Automatic vertical welding method and system for titanium alloy butt joint double-sided synchronous narrow gap

By employing a double-sided synchronous narrow-gap automatic vertical welding method for titanium alloy butt joints, and utilizing dual-gun synchronous TIG welding technology and high-purity argon gas protection, the problems of low efficiency and reliance on manual labor in the longitudinal butt joint welding of large-size titanium alloy components have been solved, achieving efficient and stable welding results and stress balance.

CN123149529APending Publication Date: 2026-11-24WUCHANG SHIPBUILDING INDUSTRY GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611167679.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-03
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing titanium alloy welding technology suffers from problems such as low efficiency, reliance on manual experience for quality, large residual stress, and uneven deformation in the longitudinal butt joint welding of large-size thick plate components. In particular, the double-sided welding of longitudinal butt joints requires multiple operations and it is difficult to ensure stress balance.

Method used

The method of double-sided synchronous narrow gap automatic vertical welding of titanium alloy butt joints is adopted. The narrow gap bevel is formed by machining, and the dual-gun synchronous TIG welding technology is used to realize the vertical placement of the longitudinal butt joint. Combined with high-purity argon gas protection, single-layer single-pass automatic welding is performed to reduce the amount of filler metal and offset the welding stress.

Benefits of technology

Significantly improves welding efficiency, reduces filler metal usage by more than 30%, increases welding efficiency by more than 100%, reduces reliance on manual labor, stabilizes the first-pass yield rate at over 96%, reduces residual stress and deformation, and meets the high-precision manufacturing requirements of thick and large-sized components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149529A_ABST
    Figure CN123149529A_ABST
Patent Text Reader

Abstract

This application belongs to the field of titanium alloy welding technology, specifically disclosing a method and system for automatic vertical welding of titanium alloy butt joints with double-sided synchronous narrow gap. The automatic vertical welding method includes: beveling the edges of the titanium alloy component used to form the longitudinal butt joint; assembling and fixing the veneered titanium alloy component so that the longitudinal butt joint is set vertically and configuring two tungsten inert gas (TIG) welding torches; performing single-torch alternating root pass welding on the longitudinal butt joint to form a root pass layer at the bottom of the narrow gap bevel; measuring the angular deformation of the root pass layer and actively compensating for the angular deformation using single-torch welding to meet the requirements of subsequent automatic welding; and performing double-torch synchronous filler and capping welding on top of the pre-treated root pass layer to form a filler weld layer and a capping weld layer, respectively. This application can solve the problems of high dependence on manual welding effect and low welding efficiency in existing titanium alloy welding processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of titanium alloy welding technology, and more specifically, relates to a method and system for automatic vertical welding of titanium alloy butt joints with synchronous narrow gap on both sides. Background Technology

[0002] Currently, the main methods for butt welding of large-size thick plate titanium alloy structures include manual tungsten inert gas welding, non-narrow gap TIG welding, electron beam welding, and narrow gap flat welding. Each method has its limitations to varying degrees.

[0003] Manual tungsten inert gas (TIG) welding offers stable welding quality and strong engineering adaptability, but it is inefficient and highly dependent on the welder's experience. Any fluctuation in the welding torch angle, movement speed, and wire feed stability can lead to weld quality defects. When welding thick plates, the large bevel filler volume results in coarse grains, uneven microstructure, deformation, and residual stress. Electron beam welding is widely used in titanium alloy welding, but its application in large structures is limited by vacuum chamber size, and the high cost of vacuum chambers makes it less cost-effective. Magnetically controlled narrow-gap flat welding technology is restricted by the external environment and fixing devices, has a single welding position, and requires frequent hoisting, transportation, and flipping during structural welding, making its engineering application cumbersome.

[0004] Furthermore, titanium alloy welding requires continuous inert gas protection to prevent oxidation. Manual protection methods are difficult to reliably adapt to the welding process, easily leading to localized oxidation and affecting weld quality. Therefore, existing TIG (tungsten inert gas) welding processes are insufficient for welding narrow gaps on thick titanium alloys. Especially for the welding of longitudinal butt joints on titanium alloy components, existing manual or mechanical welding typically involves laying the component flat to weld the joint. For butt joints requiring welding on both sides, it is usually necessary to weld the component twice, sequentially. Additionally, when switching sides for welding, the component needs to be hoisted, transported, and flipped. This not only makes it difficult to ensure the balance of residual stress on both sides of the butt joint, but the sequential welding method is also inefficient.

[0005] In summary, for the welding of longitudinal butt joints on large-sized titanium alloy components, there is an urgent need to develop an automated TIG welding process for narrow gaps in titanium alloys, in order to improve welding efficiency and reduce the dependence of welding quality on human experience. Summary of the Invention

[0006] To address the shortcomings or improvement needs of existing technologies, this application provides a method and system for automatic vertical welding of titanium alloy butt joints with synchronous narrow gaps on both sides. The aim is to solve the problems of high dependence on manual welding effect and low welding efficiency in existing titanium alloy welding processes, thereby realizing automatic welding of vertical joints inside titanium alloy components.

[0007] The above-mentioned technical objectives of this application are mainly achieved through the following technical solutions.

[0008] On the one hand, this application provides a method for automatic vertical welding of titanium alloy butt joints with double-sided synchronous narrow gap, which is used for welding longitudinal butt joints extending in the vertical direction on upright titanium alloy components. The automatic vertical welding method includes steps S10-S60, as follows.

[0009] Step S10: The two sides of the longitudinal butt joint are machined by means of mechanical processing to form a narrow gap bevel extending along the longitudinal butt joint on both sides of the titanium alloy component.

