Semiconductor device
The semiconductor device integrates a translucent oxide semiconductor electrode and a stacked dielectric film to enhance capacitor capacity and aperture ratio, addressing the limitations of conventional designs by maintaining display quality and reducing power consumption.
Patent Information
- Application Number
- DE102013216824
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2013-08-23
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2033-08-23
AI Technical Summary
Conventional semiconductor devices face challenges in achieving a high aperture ratio and low power consumption while maintaining a high capacity for capacitors, often compromising display quality due to increased electrode overlap areas which reduce the pixel's light transmission.
The semiconductor device incorporates a translucent capacitor with one electrode formed from a light-transmitting oxide semiconductor film, connected to a scan line of an adjacent pixel, and a dielectric film made from a stack of oxide and nitride insulating films, allowing for increased capacitor capacity without additional components, thus enhancing the aperture ratio and reducing power consumption.
This design results in a semiconductor device with improved aperture ratio, higher capacity capacitors, and reduced power consumption, maintaining excellent display quality even at high pixel densities.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Background of the invention 1. Field of the invention
[0001] The invention disclosed in this specification and the like relates to semiconductor devices. 2. Description of the state of the art
[0002] In recent years, flat panel displays such as liquid crystal displays have become widely used. In each of the Pixels arranged in the row direction and in the column direction in a display device such as a flat panel display are a transistor that serves as a switching element, a liquid crystal element that is electrically connected to the transistor and a capacitor connected in parallel with the liquid crystal element.
[0003] As a semiconductor material for forming a semiconductor film of the transistor, a silicon semiconductor is generally used such as amorphous silicon or polysilicon (polycrystalline silicon).
[0004] In addition, metal oxides with semiconductor properties (hereinafter referred to as oxide semiconductors) can be used for Semiconductor films of transistors are used. For example, techniques for forming transistors that zinc oxide or an In-Ga-Zn-based oxide semiconductor (see Patent Documents 1 and 2). [Reference] [Patent document] [Patent Document 1] Japanese Patent Laid-Open No. JP 2007-123861 A [Patent Document 2] Japanese Patent Laid-Open No. JP 2007-096055 A Summary of the invention
[0005] In a capacitor, a dielectric film is arranged between a pair of electrodes, wherein at least one of the pair of electrodes often using a conductive, opaque film to form a gate electrode, a source electrode, a drain electrode or the like of a transistor.
[0006] If the capacitance value of a capacitor is increased, a period can be made longer during whose alignment of liquid crystal molecules of a liquid crystal element is constant in the state when a electric field is applied to it. If this period of time is in a still image displaying display device can be made longer, the frequency of the process of rewriting the Image data can be reduced, resulting in reduced power consumption.
[0007] In one of the methods for increasing the capacitance of a capacitor, the area of the capacitor increased, in particular, the area of an area where a pair of electrodes overlaps each other is increased. However, is when the area of a conductive light-blocking film is increased to increase the area of an area where a pair of electrodes overlaps each other, reducing the aperture ratio of a pixel and thus the display quality of an image deteriorates.
[0008] In view of the above, an object of an embodiment of the present invention is to provide a semiconductor device having a high aperture ratio and including a capacitor having a A further object is to provide a semiconductor device that can have a high aperture ratio, contains a capacitor that can have a higher capacity, and low power consumed.
[0009] An embodiment of the present invention is a semiconductor device in which pixels in the row direction and arranged in the column direction. Each of the pixels contains a transistor and a light-transmitting capacitor. One of a pair of electrodes contained in the capacitor is electrically connected to a scan line contained in a pixel adjacent in the row direction.
[0010] An electrode of the capacitor may be formed of a semiconductor film having a light-transmitting property The semiconductor film with a translucent property can be made of, for example, an oxide semiconductor which has an energy gap greater than or equal to 3.0 eV and a high permeability for visible light.
[0011] The light-transmitting capacitor can be manufactured by applying a manufacturing process of the transistor An electrode of the capacitor can be formed by applying a manufacturing process of a semiconductor film of the An oxide semiconductor film can be used as the semiconductor film of the transistor, and a Transistor having an appropriately processed oxide semiconductor film has a very small off-state current (off-state current). Therefore, the power consumption of a semiconductor device containing such a transistor can be reduced.
[0012] An embodiment of the present invention is a semiconductor device including pixels defined by x (x is an integer 2 or greater) scanning lines and y (y is an integer 1 or greater) signal lines are fixed, and each of the pixels contains a transistor and a capacitor. The transistor contains a Semiconductor film with a light-transmitting property. The capacitor contains a dielectric film between a pair of electrodes and is electrically connected to the transistor. In the capacitor between an (m-1)-th (m is an integer that is 2 or larger and x or smaller) scanning line and an m-th scanning line is used Semiconductor film on the same surface as the semiconductor film with a light-transmitting property of the transistor as one of the pair of electrodes and is electrically connected to the (m-1)th scanning line.
[0013] The dielectric film of the capacitor can be formed by applying a manufacturing process of an insulating film which is arranged above the semiconductor film of the transistor. The other electrode of the capacitor can be formed by applying a manufacturing process of a pixel electrode that is electrically connected to the transistor is connected.
[0014] In other words, the semiconductor device of one embodiment of the present invention includes a Pixel electrode that is electrically connected to the transistor. The pixel electrode serves as the other of the pair of electrodes, and an insulating film over the semiconductor film of the transistor with a light-transmitting property serves as dielectric film.
[0015] With such a structure, the capacitor has a translucent property and can thus be large (in a large area) in a region of the pixel where the transistor is not formed. Consequently, An embodiment of the present invention provides a semiconductor device whose aperture ratio and capacity are increased. In addition, increasing the aperture ratio can make a semiconductor device with excellent display quality. It should be noted that in the semiconductor device of an embodiment of the present invention, the scanning line in the pixel adjacent in the row direction is also referred to as a line (capacitor line) is used to supply a potential to one electrode of the capacitor. As a result, a Capacitor line is not additionally arranged in the pixel; this allows the aperture ratio of the pixel to be higher than that of a conventional semiconductor device.
[0016] In the semiconductor device, when the insulating film over the semiconductor film of the transistor is a stack of an oxide insulating film and a nitride insulating film, the dielectric film of the capacitor is a stack of the oxide insulating film and the nitride insulating film.
[0017] In the case where the insulating film over the semiconductor film of the transistor is a stack of an oxide insulating film and a nitride insulating film, the oxide insulating film is only removed in an area above the capacitor, so that the dielectric film of the capacitor can be a single layer of the nitride insulating film. In other words, the Nitride insulating film is in contact with the oxide semiconductor film, which serves as one electrode of the capacitor. Structure in which a nitride insulating film is in contact with an oxide semiconductor film, a defect level (interface state) at the interface between the nitride insulating film and the oxide semiconductor film When the nitride insulating film is formed by a plasma CVD method or a sputtering method, the Semiconductor film is exposed to a plasma; therefore, oxygen vacancies are created. Furthermore, Nitrogen and / or hydrogen in the nitride insulating film to the semiconductor film. When hydrogen in the nitride insulating film enters the defect levels or the When oxygen vacancies occur, electrons are generated that serve as charge carriers. Consequently, the electrical Conductivity of the semiconductor film is increased, and the semiconductor film has N-type conductivity and serves as a conductive film. The conductivity of the oxide semiconductor film is increased, so that the oxide semiconductor film can be sufficiently and easily used as a electrode of the capacitor. Since the dielectric film can be made thin, the capacitance of the capacitor can be increased.
[0018] An embodiment of the present invention is a semiconductor device including pixels defined by x (x is an integer 2 or greater) scanning lines and y (y is an integer 1 or greater) signal lines are fixed, and each of the pixels contains a transistor and a capacitor. The transistor contains a Semiconductor film with a light-transmitting property. The capacitor contains a dielectric film between a pair of electrodes. Inside the transistor is an insulating film, which is a stack of an oxide insulating film and a Nitride insulating film over the semiconductor film with a translucent property. In the capacitor between an (m-1)-th (m is an integer 2 or greater and x or less) scanning line and an m-th Scanning line is a semiconductor film on the same surface as the semiconductor film with a light-transmitting Property of the transistor as one of the pair of electrodes and is electrically connected to the (m-1)th scanning line. The nitride insulating film in the insulating film serves as a dielectric film.
[0019] Also, in the semiconductor device, a pixel electrode electrically connected to the transistor serves as the other of the pair of electrodes.
[0020] An oxide semiconductor film serving as an electrode of the capacitor may be in direct contact with a scanning line, which serves as a capacitor line and is contained in the adjacent pixel; thus, the Oxide semiconductor film electrically connected to the scanning line. Alternatively, the oxide semiconductor film, which serves as an electrode be electrically connected to the scanning line via a conductive film which is used in a process for forming a source electrode or a drain electrode of the transistor.
[0021] In particular, the conductive film may be in contact with an end portion of the oxide semiconductor film which serves as a For example, the conductive film may be provided in contact with the oxide semiconductor film along its outer periphery. With such a structure, the conductivity of the oxide semiconductor film can be increased The oxide semiconductor film can be easily used as an electrode of the capacitor by increasing its conductivity serve.
[0022] In the semiconductor device, the oxide semiconductor film serving as an electrode of the capacitor is preferably N-type, and its electrical conductivity is preferably increased. In other words, an electrode of the capacitor is preferably an N-type oxide semiconductor film formed on the same surface as the oxide semiconductor film of the transistor and includes an area whose electrical conductivity is higher than that of the oxide semiconductor film. With such a structure, the oxide semiconductor film can be sufficiently and easily used as a electrode of the capacitor. Furthermore, the capacitor can operate stably throughout its entire operating period.
[0023] In order for the oxide semiconductor film to have N-type conductivity and increase its electrical conductivity For example, one or more elements consisting of boron, nitrogen, fluorine, aluminum, phosphorus, arsenic, Indium, tin, antimony and a noble gas element are preferably added to the oxide semiconductor film. Any of the above elements may be added to the oxide semiconductor film by an ion implantation method, a ion doping process or the like, or by exposing the oxide semiconductor film to a plasma containing any of the above elements. In this case, the electrical conductivity of the oxide semiconductor film, which serving as an electrode of the capacitor, higher than or equal to 10 S / cm and lower than or equal to 1000 S / cm, preferably higher than or equal to 100 S / cm and lower than or equal to 1000 S / cm.
[0024] It should be noted that with a structure in which an oxide semiconductor film serving as an electrode of a capacitor serves, as in the above semiconductor device in contact with a nitride insulating film, a step for adding one of the above elements by an ion implantation method, an ion doping method or the like can be omitted. Thus, the yield of a semiconductor device can be improved, and its Manufacturing costs can be reduced.
[0025] In the case where the insulating film disposed over the oxide semiconductor film of the transistor in the semiconductor device is a stack of an oxide insulating film and a nitride insulating film, it is preferable that the oxide insulating film is not easily allows nitrogen to pass through, i.e. has a barrier property against nitrogen.
[0026] With such a structure, it can be prevented that nitrogen enters the oxide semiconductor film of the transistor diffused; thus, fluctuations in the electrical properties of the transistor can be prevented. Consequently, the reliability of the semiconductor device can be improved.
