A ceramicized functional mica composite material

By forming textured and slotted microstructures on the surface of mica substrate and compounding it with a ceramic-compatible high-temperature resistant coating, the problem of poor bonding strength of mica composite materials is solved, flame retardancy and service life are improved, and the safety of lithium battery cell modules is ensured.

CN224981529UActive Publication Date: 2026-11-17浙江荣泰电工器材股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522357653.1
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-11-06
Publication Date
2026-11-17
Estimated Expiration
2035-11-06

AI Technical Summary

Technical Problem

In existing mica composite materials, the bonding force between the mica substrate and the ceramicizable high-temperature resistant coating is poor, leading to delamination problems and affecting the stability of flame-retardant and fire-resistant performance and service life.

Method used

A textured microstructure that improves interfacial bonding and a slotted microstructure that relieves interfacial stress are formed on the surface of the mica substrate, and a ceramicizable high-temperature resistant coating with a thickness of 5-40μm is laminated to form a dense ceramic coating to protect the mica substrate.

Benefits of technology

It improves the interfacial bonding performance of mica composite materials, enhances flame retardancy and burn-through resistance, extends service life, and forms a dense ceramic layer at high temperatures to insulate heat, thereby improving the thermal runaway safety of lithium battery cell modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224981529U_ABST
    Figure CN224981529U_ABST
Patent Text Reader

Abstract

This application relates to the field of high fire-resistant and burn-through functional mica materials, and in particular to a ceramicized functional mica composite material. The ceramicized functional mica composite material includes a mica substrate, the surface of which is formed by embossing and hot-pressing to create a textured microstructure that improves interfacial bonding; the surface of the mica substrate is also formed by embossing and hot-pressing to create a plurality of dot-matrix distributed slotted microstructures that relieve interfacial stress; and the surface of the mica substrate is coated with a ceramicizable high-temperature resistant coating. The mica composite material in this application is made from mica sheet / mica paper combined with a ceramicizable coating technology, exhibiting excellent flame retardancy, burn-through resistance, and good interfacial bonding performance, giving it a relatively long service life, and is particularly suitable for packaging and protection materials for lithium battery cell modules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of high fire-resistant and breakdown-resistant functional mica materials, and in particular to a ceramicized functional mica composite material, especially suitable for packaging and protection materials for lithium battery cell modules. Background Technology

[0002] Mica materials possess excellent mechanical properties, flame retardancy, high-temperature resistance, and low manufacturing cost, making them widely used in new energy vehicles, aerospace, and other fields. Mica materials are made from mica powder and binders, which can be either silicone binders or epoxy resin binders. Mica materials prepared with silicone binders exhibit better resistance to low and high temperatures, weather resistance, and impact toughness, making them the mainstream mica material for thermal runaway protection in lithium battery cell modules. However, the silicone binder content in this type of mica material is typically 10-16 wt%, resulting in poor adhesion of the mica powder to the surface. This leads to lower wear resistance and a tendency for surface "powder shedding," which is detrimental to thermal runaway protection in lithium battery cell modules.

[0003] Existing technologies utilize mica composite materials formed from a ceramicizable high-temperature resistant coating / mica substrate, which solves the "powder shedding" problem of such mica composites. However, during the widespread use of this mica composite material, the following problem was discovered: poor bonding between the mica substrate and the ceramicizable high-temperature resistant coating leads to "delamination" during use, resulting in unstable flame-retardant and fire-resistant properties and affecting its service life. Therefore, the inventors have provided a ceramicizable functional mica composite material. Utility Model Content

[0004] To address the aforementioned technical problems, this application provides a ceramicized functional mica composite material.

[0005] The ceramicized functional mica composite material provided in this application is achieved through the following scheme: A ceramicized functional mica composite material includes a mica substrate, wherein the surface of the mica substrate is embossed to form a textured microstructure that improves interfacial bonding; the surface of the mica substrate is embossed to form a plurality of slotted microstructures that relieve interfacial stress; and the surface of the mica substrate is coated with a ceramicizable high-temperature resistant coating with a thickness of 5-40 μm.

[0006] The ceramic-like high-temperature resistant coating can form a dense ceramic coating under the high-temperature thermal runaway of lithium batteries. This coating can protect the mica substrate from direct contact with air and fire sources, and delay the burning rate of the mica substrate in a fire. Thus, the application of the ceramic-like high-temperature resistant coating improves the overall fire resistance, flame retardancy, and burn-through resistance.

