Anode sheet, electrode assembly, and electrochemical device
By setting grooves on the surface of the active material layer of the anode plate and coating it with an ion-permeable coating, the problem of difficult cleaning of anode powder in the grooves is solved, thereby improving the safety performance and service life of the electrochemical device.
Patent Information
- Application Number
- CN202522562197.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2035-12-02
AI Technical Summary
During the laser etching process of the electrode, the anode powder in the groove is difficult to clean, causing it to fall off during the winding process, affecting the self-discharge performance and safety performance of the battery cell.
Grooves are formed on the surface of the active material layer of the anode sheet, and an ion-permeable coating is coated in the grooves. The thickness of the ion-permeable coating is 7.5 μm to 15 μm to prevent the active material powder from falling off during winding.
This effectively prevents active material powder from falling off the separator, reduces the K value of the battery cell, and improves the safety performance and service life of the electrochemical device.
Smart Images

Figure CN224986282U_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electrochemical energy storage technology, and in particular to an anode plate, electrode assembly and electrochemical device. Background Technology
[0002] In recent years, with the booming development of industries such as consumer electronics and new energy vehicles, the performance requirements for battery products have become increasingly stringent, showing a significant trend towards smaller size and higher energy density (high ED). Smaller batteries can better fit into compact electronic devices, meeting their design requirements for thinness and portability; while high energy density means that batteries can store more electrical energy in the same volume or weight, thereby extending the device's battery life and improving the user experience. To meet these demands, more battery production projects are adopting new processes such as double-layer coating and electrode laser etching.
[0003] In electrode laser etching projects, laser etching is widely used to carve specific grooves on the anode sheet to improve the electrolyte's wetting effect on the electrode and optimize the ion transport path of the battery, thereby improving the battery's charge and discharge efficiency and energy density. However, this process can also easily lead to the accumulation of anode powder in the grooves. This anode powder adheres to the inside of the grooves after laser etching, and due to the special structure of the grooves, it is difficult to completely remove it in subsequent conventional cleaning processes. During the winding process, there is a risk that the anode powder accumulated in the grooves may fall off. As the winding equipment operates, the anode powder may fall from the grooves and scatter, adhering to the separator. The adhesion of anode powder to the separator may affect the cell's self-discharge performance, leading to an increase in the cell's K-value (self-discharge rate). Utility Model Content
[0004] The main purpose of this application is to provide an anode plate, electrode assembly, and electrochemical device, which aims to improve the problem of powder shedding from the grooves of the anode plate and enhance the safety performance of the electrochemical device.
[0005] To achieve the above objectives, this application proposes an anode sheet, which includes a current collector and an active material layer. The active material layer is disposed on both sides of the current collector along its thickness direction. The surface of the active material layer is provided with grooves, and the surface of the grooves is provided with an ion-permeable coating. The thickness of the ion-permeable coating is 7.5 μm to 15 μm.
[0006] In some embodiments, the current collector has grooves on the active material layer on both sides along its thickness direction, and there are multiple grooves arranged side by side along the width direction of the current collector.
[0007] In some embodiments, the distance between two adjacent grooves along the length of the anode sheet is 1 mm to 2.5 mm.
[0008] In some embodiments, the depth of the groove along the thickness direction of the anode sheet is 10 μm to 20 μm.
[0009] In some embodiments, the width of the groove along the length of the anode sheet is 50 μm to 90 μm.
[0010] In some embodiments, the distance from one end of any of the grooves to the edge of the adjacent active material layer along the width direction of the anode sheet is 0.1 mm to 1.5 mm.
[0011] In some embodiments, the distance from one end of any of the grooves to the edge of the adjacent active material layer along the width direction of the anode sheet is 0.5 mm to 1 mm.
[0012] In some embodiments, the ion-permeable coating comprises one of polyvinylidene fluoride, polyacrylic acid, sodium carboxymethyl cellulose, and polyethylene oxide.
[0013] A second aspect of this application also provides an electrode assembly comprising an anode sheet, a cathode sheet, and a diaphragm arranged in a stacked and wound manner, wherein the anode sheet is the aforementioned anode sheet.
[0014] A third aspect of this application also provides an electrochemical device comprising the electrode assembly described above.
