Nitride vertical power device

The laminated nitride transition layer is formed through staged growth, which solves the leakage problem of nitride vertical power devices and improves their voltage resistance and breakdown resistance.

CN221861668UActive Publication Date: 2024-10-18JIANGSU INST OF ADVANCED SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323546216.1
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-10-18
Estimated Expiration
2033-12-25

AI Technical Summary

Technical Problem

Nitride vertical power devices have leakage problems, which affect their voltage resistance and breakdown resistance.

Method used

Staged growth is used to form a stacked first nitride transition layer and a second nitride transition layer. The density of the first nitride transition layer is smaller than that of the second nitride transition layer. The surface of the first nitride transition layer is planarized through annealing. A dense nitride transition layer is formed to cover the gate trench structure.

Benefits of technology

The unevenness of the inner wall of the gate trench structure is eliminated, the surface flatness of the nitride transition layer is improved, leakage problems are avoided, and the voltage resistance and breakdown resistance of the device are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221861668U_ABST
    Figure CN221861668U_ABST
Patent Text Reader

Abstract

The utility model discloses a nitride vertical power device. The nitride vertical power device comprises a device main body structure, a gate layer structure, a source electrode, a drain electrode and a gate electrode, the device main body structure comprises a drain electrode contact layer, a drift layer, a p-type nitride layer with a first through groove and a source electrode contact layer with a second through groove, the first through groove and the second through groove are communicated to form a gate groove structure; the gate layer structure comprises a nitride transition layer and a first insulating layer, the nitride transition layer covers the side wall and the groove bottom of the gate groove structure, and the first insulating layer is arranged on the nitride transition layer; at least one part of the gate electrode is arranged in the gate groove structure; the nitride transition layer comprises a first nitride transition layer and a second nitride transition layer which are arranged in a stacked mode, and the density of the first nitride transition layer is smaller than that of the second nitride transition layer. According to the utility model, the electric leakage problem of the device is avoided, and the voltage resistance and breakdown resistance of the device are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of semiconductor devices, and particularly relates to a nitride vertical power device. Background Art

[0002] As early as the mid-1990s, the trench gate structure has been applied to double-diffused metal oxide semiconductor (DMOS) devices and has been commercialized, called U-shaped groove metal-oxide-semiconductor (UMOS) devices. UMOS devices have a high trench density and low drain diffusion resistance, and their on-state characteristic resistance is extremely low. Trench gates are generally used in vertical DMOS devices. The main reason is that the trench gate introduces the channel current from the device surface into the body, which is consistent with the current flow direction of the vertical structure. This structure can also increase the breakdown voltage value. At the same time, the trench gate can well control the channel length, reduce the hot carrier effect, and reduce the drift of the threshold voltage. Therefore, this device structure can improve the saturation region characteristics and improve the linearity of the transfer characteristic curve, thereby improving the reliability and life of the device, but there is a leakage problem. Utility Model Content

[0003] The main purpose of the utility model is to provide a nitride vertical power device to solve the leakage problem of the nitride vertical power device and improve the pressure resistance and anti-breakdown performance of the device.

[0004] In order to achieve the above-mentioned utility model purpose, the technical solution adopted by the utility model includes:

[0005] The utility model provides a nitride vertical power device, comprising:

[0006] The device main body structure comprises a drain electrode contact layer, a drift layer, a p-type nitride layer, and a source electrode contact layer which are stacked in sequence, wherein the p-type nitride layer has a first through-groove, and the source electrode contact layer has a second through-groove connected to the first through-groove, and the first through-groove and the second through-groove constitute a gate trench structure;

[0007] A gate layer structure, the gate layer structure comprising a nitride transition layer and a first insulating layer, the nitride transition layer covers the sidewalls of the gate trench structure and the bottom of the gate trench structure, and the first insulating layer is disposed on the nitride transition layer;

[0008] a source electrode, the source electrode being disposed on the source electrode contact layer and electrically connected to the source electrode contact layer;

[0009] a drain electrode, the drain electrode being arranged at a side of the drain electrode contact layer away from the drift layer and being electrically connected to the drain electrode contact layer;

[0010] a gate electrode, at least a portion of which is disposed in the gate trench structure, and a portion of the gate electrode located in the gate trench structure is surrounded by the first insulating layer;

[0011] The nitride transition layer includes a first nitride transition layer and a second nitride transition layer which are stacked, and the density of the first nitride transition layer is smaller than the density of the second nitride transition layer.

