Device for preparing high-purity and high-uniformity powder high-temperature alloy cast ingot
By using plasma gun smelting technology and water-cooled copper crystallizer in a high vacuum environment, the problems of inclusion removal and composition uniformity control in metallurgical technology are solved, and the preparation of high-temperature alloy ingots with high purity, high uniformity and high-temperature strength is achieved. , reducing production costs.
Patent Information
- Application Number
- CN202420418590.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2034-03-05
AI Technical Summary
When preparing high-temperature alloy ingots with existing metallurgical technology, it is difficult to completely remove inclusions and control composition uniformity, resulting in insufficient high-temperature structural stability and oxidation resistance of turbine disks.
Using plasma gun smelting technology in a high vacuum smelting environment, combined with a water-cooled copper crystallizer and telescopic components, it significantly reduces the gas impurities and inclusion content in the ingot, accelerates the dissolution and removal of inclusions through the plasma flame, and accelerates the rapid cooling process Reduce thermal stress.
It significantly improves the purity and uniformity of high-temperature alloys, enhances high-temperature strength, reduces production costs, avoids the occurrence of internal cracks, and achieves the preparation of high-purity and uniform powder high-temperature alloy ingots.
Smart Images

Figure CN221895082U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of metallurgy, and in particular relates to a device for preparing high-purity and high-uniform powder high-temperature alloy ingots. Background Art
[0002] Due to the harsh working environment and complex forces of engine turbine disks, the material is required to have excellent high-temperature strength, low / high-cycle fatigue resistance, oxidation resistance and thermal corrosion resistance, as well as long-term high-temperature structural stability. The turbine disks and other components currently used in aircraft engines are usually made of nickel-based powder high-temperature alloys. The purity of the alloy and the uniformity of the structure and composition are important factors affecting the safety and reliability of the turbine disk. The quality of the master alloy ingot is the primary factor that determines the performance of the final turbine disk. Selecting an appropriate smelting production process can effectively control the segregation and purity of the master alloy.
[0003] At present, double or triple melting processes are usually used to prepare powder high-temperature alloy ingots, but the control of impurity content and uniformity of structure and composition is still far behind that of advanced countries such as the United States.
[0004] Powder high-temperature alloy master alloy is usually melted once by vacuum induction melting. In order to improve its purity, slag filtration and high-temperature treatment of the melt are taken during the melting process, but its purity still has certain problems; therefore, on the basis of vacuum induction melting, electroslag remelting or vacuum consumable remelting is also used for secondary melting, or even tertiary melting to improve its purity. The removal of inclusions by vacuum consumable melting technology mainly relies on its flotation effect, that is, during the melting process, the inclusions will float to the surface of the molten pool, then move around and be repelled to the edge of the molten pool by the arc. After contacting and solidifying with the water-cooled crystallizer, they are concentrated on the surface of the ingot and finally removed by machining. However, this removal process cannot completely remove the inclusions in the ingot, and may also cause larger inclusions in the remelted ingot. At the same time, due to the fast solidification cooling rate, metal volatilization and splashing will occur during melting. These deposits condensed on the wall of the crystallizer are very likely to fall into the ingot during the melting process and reduce the uniformity of the structure of the remelted ingot. In addition, during vacuum consumable remelting, due to the large molten pool and the strong flow of solute-rich interdendritic liquid in the mushy area of the molten pool, macro segregation of the remelted rod is very likely to occur. The electroslag remelting technology mainly relies on slag adsorption to remove inclusions in the molten pool. Although the removal rate of original inclusions in vacuum induction melting electrode rods is high (>80%), the electrode surface is very easy to oxidize at high temperatures, which will increase the oxygen content in the ingot. During the cooling process of the molten pool, the oxygen solubility will decrease, and the supersaturated oxygen will interact with certain alloying elements in the molten pool to produce new oxide inclusions. In addition, due to the low melting and solidification rates of this technology, the active elements in the melting process are difficult to control, which will cause component segregation in some areas of the ingot.
