in a thermostatic bath at 25°C. The above charging and discharging cycle was performed for 50 cycles.
[0202] As the capacity retention rate after charge-discharge cycles, the percentage of the discharge capacity of the 50th cycle relative to the discharge capacity of the 1st cycle in the above charge-discharge cycle test was calculated as the capacity retention rate. The results are shown in Table 1. It should be noted that the values shown in Table 1 are relative values with the capacity retention rate of Comparative Example 6 set to 100.0.
[0203]
[0204] As shown in Table 1, Comparative Example 1, which uses small-diameter solid graphite particles as the first graphite particle and whose content ratio is 0.2 or less, has an initial DCR of 100.0. Comparative Example 2, which uses small-diameter hollow graphite particles as the first graphite particle, has a lower initial DCR, but a capacity retention rate of less than 100.4. Comparative Examples 3-5, where either the first or second graphite particle is artificial graphite, have an initial DCR of 100.0 or higher. Comparative Examples 6-12, where all graphite particles are large-diameter, have a large initial DCR and a capacity retention rate of less than 100.4. Comparative Examples 13-16, where all graphite particles are small-diameter, also have a large initial DCR and a capacity retention rate of less than 100.4. In contrast, Examples 1 and 2, which use small-diameter solid particles as the first graphite particle and large-diameter natural graphite particles as the second graphite particle and mix them within an appropriate range, have a low initial DCR and a capacity retention rate of 100.4 or higher.
[0205] Industrial availability
[0206] This invention is suitable for use as a power storage element in personal computers, communication terminals and other electronic devices, automobiles, industrial applications and other power sources.
[0207] Symbol Explanation
[0208] 1. Energy storage components
[0209] 2 Electrode Body
[0210] 3 containers
[0211] 4 positive leads
[0212] 5 Positive External Terminals
[0213] 6 negative leads
[0214] 7 Negative External Terminals
[0215] 20 energy storage units
[0216] 30 energy storage devices
Claims
1. A negative electrode active material particle, comprising a first graphite particle and a second graphite particle different from the first graphite particle. The first graphite particle is natural graphite with an average particle size of 3μm to 8μm and a solid structure. The second graphite particle is natural graphite with an average particle size of 10μm to 20μm. The ratio of the content of the first graphite particle to the total content of the first graphite particle and the second graphite particle, on a volume basis, is greater than 0.2 and less than 0.
6.
2. The negative electrode active material particles according to claim 1, wherein, The second graphite particle has a solid structure.
3. The negative electrode active material particles according to claim 1 or 2, wherein, The sphericity of the first graphite particle and the second graphite particle is greater than 0.
6.
4. The negative electrode active material particles according to claim 1 or 2, wherein, The ratio of the average particle size of the first graphite particle to the average particle size of the second graphite particle is less than 0.
6.
5. A negative electrode for an energy storage element, comprising a negative electrode active material layer containing negative electrode active material particles as described in claim 1 or 2.
6. The negative electrode for the energy storage element according to claim 5, wherein, The BET specific surface area of the negative electrode active material layer is 3.0 m². 2 / g~4.3m 2 / g.
7. An energy storage element having a negative electrode as described in claim 5.
Citation Information
Patent Citations
Power storage element
WO2021015194A1