A black shading reflective film and a black photovoltaic module
The multi-layered black shading and reflective film solves the problems of displacement and wrinkles in black photovoltaic modules during the lamination process, improving power generation efficiency and weather resistance, and ensuring the aesthetics and stable performance of the modules.
Patent Information
- Application Number
- CN202522561236.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-02
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2035-12-02
AI Technical Summary
In existing black photovoltaic modules, the black shading film is prone to shifting and wrinkling during the lamination process. The thickness of the busbars leads to visual unevenness, and the black coating is prone to aging and fading, affecting the performance and aesthetics of the modules.
The black reflective film with a multi-layer structure includes an adhesive layer, a black coating, a substrate layer, and a composite reflective layer. The adhesive layer ensures reliable bonding and prevents misalignment and wrinkles. The black coating is placed between the substrate layer and the composite reflective layer for protection. The composite reflective layer reflects light to improve power generation efficiency.
It improved production yield and automation, reduced optical loss, enhanced the weather resistance of materials, and ensured the stable performance and aesthetic durability of components in long-term humid and hot environments.
Smart Images

Figure CN224959975U_ABST
Abstract
Description
Technical Field
[0001] This utility model belongs to the field of photovoltaic technology and relates to a black shading reflective film and a black photovoltaic module. Background Technology
[0002] All-black or black monocrystalline modules are primarily used in applications with extremely high aesthetic requirements, particularly high-end residential rooftops, commercial and public buildings, and building-integrated photovoltaic (BIPV) projects. Black encapsulation and concealed grid technologies enable them to achieve a significant visual enhancement while maintaining excellent power generation performance. Although the price is typically slightly higher than traditional modules, their aesthetic value and potential property appreciation make them highly competitive in their target market. With the development of BIPV and the increasing aesthetic demands of consumers, the application scenarios for black photovoltaic modules will continue to expand.
[0003] Currently, the black appearance of black photovoltaic modules is mainly achieved through various black auxiliary materials, such as black solder strips, black busbars, black backsheets, and black shading films. The black shading film is typically manually applied directly above the busbars to shield them from the silver-white surface, achieving a uniform black appearance. However, manually applied black shading films often exhibit defects such as misalignment and wrinkles after lamination. The busbars themselves have a certain thickness, which can cause the film strip to have a higher center and lower edges, resulting in an undesirable appearance. Furthermore, manually applying the film strip and then removing the fixture from the module can easily cause scratches on the solar cells. In addition, this type of black shading film structure mainly consists of an EVA (ethylene-vinyl acetate copolymer) layer and a black coating. The black film strip may absorb some scattered light while shielding the metal electrodes, reducing the overall efficiency of the module. Simultaneously, the black coating is prone to aging and fading when exposed to humid and hot environments for extended periods, and micro-cracks can easily form at the interface with the metal electrodes, increasing resistance.
[0004] Therefore, how to avoid the risks associated with manual application, solve the visual unevenness caused by the thickness of the busbar, and improve the long-term weather resistance and light reflection efficiency of the black masking material are urgent technical challenges to be addressed. Utility Model Content
[0005] To address the shortcomings of existing technologies, the purpose of this invention is to provide a black shading and reflective film and a black photovoltaic module. This invention provides a multi-layered black shading and reflective film that effectively solves many problems caused by manual application of the black shading film, while also resolving the visual unevenness issue caused by the thickness of the busbars. Specifically, an adhesive layer ensures reliable bonding with the module structure, avoiding misalignment and wrinkles during lamination, thus improving production yield and automation. In particular, the highly reflective black coating absorbs almost no light, so light incident on the black coating is fully transmitted and reflected back to the front of the solar cell for utilization, thereby improving power generation efficiency while ensuring a uniform pure black appearance for the module. Furthermore, this multi-layered structure protects the easily aging black coating by placing it between the substrate layer and the composite reflective layer, greatly enhancing the material's weather resistance, preventing fading and interface degradation, and ensuring the module's stable performance and lasting aesthetic appeal under long-term humid and hot environments.
