Semiconductor device
By forming a second isolation structure on the fin base of the fully wound gate field effect transistor, the problem of leakage current between adjacent source/drain regions on the fin base is solved and a more efficient circuit is achieved. isolation and more reliable device performance.
Patent Information
- Application Number
- CN202420095830.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-14
- Filing Date
- 2024-01-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2034-01-15
AI Technical Summary
In semiconductor devices, as dimensions shrink, the problem of leakage current between adjacent source/drain regions on the fin substrate becomes more serious, affecting the performance and reliability of fully wound gate field effect transistors. .
By forming a second isolation structure on the fin base of the fully wound gate field effect transistor, plasma etching techniques are used to form isolation trenches between the shallow trench isolation regions, ensuring that portions of the fin base are fully removed , to avoid leakage current caused by residual materials, and use insulating material filling to enhance electrical isolation.
It effectively avoids or minimizes the leakage current between the source/drain regions, improves the device performance and reliability of the fully wound gate field effect transistor, and improves the performance and reliability of the device.
Smart Images

Figure CN221861663U_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the utility model relate to a field effect transistor, and more particularly to an isolation structure thereof. Background Art
[0002] As semiconductor technology advances, the demand for higher storage capacity, faster processing systems, higher performance, and lower costs increases. In order to meet these demands, the semiconductor industry continues to reduce the size of semiconductor devices such as metal oxide semiconductor field effect transistors, fin field effect transistors, and all-around gate field effect transistors. The reduction in size tends to increase the complexity of the semiconductor manufacturing process. Utility Model Content
[0003] In some embodiments, a method for forming a semiconductor device includes: forming a first fin base and a second fin base on a substrate; forming multiple first nanostructure layers and multiple second nanostructure layers on the first fin base and the second fin base, respectively; forming multiple coatings on the side walls of the first nanostructure layer and the second nanostructure layer; forming a polysilicon structure on the first nanostructure layer, the second nanostructure layer, and the coating; removing a portion of the polysilicon structure to form a first opening on the second nanostructure layer; removing a portion of the second nanostructure layer through the first opening to form a second opening on the second fin base; removing a portion of the second fin base through the second opening to form a third opening on the substrate; removing a portion of the substrate through the third opening to form a fourth opening in the substrate; and depositing insulating material to fill the first opening, the second opening, the third opening, and the fourth opening.
[0004] In some embodiments, a method for forming a semiconductor device includes forming a first fin substrate and a second fin substrate on a substrate; forming a plurality of first nanostructure layers and a plurality of second nanostructure layers on the first fin substrate and the second fin substrate, respectively; forming a first isolation structure between the first fin substrate and the second fin substrate; forming a second isolation structure above the first isolation structure and between the first nanostructure layer and the second nanostructure layer; forming a polysilicon structure on the first nanostructure layer and the second nanostructure layer; and forming a third isolation structure, including forming a first isolation portion and a second isolation portion of the third isolation structure in the substrate; forming a third isolation portion and a fourth isolation portion of the third isolation structure on both sides of the first isolation structure; forming a fifth isolation portion and a sixth isolation portion of the third isolation structure on both sides of the second isolation structure; and forming a seventh isolation portion of the third isolation structure in the polysilicon structure.
[0005] In some embodiments, the semiconductor device includes: a substrate; a first fin substrate and a second fin substrate, located on the substrate; a plurality of first nanostructure layers and a plurality of second nanostructure layers, respectively located on the first fin substrate and the second fin substrate; a first gate structure and a second gate structure, respectively surrounding the first nanostructure layer and the second nanostructure layer; a first shallow trench isolation region and a second shallow trench isolation region, located on both sides of the first fin substrate and the second fin substrate; a first first isolation structure and a second first isolation structure, respectively located on the first shallow trench isolation region and the second shallow trench isolation region; and a second isolation structure. The second isolation structure includes a first isolation portion, located between the first gate structure and the second gate structure; a second isolation portion, located between the first first isolation structure and the second first isolation structure and contacting the first first isolation structure and the second first isolation structure; a third isolation portion, located between the first shallow trench isolation region and the second shallow trench isolation region and contacting the first shallow trench isolation region and the second shallow trench isolation region; and a fourth isolation portion, located in the substrate, wherein the first isolation portion is wider than the second isolation portion and the third isolation portion.
[0006] In some embodiments, the fourth isolation portion overlaps lower surfaces of the first shallow trench isolation region and the second shallow trench isolation region.
[0007] In some embodiments, the fourth isolation portion comprises a curved sidewall profile, and a bottom end has an obtuse angle.
[0008] In some embodiments, a width of an upper surface of the fourth isolation portion is 35 nm to 45 nm.
[0009] In some embodiments, the obtuse angle is between 110 and 115 degrees.
[0010] In some embodiments, the height of the fourth isolation portion is 25 nm to 40 nm.
[0011] In some embodiments, the fourth isolation portion includes a tapered sidewall profile and a substantially flat bottom profile.
[0012] In some embodiments, a width of an upper surface of the fourth isolation portion is 35 nm to 40 nm.
[0013] In some embodiments, the height of the fourth isolation portion is 45 nm to 75 nm.
[0014] In some embodiments, an angle between a sidewall and a lower surface of the fourth isolation portion is 95 degrees to 97 degrees.
[0015] At least one embodiment of the present invention has the following advantages or technical effects: it can avoid or minimize the leakage current between the source / drain regions on the fin substrate caused by any residual material in the etched portion of the fin substrate, and can improve the device performance and reliability of the fully wrapped gate field effect transistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1A is an isometric diagram of a semiconductor device having an isolation structure in some embodiments.
[0017] Figure 1B is a top view of a semiconductor device with an isolation structure in some embodiments.
[0018] Figures 1C to 1J 2 are different cross-sectional views of a semiconductor device having an isolation structure in some embodiments.
[0019] Figure 2 is a flow chart of a method for manufacturing a semiconductor device with an isolation structure in some embodiments.
[0020] Figures 3A to 3C , 4A to 4C, 5A to 5C, 6A to 6C, 7A to 7C, 8A to 8C, 9A to 9C, 10A to 10C, 11A to 11C, 12A to 12M, and 13A to 13C, 14A to 14C, and 15A to 15C are isometric views and cross-sectional views of semiconductor devices with isolation structures at various stages of the manufacturing process in some embodiments.
[0021] The accompanying drawings are described as follows:
[0022] AA,BB: Section line
[0023] B,C: Angle
[0024] D1,D2,D3: distance
[0025] GL1, GL2: Gate length
[0026] H1,H2,H3: Total height
[0027] W1,W2,W3,W4,W5: Width
[0028] 100: Field Effect Transistor
[0029] 104:Substrate
[0030] 106A, 106B, 106C, 106D: Fin base
[0031] 106Br1,106Br2,106Br3,106Cr1,106Cr2,106Cr3: Residual semiconductor materials
[0032] 106B1, 106B2, 106C1, 106C2: Fin base
[0033] 106t: Upper surface
[0034] 108A, 108B, 108C, 108D, 108E: Shallow trench isolation area
[0035] 108bs: Bottom side wall
[0036] 110A1,110A2,110A3,110A4,110B1,110B2,110B3,
[0037] 110B4,110C1,110C2,110C3,110C4,110D1,110D2,110D3,110D4: Source / drain region
[0038] 112A, 112B, 112C, 112D, 112E, 112F: Gate structure
[0039] 113A: High dielectric constant gate dielectric layer
[0040] 113B: Conductive layer
[0041] 114: Outer gate spacer
[0042] 115: Inner gate spacer
[0043] 116A, 116B, 116C, 116D, 116E: first isolation structure
[0044] 117A,121: Insulation pad
[0045] 117B,123: Insulation filling layer
[0046] 118A, 118B, 118C, 118D, 118E: Barrier layer
[0047] 119: Second isolation structure
[0048] 119A, 119B, 119C, 119D: Isolation section
[0049] 120: Etching stop layer
[0050] 122: Interlayer dielectric layer
[0051] 124A, 124B, 124C, 124D: Nanostructured channel region
[0052] 125,836A,836B: Hard mask layer
[0053] 200: Method
[0054] 205,210,215,220,225,230,235,240: Steps 323A,323B,323C,323D,: Superlattice Structure
[0055] 324A, 324B, 324C, 324D: Nanostructured layer
[0056] 336A,336B,936: Mask layer
[0057] 438: Coating
[0058] 812A,812B,812C,812CD,812D,812E,812F: Polysilicon structure
[0059] 1040,1140,1219,1240,1242: Open
[0060] 1521: Insulating oxide layer
[0061] 1523: Insulating nitride layer DETAILED DESCRIPTION
[0062] The following content is described in detail with the accompanying drawings to facilitate understanding of the embodiments of the present utility model. The following content is described with the accompanying drawings to illustrate exemplary embodiments. In the accompanying drawings, similar reference numerals generally represent identical, functionally similar, and / or structurally similar units.
