Electroslag remelting device based on rare earth kovar alloy
By using a funnel-shaped gate and a rotating magnetic field structure in electroslag remelting technology, the problems of low refining efficiency and poor purification effect in traditional technology are solved, achieving efficient smelting and purification of rare earth Kovar alloys, reducing production costs and energy consumption.
Patent Information
- Application Number
- CN202420302489.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2034-02-19
AI Technical Summary
Traditional electroslag remelting technology has problems such as low refining efficiency and incomplete removal of non-metallic inclusions, which makes it difficult to meet the requirements for smelting purity and high production efficiency and energy consumption.
An electroslag remelting device based on rare earth Kovar alloy is used. The funnel-shaped gate is used to evenly inject the Kovar alloy liquid into the slag layer in the form of droplets, and combined with the rotating magnetic field structure, the rotation of the droplets in the slag layer is enhanced. and contact area to improve the purification effect.
It improves the smelting efficiency and purification effect, reduces production costs, avoids central segregation and loosening problems caused by heat accumulation in traditional technology, and significantly improves the cleanliness of materials.
Smart Images

Figure CN221810401U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the field of kovar alloys, in particular to an electroslag remelting device based on rare earth kovar alloys. Background Art
[0002] Kovar alloy is a high-performance precision alloy, which is composed of metal elements such as steel, nickel, and cobalt. It has excellent thermal expansion performance, processing performance, welding performance, corrosion resistance, and low thermal expansion coefficient. It usually has a relatively stable thermal expansion coefficient in the range of -180℃ to +450℃, and can be made into parts of various shapes. Therefore, it is widely used in aviation, aerospace, shipbuilding, electronics and other fields. With the development needs of the country for aerospace, military nuclear power, higher requirements are put forward for alloy materials, especially the requirements for the smelting purity of materials are getting higher and higher.
[0003] Electroslag remelting technology is one of the key refining processes for preparing Kovar alloy. Traditional electroslag remelting (ESR) uses the resistance heat generated when current passes through the molten slag as a heat source to melt the alloy parent material of the consumable conductive ring. The liquid metal falls through the slag layer into the metal molten pool in the water-cooled crystallizer in the form of molten droplets, that is, the slag washes the Kovar alloy liquid to achieve the method of refining the alloy.
[0004] However, the traditional electroslag remelting technology still has the problems of low refining efficiency and incomplete removal of non-metallic inclusions. There are even non-metallic inclusions larger than 20um. In order to obtain pure electroslag ingots, the electroslag remelting process has to be used multiple times, which not only reduces the production efficiency of electroslag, but also greatly increases the unit energy consumption of electroslag ingots. Utility Model Content
[0005] One purpose of the utility model is to provide an electroslag remelting device based on rare earth Kovar alloy, which allows Kovar alloy liquid to be uniformly injected into a slag layer in the form of droplets through a funnel-shaped pouring gate to improve refining efficiency.
[0006] This purpose is achieved by adopting the following technical solutions:
[0007] An electroslag remelting device for rare earth Kovar alloy comprises a crystallizer and a conductive ring, wherein the lower part of the crystallizer is a metal pool for containing Kovar alloy liquid, the middle part of the crystallizer is a slag layer, the lower end of the conductive ring extends into the slag layer, a casting device for placing Kovar alloy liquid is arranged on the crystallizer, and a plurality of funnel-shaped gates are arranged at the lower end of the casting device, and the funnel-shaped gates are used to inject the Kovar alloy liquid into the slag layer in the form of droplets. A heating structure is arranged in the casting device, and the heating structure heats the Kovar alloy liquid in the casting device.
[0008] Compared with the existing devices, the present device places the molten Kovar alloy directly in the casting equipment, and there is no need to process the molten Kovar alloy into consumable conductive rings. This not only reduces the cooling, annealing, transportation, cleaning, welding and other processes of the solid consumable conductive ring blanks, but also the direct electroslag smelting of the molten Kovar alloy during remelting, and the thermal efficiency and melting rate are much higher than those of the traditional electroslag technology, and the production costs such as energy consumption, transportation and manufacturing are greatly reduced.