[0005] In view of this, the inventor provides a device for preparing high-purity and high-uniformity powder high-temperature alloy ingots to solve the above technical problems. Utility Model Content
[0006] The purpose of the utility model is to overcome the shortcomings of the above-mentioned prior art and propose a device for preparing high-purity and high-uniformity powder high-temperature alloy ingots. The device melts electrode rods through a plasma gun in a high vacuum melting environment, and is provided with a water-cooled copper crystallizer and a telescopic component, which can significantly reduce the gas impurity content inside the ingot and the inclusion content in the ingot, and solves the problem of component segregation commonly existing in traditional smelting devices in the preparation of high-temperature alloy ingots.
[0007] In order to achieve the above purpose, the utility model adopts the following technical solutions:
[0008] A device for preparing high-purity and high-uniformity powder high-temperature alloy ingots, comprising a smelting chamber, a plasma gun control system is arranged on one side of the smelting chamber, and a driving mechanism is arranged on the other side, the driving mechanism is connected to an electrode rod inserted into the smelting chamber and arranged horizontally, and in the smelting chamber, a plasma flame generated by the plasma gun control system melts the electrode rod into liquid metal;
[0009] Wherein, a water-cooled copper crystallizer is arranged inside the smelting chamber and below the electrode rod;
[0010] Specifically, the wall thickness of the water-cooled copper crystallizer is 30 mm, the inner diameter is 100 mm, and the total height of the solidification chamber is 1 m; the diameter of the cooling water channel is 6 mm.
[0011] The top of the smelting chamber is connected to a vacuum control system through a vacuum pipeline, and a telescopic component is installed at the bottom of the smelting chamber, one side of the telescopic component extends into the interior of the smelting chamber and contacts the bottom of the water-cooled copper crystallizer.
[0012] Specifically, the electrode rod material has a diameter φ of 55 mm to 110 mm and a length of 500 mm to 800 mm.
[0013] Further, the plasma gun control system includes a control cabinet and a gas storage assembly arranged outside the smelting chamber and a plasma gun located inside the smelting chamber;
[0014] The plasma gun comprises a plasma gun cathode and a plasma gun anode arranged around the plasma gun cathode, a water cooling channel is arranged inside the plasma gun anode, the water cooling channel is connected to the control cabinet through a cooling pipeline, the plasma gun cathode is connected to the control cabinet through a gas pipeline, and the gas pipeline of the gas storage assembly is connected to the gas pipeline and transports Ar+He mixed gas to the plasma gun;
[0015] The central axis of the plasma gun and the electrode rod are located on the same horizontal line.
[0016] Specifically, the melting power of the plasma gun is 10 kW to 20 kW.
[0017] Furthermore, the driving mechanism includes a push rod and a first driving motor connected thereto, and the push rod is connected to the electrode rod.
[0018] Furthermore, it also includes an oxygen content monitoring probe, which is installed on the top of the smelting chamber.
[0019] Furthermore, a solidification chamber is axially opened at the center of the water-cooled copper crystallizer, a cooling water channel is arranged inside the water-cooled copper crystallizer and on the outer periphery of the solidification chamber, a movable baffle is arranged in the solidification chamber and is slidably connected to the inner wall of the water-cooled copper crystallizer, the top of the movable baffle is used to accommodate liquid metal generated by the electrode rod during the melting process, the lower part of the cooling water channel, located on the outside of the smelting chamber, is connected to a water inlet through a cooling pipe, and a water outlet is arranged above the water inlet.
[0020] Furthermore, a first flow regulating valve is provided on the cooling pipe between the water inlet and the smelting chamber, and a second flow regulating valve is provided on the cooling pipe between the water outlet and the smelting chamber.
[0021] Furthermore, the telescopic assembly includes a telescopic rod and a second drive motor arranged outside the smelting chamber, one end of the telescopic rod is connected to the transmission shaft of the second drive motor, and the other end extends into the smelting chamber and contacts the bottom of the movable baffle, and a sealing assembly is arranged at the position where the telescopic rod contacts the smelting chamber.