[0063] The following content provides different embodiments or examples that can implement different structures of the utility model. The following specific components and arrangement embodiments are used to simplify the content of the utility model and are not intended to limit the utility model. For example, the description of forming a first component on a second component includes an embodiment in which the two are in direct contact, or an embodiment in which the two are separated by other additional components but not in direct contact. In addition, multiple examples of the utility model may repeatedly use the same number for simplicity, but the elements with the same number in multiple embodiments and / or settings do not necessarily have the same corresponding relationship.
[0064] Spatially relative terms such as "below," "beneath," "below," "above," "upper," or similar terms may be used to simplify the description of the relative relationship of one element to another element in a diagram. Spatially relative terms may be extended to elements used in other orientations, not limited to the orientation shown. Elements may also be rotated 90 degrees or other angles, so directional terms are only used to describe the orientation shown in the diagram.
[0065] It is worth noting that the embodiments described in the following content as "an embodiment", "an exemplary embodiment", "exemplary", or similar terms may include specific features, structures, or characteristics, but each embodiment may not necessarily include specific features, structures, or characteristics. In addition, these terms do not necessarily refer to the same embodiment. In addition, when specific features, structures, or characteristics are described in conjunction with an embodiment, whether or not explicitly stated, those skilled in the art can implement these features, structures, or characteristics in conjunction with other embodiments.
[0066] It should be understood that the purpose of the words or terms herein is for explanation rather than limitation, and thus those skilled in the art may interpret the words or terms of the following description based on the description herein.
[0067] In some embodiments, the terms "approximately" and "substantially" refer to a given value that varies within 5% (e.g., a value of ±1%, ±2%, ±3%, ±4%, or ±5%). These values are used for example only and are not intended to limit the embodiments of the present invention. The terms "approximately" and "substantially" may refer to a percentage of a value as interpreted by a person skilled in the art based on the context of the present invention.
[0068] The all-around gate transistor may be patterned by any suitable method. For example, the structure may be patterned using one or more photolithography processes, including double patterning or multiple patterning processes. Generally, the double patterning or multiple patterning process combines photolithography with a self-alignment process to produce a pattern pitch that is less than the pattern pitch obtained using a single direct photolithography process. For example, one embodiment forms a sacrificial layer on a substrate and patterns the sacrificial layer using a photolithography process. A self-alignment process is used to form spacers along the sidewalls of the patterned sacrificial layer. The sacrificial layer is then removed, and the retained spacers can then be used to pattern the all-around gate structure.
[0069] A fully wrapped gate field effect transistor may include a fin substrate located on a substrate, a stack of nanostructure channel regions located on a first portion of the fin substrate, a source / drain region located on a second portion of the fin substrate, a gate structure surrounding each nanostructure channel region, and a shallow trench isolation region located between adjacent fin substrates. The fully wrapped gate field effect transistor may further include a first isolation structure and a second isolation structure. The first isolation structure may be located on the shallow trench isolation region and configured to electrically isolate adjacent source / drain regions on different fin substrates. The second isolation structure may be configured to electrically isolate adjacent grouped source / drain regions on the same fin substrate. The method for forming the second isolation structure may be to replace the semiconductor material of the first portion of the fin substrate with a dielectric material. However, the reduction in the size of the semiconductor device increases the challenge of fully removing the semiconductor material of the first portion of the fin substrate. In this way, the challenge of avoiding leakage current between adjacent grouped source / drain regions on the same fin substrate increases. The presence of leakage current between adjacent sets of source / drain regions may degrade the performance and reliability of the all-wrap-gate field effect transistor.
[0070] In order to solve the above challenges, the utility model embodiment provides a method for forming a second isolation structure on the same fin substrate of a fully wrapped gate field effect transistor, which can avoid or minimize the leakage current between the grouped source / drain regions that should be electrically isolated from each other on the same fin substrate. In some embodiments, the method for forming the second isolation structure may be to replace a portion of the fin substrate with a dielectric material. A portion of the fin substrate may be located between a pair of shallow trench isolation regions and does not overlap with the source / drain regions on other portions of the fin substrate portion. The step of replacing a portion of the fin substrate may include plasma etching a portion of the fin substrate to form an isolation groove between a pair of shallow trench isolation regions. By controlling the plasma etching process parameters (such as etching gas type, etching gas flow rate, process chamber pressure, bias power, and similar parameters), the isolation groove profile can be controlled to ensure that a portion of the fin substrate is fully removed. In some embodiments, the width of the cross-sectional profile of the isolation groove may gradually increase along the height of the shallow trench isolation region and gradually decrease at a lower surface below the shallow trench isolation region. These cross-sectional profiles of the isolation trench ensure that portions of the fin substrate are substantially completely removed from the sidewalls and bottom edges of the shallow trench isolation region. This avoids or minimizes leakage current between the source / drain regions on the fin substrate due to any residual material from the etched portion of the fin substrate, and improves device performance and reliability of the all-around gate field effect transistor.
[0071] Figure 1A An isometric diagram of a field effect transistor 100 (eg, a fully wrapped gate field effect transistor) is shown in some embodiments. Figure 1B is a top view of the field effect transistor 100 in some embodiments. Figure 1C , 1E , 1G, and 1I are some embodiments in which the field effect transistor 100 is arranged along Figure 1A and 1B Different cross-sectional views of section line AA. Figure 1D , 1F , 1H, and 1J are some embodiments in which the field effect transistor 100 is arranged along Figure 1A and 1B Different cross-sectional views of section line BB. Figure 1C , 1D 1E, 1F, 1G, 1H, 1I, and 1J show cross-sectional views of field effect transistor 100, which has Figure 1A and 1B Additional structures are not shown (to simplify the drawing). The contents of elements with the same reference numerals can be interchanged with each other unless otherwise stated.
[0072] like Figures 1A to 1J In some embodiments shown, the field effect transistor 100 may include (i) a substrate 104, (ii) fin substrates 106A to 106D located on the substrate 104, (iii) shallow trench isolation regions 108A to 108E located on the substrate 104, (iv) source / drain regions 110A1 to 110D4 located on the fin substrates 106A to 106D, (v) gate structures 112A to 112F, (vi) outer gate spacers 114, (vii) inner gate spacers 115, and (viii) The first isolation structures 116A to 116E are respectively located on the shallow trench isolation regions 108A to 108E, (ix) the barrier layers 118A to 118E are respectively located on the first isolation structures 116A to 116E, (x) the second isolation structure 119 is located on the substrate 104, (xi) the etch stop layer 120, (xii) the interlayer dielectric layer 122, (xiii) the nanostructure channel regions 124A to 124D are respectively located on the fin bases 106A to 106D (the nanostructure channel region 124C is not shown in FIG. 1 ). Figures 1A to 1J , but displayed in Fig. 9C (xiv) a hard mask layer 125 is located on the interlayer dielectric layer 122. The term "nanostructure" as used herein is defined as a structure, layer, and / or region having a horizontal dimension (e.g., along the X and / or Y axis) and / or a vertical dimension (e.g., along the Z axis) less than about 100 nm, such as about 90 nm, about 50 nm, about 10 nm, or other values less than about 100 nm. In some embodiments, the nanostructure channel regions 124A to 124D may be nanosheets, nanowires, nanorods, nanotubes, or other suitable nanoshapes.
[0073] In some embodiments, the substrate 104 may be a semiconductor material such as silicon, germanium, silicon germanium, silicon-on-insulator structure, or a combination thereof. In addition, the substrate 104 may be doped with p-type dopants (such as boron, indium, aluminum, or gallium) or n-type dopants (phosphorus or arsenic).