[0012] Furthermore, the first nitride transition layer is continuously disposed on the sidewalls of the gate trench structure and the bottom surface of the gate trench structure, the second nitride transition layer is continuously disposed on the first nitride transition layer, and the first insulating layer is continuously disposed on the second nitride transition layer.

[0013] Furthermore, a surface of the first nitride transition layer facing the gate trench structure has a concave-convex structure conforming to the surface of the sidewall and / or bottom of the gate trench structure, and the other surface of the first nitride transition layer facing away from the gate trench structure is a continuous flat structure.

[0014] Furthermore, the first nitride transition layer is an aluminum nitride layer having a plurality of holes therein, and the second nitride transition layer is a dense aluminum nitride layer.

[0015] Furthermore, the thickness of the first nitride transition layer is smaller than the thickness of the second nitride transition layer.

[0016] Furthermore, the total thickness of the nitride transition layer is 50nm-100nm.

[0017] Furthermore, the thickness of the first nitride transition layer is 5nm-20nm.

[0018] Furthermore, top surfaces of the first nitride transition layer, the second nitride transition layer, and the first insulating layer are flush with a top surface of the source electrode contact layer.

[0019] Furthermore, the nitride vertical power device also includes a second insulating layer, which covers the source electrode contact layer, the first nitride transition layer, the second nitride transition layer, and the top surface of the first insulating layer, and the second insulating layer is arranged between the source electrode and the gate electrode.

[0020] Furthermore, a top surface of the gate electrode is flush with a top surface of the second insulating layer.

[0021] Furthermore, the source electrode is arranged at an edge of the second insulating layer, and a top surface of the source electrode is flush with an upper surface of the second insulating layer.

[0022] Furthermore, the doping concentration of the drift layer is lower than the doping concentration of the drain electrode contact layer.

[0023] Furthermore, the doping concentration of the drift layer is less than the doping concentration of the source electrode contact layer.

[0024] Furthermore, the drain electrode contact layer is a heavily doped N-type gallium nitride layer, the thickness of the drain electrode contact layer is 50nm-500nm, and the doping concentration is 10 17 cm -3 -10 20 cm -3 .

[0025] Furthermore, the drift layer is a lightly doped N-type gallium nitride layer, and the doping concentration of the drift layer is 10 14 cm -3 -10 17 cm -3 , the thickness of the drift layer is 500nm-20μm.

[0026] Furthermore, the doping concentration of the p-type nitride layer is 10 17 cm -3 -10 20 cm -3 , the thickness of the p-type nitride layer is 150nm-5500nm.

[0027] Furthermore, the source electrode contact layer is a heavily doped N-type gallium nitride layer, and the doping concentration of the source electrode contact layer is 10 17 cm -3 -10 20 cm -3 , the thickness of the source electrode contact layer is 50nm-500nm.

[0028] Compared with the prior art, the advantages of the utility model include:

[0029] The utility model provides a nitride transition layer of a nitride vertical power device, which is formed by a first nitride transition layer and a second nitride transition layer, and the first nitride transition layer has a lower density than the second nitride transition layer, thereby eliminating the adverse effect of the uneven structure of the inner wall of the gate trench structure on the nitride transition layer, so that the surface flatness of the obtained nitride transition layer is better, thereby avoiding the leakage problem of the device, and further improving the voltage resistance and anti-puncture performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a structural schematic diagram of a nitride vertical power device provided in a typical implementation case of the utility model;

[0031] Figure 2 It is a schematic diagram of the structure after a drain electrode contact layer is formed on a substrate in a typical implementation case of the utility model;