[0009] At the same time, a plurality of funnel-shaped gates are provided at the lower end of the casting equipment, and the Kovar alloy liquid is injected into the slag layer in the form of droplets at the lower end of the funnel-shaped gate. The funnel-shaped gates are evenly distributed above the slag layer. Therefore, compared with the existing structure, the metal droplets in the device no longer converge centripetally but are evenly distributed and separated, making the temperature of the slag layer and the metal pool more uniform, forming a shallower metal molten pool. This solves the problem that the molten droplets formed by the melting of the conductive ring in the traditional electroslag remelting process are too concentrated, so that the heat transmitted to the metal pool accumulates in the center of the ingot, which is easy to form a deep V-shaped molten pool, resulting in the inevitable generation of center segregation, channel segregation (black spots), looseness and other technical difficulties during the solidification process.
[0010] Secondly, the opening at the lower end of the funnel-shaped gate of the device can be adjusted as needed to keep the Kovar alloy liquid in a droplet shape and reduce the size of the droplets, which is beneficial to improving the cleanliness of the material. Under the action of gravity, the droplets leaking from the funnel-shaped gate are smaller in size, so the possibility of non-metallic inclusions being adsorbed by the flux at the phase interface and then assimilated is increased.
[0011] Preferably, a plurality of liquid outlet holes are provided on the side of the funnel-shaped gate. A plurality of drainage grooves are provided on the side of the funnel-shaped gate, and the drainage grooves are used to transfer the liquid droplets flowing out of the liquid outlet holes to the liquid droplets flowing out of the lower end of the funnel-shaped gate. Preferably, the drainage grooves are spirally distributed on the side of the funnel-shaped gate. Preferably, the angle between the axis of the liquid outlet hole and the vertical line is an acute angle to prevent the liquid droplets from falling quickly when flowing out of the side of the funnel-shaped gate.
[0012] During the outflow process, the Kovar alloy liquid flows out through several outlet holes on the side of the funnel-shaped gate and converges on the droplets at the lower end of the funnel-shaped gate through the drainage groove. During the process of the droplets gradually converging and dripping, any part of the inclusions may contact the molten droplets and react with the slag, which can better improve the accuracy.
[0013] Furthermore, a rotating magnetic field structure is provided on the crystallizer, and the rotating magnetic field structure enables the droplets to move downward in a spiral in the slag layer. In the existing rotating magnetic field structure, for example, an electroslag casting device and method with an external electromagnetic stirring, which is application number 2009100102413, the metal droplets melted by the consumable conductive ring fall in a spiral line in the non-conductive slag layer under the action of the rotating magnetic field. Compared with the refining process in which the magnetic field is not applied and the metal droplets fall directly, the movement distance is increased, and the relative speed with the slag layer is increased, thereby enhancing the ability of the metal droplets to remove impurities and perform deep desulfurization, and the effect of improving the refining efficiency can be achieved. However, in actual use, the inventor of the utility model found that in the magnetic field structure, the droplets are always spirally rotating in the slag layer. When the droplets in the funnel-shaped gate continue to be injected and superimposed on the spirally rotating droplets in the slag layer, so that their weight increases, they break through the suction force of the magnetic field and fall into the metal pool. Therefore, the volume of the droplets in the rotating magnetic field structure is large relative to the volume of the droplets flowing down from the consumable conductive ring, and the large-sized droplets are less likely to be adsorbed by the flux at the interface, resulting in poor purification effect.
[0014] Based on this, the utility model provides another rotating magnetic field, the rotating magnetic field structure includes a conical stator winding, the axial force generated by the conical stator winding gradually decreases from top to bottom. Therefore, when the droplets are in the rotating magnetic field generated by the conical stator winding, they first rotate under the action of the relatively large axial force above. Since the axial force gradually decreases from top to bottom, the droplets can achieve the effect of spirally falling from top to bottom, which increases the time the droplets stay in the slag layer, and also achieves the purpose of keeping the droplets in a small size and rotating in the slag layer, increasing the contact area and improving the purification effect.
[0015] On the other hand, a method for electroslag remelting of a rare earth kovar alloy comprises the following steps:
[0016] The Kovar alloy liquid in the casting equipment is injected into the slag layer in the form of droplets through a number of funnel-shaped gates;
[0017] The rotating magnetic field structure on the crystallizer causes the droplets to move downward in a spiral in the slag layer.