[0074] In some embodiments, fin substrates 106A-106D may include materials similar to substrate 104. Fin substrates 106A-106D may have elongated sides extending along the X-axis. Figure 1B As shown, (i) the fin base 106A may be substantially parallel to the shallow trench isolation regions 108A and 108B and extend between the shallow trench isolation regions 108A and 108B, and extend under the gate structures 112A, 112B, 112C, 112E, and 112F and the source / drain regions 110A1 to 110D1; and (ii) the fin base portion 106D may be substantially parallel to the shallow trench isolation regions 108D and 108E and extend between the shallow trench isolation regions 108D and 108E, and extend under the gate structures 112A, 112B, 112D, 112E, and 112F and the source / drain regions 110A4 to 110D4. Figure 1B , 1C , 1E, 1G, and 1I show that the fin base 106B may include fin base portions 106B1 and 106B2, and the second isolation structure 119 may separate and electrically isolate the fin base portions 106B1 and 106B2 from each other. In some embodiments, the fin base portion 106B1 may be substantially parallel to the shallow trench isolation regions 108B and 108C and extend between the shallow trench isolation regions 108B and 108C, and extend under the gate structures 112A and 112B and the source / drain regions 110A2 and 110B2, such as Figure 1B and 1C In some embodiments, the fin base portion 106B2 may be substantially parallel to the shallow trench isolation regions 108B and 108C and extend between the shallow trench isolation regions 108B and 108C, and extend below the gate structures 112E and 112F and the source / drain regions 110C2 and 110D2, as shown in FIG. Figure 1B and 1C The fin substrate 106C is similar to the fin substrate 106B and may include fin substrate portions 106C1 and 106C2, and the second isolation structure 119 may separate and electrically isolate the fin substrate portions 106C1 and 106C2 from each other. Figure 1B In some embodiments, the fin base portion 106C1 may be substantially parallel to the shallow trench isolation regions 108C and 108D and extend between the shallow trench isolation regions 108C and 108D, and extend below the gate structures 112A and 112B and the source / drain regions 110A3 and 110B3, as shown in FIG. Figure 1B In some embodiments, the fin base portion 106C2 may be substantially parallel to the shallow trench isolation regions 108C and 108D and extend between the shallow trench isolation regions 108C and 108D, and extend below the gate structures 112E and 112F and the source / drain regions 110C3 and 110D3, as shown in FIG. Figure 1B shown.
[0075] like Figures 1A to 1J In some embodiments shown, the shallow trench isolation regions 108A to 108E, the outer gate spacers 114, the inner gate spacers 115, the etch stop layer 120, the interlayer dielectric layer 122, and the hard mask layer 125 may include insulating materials such as silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride, silicon carbon oxynitride, or silicon germanium oxide. The outer gate spacers 114, the barrier layers 118A to 118E, the etch stop layer 120, the interlayer dielectric layer 122, and the hard mask layer 125 are not shown. Figure 1B To simplify the drawings.
[0076] In some embodiments, the source / drain regions 110A1 to 110D4 may include epitaxially grown semiconductor materials such as silicon, and n-type dopants such as phosphorus or other suitable n-type dopants. In some embodiments, the source / drain regions 110A1 to 110D4 may include epitaxially grown semiconductor materials such as silicon or silicon germanium, and p-type dopants such as boron or other suitable p-type dopants.
[0077] In some embodiments, the semiconductor material included in the nanostructure channel regions 124A to 124D may be similar to or different from the substrate 104. In some embodiments, the nanostructure channel regions 124A to 124D may include silicon, silicon arsenide, silicon phosphide, silicon carbide, silicon carbon phosphide, silicon germanium, silicon germanium boride, germanium boride, silicon germanium tin boride, III-V semiconductor compounds, or other suitable semiconductor materials. Although the nanostructure channel regions 124A to 124D in the drawings have a rectangular cross-section, the nanostructure channel regions 124A to 124D may have other geometric shapes such as a circular, elliptical, triangular, or polygonal cross-section.
[0078] In some embodiments, gate structures 112A, 112B, 112E, and 112F may each surround each nanostructure channel region 124A, 124B, 124C, and 124D. In some embodiments, gate structure 112C may surround nanostructure channel region 124A, and gate structure 112D may surround nanostructure channel region 124D. In some embodiments, second isolation structure 119 may separate and electrically isolate gate structures 112C and 112D from each other. Outer gate spacers 114 and inner gate spacers 115 may electrically isolate gate structures 112A to 112F from adjacent source / drain regions 110A1 to 110D4. In some embodiments, field effect transistor 100 may be a fin field effect transistor and may have a fin region (not shown) instead of nanostructure channel regions 124A to 124D.
[0079] In some embodiments, the gate structures 112A to 112F may each include (i) an interfacial oxide layer (not shown), (ii) a high-k gate dielectric layer 113A located on the interfacial layer, and (iii) a conductive layer 113B located on the high-k gate dielectric layer 113A. In some embodiments, the interfacial layer may include silicon oxide, silicon germanium oxide, or germanium oxide. In some embodiments, the high-k gate dielectric layer 113A may include a high-k dielectric material such as hafnium oxide, titanium oxide, hafnium zirconium oxide, tantalum oxide, hafnium silicate, zirconium oxide, or zirconium silicate. In some embodiments, the conductive layer 113B may be a multilayer structure. The different layers of the conductive layer 113B are not shown to simplify the drawing. The conductive layer 113B may each include a work function metal layer located on the high-k gate dielectric layer 113A, and a gate metal fill layer located on the work function metal layer. In some embodiments, the work function metal layer may include titanium aluminum, titanium aluminum carbide, tantalum aluminum, tantalum aluminum carbide, aluminum-doped titanium, aluminum-doped titanium nitride, aluminum-doped tantalum, aluminum-doped tantalum nitride, or other suitable aluminum-doped materials for use in the all-around gate n-type field effect transistor 100. In some embodiments, the work function metal layer may include substantially aluminum-free titanium-based or tantalum-based nitrides or alloys, such as titanium nitride, titanium silicon nitride, titanium aluminum alloy, titanium copper alloy, tantalum nitride, tantalum silicon nitride, tantalum gold alloy, or tantalum copper for use in the all-around gate p-type field effect transistor 100. The gate metal fill layer may include suitable conductive materials such as tungsten, titanium, silver, ruthenium, molybdenum, copper, cobalt, aluminum, iridium, nickel, metal alloys, or combinations thereof.
[0080] In one embodiment, the first isolation structures 116A to 116E can electrically isolate (i) the source / drain regions 110A1 to 110A4 from each other along the Y axis, (ii) the source / drain regions 110B1 to 110B4 from each other along the Y axis, (iii) the source / drain regions 110C1 to 110C4 from each other along the Y axis, and (iv) the source / drain regions 110D1 to 110D4 from each other along the Y axis. Figure 1B In addition, the first isolation structures 116A to 116E can prevent (i) epitaxially grown semiconductor materials of the source / drain regions 110A1 to 110A4 from merging along the Y axis, (ii) epitaxially grown semiconductor materials of the source / drain regions 110B1 to 110B4 from merging along the Y axis, (iii) epitaxially grown semiconductor materials of the source / drain regions 110C1 to 110C4 from merging along the Y axis, and (iv) epitaxially grown semiconductor materials of the source / drain regions 110D1 to 110D4 from merging along the Y axis. In some embodiments, the elongated side of the first isolation structure 116A can extend below the gate structures 112A, 112B, 112C, 112E, and 112F along the X axis. In some embodiments, the elongated side of the first isolation structure 116B may extend along the X-axis below the gate structures 112A, 112B, 112C, 112E, and 112F and the second isolation structure 119. In some embodiments, the elongated side of the first isolation structure 116C may extend along the X-axis below the gate structures 112A, 112B, 112E, and 112F and the second isolation structure 119. In some embodiments, the elongated side of the first isolation structure 116D may extend along the X-axis below the gate structures 112A, 112B, 112D, 112E, and 112F and the second isolation structure 119. In some embodiments, the elongated side of the first isolation structure 116A may extend along the X-axis below the gate structures 112A, 112B, 112D, 112E, and 112F. In some embodiments, the first isolation structures 116A to 116E may each include an insulating liner 117A and an insulating filling layer 117B. In some embodiments, the insulating liner 117A and the insulating filling layer 117B may include silicon oxide, silicon nitride, silicon carbonitride, silicon carbon nitride oxide, or silicon germanium oxide.