[0032] Figure 3 It is a schematic diagram of the structure after a drift layer is formed on the drain electrode contact layer in a typical implementation case of the utility model;

[0033] Figure 4 It is a schematic diagram of the structure after a p-type nitride layer and a source electrode contact layer are formed on the drift layer in a typical implementation case of the utility model;

[0034] Figure 5 It is a schematic diagram of the structure after etching to form a gate trench structure in a typical implementation case of the utility model;

[0035] Figure 6 It is a schematic diagram of the structure after a first nitride transition layer is formed on the inner wall of the gate trench structure in a typical implementation case of the utility model;

[0036] Figure 7 It is a schematic structural diagram of a typical implementation case of the utility model after a second nitride transition layer is formed on the surface of the first nitride transition layer;

[0037] Figure 8a It is a schematic diagram of a local structure after a first nitride transition layer is formed on the inner wall of a gate trench structure in a typical implementation case of the utility model in the first growth stage;

[0038] Figure 8b It is a schematic diagram of the local structure after a second nitride transition layer is grown on the surface of the first nitride transition layer in a typical implementation case of the utility model in the second growth stage;

[0039] Fig. 9 It is a schematic diagram of the structure after the insulating layer is formed in a typical implementation case of the utility model. DETAILED DESCRIPTION

[0040] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the utility model after long-term research and extensive practice. The technical solution, its implementation process and principle, etc. will be further explained in conjunction with the accompanying drawings and specific implementation cases. Unless otherwise specified, the semiconductor epitaxial equipment and related processes, photolithography and etching equipment and related processes used in the utility model are all known to those skilled in the art, and no specific limitation or description is made here.

[0041] Explanation of terms involved in the embodiments of the present invention: the source electrode region refers to the region corresponding to the source electrode or the positive projection region of the source electrode; the gate electrode region refers to the region corresponding to the gate electrode or the positive projection region of the gate electrode.

[0042] See also Figure 1 , Figure 1 It is a structural schematic diagram of a nitride vertical power device provided in a typical implementation case of the utility model. The nitride vertical power device includes a device main structure and an electrode matching the device main structure. The device main structure includes a drain electrode contact layer 11, a drift layer 12, a p-type nitride layer 13, and a source electrode contact layer 14 stacked in sequence along the longitudinal direction of the device. The electrodes include a source electrode 21, a drain electrode (i.e., drain electrode, the same below) 22 and a gate electrode 23.

[0043] The gate electrode region of the device main structure has a gate trench structure, the bottom of the gate trench structure is located on the surface of the drift layer 12 away from the drain electrode contact layer 11, and the groove is flush with the surface of the source electrode contact layer 14 away from the p-type nitride layer 13; specifically, the p-type nitride layer 13 has a first through groove, the groove of the first through groove is flush with the surface of the source electrode contact layer 14 away from the p-type nitride layer 13, the source electrode contact layer 14 has a second through groove connected to the first through groove, the bottom of the second through groove is located on the surface of the drift layer 12 away from the drain electrode contact layer 11, the first through groove and the second through groove are continuously connected and constitute a gate trench structure, the gate electrode 23 is arranged in the gate trench structure, and is insulated from the device main structure; the source electrode 21 is arranged on the source electrode contact layer 14 and is electrically connected to the source electrode contact layer 14; the drain electrode 22 is arranged on the side of the drain electrode contact layer 11 facing away from the drift layer 12, and is electrically connected to the drain electrode contact layer 11.

[0044] Specifically, the drain electrode contact layer 11 is a heavily doped n-type gallium nitride layer, and the doping concentration of the drain electrode contact layer 11 is (10 17 -10 20 )cm -3 The thickness of the drain electrode contact layer 11 is 50nm-500nm. The drift layer 12 is a lightly doped (also referred to as low-doped, the same below) n-type gallium nitride layer, and the doping concentration of the drift layer 12 is (10 14 -10 17 )cm -3 The thickness of the drift layer 12 is usually 500 nm-20 μm. The p-type nitride layer 13 is a p-type gallium nitride layer, and the doping concentration of the p-type nitride layer 13 is (10 17 -10 20 )cm -3 The thickness of the p-type nitride layer 13 is 150nm-5500nm. The source electrode contact layer 14 is a heavily doped n-type gallium nitride layer, and the doping concentration of the source electrode contact layer 14 is (1017 -10 20 )cm -3 The thickness of the source electrode contact layer 14 is usually 50nm-500nm.