[0015] This application discloses an anode sheet, an electrode assembly, and an electrochemical device. The anode sheet is used in the electrode assembly, which is a wound battery cell. By setting grooves on the anode sheet and setting an ion-permeable coating in the grooves, the active material layers at the grooves are tightly bonded together, preventing the active material powder from falling onto the diaphragm during the winding of the anode sheet and preventing the diaphragm from being punctured by the active material powder, thereby improving safety performance. It also helps to reduce the K value of the electrode assembly, thereby extending the service life of the electrochemical device. Attached Figure Description
[0016] Figure 1 This is a side cross-sectional view of the anode sheet in one embodiment of this application; Figure 2 This is a top view of the anode sheet in one embodiment of this application.
[0017] Explanation of reference numerals in the attached figures: Anode plate 100; current collector 110; active material layer 120; groove 130; ion-permeable coating 140. Detailed Implementation
[0018] The solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments in this application, and not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0019] It should be noted that all directional indicators (such as up, down, left, right, front, back, etc.) in the embodiments of this application are only used to explain the relative positional relationship and movement of each component in a certain specific posture (as shown in the figure). If the specific posture changes, the directional indicator will also change accordingly.
[0020] It should also be noted that when a component is described as "fixed to" or "set on" another component, it can be directly on the other component or there may be an intervening component present. When a component is described as "connected to" another component, it can be directly connected to the other component or there may be an intervening component present.
[0021] Furthermore, the use of terms such as "first" and "second" in this application is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. Additionally, the technical solutions of the various embodiments can be combined with each other, but only on the basis of being achievable by those skilled in the art. When the combination of technical solutions is contradictory or impossible to implement, such a combination of technical solutions should be considered non-existent and not within the scope of protection claimed in this application.
[0022] Please see Figure 1 This application discloses an anode sheet 100, which includes a current collector 110 and an active material layer 120. The active material layer 120 is disposed on both sides of the current collector 110 along its thickness direction. A groove 130 is provided on the surface of the active material layer 120, and an ion-permeable coating 140 is provided on the surface of the groove 130. The thickness of the ion-permeable coating 140 is 7.5 μm to 15 μm.
[0023] In this embodiment, the anode sheet 100 includes a current collector 110, an active material layer 120, grooves 130, and an ion-permeable coating 140. Viewed along the thickness direction of the anode sheet 100, the current collector 110 includes a first surface and a second surface disposed opposite to each other, and an active material layer 120 is disposed on both the first and second surfaces. The anode sheet 100 proposed in this application is suitable for wound battery cells. Grooves 130 are disposed on the active material layer 120 on both the first and second surfaces of the current collector 110. The grooves 130 are disposed on the surface of the active material layer 120, and the thickness of the grooves 130 is less than the thickness of the active material layer 120. Because the active material layer 120 undergoes significant volume changes before and after charge-discharge cycles, and the anode sheet 100 is wound, the active material layer 120 experiences high stress and is prone to cracking during charge-discharge cycles. By using laser etching to create grooves 130 on the surface of the active material layer 120, the stress on the active material layer 120 can be buffered, thereby improving the cracking situation of the active material layer 120. In addition, it can shorten the ion transport distance, thereby increasing the charging and discharging speed of the wound battery cell.
[0024] In actual production, since the groove 130 is set on the surface of the active material layer 120, some active material powder inevitably remains in the groove 130 after laser etching. During the manufacturing process of the wound cell, the anode sheet 100, cathode sheet and separator are stacked and wound together. Therefore, the active material powder in the groove 130 is easy to fall onto the separator during winding, which may cause the separator to be punctured by these fallen active material powders during charge and discharge cycles, resulting in an increase in K value and reducing the storage performance and service life of the cell.
[0025] It should be particularly noted that an ion-permeable coating 140 is also provided on the surface of the groove 130. In this embodiment, the ion-permeable coating 140 can be applied by spraying. It is understood that in other embodiments, the ion-permeable coating 140 can also be applied by other coating methods, such as dot coating, etc. This application does not impose any limitations here. By providing the ion-permeable coating 140 on the surface of the groove 130, the active material powder in the groove 130 can be prevented from falling off. The adhesive force of the ion-permeable coating 140 is used to bond the active material layer 120 on the surface of the groove 130 together, thereby preventing the active material powder in the groove 130 from falling off during the winding of the anode sheet 100, thus improving the powder shedding problem after the anode sheet 100 is provided with the groove 130.