[0027] It should be noted that a method of manufacturing a semiconductor device of an embodiment of the present invention is also an embodiment of the present invention.
[0028] According to an embodiment of the present invention, a semiconductor device can be provided which includes a capacitor whose capacitance is increased while the aperture ratio is improved. Furthermore, a semiconductor device can be provided which has a high aperture ratio and low power consumption and contains a high-capacity capacitor. Short description of the drawings Fig. 1A is a diagram showing a semiconductor device, and Fig. 1B is a circuit diagram of a pixel. Fig. 2 is a diagram showing the relationship between the voltage and capacitance of a capacitor in a semiconductor device. Fig. 3 is a timing chart showing an operating method of a capacitor in a semiconductor device. Fig. 4A and Fig. 4B are diagrams for showing an operating method of a capacitor in a semiconductor device. Fig. 5 is a plan view showing a semiconductor device. Fig. 6 is a cross-sectional view showing a semiconductor device. Fig. 7A and Fig. 7B are cross-sectional views showing a method of manufacturing a semiconductor device show. Fig. 8A and Fig. 8B are cross-sectional views showing a method of manufacturing a semiconductor device show. Fig. 9 is a plan view showing a semiconductor device. Fig. 10A and Fig. 10B are cross-sectional views showing a semiconductor device. Fig. 11 is a plan view showing a semiconductor device. Fig. 12 is a plan view showing a semiconductor device. Fig. 13A and Fig. 13B are cross-sectional views showing a semiconductor device. Fig. 14 is a plan view showing a semiconductor device. Fig. 15 is a cross-sectional view showing a transistor used in a semiconductor device can be. Fig. 16 is a cross-sectional view showing a transistor used in a semiconductor device can be. Fig. 17 is a cross-sectional view showing a transistor used in a semiconductor device can be. Fig. 18 is a plan view showing a semiconductor device. Fig. 19 is a cross-sectional view showing a semiconductor device. Fig. 20A and Fig. 20B are cross-sectional views showing a method of manufacturing a semiconductor device show. Fig. 21 is a cross-sectional view showing a method of manufacturing a semiconductor device. Fig. 22 is a cross-sectional view showing a semiconductor device. Fig. 23 is a plan view showing a semiconductor device. Fig. 24 is a cross-sectional view showing a semiconductor device. Fig. 25A and Fig. 25B are cross-sectional views showing a method of manufacturing a semiconductor device show. Fig. 26A and Fig. 26B are cross-sectional views showing a method of manufacturing a semiconductor device show. Fig. 27 is a cross-sectional view showing a transistor used in a semiconductor device can be. Fig. 28A to Fig. 28C are plan views each showing a semiconductor device. Fig. 29 is a cross-sectional view showing a semiconductor device. Fig. 30A and Fig. 30B are a plan view and a cross-sectional view showing a part of a Scan line driver circuit of a semiconductor device. Fig. 31A to Fig. 31C are a plan view and cross-sectional views, each showing a common Show connection section of a semiconductor device. Fig. 32A to Fig. 32C each show an electronic device incorporating a semiconductor device. Fig. 33A to Fig. 33C show an electronic device incorporating a semiconductor device. Figures 34A to 34D each show a structure of a sample. Fig. 35 is a diagram showing the sheet resistance. Fig. 36A and Fig. 36B show results of SIMS measurements. Figures 37A to 37C show results of ESR measurements. Fig. 38 shows a result of an ESR measurement. Fig. 39 is a graph showing the sheet resistance. Fig. 40 is a graph showing the sheet resistance. Fig. 41A and Fig. 41B each show a bulk model of InGaZnO . 4 Fig. 42A and Fig. 42B show the formation energy and the thermodynamic transition level of VoH. Detailed description of the invention
[0029] Embodiments and examples of the present invention will be described in detail below with reference to accompanying drawings. However, the present invention is not limited to the following description limited, and it will be easily understood by a person skilled in the art that the modes and details can be For this purpose, the present invention should not be considered as limited to the description in the following Embodiments and examples are to be considered limited.
[0030] It should be noted that in structures of the present invention described below, the same sections or sections having similar functions are identified in different drawings by the same reference numerals and that the description thereof is not repeated. In addition, the same hatching pattern is used for Sections that have similar functions, and in some cases the sections are not particularly designated by reference symbols.
[0031] It should be noted that in each drawing in this specification, the size, thickness of a film or area each component is exaggerated in some cases for the sake of clarity. Thus, the embodiments and examples the present invention is not limited to such proportions.
[0032] It should be noted that the ordinal numbers such as ´´first´´ and ´´second´´ in this description and the like used for simplicity and not the order of steps or the sequence sequence of stacked layers. In addition, the ordinal numbers in this description and the like, no special names that determine the present invention.
[0033] The functions of a ´´source´´ and a ´´drain´´ in the present invention are sometimes confused swapped, e.g., when the direction of current flow is changed during circuit operation. Therefore, the expressions ´´Source´´ and ´´Drain´´, in this description are also used to indicate the drain and the source respectively. describe.
[0034] It should be noted that a voltage denotes a difference between potentials of two points, and that a potential is an electrostatic energy (electrical potential energy) of a unit charge on a given point in an electrostatic field. In general, a distinction is made between a Potential of a point and a reference potential (e.g. an earth potential) simply a potential or a voltage and a potential and a voltage are often used as synonyms. Therefore, in this Description a potential can also be expressed as a voltage, and a voltage can also be expressed as a potential unless otherwise specified.
[0035] In this description, in the case where an etching treatment is carried out after a photolithography process is carried out, a mask formed in the photolithography process is removed. (Embodiment 1)
[0036] In this embodiment, a semiconductor device of an embodiment of the present invention described with reference to drawings. It should be noted that in this embodiment, a Liquid crystal display device as an example of the semiconductor device of an embodiment of the present invention is described. <Struktur einer Halbleitervorrichtung>
[0037] Fig. 1A shows an example of a semiconductor device. The semiconductor device in Fig. 1A includes a pixel section 100, a scanning line driver circuit 104, a signal line driver circuit 106, x scanning lines 107, which are arranged parallel or substantially parallel to each other and whose potentials are determined by the Scan line driver circuit 104, and y signal lines 109 which are parallel or substantially parallel to each other and whose potentials are controlled by the signal line driver circuit 106. Let noted that x is an integer greater than or equal to 2, and y is an integer greater than or equal to 1 is.
[0038] In the pixel section 100, pixels 101 including the x scanning lines 107 and the y signal lines 109 are arranged in the row direction and in the column direction. In other words, the pixel section 100 includes the pixels 101 arranged in a matrix of x rows and y columns. In this description, the drawings and Similarly, the m-th scanning line is represented as scanning line 107_m, the n-th signal line is represented by a signal line 109_n, and a pixel in an area where the scanning line 107_m and the signal line 109_n intersect each other is represented by a pixel 101 (m, n). Note that m is an integer greater than or equal to 2 and less than or equal to x, and n is an integer greater than or equal to 1 and less than or is equal to y.
[0039] The scanning line 107_m is electrically connected to the pixels 101 arranged in the m-th row. Signal line 109_n is electrically connected to the pixels 101 arranged in the n-th column.
[0040] In addition, each of the pixels 101 arranged in the m-th row is also electrically connected to a scanning line in a pixel adjacent in the row direction. In particular, a scanning line 107_m-1 is electrically connected to the Pixels 101 arranged in the (m-1)th row and the pixels 101 arranged in the mth row, tied together.
[0041] Fig. 1B is an example of a circuit diagram of the pixel 101 (m, n) in the semiconductor device in Fig. 1A. The pixel 101 (m, n) in Fig. 1B includes a transistor 103, a capacitor 105 and a liquid crystal element 108. The Transistor 103 is electrically connected to the scanning line 107_m and the signal line 109_n. One electrode of the Capacitor 105 is electrically connected to the scanning line 107_m-1, and the other electrode of the capacitor 105 is a pixel electrode 121 which is electrically connected to the trans sistor 103. In the liquid crystal element 108 there is an electrode (counter electrode) which is connected to the pixel electrode 121 opposite, electrically connected to a line for supplying a counter potential.
[0042] In the pixel 101 (m, n), the scanning line 107_m-1 also serves as a line (capacitor line) for supplying a Potential to one electrode of the capacitor 105.
[0043] A semiconductor film included in the transistor 103 is an oxide semiconductor film. A transistor having a suitable conditions processed oxide semiconductor film as a semiconductor film with a channel formation region, can have a very small reverse current. Consequently, transistor 103 is a transistor with a very small reverse current.
[0044] The capacitor 105 has a dielectric film between the pair of electrodes and has a light-transmitting property. The capacitor 105 can be formed by applying a manufacturing process of the transistor 103 One electrode of the capacitor 105 is a semiconductor film having a light-transmitting property, in particular, an oxide semiconductor film 119. The oxide semiconductor film 119 serves as an electrode of the capacitor 105 when the oxide semiconductor film 119 is brought into a conductive state by controlling a potential applied thereto. The Oxide semiconductor film 119 is an oxide semiconductor film formed by applying a manufacturing process of an oxide semiconductor film 111 is formed in the transistor 103. The dielectric film is an insulating film that has a light-transmitting property and is arranged over the oxide semiconductor film 111 in the transistor 103. The pixel electrode 121 serves as the other electrode of the capacitor 105. Thus, the capacitor 105 can be designed as a metal oxide semiconductor (metal oxide semiconductor: MOS) capacitor. A MOS capacitor is charged when, as shown in Fig. 2, a Voltage higher than the threshold voltage (Vth) to one electrode of the MOS capacitor (to the pixel electrode 121 in the case of capacitor 105). It should be noted that in Fig. 2 the horizontal axis represents a voltage (V), applied to the pixel electrode and the vertical axis represents a capacitance (C). In the case where the Frequency of a voltage at the time of the capacitance-voltage (CV) measurement is lower than the frame rate of the semiconductor device, CV curves are obtained as shown in Fig. 2. In Fig. 2, a solid line a CV curve in the case of an I-type electrode, and a dashed line is a CV curve in the case of an N-type electrode. Type.
[0045] The liquid crystal element 108 is an element that allows the transmission or non-transmission of light through a optical modulation action of a liquid crystal between a substrate connected to the transistor 103 and the pixel electrode 121, and a substrate provided with the counter electrode. The optical Modulation action of the liquid crystal is controlled by an electric field (a vertical electric field or a diagonal electric field) applied to the liquid crystal. In the case where the counter electrode (also called common electrode) is formed over the substrate over which the pixel electrode is formed, a lateral electric field applied to the liquid crystal.
[0046] The scanning line driver circuit 104 and the signal line driver circuit 106 are each roughly divided into a logic circuit section and a switch section or a buffer section. Although concrete structures of the Scan line driver circuit 104 and the signal line driver circuit 106 are omitted here, a transistor included in both the scan line driver circuit 104 and the signal line driver circuit 106.
