Hot working die
By adjusting the thickness and aperture of the composite layer in the hot-working mold to match the curvature of the curved glass, the defects and cracking problems in the curved glass forming process were solved, improving product yield and mold life.
Patent Information
- Application Number
- CN202522471421.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2035-11-20
AI Technical Summary
Curved glass is prone to defects and cracks during the forming process, resulting in a low yield rate. Existing hot processing molds are prone to deformation or cracking under high temperature and high load conditions, affecting product quality and service life.
Design a thermal processing mold that, by adjusting the thickness and aperture of the composite layer to match the curvature of curved glass, enhances the mold's wear resistance and thermal shock resistance, and reduces stress concentration and deformation, by having the thickness of the composite layer in the mold be positively correlated with the bending angle of the forming surface.
It improves the molding yield of curved glass, reduces defects and cracks, extends the service life of molds, and enhances the overall strength and wear resistance of molds.
Smart Images

Figure CN224954529U_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of mold manufacturing technology, and more particularly to a heat treatment mold. Background Technology
[0002] As consumer electronics products trend towards thinner, lighter, and more curved designs, curved components have become core components of high-end electronic devices due to their aesthetic appeal and ergonomic design advantages. Curved components include curved glass, such as smartwatch covers and mobile phone screens. Curved glass is typically formed by pressing flat glass under high temperature and pressure.
[0003] However, curved glass is prone to defects and cracks during the forming process, resulting in a low yield rate. Utility Model Content
[0004] This application provides a thermal processing mold to achieve a high yield rate for curved glass.
[0005] This application provides a heat treatment mold, including at least one mold core, wherein the at least one mold core has a forming surface, and the mold core includes:
[0006] Matrix;
[0007] A composite layer covers at least a portion of the surface of the substrate, forming at least a portion of the shaped surface, wherein the thickness of the composite layer is positively correlated with the bending angle of the shaped surface.
[0008] In some possible implementations, the forming surface includes:
[0009] end face,
[0010] The side surface surrounds the end face and has an arc segment connected to the end face. The angle between the end of the arc segment away from the end face and the end face forms the bending angle.
[0011] In some possible implementations, the thickness of the composite layer corresponding to the side face is greater than the thickness of the composite layer corresponding to the end face.
[0012] In some possible implementations, the thickness of the composite layer is monotonically positively correlated with the bending angle of the molded surface.
[0013] In some possible implementations, the thickness of the composite layer is greater than or equal to 0.05 mm and less than or equal to 3 mm.
[0014] In some possible implementations, when the bending angle is greater than or equal to 0° and less than 30°, the thickness of the composite layer is When the bending angle is greater than or equal to 30° and less than 45°, the thickness of the composite layer is: When the bending angle is greater than or equal to 45° and less than 60°, the thickness of the composite layer is: When the bending angle is greater than or equal to 60° and less than 75°, the thickness of the composite layer is: When the bending angle is greater than or equal to 75° and less than or equal to 90°, the thickness of the composite layer is: ;
[0015] The , , , , It satisfies the following formula:
[0016] ;
[0017] ;
[0018] ;
[0019] ;
[0020] .
[0021] In some possible implementations, the aperture of the composite layer is negatively correlated with the bending angle of the shaped surface.
[0022] In some possible implementations, the pore size of the composite layer is greater than or equal to 0.2 μm and less than or equal to 30 μm.
[0023] In some possible implementations, when the bending angle is greater than or equal to 0° and less than 30°, the pore size of the composite layer is... When the bending angle is greater than or equal to 30° and less than 45°, the pore size of the composite layer is... When the bending angle is greater than or equal to 45° and less than 60°, the pore size of the composite layer is... When the bending angle is greater than or equal to 60° and less than 75°, the pore size of the composite layer is... When the bending angle is greater than or equal to 75° and less than or equal to 90°, the pore size of the composite layer is... ;
[0024] The , , , , It satisfies the following formula:
[0025] ;
[0026] ;
[0027] ;
[0028] ;
[0029] .
[0030] In some possible implementations, the hardness of the composite layer is positively correlated with the bending angle of the molded surface.
[0031] In some possible implementations, the hardness of the composite layer is greater than or equal to 80 Hv and less than or equal to 2000 Hv.
[0032] In some possible implementations, when the bending angle is greater than or equal to 0° and less than 30°, the hardness of the composite layer is [value missing]. When the bending angle is greater than or equal to 30° and less than 45°, the hardness of the composite layer is: When the bending angle is greater than or equal to 45° and less than 60°, the hardness of the composite layer is... When the bending angle is greater than or equal to 60° and less than 75°, the hardness of the composite layer is: When the bending angle is greater than or equal to 75° and less than or equal to 90°, the hardness of the composite layer is... ;
[0033] The , , , , It satisfies the following formula:
[0034] ;
[0035] ;
[0036] ;
[0037] ;
[0038] .
[0039] In some possible implementations, the compressive strength of the composite layer is positively correlated with the thickness of the composite layer;
[0040] And / or, the compressive strength of the composite layer is greater than or equal to 90 MPa.
[0041] In some possible implementations, the at least one mold core includes a first mold core, the matrix of which comprises:
[0042] A protrusion is covered with the composite layer, and the protrusion and the corresponding composite layer form a core, the surface of which forms the corresponding molding surface.
[0043] In some possible implementations, the composite layer of the core comprises:
[0044] Planar part;
[0045] The sidewall portion has at least two, and the at least two sidewall portions are arranged circumferentially along the planar portion and connected to the planar portion;
[0046] The corner section connects two sidewall sections with different extending directions, and the sidewall section connects to the planar section.
[0047] In some possible implementations, the thickness of both the corner portion and the sidewall portion is greater than the thickness of the planar portion; and / or,
[0048] The apertures of the corner portion and the sidewall portion are both smaller than the aperture of the planar portion.