[0026] Looking along the thickness direction of the anode sheet 100, the thickness of the ion-permeable coating 140 is denoted as t, and the value of t is set in the range of 7.5 μm to 15 μm. In actual production, the thickness t of the ion-permeable coating 140 can be set to different values such as 7.5 μm, 10 μm, and 15 μm. Specifically, if the thickness of the ion-permeable coating 140 is too low, the adhesion will decrease, and the active material layer 120 on the surface of the groove 130 will not be tightly bonded together, making it easy for the active material powder to fall off during winding; if the thickness of the ion-permeable coating 140 is too high, the groove 130 will be almost filled by the ion-permeable coating 140, failing to accelerate the ion transport speed and seriously affecting the effect of setting the groove 130. In addition, if the ion-permeable coating 140 is too thick, it will overflow the groove 130, resulting in uneven thickness of the ion-permeable coating 140. Taking a thickness t of 7.5 μm for the ion-permeable coating 140 as an example, if it is less than 7.5 μm, the ion-permeable coating 140 is too thin, resulting in insufficient adhesion strength. This would prevent the active material layer 120 at the groove 130 from being bonded together, and powder shedding would still occur during the winding of the anode sheet 100. Taking a thickness t of 15 μm for the ion-permeable coating 140 as an example, if it is greater than 15 μm, the ion-permeable coating 140 is too thick, almost filling the groove 130 completely, increasing the ion transport distance, and violating the original intention of setting the groove 130.
[0027] Because the active material powder that falls onto the separator is sharp and has a large particle size, it can easily puncture the separator, leading to micro-short circuits inside the final wound cell and causing physical self-discharge, resulting in an increase in the K value. In this embodiment, by providing an ion-permeable coating 140 in the groove 130 and limiting the thickness of the ion-permeable coating 140 to 7.5µm to 15µm, the adhesion strength of the ion-permeable coating 140 can be ensured. This prevents the active material layer 120 at the groove 130 from dropping active material powder onto the production equipment or separator during the winding of the anode sheet 100, reducing the probability of separator puncture and preventing the K value of the wound cell from increasing. Here, the K value refers to the voltage drop of the cell per unit time, used to measure the self-discharge rate of the cell. The higher the K value, the faster the self-discharge of the cell, the more severe the capacity decay, and the shorter the service life. Therefore, the provision of the ion-permeable coating 140 helps to reduce the K value of the wound cell, thereby extending the service life of the wound cell.
[0028] Please see Figure 1 and Figure 2 In some embodiments, the active material layer 120 on both sides of the current collector 110 along its thickness direction is provided with the groove 130, and multiple grooves 130 are provided, which are arranged side by side along the width direction of the current collector 110.
[0029] In some embodiments, the distance between two adjacent grooves 130 along the length of the anode plate 100 is 1 mm to 2.5 mm.
[0030] In this embodiment, grooves 130 are provided on both the front and back sides of the anode plate 100. Specifically, the grooves 130 are disposed on the surfaces of the active material layers 120 on both sides of the current collector 110, with the grooves 130 located on the side of the active material layer 120 facing away from the current collector 110. The grooves 130 are arranged in parallel lines on the active material layers 120 on each side of the current collector 110, and the grooves 130 on both sides are symmetrically arranged with respect to the current collector 110. Providing grooves 130 on the anode plate 100 can shorten the ion transport path on the anode plate 100, reduce the tortuosity of ion transport, and allow ions to move more smoothly between the anode and cathode, reducing energy loss during ion transport and thus improving the charging and discharging efficiency of the wound battery cell.