[0018] A plurality of liquid outlet holes and drainage grooves are arranged on the side of the funnel-shaped gate. Liquid droplets flowing out of the liquid outlet holes converge with liquid droplets flowing out of the lower end of the funnel-shaped gate under the action of the drainage grooves.
[0019] Compared with the prior art, the utility model has the following advantages and beneficial effects:
[0020] The utility model discloses an electric slag remelting device based on rare earth Kovar alloy. The utility model adopts a method of injecting a slag layer in the form of droplets using multiple funnel-shaped gates to replace the existing smelting method of remelting a solid consumable conductive ring, thereby reducing the processes of cooling, annealing, transporting, cleaning, welding, etc. of the consumable conductive ring blank, and can effectively reduce costs and improve production efficiency.
[0021] Secondly, the multiple funnel-shaped gates of the device are evenly distributed above the slag layer, so that the molten metal droplets no longer converge centripetally but are evenly distributed and separated, making the temperature of the slag layer and the metal pool more uniform, forming a shallower molten metal pool. This solves the problem that the molten droplets formed by the melting of the conductive ring in the traditional electroslag remelting process are too concentrated, causing the heat transmitted to the molten metal pool to accumulate in the center of the ingot, easily forming a deep V-shaped molten pool, and inevitably causing technical problems such as center segregation, channel segregation (black spots), and looseness during the solidification process;
[0022] In addition, the size of the liquid outlet at the lower end of the funnel-shaped gate of the utility model is adjustable, which can better reduce the droplet size of the molten metal droplets, increase the refining reaction area, and improve the cleanliness. In addition, the multiple liquid outlet holes and drainage grooves on the side of the funnel-shaped gate allow the metal droplets to move along the drainage grooves on the side of the funnel-shaped gate, increasing the contact time and area with the slag layer and improving the purification effect. At the same time, the droplets on the side of the funnel-shaped gate and the droplets at the lower end of the funnel-shaped gate converge and are injected into the slag layer. The size of the converged droplets is smaller than the droplet size of the existing device, which is more conducive to removing impurities. At the same time, the droplets on the side of the funnel-shaped gate contact and react with the slag during the movement of the side of the funnel-shaped gate before converging, so that a large number of inclusions can be initially removed.
[0023] At the same time, compared with the existing rotating magnetic field, the rotating magnetic field structure of the device can make the droplets injected into the slag layer fall in a spiral, solving the problem that the existing rotating magnetic field needs to accumulate more droplets into large droplets until they are greater than the magnetic field force and fall, and cannot always keep small droplets, thus affecting the final purification effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The drawings described herein are used to provide a further understanding of the embodiments of the present utility model, constitute a part of this application, and do not constitute a limitation of the embodiments of the present utility model. In the drawings:
[0025] Figure 1 This is a schematic diagram of the structure of the device in Example 1;
[0026] Figure 2 is a cross-sectional view of the funnel-shaped gate in Example 2;
[0027] Figure 3 It is a schematic diagram of the structure in which the drainage grooves are spirally distributed on the side of the funnel-shaped gate in Example 2;
[0028] Figure 4 Schematic diagram of the conical stator winding structure in Example 3;
[0029] Figure 5 This is a schematic diagram of the structure of the device in Example 4.
[0030] Marks and corresponding parts names in the attached drawings:
[0031] 1-crystallizer, 2-conductive ring, 3-slag layer, 4-metal pool, 5-casting equipment, 6-funnel-shaped gate, 61-drainage groove, 62-liquid outlet hole, 7-conical stator winding, 8-controller, 9-stirring rod. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the utility model more clearly understood, the utility model is further described in detail below in conjunction with embodiments and drawings. The schematic implementation manner of the utility model and its description are only used to explain the utility model and are not intended to limit the utility model.
[0033] In the description of the present invention, it should be understood that the terms "front", "rear", "left", "right", "up", "down", "vertical", "horizontal", "high", "low", "inside", "outside", etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as limiting the scope of protection of the present invention.