[0049] In some possible implementations, the thickness of the corner portion is greater than or equal to the thickness of the sidewall portion, and the thickness of the sidewall portion is greater than the thickness of the planar portion; and / or,
[0050] The diameter of the hole at the corner is less than or equal to the diameter of the hole in the sidewall portion, and the diameter of the hole in the sidewall portion is less than the diameter of the hole in the flat portion.
[0051] In some possible implementations, the at least one mold core further includes a second mold core, the matrix of which comprises:
[0052] A recessed portion, wherein the composite layer is covered within the recessed portion, and the composite layer within the recessed portion encloses and forms a cavity, and the surface of the cavity forms a corresponding molding surface;
[0053] The thickness of the composite layer within the recess is positively correlated with the bending angle of the corresponding molded surface.
[0054] In some possible implementations, the substrate is a graphite substrate, and the composite layer is a silicon carbide and graphite composite layer.
[0055] In some possible implementations, the composite layer forms an integral structure with the substrate.
[0056] The thermal processing mold provided in this application includes at least one mold core, which has a forming surface. The mold core includes a substrate and a composite layer. The composite layer covers at least a portion of the surface of the substrate, forming at least a portion of the forming surface. The thickness of the composite layer is positively correlated with the curvature angle of the forming surface. The thickness of the composite layer is adjusted according to the curvature angle of the forming surface, as well as the thickness of different regions of the composite layer. The thicker the composite layer, the better its density, oxidation resistance, hardness, and wear resistance. It can withstand greater thermo-mechanical stress, improving local strength and wear resistance. The thickness of the composite layer is adapted to the curvature of the forming surface, thereby adapting the thickness of the composite layer to the curvature of the formed curved glass. This reduces stress concentration and large deformation at high curvature positions under thermo-mechanical coupling cyclic conditions, which can lead to glass defects and cracks, ensuring product yield. Furthermore, it can improve the overall strength, wear resistance, and thermal shock resistance of the mold, extending its service life. Attached Figure Description
[0057] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0058] Figure 1 A schematic diagram of the heat treatment mold provided in this application;
[0059] Figure 2 A schematic diagram of the first mold core provided for this application;
[0060] Figure 3 A schematic diagram of the core provided in this application;
[0061] Figure 4 Top view of the core provided in this application;
[0062] Figure 5 A schematic diagram of the second mold core provided in this application.
[0063] Explanation of reference numerals in the attached figures:
[0064] 10-First mold kernel;
[0065] 11-Protrusion;
[0066] 12-First substrate;
[0067] 13-First circumferential section;
[0068] 14-Second circumferential section;
[0069] 15 - Air outlet;
[0070] 16-Core;
[0071] 20 - Second mold kernel;
[0072] 21-Depression;
[0073] 22-Second substrate;
[0074] 23-First groove;
[0075] 24 - Second groove;
[0076] 30-Flat glass;
[0077] 40-Composite layer;
[0078] 41-Flat section;
[0079] 42-Side wall portion;
[0080] 43 - Corner.
[0081] The accompanying drawings illustrate specific embodiments of this application, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the concept in any way, but rather to illustrate the concept of this application to those skilled in the art through reference to particular embodiments. Detailed Implementation
[0082] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims.
[0083] Curved components are typically formed by hot bending, meaning they can be manufactured using hot-working molds. For example, 3D curved glass often uses hot-working molds made of homogeneous graphite material. However, during the manufacturing process, cracks are prone to appear in the high-curvature areas at the four corners of the curved glass. These cracks often propagate from the corners towards the center, rendering the finished product unusable. Furthermore, the hot-working mold operates under cyclical conditions of high temperature and high load, causing deformation or cracking in some areas, shortening its lifespan, and increasing the thickness and curvature error of the curved glass, thus affecting optical quality.
[0084] When hot-pressing 3D curved glass, the hot-processing mold exhibited cracks at the four corners, pits on the curved glass surface, and a low yield rate. Analysis revealed that the cause was that the sidewalls, bottom, and four corners experienced different heating and stress conditions during the hot-pressing process. Using the same material resulted in a large thermal gradient and localized stress concentration, leading to significant deformation in the sidewalls and corners with greater curvature. Under cyclic thermo-mechanical loading, these structural defects were amplified, ultimately resulting in defects, cracks, and mold warping in the curved glass.
[0085] The thermal processing mold provided in this application adjusts the thickness of the composite layer and the thickness of different areas of the composite layer according to the curvature of the forming surface, so that the thickness of the composite layer can be adapted to the curvature of the formed curved glass. This reduces stress concentration and large deformation of the mold at high curvature positions under thermo-mechanical coupling cycle conditions, which can lead to glass defects and cracks, and ensure product yield.
[0086] The technical solution of this application and how the technical solution of this application solves the above-mentioned technical problems are described in detail below with specific embodiments. These specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described again in some embodiments. The embodiments of this application will now be described with reference to the accompanying drawings.
[0087] See Figures 1 to 5 This application provides a hot working mold, which can be, for example, a hot bending mold. The hot working mold includes at least one mold core, the at least one mold core having a forming surface, the mold core including a substrate and a composite layer 40; the composite layer 40 covers at least a portion of the surface of the substrate, forming at least a portion of the forming surface, and the thickness of the composite layer 40 is positively correlated with the bending angle of the forming surface. Exemplarily, the hot working mold includes one mold core, two or more mold cores, wherein some or all of the mold cores include a substrate and a composite layer 40.