[0047] It should be noted that the transistor in the scan line driver circuit 104 and / or the Signal line driver circuit 106 can be formed by applying the manufacturing process of the transistor 103 In other words, the scan line driver circuit 104 and / or the signal line driver circuit 106 can be provided over a substrate over which the transistor 103 and the pixel electrode 121 are arranged. On In this way, the scanning line driver circuit 104 and / or the signal line driver circuit 106 are the same substrate, whereby the number of components of the semiconductor device can be reduced and the production costs can be reduced.
[0048] The capacitor 105 has, as described above, a light-transmitting property and can therefore be large (in a large area) in a region of the pixel 101 (m, n) in which the transistor 103 is not formed. The semiconductor device in Fig. 1A and Fig. 1B is a semiconductor device whose aperture ratio and capacitance are increased and their display quality is excellent. Furthermore, in the semiconductor device in Fig. 1A and Fig. 1B the sampling line 107_m-1 also as capacitor line of the capacitor 105; thus, a capacitor line does not need to be provided additionally. Consequently, the Aperture ratio of the pixel in the semiconductor device in Fig. 1A and Fig. 1B is higher than that of a pixel in a conventional semiconductor device. For example, if the pixel density of the semiconductor device in one embodiment of the present invention is about 300 ppi, the aperture ratio of the pixel is 50% or higher, 55% or higher, or even 60% or higher. In one embodiment of the present invention, a Semiconductor device whose aperture ratio of a pixel is higher than that of the pixel in the conventional semiconductor device is made can be easily achieved.
[0049] Now, the operation of the capacitor 105 in the pixel 101 (m, n) will be described. Fig. 3 is a timing diagram of the Signal line 109_n, scanning line 107_m-1, scanning line 107_m and pixel electrode 121. The timing diagram shows a change in the potential of each of the signal line 109_n, the scanning line 107_m-1, the scanning line 107_m and the pixel electrode 121. The potential of each of the signal line 109_n, the scanning line 107_m-1, the scanning line 107_m and the pixel electrode 121 is changed when a signal is input.
[0050] In a period before a time T1, a certain signal (image signal or the like) is extracted from the signal line driver circuit 106 into the signal line 109_n. During this period, a signal is Turning on the transistor 103 from the scan line driver circuit 104 neither into the scan line 107_m-1 nor into the Scanning line 107_m is input. Furthermore, no signal is input to pixel electrode 121 during this period.
[0051] In a period from time T1 to time T2 (period T1T2), a certain signal such as in the period before time T1 is input to the signal line 109_n. In the period T1T2, a signal is input to the Turning on a transistor in a pixel 101 (m-1, n) is input to the scanning line 107_m-1 so that the potential the scanning line 107_m-1 is increased. A signal to turn on the transistor 103 is not input to the scanning line 107_m entered in the period T1T2.
[0052] Furthermore, the potential of the pixel electrode 121 is increased in the period T1T2. The potential of the pixel electrode 121 is increased (changed) in the following way. Since the scanning line 107_m-1 is electrically connected to the oxide semiconductor film 119 which serves as one electrode of the capacitor 105, the potential of one electrode (the oxide semiconductor film 119) is changed when the potential of the scanning line 107_m-1 is changed. The pixel electrode 121, the serves as the other electrode of the capacitor 105, faces one electrode, wherein the dielectric film in between. Therefore, the potential of the pixel electrode 121 is changed according to the potential of one electrode. Consequently, the potential of the pixel electrode 121 is changed according to the potential of the scanning line 107_m-1. noted that the potential of the pixel electrode 121 is set in a manner similar to that of the scanning line 107_m-1, is changed.
[0053] In a period from time T2 to time T3 (period T2T3), a signal is sent to Turning off the transistor in the pixel 101 (m-1, n) is input to the scanning line 107_m-1, so that the potential of the Scanning line 107_m-1 is reduced at time T2. Since the potential of the pixel electrode 121 is reduced according to the potential the scanning line 107_m-1 is changed, the potential of the pixel electrode 121 at the time T2 is as in the Scan line 107_m-1 reduced.
[0054] In the period T2T3, a signal for turning on the transistor 103 is input to the scanning line 107_m, so that the potential of the scanning line 107_m is increased. A signal for the desirable operation of the Liquid crystal element 108 is input to the signal line 109_n in the period T2T3. The transistor 103 is in the period T2T3, so that the signal input to the signal line 109_n is input to the pixel electrode 121 which is electrically connected to the transistor 103. As a result, the potential of the pixel electrode 121 to the same level as the potential of the signal line 109_n. The potential of the pixel electrode 121 is increased as above described; thus the capacitor 105 can operate.
[0055] It should be noted that in a period after the time T3, a certain signal as in the period before the time T1 is input into the signal line 109_n. In the period after the time T3, the potential the pixel electrode 121 is maintained at the potential that has been increased in the period T2T3. In particular, the Potential is held until the potential of the scanning line 107_m-1 is changed again.
[0056] It should be noted that the period T1T2 is very short. The period T1T2 ends before liquid crystals in the liquid crystal element 108. Therefore, it can be said that an influence of the optical modulation action on the Liquid crystal is very small and that the optical modulation action does not affect the display quality of the semiconductor device affected even if the potential of the pixel electrode 121 is changed.
[0057] Here, the relationship between the threshold voltage (Vth) of the capacitor, the potential of the scanning line 107_m, the potential of the scanning line 107_m-1, the intermediate potential of an image signal and the potential the pixel electrode 121 is described below using Fig. 4A and Fig. 4B.
[0058] Fig. 4A shows an example in which a capacitor with properties indicated by the solid line CV curve shown in Fig. 2. Fig. 4B shows an example using a capacitor with properties represented by the dashed CV curve in Fig. 2. It should be noted that in Fig. 4A and Fig. 4B the The lowest potential supplied to the scanning line 107_m is represented by GVss and the highest potential supplied to the scanning line 107_m is represented by GVdd.
[0059] The capacitor includes a dielectric film between the pair of electrodes. In other words, the The operation of the capacitor depends on the potential difference between the pair of electrodes. For example, when the threshold voltage of the capacitor, the potential of the pixel electrode 121 and the potential of the oxide semiconductor film 119, which serves as the electrode of the capacitor, are represented by Vth, Vd and Vc, respectively, the relationship Vd ≥ Vc + Vth required.
[0060] As shown in Fig. 4A and Fig. 4B, the potential of the pixel electrode 121, which is the electrode of the capacitor 105 is, according to a signal input to the signal line 109_n, in the positive direction or in the negative direction. In particular, the potential of the pixel electrode 121 is changed in the positive direction or in the negative direction changed with respect to the average level of an image signal.
[0061] In the case of Fig. 4A, the potential of the scanning line 107_m-1 is set to Vth of the capacitor or to be lower than the lowest potential of the pixel electrode 121 so that the above relationship can be satisfied; Thus, the capacitor can be operated (see Fig. 4A). This is because, since the electrode of the capacitor is Properties represented by the solid CV curve in Fig. 2, is of I-type and Vth is a positive value is, the oxide semiconductor film 119 may be in a conductive state when the potential of the scanning line 107_m- 1 is set lower than the lowest potential of the pixel electrode 121 by Vth of the capacitor or more (turn shifts in a negative direction).
[0062] On the other hand, in the case of Fig. 4B, the potential of the scanning line 107_m-1 is set to be Vth of the capacitor or more higher than the lowest potential of the pixel electrode 121, so that the above relationship can be fulfilled; thus, the capacitor can be operated (see Fig. 4B). This is because, since the electrode of the capacitor with properties represented by the dashed CV curve in Fig. 2 is of N-type and Vth is a negative value, the oxide semiconductor film 119 may be in a conductive state when the potential of the Scanning line 107_m-1 to higher than the lowest potential of the pixel electrode 121 by Vth of the capacitor or more is adjusted (shifts in a positive direction).
[0063] Next, the concrete structural example for the pixel 101 will be described. Here, the pixel 101 (m, n) is defined as example. Note that Fig. 5 is a top view of pixel 101 (m, n). In Fig. 5, some Components (e.g., the liquid crystal element 108) of the semiconductor device are omitted for clarity.
[0064] In Fig. 5, the scanning line 107_m-1 and the scanning line 107_m are arranged such that they are in the direction which is substantially perpendicular to the signal line 109_n and a signal line 109_n+1 (in transverse direction in the drawing). The signal line 109_n and the signal line 109_n+1 are arranged to be in the direction that is substantially perpendicular to the scanning line 107_m-1 and the scanning line 107_m (in longitudinal direction in the drawing). It should be noted that the scanning line 107_m-1 and the scanning line 107_m are electrically connected to the scanning line driver circuit 104, while the signal line 109_n and the Signal line 109_n+1 are electrically connected to the signal line driver circuit 106 (see Fig. 1A).
[0065] The transistor 103 is arranged in a region in which the scanning line 107_m and the signal line 109_n The transistor 103 includes at least the oxide semiconductor film 111 having a channel formation region, a Gate electrode, a gate insulating film (not shown in Fig. 5), a source electrode and a drain electrode.
[0066] In addition, the scanning line 107_m includes a region serving as the gate electrode of the transistor 103, and The signal line 109_n includes a region that serves as the source electrode of the transistor 103. A conductive film 113 includes a region serving as the drain electrode of the transistor 103 and is electrically connected to the pixel electrode 121 connected by an opening 117. In Fig. 5, the hatching pattern of the pixel electrode 121 is not shown.
[0067] The region in the scanning line 107_m serving as a gate electrode overlaps at least with the Oxide semiconductor film 111. The region in the signal line 109_n serving as a source electrode overlaps at least with the Oxide semiconductor film 111. The region in the conductive film 113 serving as a drain electrode overlaps at least with the Oxide semiconductor film 111. It should be noted that in the following description, the scanning line 107_m is referred to as the Scanning line 107_m is referred to, even if it indicates the gate electrode of the transistor 103, the signal line 109_n referred to as the signal line 109_n, even though it indicates the source electrode of the transistor 103, and the conductive film 113 is referred to as the conductive film 113 even though it indicates the drain electrode of the transistor 103.
[0068] The capacitor 105 is arranged in a region separated by the scanning line 107_m, the scanning line 107_m-1, the signal line 109_n and the signal line 109_n+1. The capacitor 105 includes the oxide semiconductor film 119, the pixel electrode 121 having a light-transmitting property and the insulating film (not shown in Fig. 5) having a light-transmitting property in the transistor 103, and has a light-transmitting property. In addition, since the Oxide semiconductor film 119 is in contact with the scanning line 107_m-1 through an opening 123, the capacitor 105 electrically connected to the scanning line 107_m-1. In other words, the scanning line 107_m-1 also serves as Capacitor line of the capacitor 105. Thus, the capacitor 105 can be used without additional capacitor line in the Pixel 101 (m, n) work.
[0069] The capacitance of a capacitor changes depending on the overlapping area of a pair of electrodes. When the size of a pixel is reduced to increase the resolution, the size of a capacitor is also reduced; thus, the capacitance of the capacitor is reduced. As a result, a liquid crystal element may not be effective Since the capacitor 105 transmits light, the capacitor 105 can be used in the entire operating range of the liquid crystal element 108, and thus the capacitor 105 can be made as large as possible (in a large area) in the pixel. As long as the capacitance required to operate the liquid crystal element 108 is enough, the pixel density can be increased to achieve high resolution.