[0081] In some embodiments, the barrier layers 118A to 118E may prevent the first isolation structures 116A to 116E from being etched when the source / drain regions 110A1 to 110D4 are formed, as described in detail below. In some embodiments, the barrier layers 118A to 118E may include a rare earth metal oxide layer having a rare earth metal such as hafnium, lanthanum, indium, rhodium, palladium, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, or a combination thereof. The rare earth metal atomic concentration in the rare earth metal oxide layer may be about 1×1020 Atom / cm 3 About 3x10 22 Atom / cm 3 If the concentration is less than about 1x10 20 Atom / cm 3 , the barrier layers 118A to 118E may not be able to adequately protect the first isolation structures 116A to 116E from being etched when the source / drain regions 110A1 to 110D4 are formed. On the other hand, if the concentration is higher than about 3×10 22 Atom / cm 3 , which increases the manufacturing cost of the device.
[0082] In some embodiments, the second isolation structure 119 may include an insulating liner 121 and an insulating filling layer 123. In some embodiments, the insulating liner 121 may include an oxide material such as silicon oxide, silicon germanium oxide, or other suitable insulating oxide materials. In some embodiments, the insulating filling layer 123 may include a nitride material such as silicon nitride, silicon carbonitride, silicon carbonitride oxide, or other suitable insulating nitride materials. Although the second isolation structure 119 in the accompanying drawings is located between the fin base portions 106B1 and 106B2 and between the fin base portions 106C1 and 106C2, the second isolation structure 119 of some embodiments may also be located between the fin base portions 106B1 and 106B2 or between the fin base portions 106C1 and 106C2. In some embodiments, the second isolation structure 119 may also extend through the fin base 106A and / or 106D and divide it into two parts (similar to the fin base 106B and 106C). In some embodiments, the second isolation structure 119 may be located between the gate structures 112C and 112D and directly contact the gate structures 112C and 112D. In some embodiments, the elongated side of the second isolation structure 119 may extend along the Y-axis and be substantially parallel to the elongated sides of the gate structures 112A, 112B, 112E, and 112F, such as Figure 1B shown.
[0083] In some embodiments, the upper surface of the second isolation structure 119 may be substantially coplanar with the upper surfaces of the gate structures 112C and 112D and / or the upper surface of the hard mask layer 125. The upper surface of the second isolation structure 119 and / or the widest portion of the second isolation structure 119 may have a width W1 along the X-axis and a width W2 along the Y-axis, and the width W2 is greater than the width W1. In some embodiments, the width W1 is substantially equal to the gate length GL1 of the gate structure 112C and / or the gate length GL2 of the gate structure 112D. In some embodiments, the width W2 may be greater than or equal to twice the fin pitch and less than three times the fin pitch, such as Figure 1BAs shown. The fin pitch is defined as the sum of the distance between adjacent fin bases (such as fin base portions 106B1 and 106C1) along the Y axis and the width of the fin base (such as fin base portion 106B1) along the Y axis. In some embodiments, width W2 may be greater than or equal to the fin pitch and less than twice the fin pitch (not shown). These widths W1 and W2 allow the second isolation structure to provide sufficient electrical isolation between the source / drain regions without affecting the device manufacturing cost.
[0084] The second isolation structure 119 may extend below the lower surface of the shallow trench isolation regions 108A to 108E and extend into the substrate 104. Figures 1C to 1J As described in detail below, the second isolation structure 119 may have a non-triangular cross-sectional profile along the bottom of the YZ plane and the bottom end may be an obtuse angle to avoid or minimize leakage current between the source / drain regions 110B2 and 110C2 and between the source / drain regions 110B3 and 110C3. Figure 1D If the fin substrate 106B and the bottom end are sharp angles, the residual semiconductor material of the fin substrate 106B and 106C may remain on the bottom sidewalls 108bs of the shallow trench isolation regions 108B, 108C, and 108D when the second isolation structure 119 is formed, as described in detail below. The residual semiconductor material may form a leakage current path between the source / drain regions 110B2 and 110C2 and between the source / drain regions 110B3 and 110C3, and degrade the performance and reliability of the field effect transistor 100.
[0085] The cross-sectional profiles of the second isolation structure 119 along the XZ plane and along the YZ plane may be different from each other. In some embodiments, the cross-sectional profile of the second isolation structure 119 along the XZ plane is as follows: Figure 1C , 1E , 1G, or 1I, and the cross-sectional profile along the YZ plane is as shown Figure 1D , 1F , 1H, or 1J.
[0086] like Figure 1C , 1E In some embodiments shown in FIGS. 1G and 1I, the top of the second isolation structure 119 above the upper surface 106t of the fin base portions 106B1 and 106B2 may have a substantially straight cross-sectional profile, while the bottom of the second isolation structure 119 below the upper surface 106t may have a tapered cross-sectional profile. In some embodiments, the width along the top of the second isolation structure 119 is substantially equal to the width W1. Figure 1E , 1G, and 1I, the bottom width of the second isolation structure 119 may gradually increase along a vertical distance of about 10 nm to about 25 nm below the upper surface 106t, and gradually decrease along the remaining height of the bottom of the second isolation structure 119. In some embodiments, the distance that the second isolation structure 119 extends into the substrate 104 may be a distance D1 (about 25 nm to about 40 nm, such as Figure 1E As shown), distance D2 (about 45nm to about 75nm, as Figure 1G As shown), or a distance D3 (about 25nm to about 45nm, as Fig. 1I shown).
[0087] like Figure 1D , 1F , 1H, and 1J, the cross-sectional profiles of the isolation portions 119A, 119B, 119C, and 119D of the second isolation structure 119 along the YZ plane may be different from each other. The isolation portion 119A may be located on the barrier layers 118B, 118C, and 118D. The isolation portion 119B may extend between the upper surface of the barrier layers 118B, 118C, and 118D and the upper surface of the shallow trench isolation regions 108B, 108C, and 108D. The isolation portion 119C may extend between the upper surface and the lower surface of the shallow trench isolation regions 108B, 108C, and 108D. The isolation portions 119A, 119B, and 119C may have substantially straight cross-sectional profiles and may have different widths from each other along the Y axis. In some embodiments, the isolation portion 119A may be wider than the isolation portion 119B, which may be wider than the isolation portion 119C. The isolation portion 119B may be wider than the isolation portion 119C to avoid forming a void in the isolation portion 119C and 119D when forming the second isolation structure 119, as described in detail below. Similarly, the isolation portion 119A may be wider than the isolation portion 119B to avoid forming a void in the isolation portion 119B when forming the second isolation structure 119. The distance that the isolation portion 119D extends from the lower surface of the shallow trench isolation regions 108B, 108C, and 108D into the substrate 104 may be a distance D1 (about 25 nm to about 40 nm, as shown in FIG. 1 ). Figure 1F As shown), distance D2 (about 45nm to about 75nm, as Figure 1H As shown), or a distance D3 (about 25nm to about 45nm, as Figure 1J shown).
[0088] like Figure 1DIn some embodiments shown, the sidewalls of the second isolation structure 119 may be directly located on all sidewalls of the shallow trench isolation regions 108B, 108C, and 108D to ensure that there is no residual semiconductor material of the fin substrates 106B and 106C between the sidewalls of the isolation portion 119C and the sidewalls of the shallow trench isolation regions 108B, 108C, and 108D. To further confirm that there is no residual semiconductor material, the upper surface of the isolation portion 119D may directly contact the lower surface and / or the lower surface edge of the shallow trench isolation regions 108B, 108C, and 108D. In some embodiments, the upper surface of the isolation portion 119D along the Y-axis may be wider than the lower surface of the isolation portion 119C and overlap with the lower surface of the shallow trench isolation regions 108B, 108C, and 108D. In some embodiments, the lower surface angle of the isolation portion 119C is greater than 90 degrees, thereby reducing the local maximum electric field and improving reliability. In some embodiments, the lower surface of the isolation portion 119C is substantially circular.