[0045] Specifically, a gate layer structure is further arranged between the gate trench structure and the gate electrode 23, and the gate layer structure includes a nitride transition layer 15 and an insulating layer 16. The nitride transition layer 15 is continuously arranged on the side wall and the surface of the bottom of the gate trench structure, and the insulating layer 16 is continuously arranged on the surface of the nitride transition layer 15 and the surface of the source electrode contact layer 14. It should be noted that the side wall and the bottom of the gate trench structure constitute the inner wall (or trench wall) of the gate trench structure.

[0046] Specifically, the nitride transition layer 15 is formed of aluminum nitride, which has a good lattice match with gallium nitride, and aluminum nitride can be formed in equipment such as metal organic chemical vapor deposition (Metal-organic Chemical Vapor Deposition, MOCVD) without additional equipment. More specifically, the growth reaction source (i.e., raw material gas, the same below) used in the MOCVD process to grow aluminum nitride can be trimethylaluminum (TMA) and ammonia (NH 3 ), during the growth process, nitrogen is used as a carrier gas to provide a growth reaction source.

[0047] It should be noted that the inner wall of the gate trench structure has micro-nano-scale protrusions and / or pits formed by etching, which makes the flatness of the inner wall of the gate trench structure poor. Therefore, when aluminum nitride grows on the inner wall of the gate trench structure, since the growth reaction source has less contact with the pits on the inner wall of the gate trench structure, the growth rate of aluminum nitride here is slower, while there are more growth reaction sources that undergo contact reactions at the protrusions, and the growth rate of aluminum nitride is faster. Therefore, when aluminum nitride grows, scattered aluminum nitride protrusions and aluminum nitride pits are formed, which in turn causes the surface of the formed aluminum nitride layer to be uneven, specifically manifested as a concave-convex structure that imitates the inner wall of the gate trench structure, thereby affecting the performance of the device. Based on this, the nitride transition layer 15 in the utility model is grown and formed in stages. The utility model first forms a first aluminum nitride layer as a first nitride transition layer 1510 on the inner wall of the gate trench structure under a first temperature condition, and then anneals the first aluminum nitride layer under a nitrogen atmosphere and a second temperature condition, and then forms a second aluminum nitride layer as a second nitride transition layer 1520 on the surface of the first aluminum nitride layer under a third temperature condition. The first nitride transition layer 1510 and the second nitride transition layer 1520 together form a nitride transition layer 15, the thickness of the nitride transition layer 15 is 50nm-100nm, wherein the density of the first nitride transition layer 1510 is less than the density of the second nitride transition layer 1520, the thickness of the first nitride transition layer 1510 is relatively small, generally 5nm-20nm, and after annealing treatment, the first aluminum nitride layer can form a flat surface. More specifically, the first temperature is 1000℃-1150℃, and the third temperature is 1200℃-1300℃.

[0048] Specifically, the insulating layer 16 includes a first insulating layer 1610 and a second insulating layer 1620. The first insulating layer 1610 is continuously arranged on the surface of the second nitride transition layer 1520. The top surfaces of the first nitride transition layer 1510, the second nitride transition layer 1520, and the first insulating layer 1610 are flush with the top surface of the source electrode contact layer 14. The second insulating layer 1620 is arranged between the source electrode 21 and the gate electrode 23. The second insulating layer 1620 covers the top surfaces of the source electrode contact layer 14, the first nitride transition layer 1510, the second nitride transition layer 1520, and the first insulating layer 1610. The top surface of the gate electrode 23 is flush with the top surface of the second insulating layer 1620. The source electrode 21 is arranged at the edge of the second insulating layer 1620, and the top surface of the source electrode 21 is flush with the upper surface of the second insulating layer 1620.