[0088] The thickness of the composite layer 40 is adjusted according to the curvature angle of the forming surface; a thicker composite layer 40 corresponds to a forming surface with high curvature, and a thinner composite layer 40 corresponds to a forming surface with low curvature. A thicker composite layer 40 has better density, oxidation resistance, hardness, and wear resistance, and can withstand greater thermo-mechanical stress, improving local strength and wear resistance. The thickness of the composite layer 40 is matched to the curvature of the forming surface, thus adapting the thickness of the composite layer 40 to the degree of curvature of the formed curved component (e.g., curved glass). This allows for adjustment of the thickness of the composite layer 40 according to the curvature of different curved glass surfaces, and also adjusts the thickness of the composite layer 40 in different areas. This reduces stress concentration and large deformation in high-curvature locations under thermo-mechanical coupling cyclic conditions, thus reducing glass defects and cracking, ensuring product yield. Furthermore, it improves the overall strength, wear resistance, and thermal shock resistance of the mold, extending its service life.
[0089] The composite layer 40 covers at least one surface of the substrate, for example, the composite layer 40 covers all or part of the surface of the substrate. The composite layer 40 also forms at least a portion of the molding surface, for example, the composite layer 40 forms all or part of the molding surface, and the thickness of the composite layer 40 is positively correlated with the curvature angle of the molding surface. For example, the composite layer 40 covers the entire surface of the substrate and forms all the molding surfaces. Thus, by adjusting the thickness of the composite layer 40 so that its thickness changes in the same direction as the curvature angle of the partial molding surface, i.e., in the same direction as the curvature of the curved glass, the wear resistance and thermal gradient of the molding surface can be adjusted, ensuring the molding quality of the product.
[0090] The forming surface includes an end face and a side face. The side face surrounds the end face and has an arc segment that connects to the end face. The angle between the end of the arc segment furthest from the end face and the end face forms a bending angle. The end face is flat, and the side face surrounds the entire end face. The side face includes an arc segment, and the transition between the arc segment and the end face is smooth; that is, the end of the side face connecting to the end face is the arc segment. The angle between the end of the arc segment furthest from the end face and the end face forms a bending angle. Therefore, the bending angle of the forming surface refers to the bending angle of the arc segment portion of the side face. Figure 3 As shown in Figure a, the bending angle is specifically the angle between the tangent at the end of the arc segment furthest from the end face and the end face.
[0091] In some possible examples, the sides are all curved segments, meaning the sides form curved surfaces. In other possible examples, the sides also include straight segments that connect to the ends of the curved segments away from the end face, and the curvature angle of the straight segments is zero.
[0092] In some possible examples, the composite layer 40 forms the molded surface, and the thickness of the composite layer 40 corresponding to the side surface is greater than the thickness of the composite layer 40 corresponding to the end surface. The curvature of the arc segment of the sidewall is often larger, which matches the curvature of the curved glass. The thickness of the composite layer 40 corresponding to the end surface is smaller, and the thickness of the composite layer 40 corresponding to the side surface is larger, so that the composite layer 40 corresponding to the side with a greater curvature is denser, harder, and more wear-resistant. This can better match the curvature of different curved glass, reduce stress concentration, deformation, and thermal gradient of the composite layer 40, thereby reducing defects and cracks in the curved glass.
[0093] Among them, the composite layer 40 corresponding to the end face has the same thickness, that is, the thickness of the composite layer 40 at different positions on the end face is the same. The composite layer 40 corresponding to the side face also has the same thickness, that is, the thickness of the composite layer 40 at different positions on the side face is the same. For example, the thickness of the composite layer 40 corresponding to the arc segment is the same as the thickness of the composite layer 40 corresponding to the straight segment, so as to facilitate the formation of the composite layer 40.
[0094] In some possible examples, the thickness of the composite layer 40 exhibits a monotonically positive correlation with the bending angle of the forming surface, meaning the thickness of the composite layer 40 increases piecewise as a constant, in a stepwise manner. The bending angle of the forming surface can be discretized into multiple intervals, with the thickness of the composite layer 40 remaining constant within each interval. As the interval increases, the thickness of the composite layer 40 also increases. This simplifies the selection of the thickness of the composite layer 40, facilitating its fabrication.
[0095] In some possible examples, the thickness of the composite layer 40 is greater than or equal to 0.05 mm and less than or equal to 3 mm. This allows for adaptation to a wider range of bending angles and flexible adjustment of the thickness of different areas of the composite layer 40. The synergistic effect of the wear resistance of the composite layer 40 and the thermal conductivity of the substrate enhances the stability and reliability of the mold in the forming of curved glass. For example, the thickness of the composite layer 40 can be any value from 0.05 mm, 0.1 mm, 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, and 3 mm, or any combination thereof.
[0096] Based on the above example, in some possible implementations, when the bending angle is greater than or equal to 0° and less than 30°, the thickness of the composite layer 40 is... When the bending angle is greater than or equal to 30° and less than 45°, the thickness of composite layer 40 is... When the bending angle is greater than or equal to 45° and less than 60°, the thickness of composite layer 40 is... When the bending angle is greater than or equal to 60° and less than 75°, the thickness of composite layer 40 is... When the bending angle is greater than or equal to 75° and less than or equal to 90°, the thickness of composite layer 40 is... ; , , , , It satisfies the following formula:
[0097] ;
[0098] ;
[0099] ;
[0100] ;
[0101] .
[0102] For example, It is 0.8mm. It is 1.2mm. It is 1.6mm. It is 2mm. The thickness is 2.5mm. With this setting, different bending angles of the forming surface correspond to different curvatures of the curved glass. As the curvature of the curved glass increases, the thickness of the composite layer 40 increases, and it is segmented and matched. On the one hand, increasing the thickness of the composite layer 40 can improve strength and wear resistance, alleviate stress concentration in thermal cycling, and avoid the formation and propagation of cracks. On the other hand, dividing the space into sections reduces the complexity of the composite layer 40 and simplifies the mold.