[0089] like Figure 1F In some embodiments shown, when the shallow trench isolation regions 108B, 108C, and 108D have a tapered cross-sectional profile along the YZ plane, the isolation portion 119C may have a tapered cross-sectional profile. The tapered cross-sectional profile of the isolation portion 119C may minimize the residual semiconductor materials 106Br1 and 106Cr1 of the fin bases 106B and 106C between the sidewalls of the isolation portion 119C and the sidewalls of the shallow trench isolation regions 108B, 108C, and 108D, respectively. In some embodiments, in order to minimize the height and / or thickness of the residual semiconductor materials 106Br1 and 106Cr1 to less than about 10 nm (e.g., between about 9.5 nm and about 5 nm), the total height H1 of the isolation portions 119B, 119C, and 119D may be about 180 nm to about 190 nm, and the isolation portion 119D may have (i) an upper surface width W3 of about 35 nm to about 45 nm, (ii) bottom end angles B and C of about 110 degrees to about 115 degrees, (iii) a height of about 25 nm to about 40 nm, and (iv) a curved sidewall profile. In some embodiments, the lower surface angle of the isolation portion 119C is an obtuse angle, thereby reducing the maximum local electric field and improving reliability.
[0090] like Figure 1HIn some embodiments shown, the isolation portion 119C may have a substantially vertical and flat sidewall profile. In some embodiments, in order to minimize the height and / or thickness of the residual semiconductor materials 106Br2 and 106Cr2 to less than about 13 nm (e.g., about 12.5 nm to about 6 nm), the total height H2 of the isolation portions 119B, 119C, and 119D may be about 200 nm to about 220 nm, and the isolation portion 119D may have (i) an upper surface width W4 of about 35 nm to about 40 nm, (ii) a substantially flat lower surface, (iii) a height of about 45 nm to about 75 nm, (iv) an angle between the sidewall and the lower surface of about 95 degrees to about 97 degrees, and (v) a tapered sidewall profile.
[0091] like Figure 1J In some embodiments shown, the isolation portion 119C may have a substantially vertical and straight sidewall profile. In some embodiments, in order to minimize the height and / or thickness of the residual semiconductor materials 106Br3 and 106Cr3 to less than about 12 nm (e.g., between about 11.9 nm and about 7 nm), the total height H3 of the isolation portions 119B, 119C, and 119D may be about 185 nm to about 200 nm, and the isolation portion 119D may have (i) an upper surface width W5 of about 35 nm to about 40 nm, (ii) a curved lower surface profile, (iii) a height of about 25 nm to about 45 nm, and (iv) a substantially vertical and straight sidewall profile. In some embodiments, the lower surface of the isolation portion 119C is substantially flat, thereby reducing the local maximum electric field and improving reliability.
[0092] In some embodiments, the second isolation structure 119 may have a plurality of different characteristics depending on key factors of transistor performance, such as whether etching damage is caused to the source / drain region or depth loading effect between densely patterned device regions and sparsely patterned device regions. Figure 1E and 1F , 1G and 1H, or 1I and 1J. If the etching damage to the source / drain region is a key factor in the performance of the field effect transistor, the second isolation structure 119 has Fig. 1I and 1J The cross-sectional profile of the second isolation structure 119 is formed by using a radical-based process to avoid strong ion etching of the passivation layer and the fin substrate 106A, 106B, and 106D. If the depth loading effect is a key factor in the performance of the field effect transistor, the second isolation structure 119 has Figure 1G and 1H The cross-sectional profile of the second isolation structure 119 is formed by using an ion orientation process to fully remove etching byproducts and a polymer passivation layer. If the etching damage to the source / drain region and the depth loading effect are both key factors in the performance of the field effect transistor, the second isolation structure 119 has Figure 1E and1F The cross-sectional profile is formed by ion and radical etching.
[0093] Figure 2 is an example of a method 200 for fabricating a field effect transistor 100 in some embodiments. For illustration purposes, Figure 2 The steps shown will be paired with Figures 3A to 11C , 12A to 12M, and 13A to 15C are illustrations of the manufacturing process of the field effect transistor 100. Figures 3A to 15A are isometric views of the field effect transistor 100 at various stages of fabrication in some embodiments. Figures 3B to 11B 12B, 12D, 12F, 12H, 12J, 12K, and 13B to 15B are some embodiments in which the field effect transistor 100 is formed at various stages along the Figure 1A and 1B Section view along section line AA. Figures 3C to 11C 12C, 12E, 12G, 12I, 12K, 12M, and 13C to 15C are some embodiments in which the field effect transistor 100 is formed at various stages along the Figure 1A and 1B BB. The steps may be performed in different orders, or some steps may not be performed, depending on the specific application. It is worth noting that method 200 may not produce field effect transistor 100. In summary, it should be understood that additional processes may be provided before, during, and after method 200, and some other processes are only briefly described here. Figures 3A to 11C , 12A to 12M, and 13A to 15C and Figures 1A to 1J The contents of the units with the same labels are as described above. Figures 1A to 1J Some units are not shown in the figure Figures 3A to 11C , 12A to 12M, and 13A to 15C are used to simplify the drawings. Figures 3B to 11B , 3C to 11C, 12B to 12M, 13B to 15B, and 13C to 15C are cross-sectional views of the field effect transistor 100, which has Figures 3A to 11A , 12A, and additional structures of 13A to 15A are not shown (to simplify the drawings).
[0094] like Figure 2 As shown, step 205 forms a superlattice structure on the fin base on the substrate. Figures 3A to 3CFor example, superlattice structures 323A and 323B are respectively formed on fin substrates 106A and 106B on substrate 104. In some embodiments, superlattice structure 323A may include staggered epitaxially grown nanostructure layers such as nanostructure channel region 124A and nanostructure layer 324A, and superlattice structure 323B may include staggered epitaxially grown nanostructure layers such as nanostructure channel region 124B and nanostructure layer 324B. Similarly, superlattice structure 323C having epitaxially grown nanostructure layers such as nanostructure channel region 124C and nanostructure layer 324C may be formed on fin substrate 106C, and superlattice structure 323D having epitaxially grown nanostructure layers such as nanostructure channel region 124D and nanostructure layer 324D may be formed on fin substrate 106D, which is not shown. Figure 3A and 3C To simplify the drawings, however, Fig. 9A and 9C In some embodiments, nanostructure layers such as nanostructure channel regions 124A to 124D may include silicon without substantially any germanium (e.g., no germanium), and nanostructure layers 324A to 324D may include silicon germanium. Nanostructure layers 324A to 324D may also be considered sacrificial layers. In subsequent processes, a gate replacement process may replace sacrificial layers such as nanostructures 324A to 324D to form portions of gate structures 112A to 112D, respectively. In some embodiments, mask layers 336A and 336B may be formed on superlattice structures 323A and 323B, respectively. In some embodiments, the materials included in mask layers 336A and 336B may be similar to the materials of nanostructure layers 324A and 324B.
[0095] like Figure 2 As shown, step 210 forms a shallow trench isolation region on the substrate. Figure 3A and 3C For example, shallow trench isolation regions 108A to 108C are formed on substrate 104. Similarly, shallow trench isolation regions 108D and 108E may be formed on substrate 104, which are not shown in FIG. Figure 3A and 3C To simplify the drawing. The shallow trench isolation region is not shown in Figure 3B in the cross-sectional view.
[0096] like Figure 2 As shown, step 215 forms a cladding layer on the superlattice structure. Figures 4A to 5CFor example, the capping layer 438 is formed on the sidewalls of the superlattice structures 323A and 323B. Similarly, the capping layer 438 is formed on the sidewalls of the superlattice structures 323C and 323D. The method of forming the capping layer 438 may include (i) depositing a material layer (e.g., silicon germanium) similar to the material of the nanostructure layers 324A to 324D by a chemical vapor deposition process of precursors such as germanium and silane. Figures 3A to 3C In terms of structure, Figures 4A to 4C and (ii) performing an etching process on the deposited material layer to form a capping layer 438 on the superlattice structures 323A and 323B, such as Figure 5A and 5C shown.
[0097] like Figure 2 As shown, step 220 forms a first isolation structure on the shallow trench isolation region. Figures 5A to 5C For example, the first isolation structures 116A to 116C are formed on the shallow trench isolation regions 108A to 108C, respectively. Similarly, the first isolation structures 116D and 116E (not shown) Figure 5A and 5C ) are formed on the shallow trench isolation regions 108D and 108E, respectively. The first isolation structures 116A to 116C are not shown. Figure 5B The method of forming the first isolation structure 116A to 116C may include sequentially performing the following steps: (i) depositing an insulating liner 117A on the cap layer 438, the shallow trench isolation regions 108A to 108E, and the mask layers 336A and 336B, such as Figure 5A and 5C As shown, (ii) depositing an insulating filling layer 117B on the insulating liner 117A, (iii) performing a chemical mechanical polishing process on the insulating liner 117A, the insulating filling layer 117B, and the capping layer 438 to make the upper surfaces of the insulating liner 117A, the insulating filling layer 117B, and the capping layer 438 substantially coplanar with each other (not shown), and (iv) performing an etching process on the insulating filling layer 117B to form Figure 5A and 5C structure.