[0049] Specifically, the first insulating layer 1610 and the second insulating layer 1620 may be integrally formed, and the material of the first insulating layer 1610 and the second insulating layer 1620 may be silicon oxide or silicon nitride, etc. The thickness of the first insulating layer 1610 and the second insulating layer 1620 is 20nm-80nm.

[0050] See also Figure 2-Figure 9 The utility model provides a method for preparing the above-mentioned nitride vertical power device, comprising the following steps:

[0051] 1) providing a substrate 30, and forming a drain electrode contact layer 11 having a high doping concentration on the substrate 30, such as Figure 2 shown.

[0052] The substrate 30 may be a gallium nitride substrate, a silicon carbide substrate, a silicon substrate or a sapphire substrate. In order to facilitate subsequent stripping of the substrate 30 and reduce costs, a silicon substrate or a sapphire substrate is preferred.

[0053] After providing the substrate 30, the surface of the substrate 30 is first cleaned and dried to prevent surface oil or other contaminants from adversely affecting subsequent material growth; after cleaning and drying, in order to improve the crystallization quality and film quality of the upper layer structure, a buffer layer (not shown) can also be formed on the substrate 30, that is, the drain electrode contact layer 11 can be stacked on the buffer layer.

[0054] In a specific embodiment, MOCVD or molecular beam epitaxy (MBE) or other processes can be used to form an n-type GaN with a thickness of 50nm-500nm on the substrate 30 as the drain electrode contact layer 11. The n-type GaN as the drain electrode contact layer 11 usually has a higher doping concentration to reduce the contact resistance. The doping concentration of the drain electrode contact layer 11 is greater than 10 17 cm -3 and less than 10 20 cm -3 The doping element of the drain electrode contact layer 11 can be Si, Ge or a combination thereof.

[0055] 2) forming a drift layer 12 with a low doping concentration on the drain electrode contact layer 11, such as Figure 3 shown.

[0056] The MOCVD process can be used to deposit n-type GaN with a thickness of 500nm-20μm on the drain electrode contact layer 11 as the drift layer 12. The doping element of the drift layer 12 can be Si, Ge or a combination thereof, and the doping concentration is 10 14 cm -3 -10 17 cm -3 .

[0057] 3) forming a p-type nitride layer 13 on the drift layer 12, and forming a source electrode contact layer 14 on the p-type nitride layer 13, as shown in FIG. Figure 4 shown.

[0058] After the drift layer 12 is grown, a p-type GaN layer with a thickness of 150 nm to 5500 nm is grown on the drift layer 12 in an MOCVD device as a p-type nitride layer 13. The doping concentration of the p-type nitride layer 13 is 10 17 cm -3 -10 20 cm -3 Then, a heavily doped n-type GaN with a thickness of 50nm-500nm is grown on the p-type nitride layer 13 as the source electrode contact layer 14, and the doping concentration of the source electrode contact layer 14 is 10 17 cm -3 -10 20 cm -3 .

[0059] 4) a mask 40 is provided in the non-gate electrode region on the surface of the source electrode contact layer 14, and the source electrode contact layer 14 and the p-type nitride layer 13 located in the gate electrode region are etched away, a first through groove is formed in the p-type nitride layer 13, and a second through groove is formed in the source electrode contact layer 14, the second through groove is connected to the first through groove and forms a gate trench structure 1010, as shown in FIG. Figure 5 shown.

[0060] A photoresist is spin-coated on the surface of the source electrode contact layer 14. After the photoresist is cured, a photoresist layer is formed. After the photoresist layer is exposed and developed, an opening is formed on the photoresist layer, and the opening corresponds to the gate electrode region. The photoresist layer with the opening is used as a mask 40, and an inductively coupled plasma (ICP) etching process is adopted to etch the source electrode contact layer 14 and the p-type nitride layer 13 exposed at the opening to expose the drift layer 12 at the bottom, so that the p-type nitride layer 13 has a first through groove and the source electrode contact layer 14 has a second through groove, thereby forming a gate trench structure 1010.