[0006] To achieve this objective, the present invention adopts the following technical solution:
[0007] In a first aspect, the present invention provides a black shielding reflective film, the black shielding reflective film comprising an adhesive layer, a black coating layer, a substrate layer and a composite reflective layer stacked sequentially.
[0008] The composite reflective layer includes a reflection angle adjustment layer near the substrate layer and a reflective layer conformally stacked with the reflection angle adjustment layer.
[0009] This invention provides a multi-layered black shading and reflective film, effectively solving many problems caused by manual application of the black shading film, and also addressing the visual unevenness caused by the thickness of the busbars. Specifically, an adhesive layer ensures reliable bonding with the module structure, avoiding misalignment and wrinkles during lamination, thus improving production yield and automation. In particular, the highly reflective black coating absorbs almost no light, so light illuminating the black coating is fully transparent and reflected back to the front of the solar cell via the reflective layer for utilization, thereby improving power generation efficiency while ensuring a uniform pure black appearance for the module. Furthermore, this multi-layered structure protects the easily aging black coating by placing it between the substrate layer and the composite reflective layer, greatly enhancing the material's weather resistance, preventing fading and interface degradation, and ensuring stable performance and lasting aesthetics of the module under long-term humid and hot conditions.
[0010] Preferably, the thickness of the adhesive layer is 50-200 μm, for example, it can be 50 μm, 100 μm, 150 μm or 200 μm. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0011] Preferably, the adhesive layer is selected from any one of an EVA layer (ethylene-vinyl acetate copolymer layer), a POE layer (polyolefin elastomer layer), or a PVB layer (polyvinyl butyral layer). For example, the EVA layer may be composed of an ethylene-vinyl acetate copolymer and a crosslinking agent.
[0012] In this invention, the adhesive layer is used to bond to the bottom surface of the battery cell.
[0013] Preferably, the black coating is selected from any one of carbon black layer, black oxide layer or tricolor powder layer.
[0014] In this invention, the black coating is used to achieve a consistent appearance. It can be matched and adjusted according to the color of the front of the battery cell, so that almost all the light passing through the gaps between the battery cells can pass through and then be reflected back to the front of the battery cell by the structural layer for use.
[0015] Preferably, the black coating further comprises a resin matrix and an antioxidant. Exemplarily, the resin matrix may be acrylic resin or epoxy resin (or a modified system thereof); the antioxidant may be, for example, a combination of a primary antioxidant (hindered phenols, such as Irganox 1010) and a secondary antioxidant (phosphites, such as Irgafos 168). Furthermore, the black coating also contains light stabilizers (such as hindered amines like HALS) or ultraviolet absorbers, which work synergistically with the antioxidants to jointly resist photo-oxidative aging.
[0016] Preferably, the thickness of the black coating is 10-50 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0017] In this invention, a suitable thickness is beneficial for achieving an all-black appearance between the battery cells.
[0018] Preferably, the substrate layer is a PET layer (polyethylene terephthalate layer).
[0019] Preferably, the thickness of the substrate layer is 10-50 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0020] Preferably, the reflection angle adjustment layer is an acrylic resin layer with an angle reflection structure.
[0021] This invention uses an acrylic resin layer as a reflection angle adjustment layer. Its specific morphology (angle reflection structure) (for example, a sawtooth morphology or a semi-ellipsoidal morphology, etc.) can control the morphology of the subsequently deposited reflective layer, so that the reflection of light by the reflective layer changes from diffuse reflection to efficient directional reflection, thereby accurately projecting more light onto the effective power generation area of the solar cell, greatly improving the light capture capability and power generation efficiency of the module.
[0022] Preferably, the thickness of the reflection angle adjustment layer is 5-50 μm, for example, it can be 5 μm, 10 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0023] In this invention, an appropriate thickness ensures that the surface morphology has a sufficient influence on the reflective layer, thereby precisely controlling the reflection direction of light and achieving optimal light capture efficiency. At the same time, the thickness must also ensure the interlayer bonding force and the stability of the preparation process, avoiding excessive thickness that could lead to increased internal stress or cost.
[0024] Preferably, the reflective layer is a metallic conductive reflective layer or a white non-conductive reflective layer.