[0022] Furthermore, the sealing assembly includes a sleeve sleeved on the telescopic rod, a skeleton oil seal is arranged on the outer peripheral surface of the sleeve, a first insulating bushing is arranged on the top of the skeleton oil seal, a sealing ring is installed on the bottom of the skeleton oil seal, a second insulating bushing is arranged on the bottom of the sealing ring, a first sealing cover is arranged on the upper surface of the sleeve, located above the first insulating bushing, and a second sealing cover is arranged on the lower surface of the sleeve, located below the second insulating bushing.
[0023] Compared with the prior art, the utility model has the following beneficial effects:
[0024] The utility model provides a device for preparing high-purity and high-uniformity powder high-temperature alloy ingots, which is provided with a high vacuum melting environment (vacuum degree ≤ 1.0×10 -3Pa), the electrode rod is melted at a high refining temperature (>2500°C) of a plasma gun, which can significantly reduce the gas impurity (O, N) content inside the ingot; at the same time, under the bombardment of the plasma flame, the dissolution and removal of inclusions in the electrode rod can be accelerated, and the inclusion content in the ingot is greatly reduced; in addition, during the smelting process, the end face of the electrode rod will quickly melt into a thin molten pool under the high temperature of the plasma flame, and the alloy droplets will be thrown out under the action of centrifugal force. The extremely high melting rate will not cause a large amount of burning of active elements (such as Al and Ti), which can significantly improve the strengthening effect of elements such as Al and Ti, and enhance the high-temperature strength of the alloy. In addition, a water-cooled copper crystallizer is set to control the water cooling rate and reduce the solidification temperature gradient, which can significantly reduce the thermal stress inside the ingot and avoid the appearance of internal cracks inside the rod after solidification. The utility model only needs to be refined once after vacuum induction melting to obtain a high-purity and high-uniform powder high-temperature alloy ingot, which greatly reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings herein are incorporated into and constitute a part of this specification, and together with the description, are used to explain the principles of the present utility model.
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the utility model or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0027] Figure 1 A schematic diagram of the structure of a device for preparing a high-purity and high-uniformity powder high-temperature alloy ingot provided by the utility model;
[0028] Figure 2 The actual picture obtained by using the utility model to prepare high-purity and high-uniformity powder high-temperature alloy ingots;
[0029] Figure 3 It is a high-magnification organization diagram of the longitudinal section of the FGH4097 powder high-temperature alloy ingot prepared by the utility model;
[0030] Figure 4 It is a high-magnification organization diagram of the longitudinal section of the FGH4096 powder high-temperature alloy ingot prepared by the utility model;
[0031] Figure 5 The high-magnification organization diagram of the longitudinal section of the FGH4095 powder high-temperature alloy ingot prepared by the utility model.
[0032] Among them: 1 is a smelting chamber; 2 is a plasma gun control system; 3 is a driving mechanism; 4 is an electrode rod; 5 is a water-cooled copper crystallizer; 6 is a vacuum control system; 7 is a telescopic component; 8 is an oxygen content monitoring probe; 21 is a control cabinet; 22 is a plasma gun; 23 is a gas storage component; 31 is a push rod; 32 is a first driving motor; 51 is a solidification chamber; 52 is a cooling water channel; 53 is a movable baffle; 54 is a water inlet; 55 is a water outlet; 71 is a telescopic rod; 72 is a second driving motor; 221 is a plasma gun anode; 222 is a plasma gun cathode; 2211 is a plasma gun anode water cooling channel; 541 is a first flow regulating valve; 551 is a second flow regulating valve. DETAILED DESCRIPTION
[0033] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present utility model. Instead, they are only examples of devices consistent with some aspects of the present utility model as detailed in the attached claims.