[0010] Step S20: Fix the titanium alloy component to the base in a vertical placement manner with the longitudinal butt joint perpendicular to the ground, and adjust the butt joint size parameters of the longitudinal butt joint. Weld an arc-starting plate and an arc-extinguishing plate to both ends of the longitudinal butt joint. Move the two tungsten inert gas (TIG) welding torches integrated on the automatic welding torch adjustment frame, which are arranged opposite each other and can be raised and lowered synchronously, to both sides of the titanium alloy component, so that the two TIG welding torches are opposite to the two narrow gap bevels.

[0011] Step S30: According to the butt joint size parameters of the longitudinal butt joint, use automatic welding or manual argon arc welding to perform single-gun alternating root pass welding. During the root pass welding process, the tungsten inert gas (TIG) welding torch on one side starts arc welding, while the tungsten inert gas (TIG) welding torch on the other side moves synchronously for gas protection.

[0012] Step S40: Clean the weld formed after the initial welding and measure the angular deformation at the weld. Use single-gun welding to control the angular deformation so that the weld meets the requirements of subsequent welding.

[0013] Step S50: After adjusting the welding parameters, perform synchronous double-gun filler welding. During the filler welding process, both tungsten electrode oscillating TIG welding guns are ignited and tungsten electrode oscillating narrow gap TIG automatic welding is performed from bottom to top in a single-layer, single-pass manner.

[0014] Step S60: After adjusting the welding parameters, perform simultaneous cap welding with two guns. During the cap welding process, both tungsten inert gas (TIG) welding guns are ignited and tungsten inert gas (TIG) welding with narrow gaps is performed from bottom to top in a single-layer, single-pass manner. After the cap welding is completed, a complete longitudinal weld is formed on the titanium alloy component.

[0015] The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding method described in this application adopts a vertical placement method that makes the longitudinal butt joint perpendicular to the ground to achieve vertical welding, which can reduce the impact of horizontal placement (flat welding or horizontal welding) on ​​the structural welding formation; combined with the dual-gun synchronous welding process, continuous welding can be achieved in one assembly without frequent hoisting, turning, and transportation; double-sided synchronous welding makes the positive and negative welding stresses cancel each other out, effectively reducing welding residual stress and deformation; at the same time, the design of narrow gap bevel greatly reduces the amount of filler metal used, significantly improving welding efficiency.

[0016] In a preferred embodiment of this application, in step S30, if the misalignment of the longitudinal butt joint is not greater than 1 mm and the assembly gap is not greater than 0.5 mm, automatic welding is used for alternating single-gun root pass welding. The tungsten inert gas (TIG) welding torch on one side initiates an arc and welds from bottom to top in a single-layer, single-pass manner, while the tungsten inert gas (TIG) welding torch on the other side does not initiate an arc but moves synchronously for gas protection. The two alternating tungsten inert gas (TIG) welding torches form two weld passes in the two narrow gap bevels on both sides, so that the deposited metal smoothly transitions to the sidewall of the narrow gap bevel.

[0017] In a preferred embodiment of this application, if the misalignment of the longitudinal butt joint is greater than 1 mm or the assembly gap is greater than 0.5 mm, manual TIG welding is used for alternating single-gun root pass welding. First, the tungsten inert gas (TIG) welding torch on one side is used to perform tack welding on the narrow gap bevel on that side from bottom to top. The length of the tack weld is 30 mm to 100 mm, and the distance between adjacent welds is no more than 300 mm. Each weld is welded with 2-3 layers. Then, the tungsten inert gas (TIG) welding torch is used to fill the gap between the welds from bottom to top. Each filling position is also welded with 2-3 layers. Then, the tungsten inert gas (TIG) welding torch is used to continue self-melting or filling a layer on the continuous weld after filling. After that, the tungsten inert gas (TIG) welding torch on the other side is used to perform root pass welding on the narrow gap bevel on the back side from bottom to top for 3 passes, so that the root of the narrow gap bevel on both sides is fully melted.

[0018] By classifying the assembly precision, the two methods of automatic welding for the root pass and manual argon arc welding for the root pass can be adapted to different assembly states, ensuring reliable root penetration under various engineering conditions.

[0019] In a preferred embodiment of this application, the narrow gap bevel has a blunt edge with a thickness of 1mm-3mm, the bevel angle of the narrow gap bevel is 3°-6°, the height of the blunt edge is 1.5mm, and the bottom chamfer of the narrow gap bevel is R4.5mm. A blunt edge design of 2mm balances the conflict between thorough penetration and preventing penetration of the base material and resulting in voids in the weld pool. A bevel angle design of 5.34° reduces the filler material while also meeting the needs of manual root pass welding, effectively reducing problems such as torch clamping, top wire clamping, and tungsten clamping. The bottom chamfer R4.5mm, combined with welding shrinkage of 2mm-3mm, ensures that the root weld bevel width is within the optimal range of 8mm-10mm.

[0020] In a preferred embodiment of this application, in step S30, the base current value of the tungsten electrode oscillating TIG welding torch for root pass welding is 100A-145A, the peak current value is 135A-155A, the wire feed speed is 0.6m / min-0.8m / min, and the welding speed is 100mm / min-120mm / min. During the root pass welding stage, the tungsten electrode on the tungsten electrode oscillating TIG welding torch does not oscillate. The above parameter combination can ensure that the root of the root pass weld is fully penetrated, the deposited metal transitions smoothly with the sidewall, and no pits are formed.