[0025] If a conductive reflective metal layer is introduced into this invention, it can be used as a conductive path to assist in collecting current, working in conjunction with the solder ribbon to reduce series resistance and improve the component fill factor. If a non-conductive white reflective white layer is introduced, it can reflect light to the maximum extent without requiring additional insulation design, simplifying the structure and ensuring long-term reliability.
[0026] Preferably, the metal conductive reflective layer is selected from any one of aluminum reflective layer, silver reflective layer, copper reflective layer or alloy reflective layer.
[0027] It should be noted that the metallic conductive reflective layer can be prepared by magnetron sputtering or thermal evaporation.
[0028] It should be noted that the white adhesive film layer can be prepared by co-extrusion or coating methods.
[0029] Preferably, the thickness of the metallic conductive reflective layer is 50-500 nm, for example, it can be 50 nm, 100 nm, 200 nm, 300 nm, 400 nm or 500 nm. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0030] Preferably, the white non-conductive reflective layer is a white adhesive film layer, which is selected from any one of a white EVA layer, a white POE layer, or a white PVB layer. For example, the white EVA layer is composed of an ethylene-vinyl acetate copolymer, a crosslinking agent, and a white filler.
[0031] Preferably, the thickness of the white non-conductive reflective layer is 10-100 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0032] Secondly, this utility model provides a black photovoltaic module, which includes a back sheet, a first encapsulating film, a battery string layer, a second encapsulating film, and a front sheet stacked sequentially from bottom to top.
[0033] The battery string layer includes a plurality of battery strings arranged in parallel, and at least the gap area between adjacent battery strings is provided with a black shielding reflective film as described in the first aspect, referred to as the first black shielding reflective film.
[0034] Preferably, the peripheral area of the battery string layer is also provided with the black shielding reflective film, referred to as the second black shielding reflective film.
[0035] Preferably, the battery string layer includes a busbar, a solder strip, a black reflective film, and the battery string along the first direction, wherein the black coating in the black reflective film is close to the battery string.
[0036] In this invention, the main purpose of setting the first and second black reflective films is to shield the welding strip.
[0037] It should be noted that the first direction refers to the direction in which the black photovoltaic module is stacked from bottom to top, consisting of the backsheet, the first encapsulant film, the cell string layer, the second encapsulant film, and the front panel.
[0038] Preferably, the busbar is disposed on the side of the solder strip near the backplate, and the projection of the busbar in the first direction does not exceed the range of the solder strip extending from one side edge of the battery string layer.
[0039] It should be noted that the busbar can be fabricated using processes such as infrared, laser, ultrasonic, or low-temperature lamination welding.
[0040] Preferably, the black shielding reflective film is disposed on the side of the solder strip near the front panel; the projection of the solder strip in the first direction does not exceed the range of the second black shielding reflective film.
[0041] Preferably, the width of the first black reflective shielding film is 2-7mm, for example, it can be 2mm, 3mm, 4mm, 5mm, 6mm or 7mm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0042] Preferably, the width of the second black reflective shielding film is 4-20mm, for example, it can be 4mm, 5mm, 10mm, 12mm, 15mm, 17mm or 20mm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0043] Preferably, the projection of the busbar in the first direction lies within the range of the second black reflective shielding film; or,
[0044] The busbar's projection in the first direction lies within the range of any battery string, and an insulating layer is provided between the busbar and the cross-string solder strips on the battery string to achieve electrical isolation, while simultaneously contacting the intra-string solder strips on the battery string. For example, the insulating layer can typically be a composite material, i.e., a three-layer co-extruded film or coated film. The most common substrate is PET, and sometimes PI or PO is used, providing the main insulation thickness and mechanical support. The top and bottom layers are functional layers, typically having good adhesion to the encapsulating film (such as EVA or POE), ensuring a firm bond with the backsheet and encapsulating film during lamination, without delamination or air bubbles.
[0045] In this invention, the distribution of the busbars is diverse and can be set at any position where a single cell of the battery string is led out. When the projection of the busbar in the first direction does not exceed the cell, the silver-white busbars cannot be seen from the front, making the overall appearance more aesthetically pleasing. The creepage distance is increased, which can be used to design wider gaps between cells to utilize more transmitted light or to use larger silicon wafers to increase the power of the same type of module.