[0070] Now, the characteristics of a transistor comprising an oxide semiconductor will be described. It should be noted that that the transistor comprising an oxide semiconductor is an N-channel transistor. Oxygen vacancies in a Oxide semiconductors could generate charge carriers, which could affect the electrical properties and reliability of the transistor For example, in some cases the threshold voltage of the transistor is negatively shifted, and a drain current flows when the gate voltage is 0 V. The properties of a transistor in which a Drain current flows when the gate voltage is 0 V, are called ´´normally on´´- (normally on) properties, while the properties of a transistor in which essentially no drain current flows, when the gate voltage is 0 V, are referred to as ´´normally off´´ characteristics.
[0071] In view of the above, it is preferable that defects, which are typically oxygen vacancies, are in a Oxide semiconductor film should be reduced as much as possible when using the oxide semiconductor film. For example, the Spin density of the oxide semiconductor film (the density of defects in the oxide semiconductor film) at a g-value of 1.93, which is measured by electron spin resonance, with a magnetic field parallel to the film surface is applied, preferably to a value lower than or equal to the lower detection limit of a measuring device If the defects, which are typically the oxygen vacancies, in the oxide semiconductor film are reduced as much as possible reduced, it can prevent the transistor from showing ´´normally on´´ behavior, which can lead to Improvement of the electrical properties and reliability of a semiconductor device.
[0072] The shift of the threshold voltage of a transistor in the negative direction is in some cases caused by hydrogen (including a hydrogen compound such as water) in an oxide semiconductor film and by oxygen vacancies Hydrogen contained in the oxide semiconductor film reacts with oxygen bound to a metal atom bound to become water, and in addition, vacancies (also called oxygen vacancies) are formed in a Grid from which oxygen is released (or in an area from which oxygen is released), In addition, part of the hydrogen reacts with oxygen, which releases electrons that serve as charge carriers Therefore, a transistor that includes an oxide semiconductor film containing hydrogen is highly likely to have ´´normally on´´ properties.
[0073] Consequently, it is preferable that hydrogen in the oxide semiconductor film 111 of the transistor 103 is as much as possible In particular, the hydrogen concentration in the oxide semiconductor film 111, which is caused by secondary ion 18 3 18 Mass spectrometry (SIMS) is lower than 5 × 10 atoms / cm , preferably lower than or equal to 1 × 10 3 17 3 atoms / cm , more preferably lower than or equal to 5 × 10 atoms / cm , even more preferably lower than or 16 3 equal to 1 × 10 atoms / cm .
[0074] Furthermore, the concentration of alkali metals or alkaline earth metals in the oxide semiconductor film 111 determined by SIMS 18 3 16 3 measured, lower than or equal to 1 × 10 atoms / cm , preferably lower than or equal to 2 × 10 atoms / cm . When an alkali metal and an alkaline earth metal are bonded to an oxide semiconductor, a charge carrier could be generated which could cause an increase in the reverse current of transistor 103.
[0075] Furthermore, when nitrogen is contained in the oxide semiconductor film, charge carriers Electrons are generated and the charge carrier density increases, so that the oxide semiconductor film easily becomes an N-type oxide semiconductor. Consequently, a transistor that includes the oxide semiconductor film containing nitrogen has most likely ´´normally on´´ properties. For this reason, nitrogen in the oxide semiconductor film 111 as much as possible; for example, the nitrogen concentration is preferably lower than 18 3 or equal to 5 × 10 atoms / cm .
[0076] Furthermore, when a group 14 element such as silicon and carbon is present in the Oxide semiconductor film is contained, electrons serving as charge carriers are generated and the charge carrier density increases, so that the oxide semiconductor film easily becomes an N-type oxide semiconductor. Therefore, in the transistor 103, which Oxide semiconductor film 111 includes, in particular, at the interface between a gate insulating film 127 (not shown in Fig. 5 shown) and the oxide semiconductor film 111, the silicon concentration measured by SIMS is lower than or equal to 18 3 17 3 3 × 10 atoms / cm , preferably lower than or equal to 3 × 10 atoms / cm . It should be noted that at the interface 18 3 the carbon concentration measured by SIMS is lower than or equal to 3 × 10 atoms / cm , preferably 17 3 less than or equal to 3 × 10 atoms / cm.
[0077] As described above, when the highly purified oxide semiconductor film 111 is used, which impurities (such as hydrogen, nitrogen, silicon, carbon, an alkali metal or an alkaline earth metal) are as much as possible, preventing the transistor 103 ´´normally on´´ behavior so that the reverse current of the transistor 103 can be greatly reduced. Therefore, an embodiment of the The present invention provides a semiconductor device with favorable electrical properties and high reliability. It should be noted that the highly purified oxide semiconductor is known as an intrinsic semiconductor or essentially intrinsic semiconductor can be considered.
[0078] It should be noted that various experiments have shown a small reverse current of a transistor which has a highly purified oxide semiconductor film. Even if, for example, an element has a channel width W of 6 1 × 10 µm and a channel length L of 10 µm, the reverse current can be less than or equal to the measurement limit of a -13 semiconductor parameter analyzer, ie less than or equal to 1 × 10 A at voltages (drain voltages) between a source and a drain of 1 V to 10 V. In this case, one finds that the reverse current is corresponding to a The value obtained by dividing the reverse current by the channel width of the transistor is less than or equal to 100 zA / µm. In addition, the reverse current was measured using a circuit in which a capacitor and a transistor are connected to each other and a charge flowing into or out of the capacitor is controlled by the transistor In the measurement, a highly purified oxide semiconductor film was used for a channel formation region of the transistor used, and the blocking current of the transistor is according to a change in the amount of charge of the capacitor per unit time. The result was that in the case where the voltage between the source electrode and the drain electrode of the transistor is 3 V, a smaller reverse current of several tens of yoctoamperes per micrometer (yA / µm) can be obtained. Accordingly The transistor, which contains a highly purified oxide semiconductor film, has a very small reverse current.
[0079] A cross-sectional view along the dot-dash line A1-A2 and the dot-dash line B1-B2 in Fig. 5 is shown in Fig. 6 shown.
[0080] A cross-sectional structure along the dot-dash line A1-A2 and the dot-dash line B1-B2 is as follows. The scanning line 107_m and the scanning line 107_m-1 are arranged on a substrate 102, each of which has a gate The gate insulating film 127 is formed over the scanning line 107_m-1 and the scanning line 107_m. The oxide semiconductor film 111 is arranged over the gate insulating film 127 in such a way that it is Scan line 107_m overlaps. The opening 123, which reaches the scan line 107_m-1, is in a region of the gate insulating film 127, which is in contact with the scanning line 107_m-1. The oxide semiconductor film 119 is arranged over the Gate insulating film 127 and in the opening 123. The signal line 109_n, which has a source electrode serving area, and the conductive film 113, which has a region serving as a drain electrode, are respectively arranged over the oxide semiconductor film 111 and the gate insulating film 127. An insulating film 129, an insulating film 131 and an insulating film 132, which serve as insulating protective films of the transistor 103, are formed over the gate insulating film 127, the signal line 109_n, the oxide semiconductor film 111, the conductive film 113 and the oxide semiconductor film 119. The Opening 117, which reaches the conductive film 113, is in the insulating film 129, the insulating film 131 and the insulating film 132 provided, and the pixel electrode 121 is provided in the opening 117. It should be noted that a base insulating film between the substrate 102, and the scanning lines 107_m-1 and 107_m and the gate insulating film 127 can.
[0081] The cross-sectional structure of the liquid crystal element 108 is as follows. An opaque film 152 is formed on a Surface of a substrate 150 facing the substrate 102, arranged to be connected at least to the transistor 103 A counter electrode 154, which is a conductive film with a light-transmitting property, is arranged to to cover the light-blocking film 152. An alignment film 156 is arranged to cover the counter electrode. On the side of the substrate 102, an alignment film 158 is disposed over the insulating film 132 and the pixel electrode 121. A Liquid crystal 160 is arranged in contact with the alignment film 156 and the alignment film 158, and is between the substrate 102 and the substrate 150.
[0082] It should be noted that in the case where the semiconductor device of an embodiment of the present invention is a liquid crystal display device, a light source such as a backlight, an optical Component (an optical substrate), such as a polarizing plate, which is arranged on the side of the substrate 102 and the side of the Substrate 105, a sealing material for fixing the substrate 102 and the substrate 150 and the like required. These components are described below.
[0083] As described above, in the capacitor 105 described in this embodiment, the Oxide semiconductor film 119 as one of a pair of electrodes, the pixel electrode 121 serves as the other of the pair of electrodes, and the insulating films 129, 131 and 132 serve as a dielectric film between the pair of electrodes.
[0084] The details of the components of the given structure are described below.
[0085] There is no particular limitation on the property of a material and the like of the substrate 102, as long as the material has a heat resistance high enough to withstand at least one to withstand the heat treatment carried out during the semiconductor device manufacturing process. Examples of the substrate are a glass substrate, a ceramic substrate and a plastic substrate, and as the glass substrate, a alkali-free glass substrate such as a barium borosilicate glass substrate, an aluminoborosilicate glass substrate or a Aluminosilicate glass substrate is used. Alternatively, a non-transparent substrate such as a stainless steel alloy substrate, in which case a surface of the substrate is preferably coated with a insulating film. Alternatively, one of the following can be used as the substrate 102: a quartz substrate, a Sapphire substrate, a single-crystalline semiconductor substrate, a polycrystalline semiconductor substrate, a Compound semiconductor substrate and a silicon on insulator (SOI) substrate. In the case where the semiconductor device an embodiment of the present invention is a transmissive liquid crystal display device, a substrate having a light-transmitting property is used as the substrate 102.
[0086] The scanning lines 107_m-1 and 107_m through which a large amount of current flows are preferably formed to have a single-layer structure or a stacked layer structure using a metal film, typically one made of one of metal materials such as molybdenum (Mo), titanium (Ti), tungsten (W), tantalum (Ta), Aluminium (Al), copper (Cu), chromium (Cr), neodymium (Nd) or scandium (Sc) or an alloy material which is one of of these materials as the main component.
[0087] Examples of the scanning lines 107_m-1 and 107_m are a single-layer structure made of silicon-containing Aluminum, a two-layer structure where titanium is stacked over aluminum, a two-layer structure where Titanium is stacked over titanium nitride, a two-layer structure where tungsten is stacked over titanium nitride, a two-layer structure in which tungsten is stacked over tantalum nitride, a two-layer structure in which copper is stacked over a copper-magnesium-aluminium alloy, and a three-layer structure in which titanium nitride, copper and Tungsten are stacked in this order.
[0088] As a material for the scanning lines 107_m-1 and 107_m, a light-transmitting conductive material can be used which can be used for the pixel electrode 121. It should be noted that in the case where the Semiconductor device of an embodiment of the present invention is a reflective display device, a non-transparent conductive material (e.g., a metal material) can be used for the pixel electrode 121. In In this case, a non-light-transmitting substrate may similarly be used as the substrate 102.