[0061] More specifically, the conditions of the ICP process include: the etching gas is chlorine (Cl 2 ), the flow rate of chlorine gas is 30mL / min~40mL / min, the pressure is 0.3Pa~0.5Pa, the etching time is 20s-50s, the upper field plate power is 250W~350W and the lower field plate power is 80W~150W; the etching is performed until the drift layer 12 is exposed through detection.

[0062] 5) The mask 40 is removed, and a nitride transition layer 15 is formed by depositing in two steps on the inner wall surface of the gate trench structure 1010 after the passivation treatment, such as Figure 6 , Figure 7 shown.

[0063] The mask 40 on the surface of the source electrode contact layer 14 may be removed by an ashing process.

[0064] Please also read Figure 8a , Figure 8b The nitride transition layer 15 is formed through two growth stages, both of which are carried out using the MOCVD process, and the growth reaction source and carrier gas used are the same, that is, the nitride transition layer 15 includes a stacked first nitride transition layer 1510 and a second nitride transition layer 1520, the first nitride transition layer 1510 is continuously distributed on the inner wall of the gate trench structure 1010, and the second nitride transition layer 1520 is distributed on the surface of the first nitride transition layer 1510.

[0065] In a specific embodiment, the nitride transition layer 15 is obtained by:

[0066] a. First growth stage: The temperature in the reaction chamber of the MOCVD equipment is set to 1000°C-1150°C, nitrogen is used as a carrier gas, trimethylaluminum and ammonia are introduced into the reaction chamber, and the flow rate of trimethylaluminum is controlled to be 20sccm-200sccm, the flow rate of ammonia is controlled to be 300sccm-2000sccm, and the growth time is 10s-20s, so as to form a first aluminum nitride layer with a thickness of 5nm-20nm on the inner wall of the gate trench structure 1010, and the first aluminum nitride layer is used as the first nitride transition layer 1510.

[0067] It should be noted that if Figure 8a As shown, the inner wall of the gate trench structure 1010 formed by etching has micro-nano-scale protrusions 1101 and / or pits 1102. In the process of growing aluminum nitride on the inner wall of the gate trench structure 1010 by chemical vapor deposition, since the growth reaction source has less contact at the pit 1102 on the inner wall of the gate trench structure 1010, the growth rate of aluminum nitride is slower, while the growth reaction source that has contact reaction at the protrusion 1101 is more, and the growth rate of aluminum nitride is faster. Therefore, in the first growth formation, The aluminum nitride layer will form a dispersed first part 1511 (i.e. the aforementioned aluminum nitride protrusion) and a second part 1512 (i.e. the aforementioned aluminum nitride pit). The first part 1511 is correspondingly formed on the protrusion 1101, and the second part 1512 is correspondingly formed in the pit 1102. Moreover, since the horizontal growth and the vertical growth grow together, the first aluminum nitride layer formed by the growth has a plurality of inverted trapezoidal openings, which are correspondingly distributed between the first part 1511 and the second part 1512.

[0068] b. Annealing treatment stage: stop introducing trimethylaluminum and ammonia, control the temperature in the reaction chamber, and perform high-temperature annealing on the formed first nitride transition layer 1510 in a nitrogen atmosphere. The annealing time is 5min-60min. High-temperature annealing facilitates merging the openings of the first aluminum nitride layer, thereby forming a plurality of hole structures inside the first aluminum nitride layer.

[0069] c. Second growth stage: The temperature in the reaction chamber is raised to 1200°C-1300°C, and trimethylaluminum and ammonia gases required for growing aluminum nitride are continuously introduced into the reaction chamber, thereby forming a second aluminum nitride layer (i.e., the second nitride transition layer 1520) on the surface of the first aluminum nitride layer. The high temperature facilitates the formation of a dense aluminum nitride film layer, and the total thickness of the finally formed nitride transition layer 15 is 50nm-100nm.