[0103] In some possible examples, the pore size of the composite layer 40 is negatively correlated with the curvature angle of the forming surface. The composite layer 40 has micropores; the smaller the pore size, the better the compactness, oxidation resistance, hardness, and wear resistance of the composite layer 40. Determining the pore size according to the curvature of different curved glass surfaces can reduce stress concentration, deformation, and thermal gradients in the mold at high curvature locations under thermo-mechanical coupling cyclic conditions, thereby reducing defects and cracks in curved glass. It can also improve the overall strength, wear resistance, and thermal shock resistance of the mold, extending its service life.
[0104] In some possible examples, the pore size of the composite layer 40 is greater than or equal to 0.2 μm and less than or equal to 30 μm. This allows for adaptation to a wider range of bending angles and flexible adjustment of the pore size in different regions of the composite layer 40. The synergistic effect of the wear resistance of the composite layer 40 and the thermal conductivity of the matrix enhances the stability and reliability of the mold in the forming of curved glass. Furthermore, the pore size of the composite layer 40 can coordinate with its thickness, jointly regulating the mold's performance and reducing defects and cracking in curved glass. For example, the pore size of the composite layer 40 can be any value from 0.2 μm, 0.5 μm, 0.75 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 25 μm, and 30 μm, or any combination of both.
[0105] Based on the above example, in some possible implementations, when the bending angle is greater than or equal to 0° and less than 30°, the aperture of the composite layer 40 is... When the bending angle is greater than or equal to 30° and less than 45°, the pore size of composite layer 40 is... When the bending angle is greater than or equal to 45° and less than 60°, the pore size of composite layer 40 is... When the bending angle is greater than or equal to 60° and less than 75°, the pore size of composite layer 40 is... When the bending angle is greater than or equal to 75° and less than or equal to 90°, the pore size of composite layer 40 is... ; , , , , It satisfies the following formula:
[0106] ;
[0107] ;
[0108] ;
[0109] ;
[0110] .
[0111] For example, for , for , for , for , for With this configuration, different bending angles of the forming surface correspond to different curvatures of the curved glass. As the curvature of the curved glass increases, the aperture of the composite layer 40 decreases and is segmented and matched. On the one hand, reducing the aperture of the composite layer 40 can improve strength and wear resistance, alleviate stress concentration during thermal cycling, and prevent the formation and propagation of cracks. On the other hand, dividing the space into sections reduces the complexity of the composite layer 40 and simplifies the mold.
[0112] In some possible examples, the hardness of composite layer 40 is positively correlated with the curvature angle of the forming surface. Higher hardness of composite layer 40 results in better wear resistance. Determining the hardness based on the curvature of different curved glass surfaces can reduce stress concentration, deformation, and thermal gradients in the mold at high curvature locations under thermo-mechanical coupling cyclic conditions, thereby reducing defects and cracks in curved glass. Furthermore, it can improve the overall strength, wear resistance, and thermal shock resistance of the mold, extending its service life.
[0113] In some possible examples, the hardness of composite layer 40 is greater than or equal to 80 Hv and less than or equal to 2000 Hv. This allows for adaptation to a wider range of bending angles and flexible adjustment of the hardness in different areas of composite layer 40. The synergistic effect of the wear resistance of composite layer 40 and the thermal conductivity of the matrix enhances the stability and reliability of the mold in curved glass forming. The thickness of composite layer 40 can be achieved by adjusting its pore size and thickness, or by adjusting its material. For example, the hardness of composite layer 40 can be any value from 80 Hv, 100 Hv, 200 Hv, 300 Hv, 400 Hv, 500 Hv, 600 Hv, 700 Hv, 800 Hv, 900 Hv, 1000 Hv, 1200 Hv, 1400 Hv, 1600 Hv, 1800 Hv, and 2000 Hv, or any combination thereof.
[0114] Based on the above example, in some possible implementations, when the bending angle is greater than or equal to 0° and less than 30°, the hardness of composite layer 40 is... When the bending angle is greater than or equal to 30° and less than 45°, the hardness of composite layer 40 is... When the bending angle is greater than or equal to 45° and less than 60°, the hardness of composite layer 40 is... When the bending angle is greater than or equal to 60° and less than 75°, the hardness of composite layer 40 is... When the bending angle is greater than or equal to 75° and less than or equal to 90°, the hardness of composite layer 40 is... ; , , , , It satisfies the following formula:
[0115] ;
[0116] ;
[0117] ;
[0118] ;
[0119] .
[0120] For example, 100 Hv 150 Hv 200 Hv 300 Hv The value is 500 Hv. With this setting, the different bending angles of the sidewalls of the core 16 correspond to the different curvatures of the curved glass. As the curvature of the curved glass increases, the hardness of the composite layer 40 increases, and the segmented matching can improve wear resistance by increasing the hardness of the composite layer 40, alleviate stress concentration in thermal cycling, and avoid the formation and propagation of cracks. On the other hand, by dividing the segments, the complexity of the composite layer 40 is reduced, and the mold is simplified.
[0121] In some possible examples, the compressive strength of composite layer 40 is positively correlated with its thickness, and / or, the compressive strength of composite layer 40 is greater than or equal to 90 MPa. This ensures that composite layer 40 can withstand mold closing pressure, guaranteeing dimensional accuracy and shape stability, while also ensuring the bonding strength between composite layer 40 and the substrate, preventing cracking, peeling, or wear of composite layer 40. The positive correlation between the thickness and compressive strength of composite layer 40 better protects the substrate and extends the mold's service life. For example, the compressive strength of composite layer 40 can be any value from 90 MPa, 100 MPa, 120 MPa, 150 MPa, 200 MPa, or any combination thereof.