[0089] In addition, as a material for the scanning lines 107_m-1 and 107_m, a metal oxide containing nitrogen may be used. in particular an In-Ga-Zn-based oxide containing nitrogen, an In-Sn-based oxide containing nitrogen, an oxide In-Ga base containing nitrogen, an In-Zn based oxide containing nitrogen, an Sn based oxide containing nitrogen an In-based oxide containing nitrogen, or a metal nitride (InN, SnN, or the like) may be used. These materials each have a work function greater than or equal to 5 eV (electron volts). The use of a metal oxide containing nitrogen for the scanning line (the gate electrode) allows the threshold voltage of the Transistor 103 in the positive direction; this means that the transistor is ´´normally off´´- properties. For example, in the case where an In-Ga-Zn-based oxide containing nitrogen is used, an In-Ga-Zn based oxide with a nitrogen concentration at least higher than that of the oxide semiconductor film 111, in particular an In-Ga-Zn based oxide with a nitrogen concentration of 7 atomic% or higher can be used.
[0090] It is preferable to use aluminum or copper, which is a low-resistance material, for the scanning lines 107_m-1 and 107_m. If aluminum or copper is used, signal delay is reduced, so that the Display quality can be improved. It should be noted that aluminum has low heat resistance; Therefore, defects caused by a hump, a hair, or a migration are highly likely. To prevent the migration of aluminum, a stacked layer structure is preferably used, which contains aluminum and a Metal material with a higher melting point than aluminum, such as molybdenum, titanium or tungsten, is used. When copper is used, a stacked layer structure comprising copper and a metal material having a higher melting point than copper, such as molybdenum, titanium or tungsten, is used to repair a defect resulting from to avoid migration and diffusion of copper elements.
[0091] As shown in Fig. 5 and Fig. 6, preferably the scanning line 107_m (the scanning line 107_m-1) is such arranged so that the oxide semiconductor film 111 can be arranged in a region which is connected to the scanning line 107_m It is preferable that, as shown in Fig. 5, the scanning line 107_m protrudes into an area where the oxide semiconductor film 111 is arranged, and that the oxide semiconductor film 111 is arranged in the region which is connected to the scanning line 107_m. In this way, light passing through one surface (the rear surface) of the substrate 102 which is opposite to a surface provided with the scanning line 107_m (in a Liquid crystal display device, such light corresponds to light from a light source such as a backlight), shielded from the scanning line 107_m; thus, fluctuation or deterioration the electrical properties of the transistor 103 (e.g. threshold voltage) are suppressed.
[0092] The gate insulating film 127 is provided to have a single-layer structure or a stacked layer structure which, for example, contains one or more insulating materials such as silicon zium oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, aluminum oxide, hafnium oxide, gallium oxide and a metal oxide Ga-Zn based. It should be noted that a region in the gate insulating film 127 that is at least in contact with the oxide semiconductor film 111, preferably has an oxide insulating film to improve the properties of the interface between the gate insulating film 127 and the oxide semiconductor film 111.
[0093] By providing an insulating film having a barrier property against oxygen, hydrogen, water and such as the gate insulating film 127, it is possible to diffuse oxygen in the oxide semiconductor film 111 to the outside and prevent entry of hydrogen, water or the like into the oxide semiconductor film 111 from the outside. Regarding the Insulating film with a barrier property against oxygen, hydrogen, water and the like can be a aluminum oxide film, an aluminum oxynitride film, a gallium oxide film, a gallium oxynitride film, an yttrium oxide film, a Yttrium oxynitride film, a hafnium oxide film, a hafnium oxynitride film and a silicon nitride film are given as examples become.
[0094] The gate insulating film 127 may be formed using a high-k material such as hafnium silicate (HfSiO ). x Hafnium silicate containing nitrogen (HfSi ON ), hafnium aluminate containing nitrogen (HfAl ON ), hafnium oxide or xyzxyz Yttrium oxide, so that the gate leakage current of the transistor 103 can be reduced.
[0095] The gate insulating film 127 preferably has the following stacked layer structure. In the structure, the first Silicon nitride film a silicon nitride film with fewer defects arranged, a silicon nitride film from which little hydrogen and ammonia are released, is arranged as a second silicon nitride film over the first silicon nitride film, and a of oxide insulating films applicable as the gate insulating film 127 is disposed over the second silicon nitride film.
[0096] In the second silicon nitride film, the number of released hydrogen molecules in the thermal desorption 21 3 21 3 Spectrometry preferably less than 5 × 10 molecules / cm , more preferably less than or equal to 3 × 10 molecules / cm 21 3 , more preferably less than or equal to 1 × 10 molecules / cm , and the number of released 22 3 21 Ammonia molecules is preferably less than 1 × 10 molecules / cm , more preferably less than or equal to 5 × 10 3 21 3 molecules / cm , more preferably less than or equal to 1 × 10 molecules / cm . The first silicon nitride film and the second silicon nitride film are used as parts of the gate insulating film 127, so that a gate insulating film with little Defects and little released hydrogen and released ammonia as the gate insulating film 127 formed Consequently, it is possible to control the amount of hydrogen and nitrogen in the gate insulating film 127, which is oxide semiconductor film 111.
[0097] In the case where the trap level (also called interface state) at the interface between an oxide semiconductor film and a gate insulating film or in the gate insulating film in a transistor having a oxide semiconductor is present, a change in the threshold voltage of the transistor, as typically a change in the threshold voltage in the negative direction and an increase in the sub-threshold stroke (subthreshold swing) (S value), which provides a gate voltage to change the drain current by one digit when the transistor. Thus, there is a problem that electrical properties between the transistors For this reason, if the silicon nitride film with few defects is used as the gate insulating film 127, is used, and when the oxide insulating film is arranged in a region of the gate insulating film 127 which is in contact with the oxide semiconductor film 111, a negative shift of the threshold voltage and an increase of an S value be suppressed.
[0098] The thickness of the gate insulating film 127 is greater than or equal to 5 nm and less than or equal to 400 nm, preferably greater than or equal to 10 nm and less than or equal to 300 nm, more preferably greater than or equal to 50 nm and less than or equal to 250 nm.
[0099] The oxide semiconductor film 111 may have an amorphous crystal structure, a single-crystalline structure, or a polycrystalline structure. The thickness of the oxide semiconductor film 111 is greater than or equal to 1 nm and less than or equal to 100 nm, preferably greater than or equal to 1 nm and less than or equal to 50 nm, more preferably greater than or equal to 1 nm and less than or equal to 30 nm, more preferably greater than or equal to 3 nm and less than or equal to 20 nm.
[0100] Furthermore, an oxide semiconductor that can be used for the oxide semiconductor film 111 has an energy gap of greater than or equal to 2 eV, preferably greater than or equal to 2.5 eV, more preferably greater than or equal to 3 eV. The reverse current of the transistor 103 can be reduced by using an oxide semiconductor with a large energy gap is used in this way.
[0101] An oxide semiconductor containing at least indium (In) or zinc (Zn) is preferably used for the oxide semiconductor film 111 is used. Alternatively, both In and Zn are preferably included. To compensate for fluctuations in the electrical To reduce the properties of the transistors containing the oxide semiconductor, the oxide semiconductor preferably contains one or more stabilizers in addition to In and Zn.
[0102] Regarding the stabilizers, gallium (Ga), tin (Sn), hafnium (Hf), aluminum (Al) and zirconium (Zr) can be used as Examples are given. Lanthanides such as lanthanum (La), cerium (Ce), praseodymium (Pr), Neodymium (Nd), Samarium (Sm), Europium (Eu), Gadolinium (Gd), Terbium (Tb), Dysprosium (Dy), Holmium (Ho), Erbium (Er), Thulium (Tm), ytterbium (Yb) and lutetium (Lu) are given as examples.
[0103] As the oxide semiconductor that can be used for the oxide semiconductor film 111, for example, the following used: indium oxide, tin oxide or zinc oxide; an oxide containing two types of metals such as an oxide In-Zn-based oxide, Sn-Zn-based oxide, Al-Zn-based oxide, Zn-Mg-based oxide, Sn-Mg-based oxide, In-Mg-based oxide or In-Ga-based oxide; an oxide containing three kinds of metals such as an In- Ga-Zn-based (also called IGZO), an In-Al-Zn-based oxide, an In-Sn-Zn-based oxide, an Sn-Ga-Zn-based oxide base, an Al-Ga-Zn-based oxide, an Sn-Al-Zn-based oxide, an In-Hf-Zn-based oxide, an In-Zr-Zn-based oxide, a In-Ti-Zn-based oxide, In-Sc-Zn-based oxide, In-Y-Zn-based oxide, In-La-Zn-based oxide, In- Ce-Zn-based, an In-Pr-Zn-based oxide, an In-Nd-Zn-based oxide, an In-Sm-Zn-based oxide, an In-Eu-Zn-based oxide, a In-Gd-Zn-based oxide, In-Tb-Zn-based oxide, In-Dy-Zn-based oxide, In-Ho-Zn-based oxide, In-Er-Zn-based, an In-Tm-Zn-based oxide, an In-Yb-Zn-based oxide or an In-Lu-Zn-based oxide; or one of four types oxide containing metals such as an In-Sn-Ga-Zn-based oxide, an In-Hf-Ga-Zn-based oxide, an In-Al-based oxide Ga-Zn-based, an In-Sn-Al-Zn-based oxide, an In-Sn-Hf-Zn-based oxide, or an In-Hf-Al-Zn-based oxide.
[0104] Here, an In-Ga-Zn based oxide refers to an oxide containing In, Ga and Zn as the main component, and there are no particular limitation on the ratio of In, Ga and Zn. The In-Ga-Zn based oxide can be a Contain a metal element other than In, Ga and Zn.
[0105] Alternatively, a material represented by InMO (ZnO)" (m > 0 is satisfied) can be used as an oxide semiconductor 3 It should be noted that M is one or more metal elements selected from Ga, Fe, Mn and Co. or the above element acts as a stabilizer.
[0106] For example, an In-Ga-Zn-based metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1 (= 1 / 3:1 / 3:1 / 3), 2:2:1 (= 2 / 5:2 / 5:1 / 5) or 3:1:2 (= 1 / 2:1 / 6:1 / 3) can be used. Alternatively, a metal oxide based on In-Sn- Zn-based, containing In, Sn and Zn with an atomic ratio of 1:1:1 (= 1 / 3:1 / 3:1 / 3), 2:1:3 (= 1 / 3:1 / 6:1 / 2) or 2:1:5 (= 1 / 4:1 / 8:5 / 8). It should be noted that the proportion of each atom in the atomic ratio of the metal elements in the Error range of ±20%.
[0107] However, the atomic ratio is not limited to those described above, and a material having the appropriate Atomic ratio can be varied depending on the required semiconductor properties and electrical properties (e.g. field effect mobility and threshold voltage). In order to obtain the required semiconductor properties, it is prefer that the charge carrier density, the impurity concentration, the defect density, the atomic ratio of a metal element to oxygen, the distance between atoms, the density and the like are adjusted to appropriate values For example, a high field effect mobility can be achieved relatively easily in the case where the In-Sn-Zn based metal oxide is used. However, even in the case where the In-Ga-Zn based metal oxide used, the field effect mobility can be increased by reducing the defect density in the bulk.