[0046] The numerical range described in this utility model includes not only the point values listed above, but also any point values within the numerical range not listed above. Due to space limitations and for the sake of brevity, this utility model will not exhaustively list the specific point values included in the range.
[0047] Compared with the prior art, the beneficial effects of this utility model are as follows:
[0048] This invention provides a multi-layered black shading and reflective film, effectively solving many problems caused by manual application of the black shading film, and also addressing the visual unevenness caused by the thickness of the busbars. Specifically, an adhesive layer ensures reliable bonding with the module structure, avoiding misalignment and wrinkles during lamination, thus improving production yield and automation. The composite reflective layer efficiently reflects scattered light that would otherwise be absorbed by the black coating back to the cell surface, significantly reducing optical loss. This improves power generation efficiency while ensuring a uniform pure black appearance for the module. Furthermore, the multi-layered structure protects the easily aging black coating by placing it between the substrate layer and the composite reflective layer, greatly enhancing the material's weather resistance, preventing fading and interface degradation, and ensuring stable performance and lasting aesthetics of the module under long-term humid and hot conditions. Attached Figure Description
[0049] Figure 1 This is a schematic diagram of the structure of the black reflective shielding film provided in one embodiment of the present invention.
[0050] Figure 2 This is a schematic diagram of the structure of the black reflective shielding film provided in another embodiment of the present invention.
[0051] Figure 3 This is a cross-sectional structural diagram of a black photovoltaic module provided in another embodiment of the present invention.
[0052] Figure 4 for Figure 3 A schematic diagram of the cross-sectional structure of the battery string layer.
[0053] Figure 5 This is a schematic diagram of the surface structure of a black photovoltaic module provided in another embodiment of the present invention.
[0054] Figure 6 This is a schematic diagram of the surface structure of a black photovoltaic module provided in another embodiment of the present invention.
[0055] Among them, 1-adhesive layer; 2-black coating; 3-substrate layer; 4-first composite reflective layer; 5-second composite reflective layer; 6-back plate; 7-first adhesive film; 8-battery string layer; 9-second adhesive film; 10-front plate; 11-busbar; 12-welding ribbon; 13-first black shielding reflective film; 14-second black shielding reflective film; 15-battery string; 16-insulating layer. Detailed Implementation
[0056] It should be understood that in the description of this utility model, the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used solely for the convenience of describing this utility model and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this utility model. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, features defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this utility model, unless otherwise stated, "a plurality of" means two or more.
[0057] It should be noted that, in the description of this utility model, unless otherwise explicitly specified and limited, the terms "set," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this utility model based on the specific circumstances.
[0058] Those skilled in the art should understand that this utility model necessarily includes the necessary pipelines, conventional valves and general pump equipment for achieving complete process, but the above content is not the main innovation of this utility model. Those skilled in the art can add layouts based on the process flow and equipment structure selection. This utility model does not make any special requirements or specific limitations in this regard.
[0059] The technical solution of this utility model will be further described below with reference to the accompanying drawings and specific embodiments.
[0060] Please see Figure 1 In one embodiment, the present invention provides a black shielding reflective film, which includes an adhesive layer 1, a black coating 2, a substrate layer 3 and a first composite reflective layer 4 stacked sequentially; wherein, the first composite reflective layer 4 includes a reflection angle adjustment layer close to the substrate layer 3 and a reflective layer conformally stacked with the reflection angle adjustment layer.
[0061] Furthermore, the thickness of the adhesive layer 1 is 50-200 μm, for example, it can be 50 μm, 100 μm, 150 μm or 200 μm, etc. However, it is not limited to the listed values, other unlisted values within this range are also applicable.
[0062] Further, the adhesive layer 1 is selected from any one of an EVA layer (ethylene-vinyl acetate copolymer layer), a POE layer (polyolefin elastomer layer), or a PVB layer (polyvinyl butyral layer). For example, the EVA layer may be composed of an ethylene-vinyl acetate copolymer and a crosslinking agent.
[0063] In this invention, the adhesive layer 1 is used to bond to the bottom surface of the battery cell.