[0031] Specifically, such as Figure 1 As shown, looking along the length of the anode plate 100, the distance between two adjacent grooves 130 is denoted as L1, and the value of L1 is set within the range of 1mm to 2.5mm. In actual production, the distance L1 between two adjacent grooves 130 can be set to different values such as 1mm, 1.5mm, and 2.5mm. Specifically, if the distance between two adjacent grooves 130 is too large, the number of grooves 130 on the anode plate 100 of the same length will be reduced, and the effect of improving the ion migration speed will not be obvious; if the distance between two adjacent grooves 130 is too small, the process precision requirements will be higher, the manufacturability will be insufficient, and the yield rate during production will be easily affected. Taking a distance L1 of 2.5mm between two adjacent grooves 130 as an example, because the anode plate 100 used in smaller wound cells is shorter, if the distance is greater than 2.5mm, the number of grooves 130 set on the anode plate 100 of the small-sized wound cell will be too low, and the ion migration speed will not be accelerated much, thus failing to improve the charging and discharging efficiency. Taking a spacing L1 of 1 mm between two adjacent grooves 130 as an example, if the spacing is less than 1 mm, it increases the difficulty of creating grooves 130 on the anode plate 100 and reduces the yield of the anode plate 100 during mass production. Taking a spacing L1 of 1.5 mm between two adjacent grooves 130 as an example, a balance can be achieved between process precision and improved ion migration speed.
[0032] This embodiment limits the spacing between two adjacent grooves 130 to between 1mm and 2.5mm, which can avoid the decrease in the number of grooves 130 due to excessive spacing, ensure that the grooves 130 can accelerate the ion migration speed, and at the same time reduce the production difficulty of the grooves 130 and improve the manufacturability of the anode sheet 100.
[0033] Please see Figure 1In some embodiments, the depth of the groove 130 along the thickness direction of the anode sheet 100 is 10 μm to 20 μm.
[0034] In some embodiments, the width of the groove 130 along the length of the anode sheet 100 is 50 μm to 90 μm.
[0035] In this embodiment, the depth of the groove 130 is denoted as d, viewed along the thickness direction of the anode sheet 100, and the value of d is set in the range of 10µm to 20µm. In actual production, the depth d of the groove 130 can be set to different values such as 10µm, 15µm, and 20µm. Specifically, the depth of the groove 130 does not exceed the thickness of the active material layer 120. The deeper the groove 130, the longer the laser etching time on the active material layer 120, because more active material powder is generated during etching, which is more likely to accumulate in the groove 130, making the powder shedding problem more serious. Conversely, the shallower the groove 130, the less significant the improvement effect of the groove 130 on the ion migration speed of the anode sheet 100. Taking a groove depth d of 20µm as an example, if it is greater than 20µm, the groove depth 130 is too high. On the one hand, it is easy to penetrate the active material layer 120 during laser etching, causing damage to the current collector 110. On the other hand, more active material powder tends to accumulate in the groove 130, making it easier for powder to fall off during winding and hot pressing, thus reducing the performance of the wound cell. Taking a groove depth d of 10µm as an example, if it is less than 10µm, the groove depth 130 is too low, and the improvement in the ion migration speed of the anode plate 100 is not significant, resulting in a negligible improvement in charge and discharge efficiency. Setting the groove depth d of 130 to 15µm can ensure improved charge and discharge performance of the wound cell while preventing excessive accumulation of active material powder in the groove 130.
[0036] Looking along the length of the anode sheet 100, the width of the groove 130 is denoted as w, and the value of w is set within the range of 50µm to 90µm. In actual production, the width w of the groove 130 can be set to different values such as 50µm, 70µm, and 90µm. Specifically, for the same reasons as the depth design of the groove 130, the larger the width of the groove 130, the longer the laser etching time on the active material layer 120, because more active material powder is generated during etching, and powder shedding is more likely to occur during the winding of the anode sheet 100; conversely, the smaller the width of the groove 130, the less significant the improvement effect of the groove 130 on the ion migration speed of the anode sheet 100. Taking a groove width w of 90µm as an example, if it is greater than 90µm, the width of the groove 130 is too large, the laser etching time on the active material layer 120 is longer, and too much active material powder is generated in the groove 130, leading to a serious powder shedding problem. Taking a groove width w of 50µm as an example, if it is less than 50µm, the groove width 130 is too small, and the improvement in ion transport speed of the anode plate 100 after setting the groove 130 is not significant. Setting the groove width w of 130 to 70µm can improve the ion transport speed of the anode plate 100 while improving the problem of severe powder shedding, thereby improving the overall quality of the wound cell.