[0070] Specifically, during the annealing treatment stage, only nitrogen is introduced. Nitrogen is a carrier gas for growing aluminum nitride and will not react with aluminum nitride, nor will impurity elements such as oxygen be introduced (oxygen will form aluminum nitride oxide AlON with aluminum nitride. AlON is difficult to move at high temperatures, which is not conducive to the closure of the membrane opening). High-temperature annealing is performed in a nitrogen atmosphere, and the aluminum nitride undergoes recrystallization and high-temperature migration. Since the thickness of the aluminum nitride formed in the first growth stage is relatively small (usually between 5nm-20nm), after 5min-60min annealing, the first nitride transition layer 1510 can be closed at the opening, thereby forming a flattened surface. Some closed openings, i.e., a hole structure, will be formed at the bottom of the first nitride transition layer 1510. After that, a second nitride transition layer 1520 is formed, and a stacked structure (i.e., nitride transition layer 15) including an aluminum nitride layer with holes and a dense aluminum nitride layer can be obtained. Figure 8a , Figure 8b shown.

[0071] Specifically, the growth temperature of the second growth stage is higher, and the high temperature facilitates the formation of a dense aluminum nitride film layer, thus forming a nitride transition layer 15 with a dense top layer and holes in the bottom layer. Compared with the direct formation of the aluminum nitride layer, as mentioned above, the surface of the directly formed aluminum nitride layer has unevenly distributed pits and protrusions, which will affect the formation of subsequent structural layers and then affect the performance of the device. If aluminum nitride is grown only by staged growth without annealing, the surface of the aluminum nitride layer formed in the first growth stage still has protrusions and pits, and the surface of the aluminum nitride layer cannot be merged to form a continuous surface, which is the same as the solution of directly forming aluminum nitride. It will cause an adverse effect on the leakage problem of the device, and will also affect the formation of the subsequent insulating layer, thereby reducing the voltage breakdown resistance.

[0072] 6) forming an insulating layer 16 on the surface of the nitride transition layer 15 and the surface of the source electrode contact layer 14, and forming a gate electrode 23 in the gate trench structure 1010, as shown in FIG. Fig. 9 shown.

[0073] A continuous insulating layer 16 can be formed on the surface of the source electrode contact layer 14 and the surface of the nitride transition layer in the gate trench structure 1010 by sputtering or deposition process. The thickness of the insulating layer 16 is 20nm-80nm, and the material of the insulating layer 16 can be silicon oxide or silicon nitride.

[0074] A gate electrode 23 may be formed in the gate trench structure 1010 by a deposition or sputtering process, and the gate electrode 23 is disposed on the insulating layer 16 ; the gate electrode 23 may be a Ti / Al metal stack structure or other appropriate conductive material or a combination thereof, and the gate electrode 23 fills the remaining space of the gate trench structure 1010 .

[0075] 7) removing the substrate 30, and forming a drain electrode 22 on the surface of the drain electrode contact layer 11, and forming a source electrode 21 on the surface of the source electrode contact layer 14, as shown in FIG. Figure 1 shown.

[0076] The bottom substrate 30 can be removed by laser lift-off or thinning process to expose the drain electrode contact layer 11; the drain electrode 22 is formed on the surface of the exposed drain electrode contact layer 11. The first insulating layer 16 located on the surface of the source electrode contact layer 14 is etched by photolithography, etching and other processes, and the source electrode contact layer 14 is exposed by etching in the area corresponding to the source electrode; the source electrode 21 is formed on the surface of the exposed source electrode contact layer 14.

[0077] The utility model provides a nitride vertical power device, which forms a stacked first nitride transition layer and a second nitride transition layer in a staged growth manner, and uses the stacked first nitride transition layer and the second nitride transition layer as the nitride transition layer. The density of the first nitride transition layer is less than the density of the second nitride transition layer, thereby eliminating the adverse effect of the uneven structure of the inner wall of the gate trench structure on the nitride transition layer, so that the surface flatness of the obtained nitride transition layer is better, thereby avoiding the leakage problem of the device, and further improving the voltage resistance and anti-breakdown performance of the device.