[0064] Furthermore, the black coating 2 is selected from any one of carbon black layer, black oxide layer or tricolor powder layer.
[0065] In this invention, the black coating 2 is used to achieve a consistent appearance. It can be matched and adjusted according to the color of the front of the battery cell, so that almost all the light passing through the gaps between the battery cells can pass through and then be reflected back to the front of the battery cell by the structural layer for use.
[0066] Furthermore, the black coating 2 also contains a resin matrix and an antioxidant. For example, the resin matrix may be acrylic resin or epoxy resin (or a modified system thereof); the antioxidant may be a combination of a primary antioxidant (hindered phenols, such as Irganox 1010) and a secondary antioxidant (phosphites, such as Irgafos 168). In addition, the black coating also contains light stabilizers (such as hindered amines like HALS) or ultraviolet absorbers, which work synergistically with the antioxidants to jointly resist photo-oxidative aging.
[0067] Furthermore, the thickness of the black coating 2 is 10-50 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. However, it is not limited to the listed values, other unlisted values within this range are also applicable.
[0068] In this invention, a suitable thickness is beneficial for achieving an all-black appearance between the battery cells.
[0069] Furthermore, the substrate layer 3 is a PET layer (polyethylene terephthalate layer).
[0070] Preferably, the thickness of the substrate layer 3 is 10-50 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0071] Preferably, the reflection angle adjustment layer is an acrylic resin layer with an angle reflection structure.
[0072] This invention uses an acrylic resin layer as a reflection angle adjustment layer. Its specific morphology (angle reflection structure) (for example, a sawtooth morphology or a semi-ellipsoidal morphology, etc.) can control the morphology of the subsequently deposited reflective layer, so that the reflection of light by the reflective layer changes from diffuse reflection to efficient directional reflection, thereby accurately projecting more light onto the effective power generation area of the solar cell, greatly improving the light capture capability and power generation efficiency of the module.
[0073] Furthermore, the thickness of the reflection angle adjustment layer is 5-50 μm, for example, it can be 5 μm, 10 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0074] In this invention, an appropriate thickness ensures that the surface morphology has a sufficient influence on the reflective layer, thereby precisely controlling the reflection direction of light and achieving optimal light capture efficiency. At the same time, the thickness must also ensure the interlayer bonding force and the stability of the preparation process, avoiding excessive thickness that could lead to increased internal stress or cost.
[0075] Furthermore, the reflective layer is a metallic conductive reflective layer.
[0076] If a metallic conductive reflective layer is introduced into this invention, it can be used as a conductive path to assist in collecting current, working in conjunction with the solder ribbon to reduce series resistance and improve the component fill factor.
[0077] Furthermore, the metallic conductive reflective layer is selected from any one of aluminum reflective layer, silver reflective layer, copper reflective layer or alloy reflective layer.
[0078] It should be noted that the metallic conductive reflective layer can be prepared by magnetron sputtering or thermal evaporation.
[0079] Furthermore, the thickness of the metallic conductive reflective layer is 50-500 nm, for example, it can be 50 nm, 100 nm, 200 nm, 300 nm, 400 nm or 500 nm, etc. However, it is not limited to the listed values, and other unlisted values within this range are also applicable.
[0080] Please see Figure 2 In another embodiment of the present invention, a black shielding reflective film is provided, the black shielding reflective film comprising an adhesive layer 1, a black coating layer 2, a substrate layer 3, and a second composite reflective layer 5 stacked sequentially; wherein, the second composite reflective layer 5 includes a reflection angle adjustment layer near the substrate layer 3 and a reflective layer conformally stacked with the reflection angle adjustment layer.
[0081] Furthermore, the reflective layer is a white, non-conductive reflective layer.
[0082] If a white, non-conductive reflective layer is introduced into this invention, it can reflect light to the maximum extent without requiring additional insulation design, thus simplifying the structure and ensuring long-term reliability.
[0083] Furthermore, the white non-conductive reflective layer is a white adhesive film layer, which is selected from any one of a white EVA layer, a white POE layer, or a white PVB layer. For example, the white EVA layer is composed of an ethylene-vinyl acetate copolymer, a crosslinking agent, and a white filler.