[0037] In this embodiment, by limiting the depth d of the groove 130 to between 10µm and 20µm, and the width w of the groove 130 to between 50µm and 90µm, and with the depth and width of the groove 130 being linearly related, excessive active material powder can be avoided when creating the groove 130 on the active material layer 120, thus improving the problem of powder shedding from the anode sheet 100. It also shortens the ion transport path distance and accelerates the ion transport speed. Furthermore, the depth of the groove 130 does not exceed the thickness of the active material layer 120. This method of setting the groove 130 according to the thickness of the active material layer 120 can accommodate anode sheets 100 of different thicknesses, maximizing energy density.
[0038] In some embodiments, along the width direction of the anode sheet 100, the distance from one end of any of the grooves 130 to the edge of the adjacent active material layer 120 is 0.1 mm to 1.5 mm.
[0039] In this embodiment, viewed along the width direction of the electrode, as shown... Figure 2As shown, the groove 130 is straight, including an upper end and a lower end, and the active material layer 120 includes an upper edge and a lower edge. The distance between the upper end of the groove 130 and the upper edge of the active material layer 120 is denoted as L2, and the distance between the lower end of the groove 130 and the lower edge of the active material layer 120 is denoted as L3. Both L2 and L3 are set within the range of 0.1 mm to 1.5 mm. It should be noted that the values of L2 and L3 can be the same or different. In actual production, the distance L2 between the upper end of the groove 130 and the upper edge of the active material layer 120 can be set to different values such as 0.1 mm, 0.8 mm, and 1.5 mm. Specifically, taking a distance L2 of 0.1 mm as an example, if it is less than 0.1 mm, the edge of the groove 130 and the active material layer 120 will be too close, which will make the edge of the anode sheet 100 more prone to powder shedding and damage. Conversely, taking a distance L2 between the upper end of the groove 130 and the upper edge of the active material layer 120 as 1.5mm as an example, if it is higher than 1.5mm, the groove 130 and the edge of the active material layer 120 will be too far apart. This means the length of the groove 130 is much smaller than the width of the active material layer 120, which will result in a negligible increase in the ion transport speed of the anode plate 100, thus failing to significantly improve the charge and discharge performance of the wound battery cell. Setting the distance L2 between the upper end of the groove 130 and the upper edge of the active material layer 120 to 0.8mm can improve the ion transport speed of the anode plate 100 while minimizing powder shedding and damage at the edge of the anode plate 100. It is understandable that the distance L3 between the lower end of the groove 130 and the lower edge of the active material layer 120 can also be set to values between 0.1mm and 1.5mm, such as 0.1mm, 0.8mm, and 1.5mm. The specific reasons for choosing the value of L3 are the same as those for L2, and will not be repeated here.
[0040] It should be noted that, in a more preferred embodiment, along the width direction of the anode sheet 100, the distance from one end of any groove 130 to the edge of the adjacent active material layer 120 is 0.5 mm to 1 mm. For example, the distance L2 between the upper end of the groove 130 and the upper edge of the active material layer 120, and the distance L3 between the lower end of the groove 130 and the lower edge of the active material layer 120, can be set to 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, and 1 mm. The purpose is to achieve a balance between the length of the groove 130 and the width of the active material layer 120. The length of the groove 130 is set according to the width of the active material layer 120, so that the groove 130 can be adapted to anode sheets 100 of different widths, thereby maximizing energy density.
[0041] In some embodiments, the ion-permeable coating 140 comprises one of polyvinylidene fluoride, polyacrylic acid, sodium carboxymethyl cellulose, and polyethylene oxide.
[0042] In this embodiment, the ion-permeable coating 140 is made of polyvinylidene fluoride (PVDF). The ion-permeable coating 140 formed by PVDF is adhesive, which can tightly bond the active material layer 120 at the groove 130, and also allows ions to pass through the ion-permeable coating 140 without affecting the charge and discharge performance of the wound battery cell.
[0043] In other embodiments, the material of the ion-permeable coating 140 may also be one or more of polyacrylic acid (PPA), sodium carboxymethyl cellulose (CMC), and polyethylene oxide (PEO).