[0122] In some possible examples, the substrate is a graphite matrix, which has good high-temperature stability, is easy to process, and has low cost. The composite layer 40 is a silicon carbide and graphite composite layer to obtain good thermal conductivity, thermal shock resistance, and oxidation resistance. The composite layer 40 and the substrate can form an integral structure. For example, the composite layer 40 can be formed by coating a silane coating on a graphite substrate and then reacting it at high temperature, utilizing the carbothermic reduction reaction between silicon dioxide and graphite, or utilizing the direct reaction between active silicon atoms and carbon to achieve a strong bond between the two phases at the microscale.
[0123] Based on the above possible examples, the preparation process of the mold core can specifically be as follows:
[0124] A graphite matrix is selected, with a porosity greater than or equal to 5% and less than or equal to 20%, and a pore size greater than or equal to 2μm and less than or equal to 50μm.
[0125] Prepare a silane slurry with a concentration greater than or equal to 20% and less than or equal to 50%. For example, it can be prepared by mixing a silane coupling agent (such as methyltrimethoxysilane, tetraethyl orthosilicate, etc.) with a solvent (such as ethanol, isopropanol) in a certain proportion.
[0126] A silane slurry is coated onto the surface of a graphite substrate and dried in an oven at 80°C–120°C. For example, the silane slurry can be directly brushed or sprayed onto the graphite surface. Drying allows for pre-curing / crosslinking, enabling the silanes to hydrolyze and condense, adhering firmly to the graphite surface. At this point, the silane slurry transforms into an amorphous silicon-containing oxide coating.
[0127] The dried graphite substrate is subjected to high-temperature heat treatment. For example, it is placed in a high-temperature vacuum furnace and held at 1500-1800℃ for 1-3 hours. The silicon dioxide in the coating reacts with the carbon on the surface of the graphite substrate at high temperature; or, the coating decomposes into silicon atoms at high temperature and reacts with the carbon on the surface of the graphite substrate directly to form a two-phase composite structure of graphite phase and silicon carbide phase (i.e., composite layer 40).
[0128] In some possible examples, at least one mold core includes a first mold core 10, which has a molding surface and includes a substrate and a composite layer 40 to improve the surface properties of the first mold core 10 and increase its service life. The substrate of the first mold core 10 includes a protrusion 11 covered with the composite layer 40, the protrusion 11 and the corresponding composite layer 40 forming a core 16, and the surface of the core 16 forming a corresponding molding surface.
[0129] The composite layer 40 covers the outer surface of the protrusion 11, for example, the entire outer surface of the protrusion 11. The protrusion 11 and the corresponding composite layer 40 on the protrusion 11 form a core 16. The outer surface of the core 16 forms a corresponding molding surface. That is, the composite layer 40 serves as the outer layer of the core 16, and its surface facing away from the protrusion 11 forms a corresponding molding surface to correspond to the inner surface of the molded curved glass.
[0130] The base of the first mold core 10 also includes a first substrate 12, a first surrounding portion 13, and a second surrounding portion 14. The first surrounding portion 13, the second surrounding portion 14, and the protrusion 11 are located on the same side of the first substrate 12. Along a direction away from the protrusion 11, the second surrounding portion 14 and the first surrounding portion 13 are sequentially fitted together, i.e., the first surrounding portion 13 is fitted onto the protrusion 11, and the second surrounding portion 14 is fitted onto the first surrounding portion 13. The outer peripheral surface of the second surrounding portion 14 is also aligned with the outer peripheral surface of the first substrate 12. The first surrounding portion 13 and the second surrounding portion 14 can be used for positioning. The surfaces of the first surrounding portion 13, the second surrounding portion 14, and the first substrate 12 can all be covered with a composite layer 40. This can improve the oxidation resistance and surface hardness of the hot-working mold, enhance its thermal shock resistance, prevent surface wear from repeated use, avoid fitting errors, and extend the service life of the hot-working mold.
[0131] Grooves are formed between the first surrounding portion 13 and the protrusion 11, and between the second surrounding portion 14 and the first surrounding portion 13. The shapes of the first surrounding portion 13, the second surrounding portion 14, and the protrusion 11 are matched, for example, all are rectangular. Figure 2As shown, both the first surrounding portion 13 and the second surrounding portion 14 are rounded rectangular rings, and the protrusion 11 is a rounded rectangular block. The first surrounding portion 13, the second surrounding portion 14, the protrusion 11, and the first substrate 12 can be an integral structure. The surface of the first surrounding portion 13 facing away from the first substrate 12 is also provided with an air outlet groove 15, which extends in a direction away from the protrusion 11.
[0132] In some possible examples, at least one die core includes a second die core 20, which has a molding surface and includes a matrix and a composite layer 40 to improve the surface properties of the second die core 20 and increase its service life. The second die core 20 is opposite to and adapted to the first die core 10, which is a punch and the second die core 20 is a die.
[0133] The second mold core 20 and the first mold core 10 can be joined together or separated. After the first mold core 10 and the second mold core 20 are joined together, there is a gap between the forming surface of the first mold core 10 and the forming surface of the second mold core 20 to accommodate the thickness of the curved glass. Figure 1 As shown, the flat glass 30 is located between the first mold core 10 and the second mold core 20, and is formed by pressing through the forming surfaces of the first mold core 10 and the second mold core 20 after the first mold core 10 and the second mold core 20 are assembled.
[0134] In some possible examples, the substrate in the second mold core 20 includes a recess 21, which is covered with a composite layer 40. The composite layer 40 within the recess 21 encloses a cavity, and the surface of the cavity forms a corresponding molding surface to correspond to the outer surface of the molded curved glass. The molding surface of the second mold core 20 and the molding surface of the first mold core 10 can be opposite and parallel, and their bending angles are consistent.