[0034] Example 1
[0035] like Figure 1 As shown, it includes a crystallizer 1 and a conductive ring 2. The lower part of the crystallizer 1 is a metal pool 4 for accommodating the Kovar alloy liquid. The middle part of the crystallizer 1 is a slag layer 3. The lower end of the conductive ring 2 extends into the slag layer 3. A casting device 5 for placing the Kovar alloy liquid is provided on the crystallizer 1. The lower end of the casting device 5 is provided with a plurality of funnel-shaped gates 6. The plurality of funnel-shaped gates 6 are evenly arranged above the slag layer 3. The discharge port at the lower end of the funnel-shaped gate 6 is relatively small. Preferably, the inner diameter of the discharge port at the lower end of the funnel-shaped gate 6 is less than 0.5 cm. In actual use, the inner diameter of the discharge port can be adjusted according to the Kovar alloy liquid and actual conditions, so that the Kovar alloy liquid flows down in the form of droplets after passing through the discharge port. The Kovar alloy liquid is injected into the slag layer 3 through the discharge port at the lower end of the funnel-shaped gate 6 in the casting device 5. The Kovar alloy liquid is injected into the slag layer 3 from the discharge port at the lower end of the funnel-shaped gate 6 in the form of droplets.
[0036] In some embodiments, the casting device 5 includes a heating structure, and the heating structure includes an electromagnetic coil wound around the casting device 5. The electromagnetic coil is connected to the controller 9, and the electromagnetic coil is used to heat the Kovar alloy liquid in the casting device 5.
[0037] The Kovar alloy liquid enters the funnel-shaped gate 6 in the casting equipment, and the Kovar alloy liquid is injected into the slag layer 3 from the discharge port at the lower end of the funnel-shaped gate 6 in the form of droplets.
[0038] Example 2
[0039] Based on Example 1, the cross-sectional view of the funnel-shaped gate 6 is as follows: Figure 2 As shown, the side of the funnel-shaped gate 6 is provided with a plurality of liquid outlet holes 62, and the drainage groove 61 is used to connect the discharge port at the lower end of the funnel-shaped gate 6 and at least one liquid outlet hole 62. The liquid outlet hole 62 is arranged obliquely upward, and the angle between the axis of the liquid outlet hole 62 and the vertical line is an acute angle. Preferably, the angle between the axis of the liquid outlet hole 62 and the vertical line is 30 degrees. The side of the funnel-shaped gate 6 is provided with a plurality of drainage grooves 61, such as Figure 3 As shown, the drainage grooves 61 are spirally distributed on the side of the funnel-shaped gate 6. The drainage grooves 61 are used to transfer the liquid drops flowing out of the liquid outlet through hole 62 to the liquid drops flowing out of the lower end of the funnel-shaped gate 6.
[0040] When the Kovar alloy liquid flows out from the liquid outlet through hole, the upwardly inclined liquid outlet through hole can prevent the liquid droplets from falling directly vertically when passing through the liquid outlet through hole. Through the upwardly inclined liquid outlet through hole, the liquid droplets on the side of the funnel-shaped gate 6 can move along the drainage groove, and finally converge on the liquid droplets flowing out of the discharge port at the lower end of the funnel-shaped gate 6, and fall into the slag layer together.
[0041] In some embodiments, the funnel-shaped gate 6 is completely located in the slag layer 3, and the drainage grooves 61 are spirally distributed on the side of the funnel-shaped gate 6, thereby increasing the time that the droplets flowing out of the drainage grooves 61 stay in the slag layer 3, and also increasing the contact area between the droplets flowing out of the drainage grooves 61 and the slag layer 3. When the droplets flowing out of the drainage grooves 61 converge with the droplets flowing out of the discharge port, the droplets flowing out of the drainage grooves 61 are already cleaned droplets. Therefore, after converging at the discharge port, a better cleaning effect can be achieved quickly.
[0042] Example 3
[0043] The crystallizer 1 is provided with a rotating magnetic field structure, which enables the liquid droplets to move downward in a spiral in the slag layer 3. The rotating magnetic field structure is connected to a controller 8, and the controller 8 is used to control whether the rotating magnetic field structure is powered on.
[0044] In this embodiment, the rotating magnetic field structure includes a conical stator winding 7 arranged outside the crystallizer 1, such as Figure 4As shown, the inner diameter of the conical stator winding 7 gradually increases from top to bottom, and the inner diameter of the lower end of the conical stator winding 7 is larger than the inner diameter of the upper end. When the coil on the conical stator winding 7 is energized, the conical stator winding 7 generates a rotating magnetic field in the crystallizer 1, so that the droplets of the conductive metal material Kovar alloy liquid spirally rotate in the slag layer 3. And because the axial force generated by the conical stator winding 7 gradually decreases from top to bottom, the droplets can fall in a spiral.