[0021] In a preferred embodiment of this application, in step S50, the base current value of the tungsten inert gas (TIG) welding torch used for filler welding is 130A-170A, the peak current value is 160A-185A, the wire feed speed is 0.85m / min-1.3m / min, and the welding speed is 50mm / min-70mm / min. The half-oscillation amplitude of the tungsten electrode on the TIG welding torch is 25°-30°, the dwell time at both ends is 0.3s-0.8s, the oscillation speed is 20rpm-60rpm, and the half-oscillation width is 1.0mm-1.6mm. These parameters ensure that heat is uniformly applied to the bevel sidewall, guaranteeing the fusion quality of the sidewall, while effectively controlling heat input and suppressing grain coarsening through single-layer, single-pass welding.

[0022] In a preferred embodiment of this application, in step S60, the base current value of the tungsten inert gas (TIG) welding torch for cap welding is 130A-170A, the peak current value is 150A-175A, the wire feed speed is 0.85m / min-1.3m / min, and the welding speed is 50mm / min-70mm / min. The half-oscillation amplitude of the tungsten electrode on the TIG welding torch is 25°-30°, the dwell time at both ends is 0.3s-0.8s, the oscillation speed is 20rpm-60rpm, and the half-oscillation width is 1.1mm-1.8mm. The cap welding adopts a dual-torch synchronous method to ensure symmetrical and uniform cap weld layers on both sides and reduce welding deformation.

[0023] In a preferred embodiment of this application, high-purity argon is used as the shielding gas during the welding process in steps S30 to S60. For the tungsten inert gas (TIG) welding torch that welds after arc initiation, the argon flow rate of the main nozzle is 10 L / min-20 L / min, and the argon flow rate of the back shielding gas behind the welding position is 15 L / min-25 L / min. For the tungsten inert gas (TIG) welding torch that does not arc but moves synchronously for gas protection, the argon flow rate of the back shielding gas is 15 L / min-25 L / min. Through the synergistic effect of the three gas paths—main nozzle, back shielding shroud, and back shielding—the weld and heat-affected zone are protected from oxidation throughout the welding process, fundamentally solving the problem of localized oxidation caused by unstable manual shielding.

[0024] In a preferred embodiment of this application, the tungsten electrode oscillating TIG welding torch supplies gas in advance before arc ignition and delays gas supply after arc extinguishing. The delay in gas supply is based on the weld color turning silver-white or pale yellow after cooling at the arc extinguishing point. This method ensures that the weld is always under inert gas protection during the high-temperature stage, effectively preventing discoloration or even performance degradation of the titanium alloy due to oxidation during cooling.

[0025] In a preferred embodiment of this application, the narrow-gap groove design takes into account welding shrinkage, so that the groove width at the root of the longitudinal weld is 8mm-10mm. This width range is the optimal working window for tungsten inert gas (TIG) welding with a narrow gap. If the groove width is too small, it can easily cause the torch to get stuck; if it is too large, it will affect the fusion quality of the sidewalls. By reserving shrinkage compensation during the groove design stage, it can be ensured that the groove width is always within the optimal range when each weld is applied.

[0026] On the other hand, this application also provides a double-sided synchronous narrow gap automatic vertical welding system for titanium alloy butt joints, used to implement the double-sided synchronous narrow gap automatic vertical welding method for titanium alloy butt joints as described above. The automatic vertical welding system includes: a base for placing the titanium alloy component to be welded; an automatic welding torch adjustment frame, which includes a column, a horizontal arm on the top of the column, and two head travel slides on the horizontal arm. The two head travel slides are parallel to each other and spaced apart, and the length direction of the head travel slides extends vertically; and two tungsten electrode oscillating TIG welding torches that are slidably mounted on the two head travel slides respectively.

[0027] The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding system described in this application achieves double-sided synchronous narrow gap TIG automatic vertical welding by mounting two tungsten inert gas (TIG) welding torches on two vertically extending machine head travel slides, enabling the two torches to rise and fall synchronously relative to the two sides of the titanium alloy component. The system has a compact structure and is suitable for various vertical welding scenarios.

[0028] In summary, compared with the prior art, the technical solutions conceived in this application mainly possess the following technical features and advantages: 1. The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding method described in this application adopts a narrow gap bevel and a dual-gun synchronous narrow gap TIG automatic vertical welding process. Compared with the traditional non-narrow gap bevel, the welding filler volume is reduced by more than 30%, and the welding efficiency is increased by more than 100%. The two tungsten electrode oscillating TIG welding guns move synchronously with the other gun for gas protection while one gun is welding. The two guns can provide gas protection for each other, effectively reducing the instability of manual protection. The number of construction personnel is reduced by more than 30%, and the first-pass yield rate is stabilized at more than 96%. It effectively overcomes the defects of traditional manual TIG welding, such as low efficiency and reliance on human experience for quality.

[0029] 2. The double-sided synchronous narrow gap automatic vertical welding method for titanium alloy butt joints described in this application uses a vertical placement method that makes the longitudinal butt joint perpendicular to the ground to fix the titanium alloy components on the base, realizing continuous welding in one assembly without the need for frequent hoisting, turning over, and transportation.

[0030] 3. The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding method described in this application adopts a double-sided symmetrical narrow gap bevel and a double gun synchronous welding process. The synchronous welding of the positive and negative sides makes the welding stress on both sides cancel each other out, effectively reducing the welding residual stress. It can meet the high-precision manufacturing requirements of large-thickness and large-size parts, and solves the technical defects of large residual stress and uneven microstructure in the existing methods.