[0135] The composite layer 40 covers the inner surface of the recess 21, for example, the entire inner surface of the recess 21, to improve the oxidation resistance and surface hardness of the heat-working mold, enhance its thermal shock resistance, prevent surface wear from repeated use, avoid fitting errors, and extend the service life of the heat-working mold. The composite layer 40 within the recess 21 encloses a cavity to accommodate the core 16. The inner surface of the cavity forms a corresponding molding surface, i.e., the surface of the composite layer 40 facing away from the recess 21 forms a corresponding molding surface.
[0136] The substrate of the second mold core 20 also includes a second substrate 22. A recess 21 is located on the surface of the second substrate 22, and a first groove 23 and a second groove 24 are formed on the surface of the second substrate 22. Along the direction away from the protrusion 11, the second groove 24 and the first groove 23 are sequentially fitted together, i.e., the first groove 23 is fitted onto the recess 21, and the second groove 24 is fitted onto the first groove 23. The second groove 24 also extends to the outer peripheral surface of the second substrate 22 to form an open structure. The first groove 23, the second groove 24, and the surface of the second substrate 22 can all be covered with a composite layer 40. This can improve the oxidation resistance and surface hardness of the hot-working mold, enhance its thermal shock resistance, prevent surface wear from repeated use, avoid fitting errors, and extend the service life of the hot-working mold.
[0137] The shapes of the second groove 24, the first groove 23, and the recess 21 are adapted to each other, for example, they are all rectangular. Figure 5 As shown, both the first groove 23 and the second groove 24 are rounded rectangular annular grooves, and the recessed portion 21 is a rounded rectangular groove. The first groove 23 is used to accommodate the first surrounding portion 13, and the second groove 24 is used to accommodate the second surrounding portion 14, so that the first mold core 10 and the second mold core 20 can be positioned and aligned.
[0138] In some possible examples, the composite layer 40 of the core 16 includes: a planar portion 41, a sidewall portion 42, and a corner portion 43. The sidewall portion 42 has at least two sides, which are arranged circumferentially along the planar portion 41 and connected to the planar portion 41. The corner portion 43 connects two sidewall portions 42 with different extension directions, as well as the sidewall portion 42 and the planar portion 41.
[0139] The planar portion 41 is flat and corresponds to the effective area (center zone) of the curved glass, forming the end face of the corresponding molding surface. At least two sidewall portions 42 are located at the edges of the planar portion 41 and are arranged circumferentially along the planar portion 41. A corner portion 43 connects the two sidewall portions 42 with different extending directions, as well as the sidewall portions 42 and the planar portion 41. The surfaces of the sidewall portions 42 and the corner portion 43 correspond to the side surfaces of the molding surface. For example, there are four sidewall portions 42 and four corner portions 43.
[0140] The curvature of the corner portion 43 and the sidewall portion 42 is greater than that of the flat portion 41, and the curvature angle of the flat portion 41 is zero. The curvature of the corner portion 43 can be greater than that of the sidewall portion 42, or it can be equal to the curvature of the flatness. Among them, part of the surface of the sidewall portion 42 can be flat, and another part of the surface can be curved, and the surface of the corner portion 43 can be entirely curved.
[0141] In some possible examples, the thickness of both the corner portion 43 and the sidewall portion 42 is greater than the thickness of the planar portion 41; and / or, the aperture of both the corner portion 43 and the sidewall portion 42 is smaller than the aperture of the planar portion 41. The bending angle of the corner portion 43 and the sidewall portion 42 is often large, i.e., the curvature is large. The thickness and / or aperture of the composite layer 40 vary in different zones. The composite layer 40 in the high curvature region can withstand greater thermo-mechanical stress, improving local strength and wear resistance; the composite layer 40 in the low curvature region can reduce material costs and processing difficulty.
[0142] The thickness of the corner portion 43 and the sidewall portion 42 is greater than the thickness of the flat portion 41. The thicknesses of the corner portion 43 and the sidewall portion 42 can be equal or unequal. For example, the thickness of the corner portion 43 is greater than or equal to the thickness of the sidewall portion 42, and the thickness of the sidewall portion 42 is greater than the thickness of the flat portion 41. This can effectively reduce stress concentration, deformation, and thermal gradient of the composite layer 40, thereby reducing defects and cracks in the curved glass.
[0143] The apertures of both the corner portion 43 and the sidewall portion 42 are smaller than the aperture of the flat portion 41. The apertures of the corner portion 43 and the sidewall portion 42 can be equal or unequal. For example, the aperture of the corner portion 43 can be smaller than or equal to the aperture of the sidewall portion 42, and the aperture of the sidewall portion 42 can be smaller than the aperture of the flat portion 41. This effectively reduces stress concentration, deformation, and thermal gradient in the composite layer 40, thereby reducing defects and cracking in the curved glass.
[0144] The present application will be further described below through specific embodiments.
[0145] Example 1
[0146] The bending angle of the sides of the molded surface (i.e., sidewall portion 42 and corner portion 43) is 15°. The thickness of corner portion 43 is 0.75 mm, the aperture is 20 μm, and the hardness is 150 Hv. The thickness of sidewall portion 42 is 0.5 mm, the aperture is 25 μm, and the hardness is 118 Hv. The thickness of flat portion 41 is 0.3 mm, the aperture is 30 μm, and the hardness is 83 Hv.
[0147] Example 2
[0148] The bending angle of the side surface in the forming surface is 30°, the thickness of the corner part 43 is 1mm, the pore diameter is 15μm, and the hardness is 297Hv; the thickness of the side wall part 42 is 0.75mm, the pore diameter is 20μm, and the hardness is 146Hv; the thickness of the flat part 41 is 0.5mm, the pore diameter is 25μm, and the hardness is 121Hv.