[0084] It should be noted that the white adhesive film layer can be prepared by co-extrusion or coating methods.
[0085] Furthermore, the thickness of the white non-conductive reflective layer is 10-100 μm, for example, it can be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm. However, it is not limited to the listed values; other unlisted values within this range are also applicable.
[0086] Please see Figure 3 , Figure 4 and Figure 5 In another embodiment of the present invention, a black photovoltaic module is provided, the black photovoltaic module comprising a backplate 6, a first encapsulant film 7, a battery string layer 8, a second encapsulant film 9 and a front plate 10 stacked sequentially from bottom to top.
[0087] The battery string layer 8 includes a plurality of battery strings 15 arranged in parallel. The gap area between adjacent battery strings 15 and the surrounding area of the battery string layer 8 are provided with black shielding reflective film as described above, which are respectively referred to as the first black shielding reflective film 13 and the second black shielding reflective film 14.
[0088] Furthermore, the battery string layer 8 includes a busbar 11, a solder strip 12, a black shielding reflective film, and the battery string 15 along the first direction, with the black coating in the black shielding reflective film close to the battery string 15.
[0089] In this invention, the purpose of setting the first black shielding reflective film 13 and the second black shielding reflective film 14 is mainly to shield the welding strip 12.
[0090] It should be noted that the first direction refers to the direction in which the black photovoltaic module is stacked from bottom to top, with the backsheet 6, the first encapsulant film 7, the cell string layer 8, the second encapsulant film 9, and the front panel 10 stacked sequentially.
[0091] Furthermore, the busbar 11 is disposed on the side of the solder strip 12 near the backplate 6, and the projection of the busbar 11 in the first direction does not exceed the range of the solder strip 12 extending from one side edge of the battery string layer 8.
[0092] It should be noted that the busbar 11 can be fabricated using processes such as infrared, laser, ultrasonic, or low-temperature lamination welding. Furthermore, the black reflective shielding film is disposed on the side of the solder strip 12 closest to the front panel 10; the projection of the solder strip 12 in the first direction does not exceed the range of the second black reflective shielding film 14.
[0093] Furthermore, the width of the first black reflective shielding film 13 is 2-7mm, for example, it can be 2mm, 3mm, 4mm, 5mm, 6mm or 7mm, etc. However, it is not limited to the listed values, other unlisted values within this range are also applicable.
[0094] Furthermore, the width of the second black reflective shielding film 14 is 4-20mm, for example, it can be 4mm, 5mm, 10mm, 12mm, 15mm, 17mm or 20mm. However, it is not limited to the listed values, other unlisted values within this range are also applicable.
[0095] Furthermore, the projection of the busbar 11 in the first direction is located within the range of the second black shielding reflective film 14.
[0096] Please see Figure 6 The gap area between adjacent battery strings is provided with a first black shielding reflective film 13 as described above, and the gap between the array of battery strings is initially covered by a black gap film strip to cover the busbar 11, so that the battery cells achieve a completely black appearance.
[0097] Furthermore, the projection of the busbar 11 in the first direction lies within the range of any battery string 15, and an insulating layer 16 is provided between the busbar 11 and the cross-string solder strips on the battery string 15 to achieve electrical isolation, while simultaneously contacting the intra-string solder strips on the battery string 15. Exemplarily, the insulating layer 16 can typically be a composite material, i.e., a three-layer co-extruded film or coated film. The most common substrate is PET, and sometimes PI or PO is also used. It provides the main insulation thickness and mechanical support. The upper and lower layers are functional layers, typically having good adhesion to the encapsulating film (such as EVA or POE), ensuring a firm bond with the backsheet and encapsulating film during lamination, without delamination or air bubbles.
[0098] In this invention, the distribution of the busbar 11 is varied and can be set at any position where a single cell of the battery string is led out. When the projection of the busbar in the first direction does not exceed the cell, the silver-white busbar cannot be seen from the front, making the overall appearance more aesthetically pleasing. The creepage distance is increased, which can be used to design wider gaps between cells to utilize more transmitted light or to use larger silicon wafers to increase the power of the same type of module.