[0031] 4. The double-sided synchronous narrow gap automatic vertical welding method for titanium alloy butt joints described in this application optimizes the design of the blunt edge size, bevel angle, bottom chamfer and welding shrinkage of the narrow gap bevel, so that the bevel shape fully adapts to the welding shrinkage law of titanium alloy. This ensures welding quality and controls forming accuracy, effectively solving the technical problem of incomplete fusion of the welding torch or sidewall caused by bevel shrinkage during automatic welding.

[0032] 5. The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding system described in this application has a structural design in which two machine head traveling slides on the welding torch automatic adjustment frame extend in the vertical direction. The two tungsten electrode oscillating TIG welding torches can slide up and down independently along their respective slides to achieve synchronous lifting and lowering welding of narrow gap bevels on both sides of the titanium alloy component. The system has a compact structure and is suitable for various vertical welding scenarios such as long straight plate splicing, columnar or conical cylinder longitudinal welds. Attached Figure Description

[0033] Figure 1 This is a flowchart of the automatic vertical welding method for double-sided synchronous narrow gap welding of titanium alloy butt joints described in this application; Figure 2 This is a schematic cross-sectional view of the narrow gap bevel on the titanium alloy component described in this application; Figure 3 This is a schematic diagram of the weld point structure for tack welding during the single-gun alternating root pass welding process using manual argon arc welding. Figure 4 This is a schematic diagram of the structure of the automatic vertical welding system for double-sided synchronous narrow gap titanium alloy butt joints described in this application.

[0034] In all the accompanying drawings, the same reference numerals are used to denote the same elements or structures, wherein: 10. Titanium alloy components; 11. Narrow gap bevel; 12. Blunt edge; 20. Base; 30. Automatic welding torch adjustment frame; 31. Column; 32. Horizontal arm; 33. Head travel slide plate; 40. Tungsten electrode oscillating TIG welding torch. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0036] Implementation Method 1: This application provides a method for automatic vertical welding of titanium alloy butt joints with double-sided synchronous narrow gap, applicable to welding of butt joints such as long straight plates, columnar or conical cylindrical longitudinal welds of large-sized titanium alloy components 10 with strength above 700MPa and thickness of 20mm-100mm. Figure 1 As shown, the automatic vertical welding method specifically includes the following steps: Step S10: The two sides of the longitudinal butt joint are machined by means of mechanical processing to form a narrow gap bevel 11 extending along the longitudinal butt joint on both sides of the titanium alloy component 10.

[0037] Step S20: Fix the titanium alloy component 10 onto the base 20 in a vertical placement manner with the longitudinal butt joint perpendicular to the ground, and adjust the butt joint size parameters. Weld an arc-starting plate and an arc-extinguishing plate to both ends of the longitudinal butt joint. Move the two tungsten inert gas (TIG) welding torches 40 integrated on the automatic welding torch adjustment frame 30, which are arranged opposite to each other and can be raised and lowered synchronously, to both sides of the titanium alloy component 10, so that the two TIG welding torches 40 are opposite to the two narrow gap bevels 11.

[0038] Step S30: Based on the butt joint dimensions of the longitudinal butt joint, use automatic welding or manual TIG welding to perform alternating single-gun root pass welding. During the root pass welding process, one side of the tungsten inert gas (TIG) welding torch 40 initiates arc welding, while the other side of the tungsten inert gas (TIG) welding torch 40 moves synchronously for gas protection.

[0039] Step S40: Clean the weld formed after the initial welding and measure the angular deformation at the weld. Use single-gun welding to control the angular deformation so that the weld meets the requirements of subsequent welding.

[0040] Step S50: After adjusting the welding parameters, perform synchronous double-gun filler welding. During the filler welding process, both tungsten electrode oscillating TIG welding guns 40 ignite arcs and perform tungsten electrode oscillating narrow-gap TIG automatic welding from bottom to top in a single-layer, single-pass manner.

[0041] Step S60: After adjusting the welding parameters, perform simultaneous cap welding with two guns. During the cap welding process, both tungsten electrode oscillating TIG welding guns 40 start the arc and perform tungsten electrode oscillating narrow gap TIG automatic welding from bottom to top in a single layer and single pass manner. After the cap welding is completed, a complete longitudinal weld is formed on the titanium alloy component 10.

[0042] The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding method described in this application adopts a vertical placement method that makes the longitudinal butt joint perpendicular to the ground to achieve vertical welding, which can reduce the impact of horizontal placement (flat welding or horizontal welding) on ​​the structural welding formation; combined with the dual-gun synchronous welding process, continuous welding can be achieved in one assembly without frequent hoisting, turning, and transportation; double-sided synchronous welding makes the positive and negative welding stresses cancel each other out, effectively reducing welding residual stress and deformation; at the same time, the design of the narrow gap bevel 11 greatly reduces the amount of filler metal used and significantly improves welding efficiency.

[0043] The following will describe in detail the specific process of each step of the automatic vertical welding method described in this application. This embodiment takes the processing and forming process of the longitudinal weld on the columnar titanium alloy component 10 as an example.

[0044] Step S10: Beveling the edges on the titanium alloy component 10 used to form the longitudinal butt joint.

[0045] Specifically, such as Figure 1 and Figure 2 As shown, the two sides of the longitudinal butt joint are machined by means of mechanical processing to form a narrow gap bevel 11 extending along the longitudinal butt joint on both sides of the titanium alloy component 10. The bevel is a narrow gap V-shaped bevel.

[0046] like Figure 2As shown, the bevel angle is designed to be 3°-6°, with 5.34° being the preferred design. The selection of the bevel angle needs to comprehensively consider the following factors: a smaller bevel angle can reduce the filler volume, but with continuous welding, further bevel contraction can easily lead to problems such as gun clamping, set wire clamping, and tungsten clamping; a larger bevel angle can avoid the above problems, but it increases the filler volume, and an excessively wide bevel affects sidewall fusion. A 5.34° bevel angle reduces the filler volume while also meeting the needs of manual root pass welding, effectively reducing gun clamping and tungsten clamping problems, and ensuring the quality of sidewall fusion.