[0034] See also Figure 1-2 The embodiment of the utility model provides a device for preparing a high-purity and high-uniformity powder high-temperature alloy ingot, comprising a smelting chamber 1, a plasma gun control system 2 is arranged on one side of the smelting chamber 1, and a driving mechanism 3 is arranged on the other side. The driving mechanism 3 is connected to an electrode rod 4 inserted into the smelting chamber 1 and arranged horizontally. In the smelting chamber 1, the plasma flame generated by the plasma gun control system 2 melts the electrode rod 4 into liquid metal;
[0035] A water-cooled copper crystallizer 5 is provided inside the smelting chamber 1 and below the electrode rod 4;
[0036] The top of the smelting chamber 1 is connected to a vacuum control system 6 through a vacuum pipeline, and a telescopic component 7 is installed at the bottom of the smelting chamber 1. One side of the telescopic component 7 extends into the interior of the smelting chamber 1 and contacts the bottom of the water-cooled copper crystallizer 5.
[0037] Furthermore, the preparation method of the electrode rod 4 is not limited. The high-temperature alloy electrode rod 4 selected in this embodiment is prepared by vacuum induction melting.
[0038] In this embodiment, the driving mechanism 3 drives the electrode rod 4 to move toward the plasma gun control system 2 at a constant feed speed, and the electrode rod 4 is melted, so that the molten liquid metal drips into the water-cooled copper crystallizer 5 and is quickly cooled to obtain an ingot, and the ingot continues to grow under the downward movement of the telescopic component 7 to form an ingot of a certain height.
[0039] In this embodiment, the plasma gun control system 2 includes a control cabinet 21 and a gas storage assembly 23 arranged outside the smelting chamber 1 and a plasma gun 22 located inside the smelting chamber 1;
[0040] The plasma gun 22 includes a plasma gun cathode 222 and a plasma gun anode 221 arranged around the plasma gun cathode 222. A water cooling channel 2211 is arranged inside the plasma gun anode 221. The water cooling channel 2211 is connected to the control cabinet 21 through a cooling pipeline. The plasma gun cathode 222 is connected to the control cabinet 21 through a gas pipeline. The gas pipeline of the gas storage component 23 is connected to the gas pipeline and transports Ar+He mixed gas to the plasma gun 22.
[0041] The central axis of the plasma gun 22 and the electrode rod 4 are located on the same horizontal line.
[0042] In this embodiment, the driving mechanism 3 includes a push rod 31 and a first driving motor 32 connected thereto. The push rod 31 is connected to the electrode rod 4. The first driving motor 32 drives the push rod 31 and further drives the electrode rod 4 to move forward and rotate.
[0043] In addition, the high-temperature alloy ingot casting device further includes an oxygen content monitoring probe 8 , which is installed on the top of the smelting chamber 1 and is used to measure the oxygen content in the smelting chamber 1 .
[0044] In this embodiment, a solidification chamber 51 is axially opened at the center of the water-cooled copper crystallizer 5, a cooling water channel 52 is arranged inside the water-cooled copper crystallizer 5 and on the outer periphery of the solidification chamber 51, a movable baffle 53 is arranged in the solidification chamber 51 and is slidably connected to the inner wall of the water-cooled copper crystallizer 5, the top of the movable baffle 53 is used to accommodate the liquid metal generated by the electrode rod 4 during the melting process, the lower part of the cooling water channel 52, located on the outer side of the smelting chamber 1, is connected to a water inlet 54 through a cooling pipe, and a water outlet 55 is arranged above the water inlet 54.
[0045] Specifically, the wall thickness of the water-cooled copper crystallizer 5 is 30 mm, the inner diameter is 100 mm, the total height of the solidification chamber 51 is 1 m; and the diameter of the cooling water channel 52 is 6 mm.
[0046] In this embodiment, the water-cooled copper crystallizer 5 is used to quickly cool the liquid metal dripping into the movable baffle 53 so that it solidifies into a solid ingot.
[0047] Preferably, a first flow regulating valve 541 is provided on the cooling pipe between the water inlet 54 and the smelting chamber 1 , and a second flow regulating valve 551 is provided on the cooling pipe between the water outlet 55 and the smelting chamber 1 .
[0048] In this embodiment, the first flow regulating valve 541 and the second flow regulating valve 551 are used to adjust the water flow in the cooling water channel 52 .