[0007] The mica composite material in this application is made by combining mica sheet / mica paper with a ceramicizable layer technology. It has excellent flame retardancy, burn-through resistance and good interfacial bonding performance, giving it a relatively long service life. It is especially suitable for the packaging and protection materials of lithium battery cell modules.

[0008] Preferably, the slotted microstructure is a honeycomb microstructure with a dot matrix distribution, the depth of the honeycomb microstructure is 1-5 μm, the side length of the honeycomb pores is 4-8 μm, and the interval between adjacent honeycomb microstructures is 5-25 μm.

[0009] Preferably, the mica substrate is mica paper or mica sheet, wherein the mica paper is mica paper with a standard thickness of 75-80μm or multilayer mica paper formed by hot pressing 2-5 sheets of mica paper with a standard thickness of 75-80μm; and the mica sheet is formed by hot pressing 6-20 sheets of mica paper with a standard thickness of 75-80μm.

[0010] Preferably, the thickness ratio of the ceramicizable high-temperature resistant coating to the mica substrate is 100:(5-15).

[0011] Preferably, the mica substrate is formed by hot pressing 4 or 5 sheets of mica paper with a standard thickness of 75-80μm, with a total thickness of 300-400μm; the thickness of the ceramic-like high-temperature resistant coating is 15-25μm.

[0012] Preferably, the ceramicizable high-temperature resistant coating is cured by high-temperature nano ceramic adhesive 15011; or the ceramicizable high-temperature resistant coating is cured by Shin-Etsu KE-4890 ceramic fireproof adhesive.

[0013] Preferably, the mica substrate comprises at least two layers of multilayer mica paper substrate and an aerogel paper laminated between the multilayer mica paper substrates. The upper and lower surfaces of the multilayer mica paper substrate are embossed to form a textured microstructure that improves interfacial bonding. The upper and lower surfaces of the multilayer mica paper substrate are embossed to form a plurality of slotted microstructures that relieve interfacial stress. The upper and lower surfaces of the multilayer mica paper substrate are laminated with a ceramic-like high-temperature resistant coating.

[0014] Preferably, the thickness of the multilayer mica paper substrate is 150-400 μm; the thickness of the aerogel paper is 100-300 μm.

[0015] The mica substrate formed by laminating aerogel paper between multiple layers of mica paper substrate has better flame retardancy, burn-through resistance, damping and shock absorption, thermal shock resistance, heat insulation and noise reduction, and lightweight advantages. The lithium battery cell module made using it has more reliable thermal runaway safety performance, providing key protection for battery safety and buying valuable emergency response time.

[0016] Preferably, the mica substrate comprises at least two multilayer mica paper substrates and a ceramicized silicone rubber layer laminated between the multilayer mica paper substrates. The upper and lower surfaces of the multilayer mica paper substrates are embossed to form textured microstructures that improve interfacial adhesion. The upper and lower surfaces of the multilayer mica paper substrates are embossed to form a plurality of slotted microstructures that relieve interfacial stress. The surface of the multilayer mica paper substrates facing away from the ceramicized silicone rubber layer is laminated with a ceramicizable high-temperature resistant coating. The thickness of the ceramicized silicone rubber layer is 100-600 μm.

[0017] The mica substrate formed by laminating a ceramicized silicone rubber layer between multiple layers of mica paper substrate has better flame retardancy, burn-through resistance, damping and shock absorption, thermal shock resistance, and thermal insulation and noise reduction. The lithium battery cell module prepared using it has more reliable thermal runaway safety performance, providing key protection for battery safety and buying valuable emergency response time.

[0018] In summary, this application has the following advantages: 1. The mica composite material in this application has good interfacial bonding performance, which gives it excellent flame retardancy, burn-through resistance and relatively long service life. In addition, the non-high-temperature ceramization ceramicizable high-temperature resistant coating has a certain buffering performance, which can improve the damping and shock absorption and thermal shock resistance of the mica composite material.

[0019] 2. Depending on the application location in the lithium battery cell module, the mica substrate contains aerogel paper or ceramicized silicone rubber to enhance flame retardancy, fire resistance, heat insulation and noise reduction. This can further improve the overall flame retardancy, burn-through resistance, damping and shock absorption, and thermal shock resistance of the mica composite material. The lithium battery cell module made using this material has more reliable thermal runaway safety performance, providing key protection for battery safety and buying valuable emergency response time. Attached Figure Description

[0020] Figure 1 This is a schematic diagram of the overall structure of the ceramicized functional mica composite material in Example 1.

[0021] Figure 2 This is a schematic diagram of the overall structure of the ceramicized functional mica composite material in Example 2.