[0047] like Figure 2 As shown, the narrow gap bevel 11 has a reserved blunt edge 12 with a thickness of 1mm-3mm, and the thickness of the blunt edge 12 is preferably designed to be 2mm. If the blunt edge 12 is too thin, it can ensure the penetration of the root pass, but it is easy to deform during the production process and easy to penetrate the base material during welding, resulting in voids in the weld pool; if the blunt edge 12 is too thick, it can ensure the assembly accuracy, but it will cause the root pass to be incomplete during welding, affecting the welding quality; the 2mm blunt edge 12 can well balance the above contradictions.

[0048] like Figure 2 As shown, the bottom chamfer of the narrow gap groove 11 is R4.5mm, and the height of the blunt edge 12 is 1.5mm. The bottom chamfer of R4.5mm, combined with the welding shrinkage of 2mm-3mm, ensures that the groove width of the root weld is within the optimal range of 8mm-10mm. The groove design also needs to consider the welding shrinkage of each weld pass to ensure that the groove width of each weld pass remains within the 8mm-10mm range, thus ensuring the stability of tungsten inert welding.

[0049] Step S20: Assemble and fix the titanium alloy component 10 processed in step S10 for subsequent automatic welding operations.

[0050] Specifically, such as Figure 4 As shown, the titanium alloy component 10 is fixed to the base 20 in a vertical placement manner, with the longitudinal butt joint perpendicular to the ground, and the butt joint dimensions are adjusted. For column-shell structures, it is placed vertically on the rotating platform of the welding system; for plate welding, it is placed vertically on the assembly fixture. Both cases use a vertical assembly method with the weld seam perpendicular to the ground, which can achieve continuous welding in one assembly, reducing the lifting, turning, and transportation processes during welding.

[0051] Using the outer surface or plane of the workpiece as a reference, the butt joint dimensions of the longitudinal butt joint are adjusted using temporary connecting brackets to ensure that the misalignment and assembly clearance of the longitudinal butt joint meet the welding requirements. Arc-starting plates and arc-extinguishing plates are welded to both ends of the longitudinal butt joint, with their bevels matching the workpiece bevels to ensure the quality of the arc-starting and arc-extinguishing sections of the weld.

[0052] After completing the above assembly, the two tungsten inert gas (TIG) welding torches 40 integrated on the automatic welding torch adjustment frame 30, which are arranged opposite each other and can be raised and lowered synchronously, are moved to both sides of the titanium alloy component 10, so that the two TIG welding torches 40 are opposite to the two narrow gap bevels 11, respectively, in preparation for subsequent welding operations.

[0053] The automatic torch adjustment frame 30, which integrates the tungsten inert gas (TIG) welding torch 40, can employ the automatic vertical welding system described below. Two TIG welding torches 40 are mounted at the same height on the automatic adjustment frame 30, and both torches can move synchronously up and down on the frame. Both torches 40 are equipped with rear protective covers and can perform alternating single-torch welding or simultaneous dual-torch welding, employing single-layer, single-pass welding. In this embodiment, throughout the welding process, the TIG welding torch 40 uses a tungsten electrode with a diameter of 3.2 mm, and a welding wire with a diameter of 1.2 mm.

[0054] Step S30: Perform a root pass weld on the longitudinal butt joint to form a root pass weld layer at the bottom of the narrow gap bevel.

[0055] Specifically, based on the butt joint dimensions, automatic welding or manual TIG welding is selected for alternating single-gun root pass welding. During the root pass welding process, one side of the tungsten inert gas (TIG) welding torch 40 initiates the arc welding, while the other side of the tungsten inert gas (TIG) welding torch 40 moves synchronously for gas protection.

[0056] When the misalignment of the longitudinal butt joint is no greater than 1 mm and the assembly gap is no greater than 0.5 mm, the fit precision of the longitudinal butt joint is high. Spot welding is not allowed within the weld bead, and automatic welding can be directly used for alternating single-gun root pass welding. During the automatic root pass welding process, the tungsten inert gas (TIG) welding torch 40 on one side initiates the arc and welds from bottom to top using a single-layer, single-pass method, thereby forming a continuous weld bead at the bottom of the narrow gap groove 11 on that side to initially fuse the longitudinal butt joint. At the same time, the tungsten inert gas (TIG) welding torch 40 on the other side does not initiate the arc but moves synchronously for gas protection. The two tungsten inert gas (TIG) welding torches 40 alternately initiate the arc welding, thereby forming two weld beads in each of the two narrow gap grooves 11 on both sides, so that the deposited metal smoothly transitions to the sidewall of the narrow gap groove 11. During the automatic root pass welding process, it is necessary to avoid forming pits.

[0057] Furthermore, the welding process parameters for automatic root pass welding are as follows: the base current value of the tungsten inert gas (TIG) welding torch 40 for root pass welding is 100A-145A, the peak current value is 135A-155A, the wire feed speed is 0.6m / min-0.8m / min, and the welding speed is 100mm / min-120mm / min. During the root pass welding stage, the tungsten electrode on the tungsten inert gas welding torch 40 does not oscillate. The above parameter combination can ensure that the root of the root pass weld is fully penetrated, the deposited metal transitions smoothly with the sidewall, and no pits are formed.