[0049] In this embodiment, the telescopic assembly 7 includes a telescopic rod 71 and a second drive motor 72 arranged outside the smelting chamber 1, one end of the telescopic rod 71 is connected to the transmission shaft of the second drive motor 72, and the other end extends into the smelting chamber 1 and contacts the bottom of the movable baffle 53, and a sealing assembly is arranged at the position where the telescopic rod 71 contacts the smelting chamber 1.
[0050] In this embodiment, the sealing assembly includes a sleeve sleeved on the telescopic rod 71, a skeleton oil seal is arranged on the outer peripheral surface of the sleeve, a first insulating bushing is arranged on the top of the skeleton oil seal, a sealing ring is installed at the bottom of the skeleton oil seal, a second insulating bushing is arranged at the bottom of the sealing ring, a first sealing cover is arranged on the upper surface of the sleeve, located above the first insulating bushing, and a second sealing cover is arranged on the lower surface of the sleeve, located below the second insulating bushing.
[0051] In this embodiment, the telescopic assembly 7 is used to support the movable baffle 53 and move downward at a uniform speed to gradually increase the ingot, thereby obtaining ingots of different required heights.
[0052] The present embodiment is used to prepare an ingot of a high-purity and high-uniformity FGH4097 powder high-temperature alloy, which specifically includes the following steps:
[0053] S1, preparing an electrode rod 4 and pre-treating the electrode rod 4;
[0054] Specifically, the FGH4097 master alloy electrode rod 4 is prepared by vacuum induction melting, and the FGH4097 master alloy electrode rod 4 is peeled and sawed to obtain the electrode rod 4 for melting, and the rod size is Φ55mm×800mm;
[0055] S2, insert one end of the pretreated FGH4097 master alloy electrode rod 4 into the smelting chamber 1, and connect the other end to the first drive motor 32 of the drive mechanism 3 through the push rod 31 of the drive mechanism 3;
[0056] S3, start the vacuum control system 6 to evacuate the smelting chamber 1, so that the vacuum degree in the smelting chamber 1 reaches 5.0×10 -4 Pa, and then conduct leakage rate detection, and make the pressure rise rate of the smelting chamber 1 less than or equal to 0.05 Pa / min;
[0057] S4. After the leakage rate test is qualified, the first flow regulating valve 541 and the second flow regulating valve 551 of the water-cooled copper crystallizer 5 are opened respectively and the water flow rate is adjusted to 0.5 m / s, and then the moving speed of the telescopic rod 71 of the telescopic assembly 7 is set to 9 mm / min;
[0058] S5, start smelting, start the first drive motor 32 to drive the FGH4097 master alloy electrode rod 4 to rotate, after the electrode rod 4 rotates smoothly, fill the plasma gun 22 of the plasma gun control system 2 with a constant pressure of 1.0Pa of Ar+He mixed gas, and turn on the plasma gun 22 to generate a plasma flame, control the melting power of the plasma gun 22 to be 10kW, and drive the electrode rod 4 to approach the plasma flame at a feed speed of 30mm / min by the first drive motor 32. When the distance between the front end of the plasma gun 22 and the end face of the master alloy electrode rod 4 is 35mm, start smelting, melt the top of the electrode rod 4 to form a thin molten pool, and the liquid metal molten pool is thrown out under centrifugal force to form alloy droplets, and fall into the solidification chamber 51 of the water-cooled copper crystallizer 5 to solidify, forming a semi-solid molten pool and an ingot;
[0059] Among them, the rotation speed of the FGH4097 master alloy electrode rod 4 is 20r / min; the volume ratio of Ar:He is 9:1;
[0060] S6, the ingot with increasing length is formed under the downward movement of the telescopic rod 71, and after the smelting is completed, it is cooled for 2 hours and then taken out of the furnace to obtain a high-purity and high-uniformity FGH4097 powder high-temperature alloy ingot, such as Figure 3 shown.
[0061] Furthermore, during the smelting process, the O content in the smelting chamber 1 should be less than 30 ppm; at the same time, during the smelting process, the upper surface of the semi-solid molten pool should always be located at 2 / 3 to 3 / 4 of the total height of the solidification chamber 51, wherein the total height of the solidification chamber 51 is 1 m, so the distance between the upper surface of the semi-solid molten pool and the upper end surface of the solidification chamber 51 should be in the range of 0.25 m to 0.33 m, which can prevent molten droplets from falling into the semi-solid molten pool and causing splashing.