[0022] Figure 3 This is a schematic diagram of the overall structure of the ceramicized functional mica composite material in Example 3.

[0023] Figure 4 This is a schematic diagram of the overall structure of the ceramicized functional mica composite material in Comparative Example 1.

[0024] Figure 5 This is a diagram illustrating a bending test of a ceramicized functional mica composite material.

[0025] In the figure, 1 is the mica substrate; 101 is the multilayer mica paper substrate; 102 is the aerogel paper; 103 is the ceramicized silicone rubber layer; 11 is the textured microstructure; 12 is the slotted microstructure; and 2 is the ceramicized high-temperature resistant coating. Detailed Implementation

[0026] To further understand the inventiveness and technical advancements of this application, the preferred embodiments of this application will be discussed in detail below with reference to examples and comparative examples.

[0027] Example 1: Reference Figure 1 A ceramicized functional mica composite material includes a mica substrate 1, on the surface of which is coated with a ceramicizable high-temperature resistant coating 2 with a thickness of 5-40 μm. The surface of the mica substrate 1 is embossed with textured microstructures 11 to improve interfacial bonding, and also with several slotted microstructures 12 to alleviate interfacial stress. The textured microstructures 11 and slotted microstructures 12 enhance the interfacial bonding strength between the ceramicizable high-temperature resistant coating 2 and the mica substrate 1, and alleviate interfacial stress, thereby improving the stability of the interfacial bonding and endowing the ceramicized functional mica composite material with excellent flame retardancy, burn-through resistance, and a longer service life.

[0028] The textured microstructure 11 is formed by hot pressing with an orange peel textured roller. The orange peel texture 11 has a depth of 10-15 micrometers for the deepest lines and 3-6 micrometers for the shallowest lines, depending on the depth of the laser-engraved lines on the roller. Alternatively, the textured microstructure 11 can be formed by hot pressing with a bark textured roller. The bark texture 11 also has a depth of 10-15 micrometers for the deepest lines and 3-6 micrometers for the shallowest lines, depending on the depth of the laser-engraved lines on the roller.

[0029] The slotted microstructure 12 is a honeycomb microstructure with a dot matrix distribution, which can alleviate the interfacial stress between the ceramicizable high-temperature resistant coating 2 and the mica substrate 1. The depth of the honeycomb microstructure is 1-5 μm, the side length of the honeycomb holes is 4-8 μm, and the spacing between adjacent honeycomb microstructures is 5-25 μm.

[0030] The thickness of the mica substrate 1 varies depending on its application within the lithium battery cell module. The mica substrate 1 can be either mica paper or mica sheet. The mica paper can be standard thickness 75-80μm or multilayer mica paper formed by hot pressing 2-5 sheets of standard thickness 75-80μm mica paper. The mica sheet is formed by hot pressing 6-20 sheets of standard thickness 75-80μm mica paper. Specifically, the mica substrate 1 is formed by hot pressing 4 or 5 sheets of standard thickness 75-80μm mica paper, with a total thickness of 300-400μm.

[0031] The thickness of the ceramicizable high-temperature resistant coating 2 affects the overall flame retardant and fireproof performance of the ceramicizable functional mica composite material. The thickness ratio of the ceramicizable high-temperature resistant coating 2 to the mica substrate 1 is 100:(10-25). Preferably, the thickness of the ceramicizable high-temperature resistant coating 2 is 15-25 μm.

[0032] The ceramic-resistant high-temperature coating 2 is cured by either Bezos Polymer New Materials (Dongguan) Co., Ltd.’s high-temperature nano ceramic adhesive 15011 or Shin-Etsu KE-4890 ceramic fireproof adhesive.

[0033] In this embodiment, the textured microstructure 11 is formed by hot pressing with an orange peel textured roller. The textured microstructure 11 is an orange peel texture microstructure. Depending on the depth of the laser-engraved texture on the orange peel textured roller, the deepest texture of the formed orange peel texture microstructure is 15 micrometers, and the shallowest texture is 5 micrometers. In this embodiment, the depth of the honeycomb microstructure is 5μm, the side length of the honeycomb hole is 5μm, and the interval between adjacent honeycomb microstructures is 25μm. In this embodiment, the mica substrate 1 is formed by hot pressing five sheets of phlogopite paper with a standard thickness of 75-80μm, and the total thickness of the mica substrate 1 is 375-400μm. The ceramicizable high-temperature resistant coating 2 is formed by curing high-temperature nano-ceramic adhesive 15011, and the thickness of the ceramicizable high-temperature resistant coating 2 is 20μm.