[0108] For the oxide semiconductor film 119, an oxide semiconductor can be used which is suitable for the oxide semiconductor film 111 can be used. The oxide semiconductor film 119 can be formed simultaneously with the oxide semiconductor film 111 and thus contains a metal element of an oxide semiconductor contained in the oxide semiconductor film 111.
[0109] The insulating film 129, the insulating film 131 and the insulating film 132, which serve as protective insulating films of the transistor 103 and as dielectric films of the capacitor 105 are insulating films, each of which is made using of a material that can be used for the gate insulating film 127. It is particularly prefer that the insulating films 129 and 131 are oxide insulating films and the insulating film 132 is a nitride insulating film. In addition, the use of a nitride insulating film as the insulating film 132 can prevent the entry of impurities such as hydrogen and water, into the transistor 103 (especially the oxide semiconductor film 111) from the outside. It should be noted that that the insulating film 129 is not necessarily present.
[0110] Furthermore, preferably, the insulating film 129 and / or the insulating film 131 are each an oxide insulating film which Contains oxygen in a higher proportion than the oxygen in the stoichiometric composition. In this case, it is prevented that oxygen is released from the oxide semiconductor film 111, and the oxygen in a Oxygen excess region can be transferred to the oxide semiconductor film 111 to form oxygen vacancies For example, when an oxide insulating film having the following characteristic is used, the Oxygen defects in the oxide semiconductor film 111 are compensated. The feature of the oxide insulating film is 18 that the number of oxygen molecules released from the oxide insulating film is greater than or equal to 1.0 × 10 3 molecules / cm when measured by thermal desorption spectroscopy (hereinafter referred to as TPD). It should be noted that an oxide insulating film which partially has a region containing oxygen at a higher proportion than Contains oxygen in the stoichiometric composition (oxygen excess range) than the insulating film 129 and / or the insulating film 131 can be used. If such an oxygen excess area is in an area which overlaps at least with the oxide semiconductor film 111, oxygen is prevented from oxide semiconductor film 111 is released, and the oxygen in the oxygen excess region can be transferred to the Oxide semiconductor film 111 to compensate for oxygen vacancies.
[0111] In the case where the insulating film 131 is an oxide insulating film containing oxygen at a higher ratio than oxygen in the stoichiometric composition, the insulating film 129 is preferably an oxide insulating film containing oxygen Oxygen entering the insulating film 129 from the outside does not completely penetrate through the insulating film 129 and is transferred, and a part of it remains in the insulating film 129. In addition, there is oxygen, which is in the Insulating film 129 is contained from the beginning and is transferred from the insulating film 129 to the outside. Therefore, the insulating film 129 preferably an oxide insulating film with a high oxygen diffusion coefficient.
[0112] Since the insulating film 129 is in contact with the oxide semiconductor film 111, the insulating film 129 is preferably a Oxide insulating film through which oxygen is allowed to pass and which reduces the interface state density at the interface to the oxide semiconductor film 111. For example, the insulating film 129 is preferably an oxide insulating film having a lower defect density than the insulating film 131. In particular, the spin density of the insulating film 129 is at a 17 g-value of 2.001 (E'-center), measured by electron spin resonance, less than or equal to 3.0 × 10 3 16 3 spins / cm , preferably less than or equal to 5.0 × 10 spins / cm . It should be noted that the spin density at a g- Value of 2.001, which is measured by electron spin resonance, the number of open bonds in the insulating film 129 corresponds.
[0113] The thickness of the insulating film 129 may be greater than or equal to 5 nm and less than or equal to 150 nm, preferably greater than or equal to 5 nm and less than or equal to 50 nm, more preferably greater than or equal to 10 nm and less than or be equal to 30 nm. The thickness of the insulating film 131 may be greater than or equal to 30 nm and less than or equal to 500 nm, preferably greater than or equal to 150 nm and less than or equal to 400 nm.
[0114] When an oxide insulating film which allows oxygen to pass through and which reduces the interface state density between the oxide semiconductor film 111 and the oxide insulating film than the insulating film 129 over the oxide semiconductor film 111 used, and an oxide insulating film having an oxygen excess region, or an oxide insulating film having Contains oxygen with a higher proportion than oxygen in the stoichiometric composition than the insulating film 131 is used, oxygen can be easily supplied to the oxide semiconductor film 111, the release of oxygen from the oxide semiconductor film 111 can be prevented, and the oxygen in the insulating film 131 can be transferred to the oxide semiconductor film 111 to compensate for the oxygen vacancies in the oxide semiconductor film 111. Thus, the transistor 103 can be prevented from exhibiting a ´´normally on´´ behavior.
[0115] In the case where a nitrogen-containing oxide insulating film such as a silicon oxynitride film or a Silicon nitride oxide film is used as the insulating film 129 and / or the insulating film 131, the nitrogen concentration 20 ration measured by SIMS is higher than or equal to the lower detection limit of SIMS and lower than 3 × 10 3 18 3 20 3 atoms / cm , preferably higher than or equal to 1 × 10 atoms / cm and lower than or equal to 1 × 10 atoms / cm . In In this case, the amount of nitrogen transferred to the oxide semiconductor film 111 in the transistor 103 can be can be reduced, and the number of defects in the nitrogen-containing oxide insulating film itself can be reduced.
[0116] In the case where a nitride insulating film is used as the insulating film 132, an insulating film having a barrier property against nitrogen as the insulating film 129 and / or the insulating film 131. For example, A dense oxide insulating film can provide a barrier property against nitrogen. In particular, it is preferable to use an oxide insulating film etched at a speed of less than or equal to 10 nm per minute can be achieved when the temperature is 25 °C and 0.5 wt% hydrofluoric acid is used.
[0117] As the insulating film 132, a nitride insulating film having a low hydrogen content may be provided. Nitride insulating film, for example, is as follows: the number of hydrogen molecules released from the nitride insulating film 21 3 21 3 21 3 is less than 5.0 × 10 / cm , preferably less than 3.0 × 10 / cm , more preferably less than 1.0 × 10 / cm , when measured by TPD.
[0118] Furthermore, the nitride insulating film has a good step coverage and can thus be advantageously used as a protective insulating film of the Transistor 103 can be used.
[0119] The insulating film 132 has a thickness that prevents the entry of impurities such as hydrogen and water from outside can be suppressed. For example, the thickness can be greater than or equal to 50 nm and less than or equal to 200 nm, preferably greater than or equal to 50 nm and less than or equal to 150 nm, more preferably greater than or equal to 50 nm and less than or equal to 100 nm.
[0120] The use of a nitride insulating film as the insulating film 132 over the insulating film 131 can prevent the entry of Impurities such as hydrogen and water into the oxide semiconductor film 111 and the oxide semiconductor film 119 from outside In addition, using a nitride insulating film with a low hydrogen content as the insulating film 132 suppresses fluctuations in the electrical properties of the transistor 103.
[0121] When a silicon oxide film is provided between the insulating film 131 and the insulating film 132 and the Nitride insulating film is used as the insulating film 132, the entry of impurities such as hydrogen and Water into the oxide semiconductor film 111 and the oxide semiconductor film 119 from the outside can be further suppressed.
[0122] Alternatively, a silicon oxide film formed by a CVD method using an organosilane gas formed between the insulating film 131 and the insulating film 132. The silicon oxide film has a good step coverage and can therefore be used advantageously as a protective insulating film for transistor 103. The Silicon oxide film can be formed in a thickness of 300 nm up to and including 600 nm. The organosilane gas can be one of the following silicon-containing compounds may be used: Tetraethylorthosilicate (TEOS) (chemical formula: Si (OC H ) ); Tetramethylsilane (TMS) (chemical formula: Si(CH ) ); tetramethylcyclotetrasiloxane (TMCTS); 2 5 4 3 4 Octamethylcyclotetrasiloxane (OMCTS); hexamethyldisilazane (HMDS); Triethoxysilane (SiH(OC H ) ); Trisdimethylaminosilane 2 5 3 (SiH(N(CH ) ) ); or the like. 3 2 3
[0123] The pixel electrode 121 may be formed using a light-transmitting conductive material such as Indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide contains indium tin oxide containing titanium oxide, indium zinc oxide or indium tin oxide to which silicon oxide is added, be trained.
[0124] For the substrate 150, a material that can be used for the substrate 102 can be used.
[0125] The opaque film 152 is also called a black matrix and is used, for example, in a Liquid crystal display device provided to detect leakage of light from a light source such as Backlight suppression or contrast deterioration due to color mixing that occurs when Color display is performed using a color filter. An opaque film, which is generally used can be used as the light-impermeable film 152. A metal and an organic resin containing a dye can be considered as examples of an opaque material Alternatively, the opaque film 152 may be provided in an area outside the pixel section 100, such as above the scan line driver circuit 104 and the signal line driver circuit 106 (see Fig. 1A) and in an area overlapping with the transistor 103.
[0126] Furthermore, a color film that transmits light with a predetermined wavelength may be sandwiched between opaque Films in each pixel in the pixel section 100. Furthermore, a coating film may be provided between the counter electrode, and the opaque films and the color film.
[0127] For the counter electrode 154, materials that can be used for the pixel electrode 121 can be be used as needed.
[0128] The alignment films 156 and 158 may be formed using a general-purpose material such as polyamide. be trained.
[0129] For the liquid crystal 160, a thermotropic liquid crystal, a low molecular liquid crystal, a high molecular liquid crystal, a polymer-dispersed liquid crystal, a ferroelectric liquid crystal, a antiferroelectric liquid crystal or the like. Such a liquid crystal material exhibits a cholesteric phase, a smectic phase, a cubic phase, a chiral nematic phase, an isotropic phase or the like, which depends on a fact.
[0130] Alternatively, a liquid crystal showing a blue phase for which an alignment film is not necessary may be used for the liquid crystal 160. A blue phase is one of the liquid crystal phases that is created exactly when before a cholesteric phase changes to an isotropic phase, while the temperature of the cholesteric liquid crystal. Since the blue phase only occurs in a narrow temperature range, a Liquid crystal compound in which a chiral material is mixed, used to improve the temperature range. It should be noted that the alignment film is formed using an organic resin containing hydrogen, water or the like, which determines the electrical properties of the transistor in the semiconductor device an embodiment of the present invention. In view of the above, the Use of a liquid crystal which shows a blue phase, for the liquid crystal 160 a preparation of the Semiconductor device according to an embodiment of the present invention without organic resin, so that the semiconductor device can be highly reliable.
[0131] It should be noted that the structure of the liquid crystal element 108 can be changed as needed according to the display mode of the liquid crystal element 108 can be changed as follows: the shapes of the pixel electrode 121 and the counter electrode 154 are changed, or a protrusion called a rib is formed.