[0078] It should be understood that the above embodiments are only for illustrating the technical concept and features of the utility model, and their purpose is to enable people familiar with the technology to understand the content of the utility model and implement it accordingly, and they cannot be used to limit the protection scope of the utility model. Any equivalent changes or modifications made according to the spirit of the utility model should be included in the protection scope of the utility model.

Claims

1. A nitride vertical power device, It is characterized in that include: The device main body structure comprises a drain electrode contact layer, a drift layer, a p-type nitride layer, and a source electrode contact layer which are stacked in sequence, wherein the p-type nitride layer has a first through-groove, and the source electrode contact layer has a second through-groove connected to the first through-groove, and the first through-groove and the second through-groove constitute a gate trench structure; A gate layer structure, the gate layer structure comprising a nitride transition layer and a first insulating layer, the nitride transition layer covers the sidewalls of the gate trench structure and the bottom of the gate trench structure, and the first insulating layer is disposed on the nitride transition layer; a source electrode, the source electrode being disposed on the source electrode contact layer and electrically connected to the source electrode contact layer; a drain electrode, the drain electrode being arranged at a side of the drain electrode contact layer away from the drift layer and being electrically connected to the drain electrode contact layer; a gate electrode, at least a portion of which is disposed in the gate trench structure, and a portion of the gate electrode located in the gate trench structure is surrounded by the first insulating layer; The nitride transition layer includes a first nitride transition layer and a second nitride transition layer which are stacked, and the density of the first nitride transition layer is smaller than the density of the second nitride transition layer.

2. The nitride vertical power device according to claim 1, Features: The first nitride transition layer is continuously disposed on the sidewall of the gate trench structure and the bottom surface of the gate trench structure, the second nitride transition layer is continuously disposed on the first nitride transition layer, and the first insulating layer is continuously disposed on the second nitride transition layer.

3. The nitride vertical power device according to claim 2, Features: The first nitride transition layer has a surface facing the gate trench structure on one side thereof and has a concave-convex structure conforming to the surface of the sidewall and / or bottom of the gate trench structure, and the first nitride transition layer has a continuous flat structure on the other side thereof and facing away from the gate trench structure.

4. The nitride vertical power device according to claim 2, Features: The first nitride transition layer is an aluminum nitride layer having a plurality of holes therein, and the second nitride transition layer is a dense aluminum nitride layer.

5. The nitride vertical power device according to any one of claims 2 to 4, Features: The thickness of the first nitride transition layer is smaller than the thickness of the second nitride transition layer.

6. The nitride vertical power device according to claim 5, Features: The thickness of the nitride transition layer is 50nm-100nm.

7. The nitride vertical power device according to claim 5, Features: The thickness of the first nitride transition layer is 5nm-20nm.

8. The nitride vertical power device according to claim 1, Features: Top surfaces of the first nitride transition layer, the second nitride transition layer, and the first insulating layer are flush with a top surface of the source electrode contact layer.

9. The nitride vertical power device according to claim 1 or 8, It is characterized in that The nitride vertical power device also includes a second insulating layer, which covers the source electrode contact layer, the first nitride transition layer, the second nitride transition layer, and the top surface of the first insulating layer, and the second insulating layer is arranged between the source electrode and the gate electrode.

10. The nitride vertical power device according to claim 9, Features: A top surface of the gate electrode is flush with a top surface of the second insulating layer.

11. The nitride vertical power device according to claim 9, Features: The source electrode is disposed at an edge of the second insulating layer, and a top surface of the source electrode is flush with a top surface of the second insulating layer.

12. The nitride vertical power device according to claim 1, Features: The drain electrode contact layer is a heavily doped N-type gallium nitride layer, and the thickness of the drain electrode contact layer is 50nm-500nm.

13. The nitride vertical power device according to claim 1, Features: The drift layer is a lightly doped N-type gallium nitride layer, and the thickness of the drift layer is 500nm-20μm.

14. The nitride vertical power device according to claim 1, Features: The thickness of the p-type nitride layer is 150nm-5500nm.

15. The nitride vertical power device according to claim 1, Features: The source electrode contact layer is a heavily doped N-type gallium nitride layer, and the thickness of the source electrode contact layer is 50nm-500nm.