[0045] The principle of metal rotation in a rotating magnetic field involves the effects of electromagnetic induction and the Lorentz force. According to Faraday's law of electromagnetic induction, when a conductor moves in a magnetic field or the intensity of the magnetic field changes, an induced electromotive force will be generated in the conductor. The induced electromotive force will cause current to flow in the conductor, forming an induced current. The force exerted on the charged particles moving in the electromagnetic field is the Lorentz force, that is, the axial force in this embodiment is the Lorentz force. After the conical stator winding 7 is energized, the Lorentz force generated gradually decreases from top to bottom. Therefore, when the weight of the droplet remains unchanged, it can gradually fall during the spiral rotation.
[0046] In this embodiment, the upper end of the conical stator winding 7 is flush with the upper end of the funnel-shaped gate 6, and the drainage grooves 61 on the side of the funnel-shaped gate 6 are spirally distributed on the side of the funnel-shaped gate 6, and the spiral direction of the drainage grooves is the same as the rotation direction of the rotating magnetic field. The rotating magnetic field generated by the conical stator winding 7 can promote the droplets flowing out of the side of the funnel-shaped gate 6 to flow along the drainage grooves 61, thereby improving the purification efficiency.
[0047] Example 4
[0048] Based on some embodiments, Figure 5 As described, the upper end of the conical stator winding 7 is flush with the upper end of the funnel-shaped gate 6, and a plurality of stirring rods 9 are provided in the casting device 5, and the plurality of stirring rods 9 are connected to the plurality of funnel-shaped gates 6 in a one-to-one correspondence, and the funnel-shaped gates 6 can all rotate at the connection between them and the casting device 5, and the funnel-shaped gate 6 and the casting device 5 can be connected through a rotating groove and a rotating protrusion, and the upper end of the funnel-shaped gate 6 is connected to the stirring rod 9, and the stirring rod 9 is located in the casting device 5. Moreover, the stirring rod 9 is connected to the funnel-shaped gate 6, and the funnel-shaped gate 6 is made of metal material. When the funnel-shaped gate 6 rotates under the action of the rotating magnetic field, the stirring rod 9 is driven to rotate together, and the stirring rod 9 rotates the Kovar alloy liquid in the casting device 5 to improve the flow of the Kovar alloy liquid.
[0049] Example 5
[0050] Based on the above embodiment, a method for electroslag remelting of a rare earth kovar alloy comprises the following steps:
[0051] The casting device 5 heats the Kovar alloy liquid therein through a heating structure, and the Kovar alloy liquid in the casting device enters into a plurality of funnel-shaped gates 6 under the action of gravity, and is injected into the slag layer 3 in the form of droplets through the discharge port at the lower end of the funnel-shaped gate; at the same time, the droplets on the side of the funnel-shaped gate flow along the side of the funnel-shaped gate and converge at the droplets at the lower end of the funnel-shaped gate, and enter into the slag layer together;
[0052] The coil on the conical stator winding 7 is energized, and the conical stator winding 7 generates a rotating magnetic field in the crystallizer 1, causing the droplets to move downward in a spiral in the slag layer 3; the funnel-shaped gate 6 drives the stirring rod to rotate under the action of the rotating magnetic field, and the Kovar alloy liquid in the casting equipment 5 is stirred during the rotation of the stirring rod.
[0053] Example 6
[0054] On the basis of some embodiments, rare earth elements are added to the Kovar alloy material; the main function is to improve the interface performance mechanism of the Kovar alloy material and promote the grain refinement of the Kovar alloy matrix, and the mechanism of action is as follows:
[0055] First, rare earth elements have low electronegativity, so they will be preferentially adsorbed on the grain boundaries of the metal matrix and the reinforcement phase during the smelting process, reducing their interfacial energy, increasing the adhesion work of the interface, and reducing the wetting angle, thereby improving the wettability of the matrix and the reinforcement phase.