[0098] After forming the first isolation structures 116A to 116C, barrier layers 118A to 118C may be formed on the first isolation structures 116A to 116C, respectively. Fig. 6A and 6C Similarly, barrier layers 118D and 118E (not shown) Fig. 6A and 6C ) may be formed on the first isolation structures 116D and 116E, respectively. The barrier layers 118A to 118C are not shown in FIG. Figure 6B in the cross-sectional view.
[0099] like Figure 2 As shown, step 225 forms a polysilicon structure on the first isolation structure, the capping layer, and the superlattice structure. Figures 7A to 8C For example, polysilicon structures 812A, 812B, 812CD, 812E, and 812F are formed on barrier layers 118A to 118E, capping layer 438, and superlattice structures 323A to 323D. The method of forming polysilicon structures 812A, 812B, 812CD, 812E, and 812F may include sequentially performing the following steps: (i) Figures 6A to 6C An etching process is performed on the structure to remove the mask layers 336A and 336B, such as Figures 7A to 7C As shown, (ii) a polysilicon layer (not shown) is deposited on Figures 7A to 7C and (iii) performing a patterning process (such as a photolithography process) on the polysilicon layer to form polysilicon structures 812A, 812B, 812CD, 812E, and 812F, such as Figures 8A to 8C As shown. In some embodiments, hard mask layers 836A and 836B may be formed when forming polysilicon structures 812A, 812B, 812CD, 812E, and 812F. In some embodiments, outer gate spacers 114 may be formed after forming polysilicon structures 812A, 812B, 812CD, 812E, and 812F, and the formation method thereof may be (i) depositing a spacer material layer 814 on the polysilicon structures 812A, 812B, 812CD, 812E, and 812F and the hard mask layers 836A and 836B, as shown. Figures 8A to 8C as shown, and (ii) in Figures 8A to 8C A chemical mechanical polishing process is performed on the structure to form an outer gate spacer 114, such as Figures 9A to 9C shown.
[0100] like Figure 2 As shown, step 230 forms source / drain regions on the fin substrate. Figures 9A to 9C For example, source / drain regions 110A2, 110B2, 110C2, and 110D2 are formed on fin substrate 106B. Similarly, source / drain regions 110A1, 110B1, 110C1, and 110D1 are formed on fin substrate 106A, source / drain regions 110A3, 110B3, 110C3, and 110D3 are formed on fin substrate 106C, and source / drain regions 110A4, 110B4, 110C4, and 110D4 are formed on fin substrate 106D, but are not shown. Figures 9A to 9C The source / drain regions 110A2, 110B2, 110C2, and 110D2 are not shown in the figure. Fig. 9A and 9C sectional view of .
[0101] The method for forming the source / drain regions 110A2, 110B2, 110C2, and 110D2 may include sequentially performing the following steps: (i) forming source / drain openings (not shown) in portions of the superlattice structure 323B, the fin base 106B, and the capping layer 438 that do not overlap with the outer gate spacers 114 and the polysilicon structures 812A, 812B, 812CD, 812E, and 812F, and (ii) epitaxially growing a semiconductor material in the source / drain openings, such as Fig. 9B In some embodiments, the inner spacer 115 may be formed between steps (i) and (ii) of the process for forming the source / drain regions 110A2, 110B2, 110C2, and 110D2. In some embodiments, after forming the source / drain regions 110A2, 110B2, 110C2, and 110D2, an etch stop layer 120, an interlayer dielectric layer 122, and a hard mask layer 125 may be formed, as shown in FIG. Fig. 9A and 9B shown.
[0102] like Figure 2 As shown, step 235 forms a second isolation structure on the substrate. Figures 10A to 11C , 12A to 12M, and 13A to 14C as examples, the second isolation structure 119 is formed on the substrate 104. The method for forming the second isolation structure 119 may include sequentially performing the following steps: (i) depositing a mask layer 936 (such as a photoresist), such as Figures 10A to 10C As shown, (ii)
[0103] The opening 1040 with a size of W1×W2 is formed on the polysilicon structure 812CD by using a photolithography process. Figures 10A to 10C As shown, (iii) the portion of the polysilicon structure 812CD exposed in the opening 1040 is etched to form an opening 1140 and polysilicon structures 812C and 812D, as shown in FIG. Figures 11A to 11C As shown, (iv) a first semiconductor material etching process is performed to remove the superlattice structures 323B and 323C and the portion of the cladding layer 438 exposed in the opening 1140, and to form an opening 1240, as shown in FIG. Figures 12A to 12C As shown, (v) a passivation layer (not shown) is deposited along the sidewall of the opening 1240 to protect the source / drain regions 110A1 to 110D4, and the passivation layer is deposited on the upper surfaces of the fin substrates 106B and 106C exposed in the opening 1240, (vi) an etching process is performed to remove a portion of the passivation layer on the upper surfaces of the fin substrates 106B and 106C, (vii) a second semiconductor material etching process is performed to remove the portion of the fin substrates 106B and 106C exposed in the opening 1240 to form an opening 1242, as shown in FIG. Fig.12D and 12EAs shown, (viii) a third semiconductor material etching process is performed to remove the portion of the substrate 104 exposed in the opening 1242 to form an opening 1219 having Fig.12F and 12F , Fig.12H and 12I ,or Figure 12L and 12M (ix) depositing an insulating oxide layer 1521 on Fig.12F and 12G In terms of structure, Figures 13A to 13C As shown, (x) an insulating nitride layer 1523 is deposited on the insulating oxide layer 1521 to fill the openings 1219, 1242, 1240, 1140, and 1040, as shown in FIG. Figures 13A to 13C As shown, and (xi) in Figures 13A to 13C A chemical mechanical polishing process is performed on the structure to form a second isolation structure, such as Figures 14A to 14C In some embodiments, the opening 1140 is wider than the opening 1240 , which is wider than the opening 1242 to prevent the formation of voids in the openings 1219 , 1242 , 1240 , and 1140 when the insulating nitride layer 1523 is deposited.
[0104] Although in Fig.12F and 12G The steps (ix), (x), and (xi) of the process for forming the second isolation structure 119 are performed on the structure of Fig.12H and 12I Steps (ix), (x), and (xi) are performed on the structure to form a Figure 1E and 1F The second isolation structure 119 of the cross-sectional profile, (ii) Fig.12J and 12K Steps (ix), (x), and (xi) are performed on the structure to form a Figure 1G and 1H The second isolation structure 119 of the cross-sectional profile, and (iii) Figure 12L and 12M Steps (ix), (x), and (xi) are performed on the structure to form a Fig. 1I and 1J A second isolation structure 119 having a cross-sectional profile. (i) Figure 1C and 1D The cross-sectional profile and dimensions of the second isolation structure 119 can be used to Fig.12F and 12G The cross-sectional profile and dimensions of the isolation trench such as the opening 1219, (ii) Figure 1E and 1F The cross-sectional profile and dimensions of the second isolation structure 119 can be used to Fig.12Hand 12I The cross-sectional profile and dimensions of the isolation trench such as the opening 1219, (iii) Figure 1G and 1H The cross-sectional profile and dimensions of the second isolation structure 119 can be used to Fig.12J and 12K The cross-sectional profile and dimensions of the isolation trench such as the opening 1219, and (iv) Fig. 1I and 1J The cross-sectional profile and dimensions of the second isolation structure 119 can be used to Figure 12L and 12M The cross-sectional profile and dimensions of the isolation trench such as the opening 1219 are shown in FIG.
[0105] In some embodiments, the step of performing the first semiconductor material etching process may include performing a dry etching process in a process chamber using a gas mixture of hydrogen halide (such as hydrogen bromide, hydrogen chloride, or hydrofluoric acid), oxygen, and argon. In some embodiments, the first semiconductor material etching process may further include delivering hydrogen halide gas with a flow rate of about 100 sccm to about 1000 sccm, oxygen gas with a flow rate of about 0 sccm to about 100 sccm, and argon gas with a flow rate of about 100 sccm to the process chamber.