[0062] Samples were taken from the head and tail of the ingot to detect the composition, and the results of gas content and active metal element content are shown in Table 1.
[0063] Table 1 FGH4097 powder high temperature alloy ingot composition test results (wt.%)
[0064]
[0065] The present embodiment is used to prepare an ingot of a high-purity and high-uniformity FGH4096 powder high-temperature alloy, which specifically includes the following steps:
[0066] S1, preparing an FGH4096 master alloy electrode rod 4, and pre-treating the electrode rod 4;
[0067] Specifically, the FGH4096 master alloy electrode rod 4 is prepared by vacuum induction melting, and the FGH4096 master alloy electrode rod 4 is peeled and sawed to obtain the electrode rod 4 for melting, and the rod size is Φ80mm×650mm;
[0068] S2, insert one end of the pretreated FGH4096 master alloy electrode rod 4 into the smelting chamber 1, and connect the other end to the first drive motor 32 of the drive mechanism 3 through the push rod 31 of the drive mechanism 3;
[0069] S3, start the vacuum control system 6 to vacuum the smelting chamber 1, so that the vacuum degree in the smelting chamber 1 reaches 5.0×10 -4 Pa, and then conduct leakage rate detection, and make the pressure rise rate of the smelting chamber 1 less than or equal to 0.05 Pa / min;
[0070] S4. After the leakage rate test is qualified, the first flow regulating valve 541 and the second flow regulating valve 551 of the water-cooled copper crystallizer 5 are opened respectively and the water flow rate is adjusted to 2 m / s, and then the moving speed of the telescopic rod 71 of the telescopic assembly 7 is set to 12 mm / min;
[0071] S5, start smelting, start the first drive motor 32 to drive the FGH4096 master alloy electrode rod 4 to rotate, after the electrode rod 4 rotates smoothly, fill the plasma gun 22 of the plasma gun control system 2 with a constant pressure of 1.8Pa of Ar+He mixed gas, and turn on the plasma gun 22 to generate a plasma flame, control the melting power of the plasma gun 22 to be 15kW, and drive the electrode rod 4 to approach the plasma flame at a feed speed of 18mm / min by the first drive motor 32. When the distance between the front end of the plasma gun 22 and the end face of the master alloy electrode rod 4 is 30mm, start smelting, melt the top of the electrode rod 4 to form a thin molten pool, and the liquid metal molten pool is thrown out under centrifugal force to form alloy droplets, and fall into the solidification chamber 51 of the water-cooled copper crystallizer 5 to solidify, forming a semi-solid molten pool and an ingot;
[0072] Among them, the rotation speed of the FGH4096 master alloy electrode rod 4 is 60r / min; the volume ratio of Ar:He is 9:1;
[0073] S6, the ingot with increasing length is formed under the downward movement of the telescopic rod 71, and after the smelting is completed, it is cooled for 4 hours and then taken out of the furnace to obtain a high-purity and high-uniformity FGH4096 powder high-temperature alloy ingot, such as Figure 4 shown.
[0074] Furthermore, during the smelting process, the O content in the smelting chamber 1 should be less than 30 ppm; at the same time, during the smelting process, the upper surface of the semi-solid molten pool should always be located at 2 / 3 to 3 / 4 of the total height of the solidification chamber 51, wherein the total height of the solidification chamber 51 is 1 m, so the distance between the upper surface of the semi-solid molten pool and the upper end surface of the solidification chamber 51 should be in the range of 0.25 m to 0.33 m, which can prevent molten droplets from falling into the semi-solid molten pool and causing splashing.
[0075] Samples were taken from the head and tail of the ingot to detect the composition, and the results of gas content and active metal element content are shown in Table 2.