[0132] Furthermore, in the semiconductor device of one embodiment of the present invention, a region of the pixel 101, in which the opaque film 152 is arranged, can be reduced or eliminated in the following way: a Polarization axis of a polarization component (a polarization substrate) is provided to the opaque film 152, and the display mode of the semiconductor device is set to a ´´normally black´´ mode in which the liquid crystal element 108 receives light from a light source such as a backlight does not pass through when no voltage is applied. As a result, the Aperture ratio of pixel 101 can be improved, even if the size of a pixel is as small as in a high pixel density display device. It should be noted that the aperture ratio can be adjusted using a translucent capacitor can be further increased. <Verfahren zum Herstellen einer Halbleitervorrichtung>
[0133] A method of manufacturing the above semiconductor device will be described with reference to Fig. 7A, Fig. 7B, Fig. 8A and Fig. 8B.
[0134] First, the scanning line 107_m-1 and the scanning line 107_m are formed over the substrate 102. A Insulating film to be processed into the gate insulating film 127 is formed to form the scanning line 107_m-1 and the scanning line 107_m. The opening 123 is formed in an area of the insulating film, which is in contact with the scanning line 107_m-1, so that the gate insulating film 127 is formed. The Oxide semiconductor film 111 is formed to overlap with the scanning line 107_m. The oxide semiconductor film 119 is formed over the gate insulating film 127 and in the opening 123 to form a region on which the pixel electrode 121 to be formed (see Fig. 7A) .
[0135] The scanning lines 107_m-1 and 107_m may be formed such that a conductive film is provided under Using one of the materials specified above, a mask is formed over the conductive film and the conductive film is processed by means of the mask. The conductive film can be processed by one of various Film formation methods such as an evaporation method, a CVD method, a sputtering method and a It should be noted that there is no particular restriction regarding the thickness of the conductive film, and that the thickness of the conductive film taking into account the time for the formation, the desired specific resistance or the like can be determined. As a mask, a Photoresist mask formed by a photolithography process can be used. The conductive film can processed by dry etching and / or wet etching.
[0136] The insulating film to be processed into the gate insulating film 127 may be formed using a material suitable for the Gate insulating film 127 may be used by one of various film forming methods such as CVD method and a sputtering method. In the case where gallium oxide is used for the gate insulating film 127 used, the insulating film can be deposited by a metal organic chemical vapor deposition (metal organic chemical vapor deposition: MOCVD) process.
[0137] The opening 123 can be formed as follows: a mask is formed over the insulating film, and the Insulating film is processed using the mask. It should be noted that the mask can be formed and the Processing can be carried out by referring to the manufacturing process of the scanning line 107_m-1 and the Scanning line 107_m.
[0138] The oxide semiconductor film 111 and the oxide semiconductor film 119 may be formed such that one of the above specified oxide semiconductor films is formed, a mask is formed over the formed oxide semiconductor film, and the oxide semiconductor film is processed using the mask. The oxide semiconductor film can be processed by a sputtering process, a coating process, a laser beam evaporation process, a laser ablation process or the like By using a printing method, the oxide semiconductor film 111 and the oxide semiconductor film 119 as after element separation directly on the gate insulating film 127. As a power supply device for To generate plasma in the case where the oxide semiconductor film is formed by a sputtering method, an RF Power supply device, an AC power supply device, a DC power supply device or the like as required As sputtering gas, an atmosphere of a noble gas (typically argon), oxygen or a mixture of a noble gas and oxygen is used. In the case of a mixture atmosphere of a noble gas and Oxygen, the oxygen content is preferably higher than that of a noble gas. It should be noted that the target can be appropriately selected according to the composition of the oxide semiconductor film to be formed. As a mask A photoresist mask formed by a photolithography process can be used. Oxide semiconductor film can be processed by dry etching and / or wet etching. The etching conditions (such as a Etching gas or etching solution, etching time and temperature) are adjusted appropriately depending on the material so that the Oxide semiconductor film 111 and the oxide semiconductor film 119 can be etched into desired shapes.
[0139] A heat treatment is preferably carried out after the formation of the oxide semiconductor films 111 and 119, to remove water or hydrogen from the oxide semiconductor films 111 and 119. The heat treatment is typically at a temperature higher than or equal to 150 °C and lower than the lower stress relief limit (strain point) of the substrate, preferably higher than or equal to 200 °C and lower than or equal to 450 °C, more preferably higher than or equal to 300 °C and lower than or equal to 450 °C. It should be noted that the Heat treatment can be carried out on the oxide semiconductor film which has not yet been added to the oxide semiconductor films 111 and 119 has been processed.
[0140] In heat treatment, a heat treatment device is not limited to an electric furnace; Heat treatment device can be a device that heats an object by conduction or radiation from a medium, such as a heated gas or the like. For example, a rapid thermal Rapid thermal annealing (RTA) facility, such as a GRTA (gas rapid thermal anneal) facility or a LRTA (lamp rapid thermal anneal) facility An LRTA device is a device for heating an object for processing by Irradiation with light (electromagnetic waves) emitted by a lamp, such as a halogen lamp, a metal halide lamp, a xenon arc lamp, a carbon arc lamp, a high-pressure sodium lamp or a High pressure mercury lamp. A GRTA facility is a facility for carrying out a heat treatment under Use of a high-temperature gas.
[0141] The heat treatment can be carried out in an atmosphere of nitrogen, oxygen, ultra-dry air (air in which the Water content less than or equal to 20 ppm, preferably less than or equal to 1 ppm, more preferably less than or equal to 10 ppb) or a noble gas (e.g. argon or helium). The atmosphere of nitrogen, Oxygen, ultra-dry air or a noble gas preferably does not contain hydrogen, water and the like. Alternatively, the heat treatment can be carried out first in an inert gas atmosphere and then in an oxygen atmosphere It should be noted that the treatment time ranges from 3 minutes to 24 hours.
[0142] In the case where a base insulating film is provided between the substrate 102 and the scanning line 107_m-1, the scanning line 107_m and the gate insulating film 127, the base insulating film can be formed using a Film of any of the following: silicon oxide, silicon oxynitride, silicon nitride, silicon nitride oxide, Gallium oxide, hafnium oxide, yttrium oxide, aluminum oxide, aluminum oxynitride, and the like. It should be noted that then, when the base insulating film is made using silicon nitride, gallium oxide, hafnium oxide, yttrium oxide or aluminum oxide is formed, it is possible to prevent diffusion of impurities such as an alkali metal, water and hydrogen from the substrate 102 into the oxide semiconductor film 111. The base insulating film can be formed by a sputtering method or a CVD process can be developed.
[0143] Next, the signal line 109_n having a region serving as a source electrode and the conductive film 113 having a region serving as a drain electrode is formed over the gate insulating film 127 (see Fig. 7B).
[0144] The signal line 109_n and the conductive film 113 can be formed as follows: a conductive film is formed under Using a material applicable to the signal line 109_n and the conductive film 113, a A mask is formed over the conductive film, and the conductive film is processed through the mask. The mask can be trained and the processing can be carried out with reference to the manufacturing process of the Scanning line 107_m-1 and the scanning line 107_m. It should be noted that a surface of the oxide semiconductor film 111 is cleaned after the signal line 109_n and the conductive film 113 have been formed, so that fluctuations the electrical properties of the transistor 103 can be reduced. For cleaning, for example, a diluted phosphoric acid solution may be used; in particular, a phosphoric acid solution in which 85% Phosphoric acid diluted one hundred times can be used.
[0145] Then, an insulating film 128 is formed over the oxide semiconductor film 111, the oxide semiconductor film 119, the signal line 109_n, the conductive film 113 and the gate insulating film 127, an insulating film 130 is formed over the insulating film 128 formed, and an insulating film 133 is formed over the insulating film 130 (see Fig. 8A). The insulating films 128, 130 and 133 are preferably formed one after the other, in which case the entry of impurities into each interface can be suppressed.
[0146] The insulating film 128 may be formed using a material that can be used for the gate insulating film 129. formed by one of various film formation processes such as a CVD process and a sputtering process The insulating film 130 can be formed using a material that can be used for the insulating film 131. The insulating film 133 may be formed using a material used for the insulating film 132 can be trained.
[0147] In the case where an oxide insulating film which reduces the interface state density between the oxide semiconductor film 111 and the oxide insulating film when the insulating film 129 is used, the insulating film 128 can be used under the following conditions. Here, a silicon oxide film or a silicon oxynitride film is formed as the oxide insulating film. Regarding the training conditions, the substrate, which is placed in a treatment chamber of a plasma CVD device which has been evacuated, at a temperature higher than or equal to 180 °C and lower than or equal to 400 °C, preferably higher than or equal to 200 °C and lower than or equal to 370 °C, the pressure in the Treatment chamber is higher than or equal to 20 Pa and lower than or equal to 250 Pa, preferably higher than or equal to 40 Pa and less than or equal to 200 Pa, wherein a source gas such as a silicon-containing deposition gas and an oxy ation gas is introduced into the treatment chamber, and a high-frequency power of a electrode located in the treatment chamber.
[0148] Typical examples of the silicon-containing deposition gas include silane, disilane, trisilane and silane fluoride. Examples of the oxidizing gas include oxygen, ozone, nitrous oxide and nitrogen dioxide.
[0149] By adjusting the ratio of the amount of oxidizing gas to the amount of silicon-containing deposition gas to 100 or higher, the amount of hydrogen contained in the insulating film 128 (the insulating film 129) contained, and the number of open bonds in the insulating film 128 (the insulating film 129) can Oxygen transferred from the insulating film 130 (insulating film 131) is in some cases the open bonds are trapped in the insulating film 128 (the insulating film 129). Therefore, in the case where the open Bonds in the insulating film 128 (the insulating film 129) are reduced, oxygen in the insulating film 130 (the insulating film 131) to the oxide semiconductor film 111 in an efficient manner to remove the oxygen vacancies in the oxide semiconductor film 111. Consequently, the amount of hydrogen entering the oxide semiconductor film 111 can be can be reduced and the oxygen vacancies in the oxide semiconductor film 111 can be reduced.
[0150] In the case where the above oxide insulating film having an oxygen excess region or the above Oxide insulating film containing oxygen in a higher proportion than oxygen in the stoichiometric composition, as the insulating film 131 is used, the insulating film 131 can be formed under the following formation conditions Here, a silicon oxide film or a silicon oxynitride film is formed as the oxide insulating film. Training conditions, the substrate is placed in a treatment chamber of a plasma CVD device, which has been evacuated at a temperature higher than or equal to 180 °C and lower than or equal to 260 °C, preferably higher than or equal to 180 °C and lower than or equal to 230 °C, the pressure in the treatment chamber is higher than or equal to 100 Pa and lower than or equal to 250 Pa, preferably higher than or equal to 100 Pa and lower than or equal to 200 Pa, wherein a source gas is introduced into the treatment chamber, and a high frequency power, 2 2 2 which is higher than or equal to 0.17 W / cm and lower than or equal to 0.5 W / cm , preferably higher than or equal to 0.25 W / cm 2 and is less than or equal to 0.35 W / cm, is supplied to an electrode located in the treatment chamber.
[0151] As the source gas for the insulating film 130, the source gas used to form the insulating film 128 can be used.