[0044] This application also proposes an electrode assembly, which includes the aforementioned anode plate 100, cathode plate, and diaphragm. The specific structure of the anode plate 100 is as described in the above embodiments. Since this electrode assembly adopts all the technical solutions of all the above embodiments, it possesses at least all the technical effects brought about by the technical solutions of the above embodiments, and will not be elaborated further here. The diaphragm is located between the cathode plate and the anode plate 100, serving to separate the positive anode, prevent short circuits, and allow ions to pass through. Given that the electrode assembly involved in this application has a wound structure, the cathode plate, anode plate 100, and diaphragm are stacked and wound together to form an electrode assembly, i.e., a wound battery cell. The electrode assembly also includes tabs, which can be further divided into cathode tabs and anode tabs. The cathode tabs are connected to the cathode plate, and the anode tabs are connected to the anode plate 100. The tabs are used to connect the electrode assembly and an external circuit, enabling current to flow between the electrode assembly and the external circuit, thereby ensuring that the electrode assembly can provide power to the electronic device normally and stably. Understandably, grooves 130 and ion-permeable coatings 140 can also be provided on the cathode sheet to further improve the performance of the electrode assembly.
[0045] This application further proposes an electrochemical device including the aforementioned electrode assembly. The electrochemical device is a device that converts chemical energy into electrical energy through an electrochemical reaction. In this application, the electrochemical device can be a wound lithium battery. The electrochemical device is used to provide electrical energy to electronic devices. The electronic devices in this application are not particularly limited and can be any electronic device known in the prior art, including but not limited to mobile phones, smartphones, laptops, tablets, wearable devices, smartwatches, etc.
[0046] In summary, this application proposes an anode sheet 100, an electrode assembly, and an electrochemical device. The anode sheet 100 is applied to the electrode assembly, which is a wound battery cell. By providing a groove 130 on the anode sheet 100 and providing an ion-permeable coating 140 in the groove 130, the active material layer 120 at the groove 130 is tightly bonded together, preventing the active material powder from falling onto the diaphragm when the anode sheet 100 is wound, thus preventing the diaphragm from being punctured by the active material powder, thereby improving safety performance. It also helps to reduce the K value of the electrode assembly, thereby extending the service life of the electrochemical device.
[0047] The above description is only a part or preferred embodiment of this application. Neither the text nor the drawings should limit the scope of protection of this application. All equivalent structural transformations made using the content of this application's specification and drawings under the overall concept of this application, or direct / indirect applications in other related technical fields, are included within the scope of protection of this application.
Claims
1. An anode sheet comprising a current collector and an active material layer provided on both sides of the current collector in the thickness direction thereof, characterized in that, The surface of the active material layer is provided with grooves, and the surface of the grooves is provided with an ion-permeable coating, the thickness of which is 7.5 μm to 15 μm.
2. The anode sheet according to claim 1, characterized by The current collector has grooves on the active material layer on both sides along its thickness direction. Multiple grooves are provided, and the multiple grooves are arranged side by side along the width direction of the current collector.
3. The anode sheet according to claim 2, characterized by Along the length of the anode sheet, the distance between two adjacent grooves is 1 mm to 2.5 mm.
4. The anode sheet according to claim 3, characterized by Along the thickness direction of the anode sheet, the depth of the groove is 10 μm to 20 μm.
5. The anode sheet according to claim 4, characterized by Along the length of the anode sheet, the width of the groove is 50 μm to 90 μm.
6. The anode sheet according to claim 5, characterized by Along the width direction of the anode sheet, the distance from one end of any of the grooves to the edge of the adjacent active material layer is 0.1 mm to 1.5 mm.
7. The anode sheet according to claim 6, characterized by Along the width direction of the anode sheet, the distance from one end of any of the grooves to the edge of the adjacent active material layer is 0.5 mm to 1 mm.
8. The anode sheet according to any one of claims 1 to 7, characterized by, The ion-permeable coating comprises one of polyvinylidene fluoride, polyacrylic acid, sodium carboxymethyl cellulose, and polyethylene oxide.
9. An electrode assembly comprising an anode sheet, a cathode sheet and a separator disposed in a stack of layers, characterized in that, The anode plate is the anode plate according to any one of claims 1 to 8.
10. An electrochemical device, characterized by, Includes the electrode assembly as described in claim 9.