[0149] Example 3
[0150] The side bending angle of the molded surface is 45°. The thickness of the corner part 43 is 1.5 mm, the pore diameter is 10 μm, and the hardness is 387 Hv. The thickness of the side wall part 42 is 1 mm, the pore diameter is 15 μm, and the hardness is 259 Hv. The thickness of the flat part 41 is 0.75 mm, the pore diameter is 20 μm, and the hardness is 139 Hv.
[0151] Example 4
[0152] The bending angle of the side surface in the forming surface is 60°. The thickness of the corner part 43 is 1.8 mm, the pore diameter is 5 μm, and the hardness is 680 Hv. The thickness of the side wall part 42 is 1.3 mm, the pore diameter is 10 μm, and the hardness is 472 Hv. The thickness of the flat part 41 is 1 mm, the pore diameter is 15 μm, and the hardness is 351 Hv.
[0153] Example 5
[0154] The side bending angle of the molded surface is 75°, the thickness of the corner part 43 is 2mm, the pore diameter is 2μm, and the hardness is 1288Hv; the thickness of the side wall part 42 is 1.5mm, the pore diameter is 5μm, and the hardness is 953Hv; the thickness of the flat part 41 is 1.2mm, the pore diameter is 10μm, and the hardness is 627Hv.
[0155] Example 6
[0156] The side bending angle of the molded surface is 90°. The thickness of the corner part 43 is 2.5 mm, the pore diameter is 0.5 μm, and the hardness is 1801 Hv. The thickness of the side wall part 42 is 2 mm, the pore diameter is 2 μm, and the hardness is 1402 Hv. The thickness of the flat part 41 is 1.5 mm, the pore diameter is 5 μm, and the hardness is 627 Hv.
[0157] Comparative Example 1
[0158] The bending angle of the side surface in the molding surface is 15°, the thickness of the composite layer 40 is consistently 0.5 mm, the pore size is consistently 25 μm, and the hardness is consistently 118 Hv.
[0159] Comparative Example 2
[0160] The bending angle of the side surface in the molding surface is 30°, the thickness of the composite layer 40 is consistently 0.75 mm, the pore size is consistently 20 μm, and the hardness is consistently 146 Hv.
[0161] Comparative Example 3
[0162] The bending angle of the side surface in the molding surface is 45°, the thickness of the composite layer 40 is 1mm, the pore size is 15μm, and the hardness is 259Hv.
[0163] Comparative Example 4
[0164] The bending angle of the side surface in the molding surface is 60°, the thickness of the composite layer 40 is 1.3mm, the pore size is 10μm, and the hardness is 472Hv.
[0165] Comparative Example 5
[0166] The bending angle of the side surface in the molding is 75°, the thickness of the composite layer 40 is consistently 1.5 mm, the pore size is consistently 5 μm, and the hardness is consistently 923 Hv.
[0167] Comparative Example 6
[0168] The bending angle of the side surface in the molding surface is 90°, the thickness of the composite layer 40 is 2mm, the pore size is 2μm, and the hardness is 1452Hv.
[0169] The hot-processing molds of Examples 1-6 and Comparative Examples 1-6 were tested, specifically measuring the number of thermal cycles, yield, and oxidation resistance.
[0170] The thermal cycling number refers to the number of times the sample is heated to 750°C and 0.8 MPa in a muffle furnace, then hot-bent to form a curved surface for exposure, and cycled several times until pits appear on the curved glass surface.
[0171] The yield rate refers to the number of curved glass pieces without quality problems and the number of times the glass is hot-bent.
[0172] Antioxidant properties are defined as follows: placing a hot-processed mold in a 700℃ high-temperature oven for 6 hours and measuring the difference in its mass before and after.
[0173] The test results are shown in Table 1:
[0174] Table 1
[0175] As can be seen from the above Examples 1 to 6 and Comparative Examples 1 to 6, by setting composite layers 40 of different thicknesses according to different degrees of curvature, stress uniformity can be achieved during thermal cycling, stress concentration no longer occurs in areas with large curvature, the oxidation resistance of the thermal processing mold is good, the yield of the formed curved glass is high, the number of thermal cycles is high, and the performance is good.
[0176] The thermal processing mold provided in this application includes at least one mold core, which has a forming surface. The mold core includes a substrate and a composite layer 40. The composite layer 40 covers at least a portion of the surface of the substrate, forming at least a portion of the forming surface. The thickness of the composite layer 40 is positively correlated with the curvature angle of the forming surface. The thickness of the composite layer 40 is adjusted according to the curvature angle of the forming surface, as well as the thickness of different regions of the composite layer 40. The thicker the composite layer 40, the better its density, oxidation resistance, hardness, and wear resistance. It can withstand greater thermo-mechanical stress, improving local strength and wear resistance. The thickness of the composite layer 40 is adapted to the curvature of the forming surface, thus adapting the thickness of the composite layer 40 to the curvature of the formed curved glass. This reduces stress concentration and large deformation at high curvature positions under thermo-mechanical coupling cyclic conditions, preventing glass defects and cracking, and ensuring product yield. Furthermore, it can improve the overall strength, wear resistance, and thermal shock resistance of the mold, extending its service life.
[0177] The embodiments or implementation methods described in this specification are presented in a progressive manner. Each embodiment focuses on the differences from other embodiments, and the same or similar parts between embodiments can be referred to accordingly. All directional indications (such as up, down, left, right, front, back, etc.) in the embodiments of this specification are only used to explain the relative positional relationships and motion relationships between components in a specific posture (as shown in the attached figure). If the specific posture changes, the directional indications will also change accordingly.
[0178] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with an embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0179] It should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, an indirect connection via an intermediate medium, or the internal connection or interaction between two components. Those skilled in the art can understand the specific meaning of these terms in the embodiments of this application based on the specific circumstances. The terms "first," "second," "third," etc. (if present) are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.