[0076] Table 2 FGH4096 powder high temperature alloy ingot composition test results (wt.%)
[0077]
[0078] The present embodiment is used to prepare an ingot of a high-purity and high-uniformity FGH4095 powder high-temperature alloy, which specifically includes the following steps:
[0079] S1, preparing an FGH4095 master alloy electrode rod 4, and pretreating the electrode rod 4;
[0080] Specifically, the FGH4095 master alloy electrode rod 4 is prepared by vacuum induction melting, and the FGH4095 master alloy electrode rod 4 is peeled and sawed to obtain the electrode rod 4 for melting, and the rod size is Φ110mm×500mm;
[0081] S2, insert one end of the pretreated FGH4095 master alloy electrode rod 4 into the smelting chamber 1, and connect the other end to the first drive motor 32 of the drive mechanism 3 through the push rod 31 of the drive mechanism 3;
[0082] S3, start the vacuum control system 6 to vacuum the smelting chamber 1, so that the vacuum degree in the smelting chamber 1 reaches 5.0×10 -4 Pa, and then conduct leakage rate detection, and make the pressure rise rate of the smelting chamber 1 less than or equal to 0.05 Pa / min;
[0083] S4. After the leakage rate test is qualified, the first flow regulating valve 541 and the second flow regulating valve 551 of the water-cooled copper crystallizer 5 are opened respectively and the water flow rate is adjusted to 4 m / s, and then the moving speed of the telescopic rod 71 of the telescopic assembly 7 is set to 15 mm / min;
[0084] S5, start smelting, start the first drive motor 32 to drive the FGH4095 master alloy electrode rod 4 to rotate, after the electrode rod 4 rotates smoothly, fill the plasma gun 22 of the plasma gun control system 2 with a constant pressure of 2.5Pa of Ar+He mixed gas, and turn on the plasma gun 22 to generate a plasma flame, control the melting power of the plasma gun 22 to be 20kW, and drive the electrode rod 4 to approach the plasma flame at a feed speed of 10mm / min. When the distance between the front end of the plasma gun 22 and the end face of the master alloy electrode rod 4 is 25mm, start smelting, melt the top of the electrode rod 4 to form a thin molten pool, and the liquid metal molten pool is thrown out under centrifugal force to form alloy droplets, and fall into the solidification chamber 51 of the water-cooled copper crystallizer 5 to solidify, forming a semi-solid molten pool and an ingot;
[0085] Among them, the rotation speed of the FGH4095 master alloy electrode rod 4 is 100r / min; the volume ratio of Ar:He is 9:1;
[0086] S6, the ingot with increasing length is formed under the downward movement of the telescopic rod 71, and after the smelting is completed, it is cooled for 6 hours and then taken out of the furnace to obtain a high-purity and high-uniformity FGH4095 powder high-temperature alloy ingot, such as Figure 5 shown.
[0087] Furthermore, during the smelting process, the O content in the smelting chamber 1 should be less than 30 ppm; at the same time, during the smelting process, the upper surface of the semi-solid molten pool should always be located at 2 / 3 to 3 / 4 of the total height of the solidification chamber 51, wherein the total height of the solidification chamber 51 is 1 m, so the distance between the upper surface of the semi-solid molten pool and the upper end surface of the solidification chamber 51 should be in the range of 0.25 m to 0.33 m, which can prevent molten droplets from falling into the semi-solid molten pool and causing splashing.
[0088] Samples were taken at the head and tail of the ingot to detect the composition, and the results of gas content and active metal element content are shown in Table 3.
[0089] Table 3 FGH4095 powder high temperature alloy ingot composition test results (wt.%)
[0090]
[0091] It can be seen from Tables 1 to 3 that the content of gas impurity elements in the powder high-temperature alloy ingot obtained by using the device is significantly lower, and the burnout of active elements is not obvious.
[0092] Depend on Figure 3 , Figure 4 as well as Figure 5 It can be seen that the internal structure of the powder high-temperature alloy ingot prepared by the utility model is fine and uniform equiaxed crystals, and there are no obvious inclusions, pores and internal cracks.