[0056] Secondly, the solubility of rare earth in Kovar alloy crystals is relatively low. Because the atomic radius of rare earth elements is large, the atomic radius of the Kovar alloy matrix is relatively small. The rare earth elements with larger radius entering the matrix lattice will cause lattice distortion and increase the energy of the system. In order to keep the free energy as low as possible, rare earth atoms can only be enriched on the grain boundaries with irregular atomic arrangement, which hinders the free growth of matrix grains to a certain extent. At the same time, the enriched rare earth elements will also adsorb other alloying elements, increase the concentration gradient of alloying elements, cause local component supercooling, and enhance the heterogeneous nucleation effect of the liquid Kovar alloy matrix. In addition, the component supercooling caused by element segregation will also promote the formation of segregated compounds and become effective heterogeneous nucleation particles, thereby promoting the refinement of Kovar alloy matrix grains.
[0057] Moreover, since rare earth elements have a strong affinity with elements such as O, S, P, and N, the standard formation free energy of their oxides, sulfides, phosphides, and nitrides is low. These compounds have a high melting point and a low density. Some of them can float up from the alloy liquid and be removed, while others are evenly distributed in the crystal, reducing the segregation of impurities at the grain boundaries, thereby purifying the grain boundaries and improving the grain boundary strength.
[0058] The terms "first", "second", "third", etc. used herein are only used to distinguish the corresponding components for the sake of clarity of description, and are not intended to limit any order or emphasize importance, etc. In addition, the term "connected" used herein, unless otherwise specified, may refer to direct connection or indirect connection via other components.
[0059] The specific implementation methods described above further illustrate the purpose, technical solutions and beneficial effects of the utility model in detail. It should be understood that the above description is only the specific implementation method of the utility model and is not used to limit the protection scope of the utility model. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the utility model should be included in the protection scope of the utility model.
Claims
1. An electroslag remelting device for rare earth Kovar alloy, comprising a crystallizer (1), wherein the lower part of the crystallizer (1) is a metal pool (4) for containing Kovar alloy liquid, and the middle part of the crystallizer (1) is a slag layer (3). It is characterized in that A conductive ring (2) is arranged on the crystallizer (1), and the lower end of the conductive ring (2) extends into the slag layer (3). A casting device (5) for placing Kovar alloy liquid is arranged above the crystallizer (1), and a plurality of funnel-shaped gates (6) are arranged at the lower end of the casting device (5), and a discharge port is arranged at the lower end of the funnel-shaped gate (6); the funnel-shaped gate (6) is located above the slag layer (3), and the discharge port allows the Kovar alloy liquid to be injected into the slag layer (3) in the form of droplets.
2. The electroslag remelting device for rare earth kovar alloy according to claim 1, It is characterized in that A plurality of liquid outlet holes (62) are arranged on the side of the funnel-shaped gate (6).
3. The electroslag remelting device for rare earth kovar alloy according to claim 2, It is characterized in that A plurality of drainage grooves (61) are arranged on the side of the funnel-shaped gate (6), and the drainage grooves (61) are used to connect the discharge port at the lower end of the funnel-shaped gate (6) and at least one liquid discharge through hole (62).
4. The electroslag remelting device for rare earth kovar alloy according to claim 3, It is characterized in that The drainage grooves (61) are spirally distributed on the side of the funnel-shaped gate (6).
5. An electroslag remelting device for rare earth kovar alloy according to any one of claims 1 to 4, It is characterized in that A rotating magnetic field structure is arranged on the crystallizer (1), and the rotating magnetic field structure comprises a conical stator winding (7), wherein the inner diameter of the conical stator winding (7) gradually increases from top to bottom.
6. The electroslag remelting device for rare earth kovar alloy according to claim 2, It is characterized in that The liquid outlet through hole (62) is arranged obliquely upward, and the angle between the axis of the liquid outlet through hole (62) and the vertical line is an acute angle.
7. The electroslag remelting device for rare earth kovar alloy according to claim 6, It is characterized in that The angle between the axis of the liquid outlet through hole (62) and the vertical line is 30 degrees.
8. The electroslag remelting device for rare earth kovar alloy according to claim 1, It is characterized in that The inner diameter of the discharge port is less than 0.5 cm.
9. The electroslag remelting device for rare earth kovar alloy according to claim 1, It is characterized in that The casting device (5) is provided with a heating structure.
10. The electroslag remelting device for rare earth kovar alloy according to claim 9, It is characterized in that The heating structure comprises an electromagnetic coil wound around the casting device (5).
Citation Information
Cited By
Electroslag remelting device and method for rare earth kovar alloy
CN118028613A