[0099] In summary, this invention provides a multi-layered black shielding and reflective film that effectively solves many problems caused by manual application of the black shielding film, while also addressing the visual unevenness caused by the thickness of the busbars. Specifically, the adhesive layer achieves reliable bonding with the module structure, avoiding misalignment and wrinkles during lamination, thus improving production yield and automation. The composite reflective layer efficiently reflects scattered light that would otherwise be absorbed by the black coating back to the cell surface, significantly reducing optical loss. This improves power generation efficiency while ensuring a uniform pure black appearance for the module. Furthermore, the multi-layered structure protects the easily aging black coating by placing it between the substrate layer and the composite reflective layer, greatly enhancing the material's weather resistance, preventing fading and interface degradation, and ensuring stable performance and lasting aesthetics of the module under long-term humid and hot conditions.
[0100] The applicant declares that the above description is only a specific embodiment of the present utility model, but the protection scope of the present utility model is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present utility model fall within the protection and disclosure scope of the present utility model.
Claims
1. A black reflective film for blocking light, characterized in that, The black shielding reflective film comprises an adhesive layer, a black coating layer, a substrate layer, and a composite reflective layer stacked sequentially. The composite reflective layer includes a reflection angle adjustment layer near the substrate layer and a reflective layer conformally stacked with the reflection angle adjustment layer.
2. The black reflective film for blocking light according to claim 1, characterized in that, The thickness of the adhesive layer is 50-200 μm; The adhesive layer is selected from any one of EVA layer, POE layer or PVB layer.
3. The black reflective film for blocking light according to claim 1, characterized in that, The black coating is selected from any one of carbon black layer, black oxide layer or tricolor powder layer; The thickness of the black coating is 10-50 μm.
4. The black reflective film for blocking light according to claim 1, characterized in that, The substrate layer is a PET layer; The thickness of the substrate layer is 10-50 μm.
5. The black reflective film for blocking light according to claim 1, characterized in that, The reflection angle adjustment layer is an acrylic resin layer with an angle reflection structure; The thickness of the reflection angle adjustment layer is 5-50 μm.
6. The black reflective film for blocking light according to claim 1, characterized in that, The reflective layer is a metallic conductive reflective layer or a white non-conductive reflective layer; The conductive metal reflective layer is selected from any one of aluminum reflective layer, silver reflective layer, copper reflective layer or alloy reflective layer; The thickness of the metallic conductive reflective layer is 50-500 nm; The white non-conductive reflective layer is a white adhesive film layer, which is selected from any one of a white EVA layer, a white POE layer, or a white PVB layer. The thickness of the white non-conductive reflective layer is 10-100 μm.
7. A black photovoltaic module, characterized in that, The black photovoltaic module includes a back sheet, a first encapsulating film, a battery string layer, a second encapsulating film, and a front sheet, which are stacked sequentially from bottom to top. The battery string layer includes a plurality of battery strings arranged in parallel, and at least the gap area between adjacent battery strings is provided with a black shielding reflective film as described in any one of claims 1-6, referred to as the first black shielding reflective film.
8. The black photovoltaic module according to claim 7, characterized in that, The surrounding area of the battery string layer is also provided with the black shielding reflective film, referred to as the second black shielding reflective film.
9. The black photovoltaic module according to claim 8, characterized in that, The battery string layer includes a busbar, a solder strip, a black shielding reflective film and the battery string along the first direction, wherein the black coating in the black shielding reflective film is close to the battery string; The busbar is disposed on the side of the solder strip near the back plate, and the projection of the busbar in the first direction does not exceed the range of the solder strip extending from one side edge of the battery string layer. The black shielding reflective film is disposed on the side of the solder strip near the front panel; the projection of the solder strip in the first direction does not exceed the range of the second black shielding reflective film; The width of the first black reflective shielding film is 2-7mm; the width of the second black reflective shielding film is 4-20mm.
10. The black photovoltaic module according to claim 9, characterized in that, The projection of the busbar in the first direction is located within the range of the second black shielding reflective film; Alternatively, the projection of the busbar in the first direction is located within the range of any battery string, and an insulating layer is provided between the busbar and the cross-string solder strips on the battery string to achieve electrical isolation, while contacting the intra-string solder strips on the battery string.