[0093] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0094] It should be understood that the present invention is not limited to the above-described contents, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A device for preparing high-purity and high-uniformity powder high-temperature alloy ingots, characterized in that: The invention comprises a smelting chamber (1), wherein a plasma gun control system (2) is arranged on one side of the smelting chamber (1), and a driving mechanism (3) is arranged on the other side thereof, wherein the driving mechanism (3) is connected to an electrode rod (4) inserted into the smelting chamber (1) and arranged horizontally, and within the smelting chamber (1), a plasma flame generated by the plasma gun control system (2) melts the electrode rod (4) into liquid metal; A water-cooled copper crystallizer (5) is arranged inside the smelting chamber (1) and below the electrode rod (4); The top of the smelting chamber (1) is connected to a vacuum control system (6) via a vacuum pipeline, and a telescopic component (7) is installed at the bottom of the smelting chamber (1), one side of the telescopic component (7) extends into the interior of the smelting chamber (1) and contacts the bottom of the water-cooled copper crystallizer (5).
2. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 1, characterized in that: The plasma gun control system (2) comprises a control cabinet (21) and a gas storage assembly (23) arranged outside the smelting chamber (1), and a plasma gun (22) located inside the smelting chamber (1); The plasma gun (22) comprises a plasma gun cathode (222) and a plasma gun anode (221) arranged in a circumferential direction of the plasma gun cathode (222); a water cooling channel (2211) is arranged inside the plasma gun anode (221); the water cooling channel (2211) is connected to the control cabinet (21) via a cooling pipeline; the plasma gun cathode (222) is connected to the control cabinet (21) via a gas pipeline; the gas delivery pipe of the gas storage component (23) is connected to the gas pipeline and delivers Ar+He mixed gas to the plasma gun (22); The central axis of the plasma gun (22) and the electrode rod (4) are located on the same horizontal line.
3. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 2, characterized in that: The driving mechanism (3) comprises a push rod (31) and a first driving motor (32) connected thereto, and the push rod (31) is connected to the electrode rod (4).
4. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 1, characterized in that: It also comprises an oxygen content monitoring probe (8), wherein the oxygen content monitoring probe (8) is installed on the top of the smelting chamber (1).
5. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 1, characterized in that: The water-cooled copper crystallizer (5) is in the shape of a hollow cylinder, with a solidification chamber (51) opened axially at the center thereof, a cooling water channel (52) is arranged inside the water-cooled copper crystallizer (5) and on the outer periphery of the solidification chamber (51), a movable baffle (53) slidably connected to the inner wall of the water-cooled copper crystallizer (5) is arranged in the solidification chamber (51), the top of the movable baffle (53) is used to contain liquid metal generated by the electrode rod (4) during the melting process, the lower part of the cooling water channel (52) and located outside the smelting chamber (1) is connected to a water inlet (54) through a cooling pipe, and a water outlet (55) is arranged above the water inlet (54).
6. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 5, characterized in that: A first flow regulating valve (541) is provided on the cooling pipe between the water inlet (54) and the smelting chamber (1), and a second flow regulating valve (551) is provided on the cooling pipe between the water outlet (55) and the smelting chamber (1).
7. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 5, characterized in that: The telescopic assembly (7) comprises a telescopic rod (71) and a second drive motor (72) arranged outside the smelting chamber (1); one end of the telescopic rod (71) is connected to the transmission shaft of the second drive motor (72), and the other end extends into the smelting chamber (1) and contacts the bottom of the movable baffle (53); and a sealing assembly is arranged at the position where the telescopic rod (71) contacts the smelting chamber (1).
8. The device for preparing high-purity and high-uniformity powder high-temperature alloy ingot according to claim 7, characterized in that: The sealing assembly comprises a sleeve sleeved on the telescopic rod (71), a skeleton oil seal is arranged on the outer peripheral surface of the sleeve, a first insulating bushing is arranged on the top of the skeleton oil seal, a sealing ring is installed on the bottom of the skeleton oil seal, a second insulating bushing is arranged on the bottom of the sealing ring, a first sealing cover is arranged on the upper surface of the sleeve, located above the first insulating bushing, and a second sealing cover is arranged on the lower surface of the sleeve, located below the second insulating bushing.