[0034] The difference between Example 2 and Example 1 is as follows: (Refer to...) Figure 2 The mica substrate 1 comprises two layers of multilayer mica paper substrate 101 and an aerogel paper 102 laminated between the multilayer mica paper substrate 101. The multilayer mica paper substrate 101 is formed by hot pressing two sheets of phlogopite paper with a standard thickness of 75-80μm, and the total thickness of the mica substrate 1 is 150-160μm. The aerogel paper 102 is provided by Honghui Technology (Henan) Co., Ltd., with a customized thickness of 200μm.

[0035] The upper and lower surfaces of the multilayer mica paper substrate 101 are embossed to form textured microstructures 11 that improve interfacial adhesion. The textured microstructures 11 are formed by hot pressing with an orange peel textured roller. The textured microstructures 11 are orange peel textured microstructures. Depending on the depth of the laser-engraved textures on the orange peel textured roller, the deepest texture of the formed orange peel textured microstructure is 15 micrometers and the shallowest texture is 5 micrometers.

[0036] The upper and lower surfaces of the multilayer mica paper substrate 101 are both embossed to form several slotted microstructures 12 to relieve interfacial stress. The depth of the honeycomb microstructure is 5μm, the side length of the honeycomb pore is 5μm, and the spacing between adjacent honeycomb microstructures is 25μm. Both the upper and lower surfaces of the multilayer mica paper substrate 101 are coated with a ceramic-like high-temperature resistant coating 2. The ceramic-like high-temperature resistant coating 2 is formed by curing high-temperature nano-ceramic adhesive 15011, and the thickness of the ceramic-like high-temperature resistant coating 2 is 20μm. During the preparation process, aerogel paper 102 is laminated between the two layers of multilayer mica paper substrate 101 using high-temperature nano-ceramic adhesive 15011.

[0037] The difference between Example 3 and Example 1 is as follows: (Refer to...) Figure 3 The mica substrate 1 comprises two multilayer mica paper substrates 101 and a ceramicized silicone rubber layer 103 laminated between the multilayer mica paper substrates 101. The multilayer mica paper substrate 101 is formed by hot pressing two sheets of phlogopite paper with a standard thickness of 75-80 μm, and the total thickness of the mica substrate 1 is 150-160 μm. The ceramicized silicone rubber layer 103 is provided by Shenzhen Yulong New Materials Co., Ltd., and its thickness is 200 μm.

[0038] The upper and lower surfaces of the multilayer mica paper substrate 101 are embossed to form textured microstructures 11 that improve interfacial adhesion. The textured microstructures 11 are formed by hot pressing with an orange peel textured roller. The textured microstructures 11 are orange peel textured microstructures. Depending on the depth of the laser-engraved textures on the orange peel textured roller, the deepest texture of the formed orange peel textured microstructure is 15 micrometers and the shallowest texture is 5 micrometers.

[0039] The upper and lower surfaces of the multilayer mica paper substrate 101 are both embossed to form several slotted microstructures 12 to relieve interfacial stress. The depth of the honeycomb microstructure is 5μm, the side length of the honeycomb pore is 5μm, and the spacing between adjacent honeycomb microstructures is 25μm. A ceramicizable high-temperature resistant coating 2 is laminated on the surface of the multilayer mica paper substrate 101 facing away from the ceramicized silicone rubber layer 103. The ceramicizable high-temperature resistant coating 2 is formed by curing high-temperature nano-ceramic adhesive 15011, and the thickness of the ceramicizable high-temperature resistant coating 2 is 20μm.

[0040] The difference between Comparative Example 1 and Example 1 is as follows: (Refer to...) Figure 4 The mica substrate 1 is formed by hot pressing five sheets of mica paper with a standard thickness of 75-80μm, and the total thickness of the mica substrate 1 is 375-400μm. The ceramicizable high-temperature resistant coating 2 is formed by curing high-temperature nano ceramic adhesive 15011, and the thickness of the ceramicizable high-temperature resistant coating 2 is 20μm.

[0041] The mica composite materials in Example 1 and Comparative Example 1 were subjected to bending tests. The diameter of the circular shaft used in the test was 5 times the thickness of the mica composite material (5R). The mica composite material was placed in a thermal shock test chamber with the following test parameters: low temperature -40℃, high temperature 85℃, holding time 30 min, temperature transition time 5 min. After 1000 cycles, the ceramic-like high-temperature resistant coating was observed to show cracking and peeling. Five test samples were used. After the high and low temperature impact test, the mica composite material in Example 1 was bent 1000 times with a 5R circular shaft (bending angle 30°). It was observed that the interface structure of the mica composite material in Example 1 was intact, and no cracking or peeling was observed. After the high and low temperature impact test, the mica composite material in Comparative Example 1 was bent 1000 times with a 5R circular shaft (bending angle 30°), and interlayer cracking and peeling were observed at the interface.