[0058] When the misalignment of the longitudinal butt joint exceeds 1mm or the assembly gap exceeds 0.5mm, the assembly accuracy of the longitudinal butt joint cannot meet the requirements of automatic welding. In this case, manual TIG welding is used for the initial welding, that is, manual TIG welding is used for alternating single-gun welding of the initial weld. Figure 3 As shown, firstly, the narrow gap groove 11 on one side is tack welded from bottom to top using the tungsten electrode oscillating TIG welding gun 40 on one side. The length of the tack weld is 30mm-100mm, and the distance between adjacent welds is no more than 300mm. Each weld is welded with 2-3 layers.

[0059] After the tack welding is completed, the gap between the weld points is filled from bottom to top using the tungsten inert gas (TIG) welding torch 40, with 2-3 layers welded at each filling position. Then, the same TIG welding torch 40 is used to continue auto-fusion or fill another layer on the continuous weld seam after filling. Next, the other TIG welding torch 40 is used to perform three root pass welding passes on the narrow gap groove 11 on the back side from bottom to top to ensure root penetration of the narrow gap groove 11 on both sides. During manual TIG welding, only one TIG welding torch 40 initiates the arc, while the other TIG welding torch 40 does not initiate the arc but moves synchronously for gas protection. This method is suitable for situations where the assembly accuracy of the titanium alloy component 10 is poor, as manual root pass welding can compensate for assembly errors and create favorable conditions for subsequent automatic welding.

[0060] Step S40: Measure and control the angular deformation of the root pass layer in step S30.

[0061] After the root pass welding is completed, the weld seam (root pass weld layer) formed by the root pass welding is cleaned, and the angular deformation at the weld seam is measured. Based on the measurement results, single-gun welding is used to control the angular deformation. By adjusting the filler amount of the welding gun on one side, the angular deformation is actively compensated to ensure that the weld seam meets the requirements of subsequent filler welding. Because the angular deformation is actively measured and controlled in step S40, the angular deformation in the weld seam area can be controlled within 1mm (100mm area on both sides of the weld seam), solving the problem of difficult deformation control in existing flat welding processes.

[0062] Step S50: Perform filler welding on top of the pre-treated root pass to form a filler pass.

[0063] Specifically, after adjusting the welding parameters, simultaneous automatic filler welding with two tungsten electrode oscillating (TIG) torches is performed. During the filler welding process, both torches ignite at 40°, and a single-layer, single-pass TIG welding process is adopted from bottom to top, using a narrow-gap TIG welding method. The weld metal must smoothly transition to the sidewall, and pitting is not allowed. The filler volume can be fine-tuned at any time during the welding process to further control weld angle deformation. The simultaneous dual-torch filler welding ensures symmetrical and uniform filler layers on both sides. Because the welding stresses on both sides cancel each other out, residual welding stress and deformation are effectively reduced.

[0064] Furthermore, the base current value for filler welding using the tungsten electrode oscillating TIG welding torch 40 is 130A-170A, the peak current value is 160A-185A, the wire feed speed is 0.85m / min-1.3m / min, and the welding speed is 50mm / min-70mm / min. The half-oscillation amplitude of the tungsten electrode on the tungsten electrode oscillating TIG welding torch 40 is 25°-30° (amplitude of unilateral oscillation), the dwell time at both ends is 0.3s-0.8s, the oscillation speed is 20rpm-60rpm, and the half-oscillation width is 1.0mm-1.6mm (width of unilateral oscillation). These parameters ensure that heat is evenly applied to the bevel sidewall, guaranteeing the fusion quality of the sidewall, while effectively controlling heat input and suppressing grain coarsening through single-layer, single-pass welding. When the tungsten electrode oscillates to a distance of 1.5mm from the bevel sidewall, the dwell time of the tungsten electrode on both sides of the bevel is preferably 0.5s, the tungsten electrode oscillation width does not exceed 10mm, and the width of the welded part does not exceed 12mm. By precisely controlling the tungsten electrode oscillation parameters, the arc heat is ensured to fully cover the bevel sidewall, effectively solving the problem of incomplete fusion of the narrow gap sidewall, while preventing poor weld formation due to excessive oscillation.

[0065] Step S60: Perform capping welding over the filler weld layer formed in step S50 to form a capping weld layer.

[0066] Specifically, after adjusting the welding parameters, simultaneous automatic capping welding with two welding torches was performed. During the capping welding process, both tungsten electrode oscillating TIG welding torches 40 were ignited, and a single-layer, single-pass method was used to perform narrow-gap TIG automatic welding from bottom to top. After the capping welding was completed, a complete longitudinal weld was formed on the titanium alloy component 10. The simultaneous dual-torch capping welding method ensured that the capping weld layers on both sides were symmetrical and uniform. Since the welding stresses on both sides canceled each other out, the residual welding stress and deformation could be effectively reduced.

[0067] Furthermore, the base current value for cap welding using the tungsten inert gas (TIG) oscillating TIG welding torch 40 is 130A-170A, the peak current value is 150A-175A, the wire feed speed is 0.85m / min-1.3m / min, and the welding speed is 50mm / min-70mm / min. The half-oscillation amplitude of the tungsten electrode on the tungsten inert gas welding torch 40 is 25°-30°, the dwell time at both ends is 0.3s-0.8s, the oscillation speed is 20rpm-60rpm, and the half-oscillation width is 1.1mm-1.8mm. When the tungsten electrode oscillates to a distance of 1.5mm from the bevel sidewall, the oscillation width should not exceed 10mm, and the width of the welded part should not exceed 12mm.