[0106] In some embodiments, the step of depositing the passivation layer may include flowing a gas mixture of a silicon precursor (such as silicon tetrachloride or silane), hydrogen bromide, argon, and oxygen into a Figures 12A to 12C In some embodiments, during the deposition process of depositing the passivation layer, the deposition chamber may further include delivering a silicon precursor having a flow rate of about 1 sccm to about 1000 sccm, a hydrogen bromide gas having a flow rate of about 100 sccm to about 500 sccm, an oxygen gas having a flow rate of about 10 sccm to about 200 sccm, and an argon gas having a flow rate of about 100 sccm to about 1000 sccm.
[0107] In some embodiments, performing an etching process to remove a portion of the passivation layer on the upper surface of the fin substrates 106B and 106C may include performing a dry etching process with a gas mixture of carbon tetrafluoride and argon in a process chamber. The etching process in some embodiments may further include delivering carbon tetrafluoride at a flow rate of about 1 sccm to about 200 sccm and argon at a flow rate of about 100 sccm to the process chamber.
[0108] In some embodiments, the step of performing the second semiconductor material etching process may include performing a dry etching process in a process chamber using a gas mixture of hydrogen halide (such as hydrogen bromide, hydrogen chloride, or hydrofluoric acid), argon gas, and carbon dioxide or oxygen. In some embodiments, the second semiconductor material etching process may further include delivering hydrogen halide gas with a flow rate of about 100 sccm to about 1000 sccm, carbon dioxide or oxygen with a flow rate of about 0 sccm to about 100 sccm, and argon gas with a flow rate of about 100 sccm to about 1000 sccm to the process chamber.
[0109] In some embodiments, a third semiconductor material etching process is performed to form Fig.12H and 12I The step of forming an isolation trench such as the opening 1219 may include performing a plasma etching process in a process chamber using a gas mixture of hydrogen bromide, argon, and carbon dioxide or oxygen, and the bromide ion concentration of the plasma is substantially equal to the concentration of bromine radicals (for example, the concentration ratio of bromide ions to bromine radicals in the plasma is substantially equal to 1). In some embodiments, the third semiconductor material etching process may further include performing a plasma etching process under a high pressure greater than or equal to about 20 mTorr (for example, between about 21 mTorr and about 200 mTorr), a low bias power less than about 100 watts (for example, between about 1 watt and about 100 watts), and a pulsed radio frequency of about 0.1 kHz to about 10 kHz. High pressure, low bias power, and substantially the same bromide ion and bromine radical concentrations as pulsed radio frequency conditions may induce anisotropic plasma etching to achieve Fig.12H and 12I The cross-sectional profile of the isolation trench is shown as an opening 1219. During the third semiconductor material etching process in some embodiments, the process may further include delivering hydrogen bromide gas with a flow rate of about 100 sccm to about 1000 sccm, carbon dioxide or oxygen gas with a flow rate of about 0 sccm to about 100 sccm, and argon gas with a flow rate of about 100 sccm to about 1000 sccm to the process chamber.
[0110] In some embodiments, a third semiconductor material etching process is performed to form Fig.12J and 12KThe step of forming an isolation trench such as the opening 1219 may include performing a plasma etching process in a process chamber using a gas mixture of hydrogen bromide, argon, and carbon dioxide or oxygen, and the bromide ion concentration of the plasma is greater than the concentration of bromine radicals (for example, the concentration ratio of bromide ions to bromine radicals in the plasma is greater than 1). In some embodiments, the third semiconductor material etching process may further include performing a plasma etching process at a low pressure of less than about 20 mTorr (for example, between about 1 mTorr and about 20 mTorr) and a high bias power of greater than about 100 watts (for example, between about 101 watts and about 200 watts). The conditions of low pressure and high bias power and a higher concentration of bromide ions can induce anisotropic and directional plasma etching along the Z axis to achieve Fig.12J and 12K The cross-sectional profile of the isolation trench is shown as an opening 1219. During the third semiconductor material etching process in some embodiments, the process may further include delivering hydrogen bromide gas with a flow rate of about 100 sccm to about 1000 sccm, carbon dioxide or oxygen gas with a flow rate of about 0 sccm to about 100 sccm, and argon gas with a flow rate of about 100 sccm to about 1000 sccm to the process chamber.
[0111] In some embodiments, a third semiconductor material etching process is performed to form Figure 12L and 12M The step of isolating the trenches such as the opening 1219 may include performing a plasma etching process in a process chamber with a gas mixture of hydrogen bromide, argon, and carbon dioxide or oxygen, and the bromide ion concentration of the plasma is less than the concentration of bromine radicals (e.g., the ratio of the bromide ion concentration to the bromine radical concentration in the plasma is less than 1). In some embodiments, the third semiconductor material etching process may further include performing a plasma etching process under a high pressure greater than or equal to about 20 mTorr (e.g., between about 21 mTorr and about 100 mTorr) and a low bias power less than about 100 watts (e.g., between about 1 watt and about 100 watts). The conditions of high pressure and low bias power and the lower concentration of bromide ions can reach Figure 12L and 12M The cross-sectional profile of the isolation trench is shown as an opening 1219. During the third semiconductor material etching process in some embodiments, the process may further include delivering hydrogen bromide gas with a flow rate of about 100 sccm to about 1000 sccm, carbon dioxide or oxygen gas with a flow rate of about 0 sccm to about 100 sccm, and argon gas with a flow rate of about 100 sccm to about 1000 sccm to the process chamber.
[0112] like Figure 2 As shown, step 240 may replace the polysilicon structure with a gate structure. Figures 15A to 15CFor example, the polysilicon structures 812A to 812F may be replaced with gate structures 112A to 112F, respectively. In some embodiments, the method for forming the gate structures 112A to 112F may include etching the polysilicon structures 812A to 812F and the nanostructure layers 324A to 324D, and replacing them with a high dielectric constant gate dielectric layer 113A and a conductive layer 113B, such as Figures 15A to 15C shown.
[0113] The present invention provides a method (such as method 200) for forming a second isolation structure (such as second isolation structure 119) on adjacent source / drain regions (such as source / drain regions 110B2 and 110C2) on the same fin substrate (such as fin substrate 106B) of a fully wrapped gate field effect transistor (such as field effect transistor 100), which can avoid or minimize leakage current between source / drain regions (such as source / drain regions 110B2 and 110C2) that should be electrically isolated from each other on the same fin substrate (such as fin substrate 106B). In some embodiments, the method for forming the second isolation structure can be to replace a portion of the fin substrate (such as fin substrate 106B) with a dielectric material (such as an insulating oxide layer such as insulating liner 121 and an insulating nitride layer such as insulating fill layer 123). A portion of the fin substrate may be located between a pair of shallow trench isolation regions (such as shallow trench isolation regions 108B and 108C) and may not overlap with source / drain regions on other portions of the fin substrate portion. The step of replacing a portion of the fin substrate may include plasma etching a portion of the fin substrate to form an isolation trench (isolation trench such as opening 1219) between the pair of shallow trench isolation regions. By controlling the plasma etching process parameters (such as etching gas type, etching gas flow rate, process chamber pressure, bias power, and similar parameters), the isolation trench profile may be controlled to ensure that the portion of the fin substrate is adequately removed. In some embodiments, the cross-sectional profile of the isolation trench (such as Figures 12F to 12M The width of the isolation trench (cross-sectional profile) can gradually increase along the height of the shallow trench isolation region and gradually decrease below the lower surface of the shallow trench isolation region. These cross-sectional profiles of the isolation trench can ensure that a portion of the fin substrate is substantially completely removed from the sidewalls (such as the bottom sidewall 108bs) and the bottom edge of the shallow trench isolation region. In this way, leakage current between the source / drain regions (such as the source / drain regions 110B2 and 110C2) on the fin substrate (such as the fin substrate 106B) due to any residual material of the etched portion of the fin substrate can be avoided or minimized, and the device performance and reliability of the all-around gate field effect transistor can be improved.
[0114] In some embodiments, a method for forming a semiconductor device includes: forming a first fin base and a second fin base on a substrate; forming multiple first nanostructure layers and multiple second nanostructure layers on the first fin base and the second fin base, respectively; forming multiple coatings on the side walls of the first nanostructure layer and the second nanostructure layer; forming a polysilicon structure on the first nanostructure layer, the second nanostructure layer, and the coating; removing a portion of the polysilicon structure to form a first opening on the second nanostructure layer; removing a portion of the second nanostructure layer through the first opening to form a second opening on the second fin base; removing a portion of the second fin base through the second opening to form a third opening on the substrate; removing a portion of the substrate through the third opening to form a fourth opening in the substrate; and depositing insulating material to fill the first opening, the second opening, the third opening, and the fourth opening.