[0042] The mica composite material in Example 1 was subjected to a flame impact of 1000 °C for 5 minutes. The entire material was not burned through and there were no cracks on the surface. The ceramic-resistant high-temperature coating forms a dense ceramic layer at high temperature, which effectively blocks heat transfer, suppresses battery explosion, provides key protection for battery safety, and buys valuable emergency response time.

[0043] In summary, the mica composite material in this application is made by combining mica sheet / mica paper with a ceramicizable layer technology. It has excellent fire resistance and flame retardancy, burn-through resistance and good interfacial bonding performance, giving it a relatively long service life. It is especially suitable for the packaging and protection materials of lithium battery cell modules.

[0044] It should be noted that this specific embodiment is merely an explanation of the technical solution of this application and is not a limitation thereof. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of this application.

Claims

1. A ceramicized functional mica composite material, characterized in that: The mica substrate (1) has a textured microstructure (11) formed on its surface to improve interfacial bonding; the mica substrate (1) has a plurality of slotted microstructures (12) formed on its surface to relieve interfacial stress; and the mica substrate (1) has a ceramic-compatible high-temperature resistant coating (2) with a thickness of 5-40 μm on its surface.

2. The ceramicized functional mica composite material according to claim 1, characterized in that: The slotted microstructure (12) is a honeycomb microstructure with a dot matrix distribution. The depth of the honeycomb microstructure is 1-5 μm, the side length of the honeycomb pores is 4-8 μm, and the interval between adjacent honeycomb microstructures is 5-25 μm.

3. The ceramicized functional mica composite material according to claim 1, characterized in that: The mica substrate (1) is mica paper or mica sheet. The mica paper is mica paper with a standard thickness of 75-80μm or multilayer mica paper made by hot pressing 2-5 sheets of mica paper with a standard thickness of 75-80μm. The mica sheet is made by hot pressing 6-20 sheets of mica paper with a standard thickness of 75-80μm.

4. The ceramicized functional mica composite material according to claim 1, characterized in that: The thickness ratio of the ceramicizable high-temperature resistant coating (2) to the mica substrate (1) is 100: (5-15).

5. The ceramicized functional mica composite material according to claim 1, characterized in that: The mica substrate (1) is formed by hot pressing 4 or 5 sheets of mica paper with a standard thickness of 75-80μm, with a total thickness of 300-400μm; the ceramic-like high-temperature resistant coating (2) has a thickness of 15-25μm.

6. The ceramicized functional mica composite material according to claim 1, characterized in that: The ceramicizable high-temperature resistant coating (2) is formed by curing high-temperature nano ceramic adhesive 15011; or the ceramicizable high-temperature resistant coating (2) is formed by curing Shin-Etsu KE-4890 ceramic fireproof adhesive.

7. The ceramicized functional mica composite material according to claim 1, characterized in that: The mica substrate (1) includes at least two layers of multilayer mica paper substrate (101) and aerogel paper (102) composited between the multilayer mica paper substrate (101). The upper and lower surfaces of the multilayer mica paper substrate (101) are embossed to form textured microstructures (11) that improve interfacial bonding. The upper and lower surfaces of the multilayer mica paper substrate (101) are embossed to form a plurality of slotted microstructures (12) that relieve interfacial stress. The upper and lower surfaces of the multilayer mica paper substrate (101) are composited with a ceramic-like high-temperature resistant coating (2).

8. The ceramicized functional mica composite material according to claim 7, characterized in that: The thickness of the multilayer mica paper substrate (101) is 150-400 μm; the thickness of the aerogel paper (102) is 100-300 μm.

9. The ceramicized functional mica composite material according to claim 1, characterized in that: The mica substrate (1) includes at least two multilayer mica paper substrates (101) and a ceramicized silicone rubber layer (103) composited between the multilayer mica paper substrates (101). The upper and lower surfaces of the multilayer mica paper substrates (101) are embossed to form textured microstructures (11) that improve interfacial bonding. The upper and lower surfaces of the multilayer mica paper substrates (101) are embossed to form a plurality of slotted microstructures (12) that relieve interfacial stress. The surface of the multilayer mica paper substrates (101) facing away from the ceramicized silicone rubber layer (103) is coated with a ceramicizable high-temperature resistant coating (2). The thickness of the ceramicized silicone rubber layer (103) is 100-600 μm.