[0180] Finally, it should be noted that other embodiments of this utility model will readily conceive of by those skilled in the art upon consideration of the specification and practice of the utility model disclosed herein. This utility model is intended to cover any variations, uses, or adaptations of this utility model that follow the general principles of this utility model and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of this utility model is limited only by the appended claims.
Claims
1. A hot working die characterized by, The mold core includes at least one mold core, at least one of the mold cores has a forming surface, the mold core includes: a base body; a composite layer (40) covering at least part of the surface of the base body, forming at least part of the forming surface, the thickness of the composite layer (40) is positively correlated with the bending angle of the forming surface.
2. The hot working die of claim 1 wherein, The forming surface includes: an end surface, a side surface surrounding the end surface, the side surface has an arc segment connected with the end surface, and the included angle between the end of the arc segment away from the end surface and the end surface forms the bending angle.
3. The hot working die of claim 2 wherein, The thickness of the composite layer (40) corresponding to the side surface is greater than the thickness of the composite layer (40) corresponding to the end surface.
4. The hot working die of claim 1 wherein, The thickness of the composite layer (40) is monotonously positively correlated with the bending angle of the forming surface in a binned manner.
5. The hot working die according to any one of claims 1 to 4, wherein The thickness of the composite layer (40) is greater than or equal to 0.05mm and less than or equal to 3mm.
6. The hot working die of any of claims 1-4, wherein, when the bending angle is greater than or equal to 0° and less than 30°, the thickness of the composite layer (40) is ; when the bending angle is greater than or equal to 30° and less than 45°, the thickness of the composite layer (40) is ; when the bending angle is greater than or equal to 45° and less than 60°, the thickness of the composite layer (40) is ; when the bending angle is greater than or equal to 60° and less than 75°, the thickness of the composite layer (40) is ; when the bending angle is greater than or equal to 75° and less than or equal to 90°, the thickness of the composite layer (40) is ; The , , , , , satisfy the following equation: ; ; ; ; 。 7. The hot working die of any of claims 1-4, wherein, The pore size of the composite layer (40) is negatively correlated with the bending angle of the forming surface.
8. The hot working die of claim 7 wherein, The pore size of the composite layer (40) is greater than or equal to 0.2μm and less than or equal to 30μm.
9. The hot working die of claim 7 wherein, when the bending angle is greater than or equal to 0° and less than 30°, the aperture of the composite layer (40) is ; when the bending angle is greater than or equal to 30° and less than 45°, the aperture of the composite layer (40) is ; when the bending angle is greater than or equal to 45° and less than 60°, the aperture of the composite layer (40) is ; when the bending angle is greater than or equal to 60° and less than 75°, the aperture of the composite layer (40) is ; when the bending angle is greater than or equal to 75° and less than or equal to 90°, the aperture of the composite layer (40) is ; The , , , , , satisfy the following equation: ; ; ; ; 。 10. The hot working die of any one of claims 1-4, wherein, The hardness of the composite layer (40) is positively correlated with the bending angle of the forming surface.
11. The hot working die of claim 10 wherein, The hardness of the composite layer (40) is greater than or equal to 80Hv and less than or equal to 2000Hv.
12. The hot working die of claim 10 wherein, when the bending angle is greater than or equal to 0° and less than 30°, the hardness of the composite layer (40) is ; when the bending angle is greater than or equal to 30° and less than 45°, the hardness of the composite layer (40) is ; when the bending angle is greater than or equal to 45° and less than 60°, the hardness of the composite layer (40) is ; when the bending angle is greater than or equal to 60° and less than 75°, the hardness of the composite layer (40) is ; when the bending angle is greater than or equal to 75° and less than or equal to 90°, the hardness of the composite layer (40) is ; The , , , , , satisfy the following equation: ; ; ; ; 。 13. The hot working die of any of claims 1-4, wherein, The compressive strength of the composite layer (40) is positively correlated with the thickness of the composite layer (40); And / or, the compressive strength of the composite layer (40) is greater than or equal to 90Mpa.
14. The hot working die of any one of claims 1-4, wherein, The at least one mold core includes a first mold core (10), the base body of the first mold core (10) includes: a protruding part (11) on which the composite layer (40) is covered, the protruding part (11) and the corresponding composite layer (40) form a core body (16), and the surface of the core body (16) forms the corresponding forming surface.
15. The hot working die of claim 14 wherein, The composite layer (40) of the core body (16) includes: a flat part (41); a side wall part (42) having at least two, the at least two side wall parts (42) are arranged along the circumference of the flat part (41) and connected with the flat part (41); a corner part (43) connecting two side wall parts (42) with different extension directions, and the side wall part (42) and the flat part (41).
16. The hot working die of claim 15 wherein, The thickness of the corner part (43) and the side wall part (42) is greater than the thickness of the flat part (41); and / or, The pore size of the corner part (43) and the side wall part (42) is smaller than the pore size of the flat part (41).
17. The hot working die of claim 15 wherein, The thickness of the corner part (43) is greater than or equal to the thickness of the side wall part (42), and the thickness of the side wall part (42) is greater than the thickness of the flat part (41); and / or, The pore size of the corner part (43) is smaller than or equal to the pore size of the side wall part (42), and the pore size of the side wall part (42) is smaller than the pore size of the flat part (41).
18. The hot working die of claim 14 wherein, The at least one mold core further includes a second mold core (20), the base body of the second mold core (20) includes: A recessed portion (21) is covered with the composite layer (40), and the composite layer (40) in the recessed portion (21) forms a cavity, and the surface of the cavity forms the corresponding molding surface; The thickness of the composite layer (40) within the recess (21) is positively correlated with the bending angle of the corresponding molding surface.
19. The hot working die of any one of claims 1-4, wherein, The substrate is a graphite substrate, and the composite layer (40) is a silicon carbide and graphite composite layer.