[0068] According to one embodiment of this application, during the welding process in steps S30 to S60, 99.999% high-purity argon gas is used as the shielding gas. For the tungsten inert gas (TIG) welding torch 40 that performs welding after arc initiation, the argon gas flow rate of its main nozzle is 10 L / min-20 L / min, and the argon gas flow rate of the rear shielding shroud is 15 L / min-25 L / min. For the tungsten inert gas (TIG) welding torch 40 that performs gas protection while not arcing in step S30 but moves synchronously, the argon gas flow rate of its back shielding is 15 L / min-25 L / min. Through the synergistic effect of the three gas streams—main nozzle, rear shielding shroud, and back shielding—the weld and heat-affected zone are protected from oxidation throughout the welding process.

[0069] Furthermore, for TIG welding torches with a tungsten electrode oscillation (TIG) torch, gas should be supplied in advance before arc ignition, and gas should be stopped with a delay after arc extinguishing. The delay should be based on the weld color turning silvery-white or light yellow after cooling at the arc extinguishing point. This method ensures that the weld is always under inert gas protection during the high-temperature stage, effectively preventing discoloration and even performance degradation of the titanium alloy due to oxidation during cooling. The arc crater should be filled before each arc extinguishing, and wind protection should be implemented throughout the process. The arc ignition and extinguishing points should be set within the arc ignition and extinguishing plates as much as possible.

[0070] If an equipment alarm occurs during welding, welding should be stopped immediately. Welding can only resume after the alarm signal is cleared and the cause of the alarm is identified.

[0071] Implementation Method Two: This application also provides a double-sided synchronous narrow-gap automatic vertical welding system for titanium alloy butt joints, such as... Figure 4 As shown, it can be used in the automatic vertical welding method described in Embodiment 1. The automatic vertical welding system includes a base 20, an automatic welding torch adjustment frame 30, and two tungsten electrode oscillating TIG welding torches 40.

[0072] The base 20 is used to place the titanium alloy component 10 to be welded. An automatic welding torch adjustment frame 30 is located on one side of the base 20, and includes a column 31, a horizontal arm 32 on top of the column 31, and two head travel slides 33 on the horizontal arm 32. The two head travel slides 33 are parallel to each other and spaced apart, both extending vertically. Two tungsten inert gas (TIG) welding torches 40 are slidably mounted on the two head travel slides 33, allowing them to rise and fall synchronously relative to both sides of the titanium alloy component 10, achieving double-sided synchronous narrow-gap TIG automatic vertical welding. The two tungsten inert gas (TIG) welding torches 40 employ a single-layer, single-pass welding method, equipped with an automatic wire feeder and a rear protective cover, enabling alternating single-torch or simultaneous dual-torch welding.

[0073] The titanium alloy butt joint double-sided synchronous narrow gap automatic vertical welding system described in this application achieves double-sided synchronous narrow gap TIG automatic vertical welding by mounting two tungsten inert gas (TIG) welding torches 40 on two vertically extending head travel slide plates 33, enabling the two torches to rise and fall synchronously relative to the two sides of the titanium alloy component 10. The system has a compact structure and is suitable for various vertical welding scenarios.

[0074] It should be understood that expressions such as "comprising" and "may include" as used in this application indicate the existence of the disclosed functions, operations, or constituent elements, and do not limit one or more additional functions, operations, and constituent elements. In this application, terms such as "comprising" and / or "having" may be interpreted as indicating a specific characteristic, number, operation, constituent element, component, or combination thereof, but should not be interpreted as excluding the existence or possibility of adding one or more other characteristics, numbers, operations, constituent elements, components, or combinations thereof.

[0075] It should be understood that the terms “center,” “upper,” “lower,” “front,” “rear,” “left,” “right,” “vertical,” “horizontal,” “inner,” “outer,” “clockwise,” “counterclockwise,” “axial,” “radial,” and “circumferential” indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0076] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0077] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0078] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A method of titanium alloy butt joint double-sided simultaneous narrow gap automatic vertical welding for welding a longitudinal butt joint extending in a vertical direction on a vertically standing titanium alloy member (10), characterized by, The automatic vertical welding method includes: Step S10: The two sides of the longitudinal butt joint are machined by means of mechanical processing to form a narrow gap bevel (11) extending along the longitudinal butt joint on both sides of the titanium alloy component (10). Step S20: Fix the titanium alloy component (10) on the base (20) in a vertical placement manner with the longitudinal butt joint perpendicular to the ground and adjust the butt joint size parameters. Weld an arc-starting plate and an arc-extinguishing plate at both ends of the longitudinal butt joint. Move the two tungsten inert gas (TIG) welding torches (40) integrated on the automatic adjustment frame (30) that are opposite to each other and can be raised and lowered synchronously to both sides of the titanium alloy component (10), so that the two tungsten inert gas (TIG) welding torches (40) are opposite to the two narrow gap bevels (11). Step S30: According to the butt joint size parameters of the longitudinal butt joint, the root welding is carried out by automatic welding or manual argon arc welding with alternating single guns. During the root welding process, the tungsten inert gas (TIG) welding gun (40) on one side starts arc welding, and the tungsten inert gas (TIG) welding gun (40) on the other side moves synchronously for gas protection. Step S40: Clean the weld formed after the initial welding and measure the angular deformation at the weld. Use single-gun welding to control the angular deformation so that the weld meets the requirements of subsequent welding. Step S50: After adjusting the welding parameters, perform synchronous double-gun filler welding. During the filler welding process, both tungsten electrode oscillating TIG welding guns (40) start arcs and perform tungsten electrode oscillating narrow gap TIG automatic welding from bottom to top in a single-layer single-pass manner. Step S60: After adjusting the welding parameters, perform simultaneous double-gun cover welding. During the cover welding process, both tungsten inert gas (TIG) welding guns (40) start arcs and perform tungsten inert gas (TIG) oscillation with narrow gaps from bottom to top in a single-layer, single-pass manner. After the cover welding is completed, a complete longitudinal weld is formed on the titanium alloy component (10).

2. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 1, characterized in that, In step S30 above: If the misalignment of the longitudinal butt joint is not greater than 1 mm and the assembly gap is not greater than 0.5 mm, then automatic welding is used to perform single-gun alternating root pass welding. The tungsten inert gas (TIG) welding gun (40) on one side starts the arc and welds from bottom to top in a single layer and single pass manner. The tungsten inert gas (TIG) welding gun (40) on the other side does not start the arc but moves synchronously for gas protection. The two tungsten inert gas (TIG) welding guns (40) alternately form two weld passes in the two narrow gap grooves (11) on both sides so that the deposited metal and the side wall of the narrow gap groove (11) can be smoothly transitioned. If the misalignment of the longitudinal butt joint is greater than 1 mm or the assembly gap is greater than 0.5 mm, manual argon arc welding is used for single-gun alternating root pass welding. First, the tungsten inert gas (TIG) welding gun (40) on one side is used to perform tack welding on the narrow gap groove (11) on the same side from bottom to top. The length of the tack weld is 30 mm to 100 mm, and the distance between adjacent welds is no more than 300 mm. Each weld is welded with 2-3 layers. Then, the tungsten inert gas (TIG) welding gun (40) is used to fill the gap between the welds from bottom to top. Each filling position is also welded with 2-3 layers. Then, the tungsten inert gas (TIG) welding gun (40) is used to continue self-melting or filling a layer on the continuous weld after filling. After that, the tungsten inert gas (TIG) welding gun (40) on the other side is used to perform root pass welding and filling 3 times on the narrow gap groove (11) on the back side from bottom to top so that the root of the narrow gap groove (11) on both sides is melted through.

3. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 1 or 2, characterized in that, The narrow gap bevel (11) has a reserved blunt edge (12) with a thickness of 1mm-3mm. The bevel angle of the narrow gap bevel (11) is 3°-6°. The height of the blunt edge (12) is 1.5mm. The bottom chamfer of the narrow gap bevel (11) is R4.5mm.

4. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 3, characterized in that, In step S30 above, the base current value of the tungsten electrode oscillating TIG welding torch (40) for root pass welding is 100A-145A, the peak current value is 135A-155A, the wire feed speed is 0.6m / min-0.8m / min, and the welding speed is 100mm / min-120mm / min. During the root pass welding stage, the tungsten electrode on the tungsten electrode oscillating TIG welding torch (40) does not oscillate.

5. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 3, characterized in that, In step S50 above, the base current value of the tungsten electrode oscillating TIG welding torch (40) for filler welding is 130A-170A, the peak current value is 160A-185A, the wire feed speed is 0.85m / min-1.3m / min, and the welding speed is 50mm / min-70mm / min; the half-oscillation amplitude of the tungsten electrode on the tungsten electrode oscillating TIG welding torch (40) is 25°-30°, the dwell time at both ends is 0.3s-0.8s, the oscillation speed is 20rpm-60rpm, and the half-oscillation width is 1.0mm-1.6mm.

6. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 3, characterized in that, In step S60 above, the base current value of the tungsten electrode oscillating TIG welding torch (40) for cover welding is 130A-170A, the peak current value is 150A-175A, the wire feed speed is 0.85m / min-1.3m / min, and the welding speed is 50mm / min-70mm / min; the half-oscillation amplitude of the tungsten electrode on the tungsten electrode oscillating TIG welding torch (40) is 25°-30°, the dwell time at both ends is 0.3s-0.8s, the oscillation speed is 20rpm-60rpm, and the half-oscillation width is 1.1mm-1.8mm.

7. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 1, characterized in that, In the welding process of steps S30 to S60 above, high-purity argon is used as the shielding gas; for the tungsten inert gas oscillating TIG welding torch (40) that performs welding after arc initiation, the argon flow rate of its main nozzle is 10L / min-20L / min, and the argon flow rate of the back shielding gas behind the welding position is 15L / min-25L / min; for the tungsten inert gas oscillating TIG welding torch (40) that does not perform arc initiation but performs gas shielding while moving synchronously, the argon flow rate of its back shielding gas is 15L / min-25L / min.

8. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 7, characterized in that, The tungsten electrode oscillating TIG welding torch (40) supplies gas in advance before ignition and stops gas after extinguishing the arc. The time of stopping gas is based on the color of the weld at the extinguishing point being silver-white or light yellow after cooling.

9. The method of butt joint double-sided simultaneous narrow gap automatic vertical welding of titanium alloys according to claim 3, characterized in that, The narrow gap bevel (11) is designed with welding shrinkage in mind so that the bevel width at the root of the longitudinal weld is 8mm-10mm.

10. A titanium alloy butt joint double-sided simultaneous narrow gap automatic vertical welding system for carrying out the titanium alloy butt joint double-sided simultaneous narrow gap automatic vertical welding method according to any one of claims 1 to 9, characterized by, The automatic vertical welding system includes: A base (20) is used to place the titanium alloy component (10) to be welded. The welding torch automatic adjustment frame (30) includes a column (31), a horizontal arm (32) on the top of the column (31), and two head travel slides (33) on the horizontal arm (32). The two head travel slides (33) are parallel to each other and spaced apart, and the length direction of the head travel slides (33) is extended in the vertical direction. Two tungsten electrode oscillating TIG welding torches (40) are respectively mounted on the two machine head travel slide plates (33) and can slide up and down.