[0115] In some embodiments, the step of removing the portion of the substrate through the third opening includes performing an etching process using a plasma containing halide ions and free radicals, and the concentration ratio of the halide ions to the free radicals is substantially equal to 1.
[0116] In some embodiments, removing the portion of the substrate through the third opening includes performing an etching process with a plasma containing halide ions and free radicals at a bias power greater than about 100 W, and a concentration ratio of halide ions to free radicals is greater than 1.
[0117] In some embodiments, removing the portion of the substrate through the third opening includes performing an etching process with a plasma containing halide ions and free radicals at a pressure greater than about 20 mTorr, and a concentration ratio of halide ions to free radicals is less than 1.
[0118] In some embodiments, the fourth opening formed by removing a portion of the substrate through the third opening has a curved sidewall profile and a bottom end that is an obtuse angle.
[0119] In some embodiments, the fourth opening formed by removing a portion of the substrate through the third opening has a tapered sidewall profile and a substantially flat bottom profile.
[0120] In some embodiments, the method further includes removing a portion of the capping layer on a sidewall of the second nanostructure layer when removing the portion of the second nanostructure layer through the first opening.
[0121] In some embodiments, the first opening formed by removing a portion of the polysilicon structure is wider than the second opening.
[0122] In some embodiments, the second opening formed by removing a portion of the second nanostructure layer is wider than the third opening.
[0123] In some embodiments, the fourth opening formed by removing a portion of the substrate through the third opening is wider than the third opening.
[0124] In some embodiments, a method for forming a semiconductor device includes forming a first fin substrate and a second fin substrate on a substrate; forming a plurality of first nanostructure layers and a plurality of second nanostructure layers on the first fin substrate and the second fin substrate, respectively; forming a first isolation structure between the first fin substrate and the second fin substrate; forming a second isolation structure above the first isolation structure and between the first nanostructure layer and the second nanostructure layer; forming a polysilicon structure on the first nanostructure layer and the second nanostructure layer; and forming a third isolation structure, including forming a first isolation portion and a second isolation portion of the third isolation structure in the substrate; forming a third isolation portion and a fourth isolation portion of the third isolation structure on both sides of the first isolation structure; forming a fifth isolation portion and a sixth isolation portion of the third isolation structure on both sides of the second isolation structure; and forming a seventh isolation portion of the third isolation structure in the polysilicon structure.
[0125] In some embodiments, the step of forming the first isolation portion and the second isolation portion includes etching a portion of the substrate with a plasma containing bromide ions and bromine radicals, and the concentration ratio of the bromide ions to the bromine radicals is substantially equal to 1.
[0126] In some embodiments, forming the first isolation portion and the second isolation portion comprises etching a portion of the substrate with a plasma at a bias power greater than about 100 watts, the plasma comprising bromide ions and bromine radicals, and a concentration ratio of the bromide ions to the bromine radicals greater than 1.
[0127] In some embodiments, forming the first isolation portion and the second isolation portion comprises etching a portion of the substrate with a plasma at a pressure greater than about 20 mTorr, the plasma comprising bromide ions and bromine radicals, and a concentration ratio of the bromide ions to the bromine radicals is less than 1.
[0128] In some embodiments, the step of forming the first isolation portion and the second isolation portion includes etching a portion of the substrate to form a first opening and a second opening having a curved sidewall profile and a bottom end having an obtuse angle.
[0129] In some embodiments, the step of forming the first isolation portion and the second isolation portion includes etching a portion of the substrate to form the first opening and the second opening having a tapered sidewall profile and a substantially flat bottom profile.
[0130] In some embodiments, the semiconductor device includes: a substrate; a first fin substrate and a second fin substrate, located on the substrate; a plurality of first nanostructure layers and a plurality of second nanostructure layers, respectively located on the first fin substrate and the second fin substrate; a first gate structure and a second gate structure, respectively surrounding the first nanostructure layer and the second nanostructure layer; a first shallow trench isolation region and a second shallow trench isolation region, located on both sides of the first fin substrate and the second fin substrate; a first first isolation structure and a second first isolation structure, respectively located on the first shallow trench isolation region and the second shallow trench isolation region; and a second isolation structure. The second isolation structure includes a first isolation portion, located between the first gate structure and the second gate structure; a second isolation portion, located between the first first isolation structure and the second first isolation structure and contacting the first first isolation structure and the second first isolation structure; a third isolation portion, located between the first shallow trench isolation region and the second shallow trench isolation region and contacting the first shallow trench isolation region and the second shallow trench isolation region; and a fourth isolation portion, located in the substrate, wherein the first isolation portion is wider than the second isolation portion and the third isolation portion.
[0131] In some embodiments, the fourth isolation portion overlaps lower surfaces of the first shallow trench isolation region and the second shallow trench isolation region.
[0132] In some embodiments, the fourth isolation portion includes a curved sidewall profile, and a bottom end has an obtuse angle.
[0133] In some embodiments, the upper surface width of the fourth isolation portion is 35 nm to 45 nm.
[0134] In some embodiments, the obtuse angle is 110 to 115 degrees.
[0135] In some embodiments, the height of the fourth isolation portion is 25 nm to 40 nm.
[0136] In some embodiments, the fourth isolation portion includes a tapered sidewall profile and a substantially flat bottom profile.
[0137] In some embodiments, the upper surface width of the fourth isolation portion is 35 nm to 40 nm.
[0138] In some embodiments, the height of the fourth isolation portion is 45 nm to 75 nm.
[0139] In some embodiments, an angle between a sidewall and a lower surface of the fourth isolation portion is 95 degrees to 97 degrees.
[0140] The features of the above embodiments are helpful for those skilled in the art to understand the present invention. Those skilled in the art should understand that the present invention can be used as a basis to design and change other processes and structures to achieve the same purpose and / or the same advantages of the above embodiments. Those skilled in the art should also understand that these equivalent substitutions do not depart from the spirit and scope of the present invention, and can be changed, replaced, or modified without departing from the spirit and scope of the present invention.
Claims
1. A semiconductor device, characterized in that: include: a substrate; A first fin substrate and a second fin substrate are located on the substrate; A plurality of first nanostructure layers and a plurality of second nanostructure layers are respectively located on the first fin substrate and the second fin substrate; A first gate structure and a second gate structure surround the first nanostructure layers and the second nanostructure layers respectively; A first shallow trench isolation region and a second shallow trench isolation region are located on both sides of the first fin substrate and the second fin substrate; A first first isolation structure and a second first isolation structure are respectively located on the first shallow trench isolation region and the second shallow trench isolation region; as well as A second isolation structure, comprising: a first isolation portion located between the first gate structure and the second gate structure; a second isolation portion, located between the first first isolation structure and the second first isolation structure and contacting the first first isolation structure and the second first isolation structure; a third isolation portion located between the first shallow trench isolation region and the second shallow trench isolation region and contacting the first shallow trench isolation region and the second shallow trench isolation region; and A fourth isolation portion is located in the substrate, wherein the first isolation portion is wider than the second isolation portion and the third isolation portion.
2. The semiconductor device according to claim 1, wherein The fourth isolation portion overlaps with lower surfaces of the first shallow trench isolation region and the second shallow trench isolation region.
3. The semiconductor device according to claim 1, wherein: The fourth isolation portion includes a curved sidewall profile, and a bottom end has an obtuse angle.
4. The semiconductor device according to claim 3, wherein: The upper surface width of the fourth isolation portion is 35 nm to 45 nm.
5. The semiconductor device according to claim 3, wherein: The obtuse angle is 110 to 115 degrees.
6. The semiconductor device according to claim 3, wherein: The height of the fourth isolation portion is 25 nm to 40 nm.
7. The semiconductor device according to claim 1, wherein The fourth isolation portion includes a tapered sidewall profile and a substantially flat bottom profile.
8. The semiconductor device according to claim 7, wherein: The width of the upper surface of the fourth isolation portion is 35nm to 40nm.
9. The semiconductor device according to claim 7, wherein: The height of the fourth isolation portion is 45 nm to 75 nm.