[0152] As the conditions for forming the insulating film 130, the high frequency power with the above Power density is supplied to the treatment chamber under the above pressure, thereby increasing the degradation efficiency of the source gas in plasma, oxygen radicals are increased, and the oxidation of the source gas is promoted. Thus, the oxygen content of the insulating film 130 is greater than that in the stoichiometric composition. In addition, the film formed at a substrate temperature in the above temperature range, the bond between silicon and oxygen weak; therefore, part of the oxygen in the film can be removed by heat treatment in the later This makes it possible to form an oxide insulating film that absorbs oxygen at a higher proportion than the stoichiometric composition and from which part of the oxygen is removed by heating In addition, the insulating film 128 is provided over the oxide semiconductor film 111. Therefore, the Insulating film 128 as a protective film of the oxide semiconductor film 111 in the process of forming the insulating film 130. Therefore Damage to the oxide semiconductor film 111 can be suppressed even if the insulating film 130 is under Using high frequency power with a high power density.
[0153] By increasing the thickness of the insulating film 130, the amount of oxygen released by heating is increased; thus, the insulating film 130 is preferably provided thicker than the insulating film 128. By the insulating film 128 is provided, a favorable coverage can be obtained even if the insulating film 130 is thick is trained.
[0154] The insulating film 132 may be formed by a sputtering method, a CVD method, or the like. In the case where a nitride insulating film having a small hydrogen content is used as the insulating film 132, the Insulating film 133 is formed under the following formation conditions. Here, the nitride insulating film is a Silicon nitride film is formed. Regarding the formation conditions, the substrate is placed in a treatment chamber the plasma CVD device, which evacuates at a temperature higher than or equal to 80 °C and lower than or equal to 400 °C, preferably higher than or equal to 200 °C and lower than or equal to 370 °C, the pressure in the treatment chamber is greater than or equal to 100 Pa and less than or equal to 250 Pa, preferably greater than or equal to 100 Pa and less than or equal to 200 Pa, wherein a source gas is introduced into the treatment chamber and a high frequency power is applied to a electrode located in the treatment chamber.
[0155] As a source gas for the insulating film 133, a silicon-containing deposition gas, nitrogen and ammonia preferably used. Typical examples of the silicon-containing deposition gas include silane, disilane, trisilane and Silane fluoride. Furthermore, the flow rate of nitrogen is 5 to 50 times, preferably 10 to 50 times higher than that of ammonia. The use of ammonia as a source gas can accelerate the degradation of the deposition gas, containing silicon and nitrogen. This is because ammonia is converted into nitrogen by plasma energy or thermal energy is dissociated, and that the energy generated by the dissociation is used to break down a bond between the molecules of the silicon-containing deposition gas and a binding of nitrogen molecules. Among the above conditions, a silicon nitride film can be formed which has a small hydrogen content and prevents the entry of Can suppress external impurities such as hydrogen and water.
[0156] In the case where a silicon oxide film formed using an organosilane gas by a CVD method formed between the insulating film 131 and the insulating film 132, the silicon oxide film is formed under Using one of the above-mentioned organosilane gases, the insulating film 130 is formed by a CVD process.
[0157] It is preferable that a heat treatment is carried out at least after the formation of the insulating film 130 so that oxygen in the insulating film 128 or in the insulating film 130 at least on the oxide semiconductor film 111 to compensate for oxygen vacancies in the oxide semiconductor film 111. The heat treatment can appropriate with reference to the details of the heat treatment to remove water or hydrogen from the oxide semiconductor film 111 and the oxide semiconductor film 119.
[0158] One of the preferred manufacturing processes of the transistor 103 is described below. Oxide insulating film whose oxygen content is greater than that in the stoichiometric composition and from which a part of oxygen is released by heating, is formed as the insulating film 130, the insulating film 130 is heated at 350 °C, a silicon oxide film is passed through a CVD process, with the substrate temperature kept at 350 °C, and a nitride insulating film, the Hydrogen content is small, is formed as the insulating film 132 at a substrate temperature of 350 °C.
[0159] Next, the opening 117 reaching the conductive film 113 is formed in a region of the insulating films 128, 130 and 133, which overlaps with the conductive film 113, so that the insulating films 129, 131 and 132 are formed (see Fig. 8B); and then the pixel electrode 121 is formed over the insulating film 132 and in the opening 117 (see Fig. 6).
[0160] The opening 117 may be formed in a manner similar to that of the opening 123. The Pixel electrode 121 is formed such that a conductive film is formed using one of the above-mentioned materials is formed to be in contact with the conductive film 113 through the opening 117, a mask over the conductive film, and the conductive film is processed by means of the mask. With reference to the Manufacturing process of the scanning line 107_m-1 and the scanning line 107_m, the mask can be formed and the processing can be carried out.
[0161] Then, the alignment film 158 is formed over the insulating film 132 and the pixel electrode 121. Thereafter, the opaque film 152 is formed on the substrate 150, the counter electrode 154 is formed to light-impermeable film 152, and the alignment film 156 is formed on the counter electrode 154. The Liquid crystal 160 is provided over the alignment film 158, the substrate 150 is provided over the substrate 102 provided so that the alignment film 156 is in contact with the liquid crystal 160, and the substrate 102 and the Substrate 150 are secured together with a sealing material (not shown).
[0162] The alignment films 156 and 158 can be formed using the above material by one of various Film forming processes such as a spin coating process and a printing process can be developed.
[0163] The opaque film 152 can be formed, for example, by a sputtering method using a Metal such as titanium or chromium can be formed and can be processed using a mask.
[0164] The counter electrode 154 can be formed using the material used for the pixel electrode 121 can be formed by one of various film formation processes such as a CVD process and a sputtering process be trained.
[0165] The liquid crystal 160 can be directly deposited on the alignment film 158 by a dispensing method (a dropping method) Alternatively, the liquid crystal 160 may be injected by means of a capillary effect or the like, after the substrate 102 and the substrate 150 have been attached to each other. In addition, the Alignment films 156 and 158 are preferably subjected to a friction treatment so that the alignment of the Liquid crystal 160 is easily performed.
[0166] Through the above process, the semiconductor device of one embodiment of the present invention can be produced (see Fig. 6). <Modifikationsbeispiel 1>
[0167] In the semiconductor device of one embodiment of the present invention, a connection between the semiconductor film (especially the oxide semiconductor film) serving as an electrode of the capacitor, and the scanning line, which serves as the capacitor line, can be changed if necessary. To increase the conductivity of the semiconductor film, For example, a conductive film may be provided in contact with a part of the semiconductor film so that the Semiconductor film and the scanning line can be electrically connected to each other via the conductive film.
[0168] It should be noted that in the drawings illustrating modification examples, the substrate 150, the opaque film 152, the counter electrode 154, the alignment film 156, the alignment film 158 and the Liquid crystal 160 are not shown for clarity. In addition, in the drawings showing the Represent modification examples, the reference numerals used in Fig. 5 or Fig. 6 are used where necessary.
[0169] A concrete example of the structure is described using Fig. 9, Fig. 10A and Fig. 10B. Here, only Parts other than those in the structure shown in Fig. 5 and Fig. 6 are described. It should be noted that Fig. 9 is a Top view of pixel 101 (m, n), Fig. 10A is a cross-sectional view along the dash-dot line A1-A2 and the dash- Dot line B1-B2 in Fig. 9, and Fig. 10B is a cross-sectional view taken along dash-dot line C1-C2 in Fig. 9.
[0170] In the pixel 101 (m, n) in Fig. 9, a conductive film 167 is in contact with the oxide semiconductor film 119 along its edge region and is in contact with the scanning line 107_m-1 through the opening 123. The conductive film 167 can by applying the manufacturing process of the signal line 109_n and the conductive film 113. The means that the conductive film 167 has an opaque property in some cases and therefore preferably a It should be noted that a larger contact area between the conductive film 167 and the Oxide semiconductor film 119 enables the oxide semiconductor film 119 to easily serve as an electrode of the capacitor 105.
[0171] Furthermore, in the pixel 101 (m, n) in Fig. 9, the shape of the oxide semiconductor film 119 is preferably selected as needed changed so that the oxide semiconductor film 119 and the scanning line 107_m-1 are in contact with the conductive film 167.
[0172] As shown in Fig. 10A and Fig. 10B, the conductive film 167 is arranged to cover an edge portion of the oxide semiconductor film 119 of the capacitor 105.
[0173] Alternatively, the conductive film 167 may be in contact with the oxide semiconductor film 119 in a loop shape having a column must be provided.
[0174] Although the conductive film 167 in the pixel 101 (m, n) in Fig. 9, Fig. 10A and Fig. 10B is formed in a loop shape, but the conductive film 167 may be in contact with only a part of the edge region of the oxide semiconductor film 119 (see Fig. 11). It should be noted that also in the pixel 101 (m, n) in Fig. 11, the oxide semiconductor film 119 and the scanning line 107_m-1 are electrically connected to each other via the conductive film 167.
[0175] In the structure in which the oxide semiconductor film 119 is in direct contact with the scanning line 107_m-1, the conductive film 167 may be provided in contact with a part of the oxide semiconductor film 119 to improve the conductivity of the oxide semiconductor film 119. In other words, the conductive film 167 can be in contact with the oxide semiconductor film 119, but not in contact with the scanning line 107_m-1. For example, as shown in Fig. 12, Fig. 13A and Fig. 13B shown, the conductive film 167 may be formed in a loop shape which is not in contact with the scanning line 107_m-1 It should be noted that Fig. 12 is a top view of the pixel 101 (m, n) with the above structure, Fig. 13A is a Cross-sectional view along the dash-dot line A1-A2 and the dash-dot line B1-B2 in Fig. 12, and Fig. 13B is a Cross-sectional view along the dash-dot line C1-C2 in Fig. 12. <Modifikationsbeispiel 2>
[0176] In the pixel 101 (m, n) in Fig. 5 and Fig. 6 or the pixels 101 (m, n) in Fig. 9, Fig. 10A, Fig. 10B, Fig. 11, Fig. 12, Fig. 13A and Fig. 13B, an organic insulating film can be arranged to reduce the parasitic capacitance that exists between the pixel electrode 121 and the conductive film 113, or the parasitic capacitance generated between the pixel electrode 121 and the conductive film 167. The organic insulating film may be in a be placed in the area where the parasitic capacitance is generated. In other words, the organic insulating film is partially arranged in the pixel 101 (m, n).
[0177] For the organic insulating film, a photosensitive organic resin or a non-photosensitive organic resin may be used; for example, an acrylic resin, a benzocyclobutene-based resin, a Epoxy resin, a siloxane-based resin or the like can be used. Alternatively, polyamide can be used for the organic Insulating film can be used.
[0178] In order to partially provide the organic insulating film in the pixel 101 (m, n), an insulating film is formed under Using one of the materials specified above and then the insulating film may need to The method for forming the organic insulating film is not particularly limited and can be can be selected as required according to the material used. For example, spin coating, Dipping, spray coating, a droplet dispensing process (an inkjet process), screen printing, offset printing or When a photosensitive organic resin is used for the organic insulating film a photoresist mask is unnecessary when forming the organic insulating film; thus, a process can be simplified become.
[0179] In general, an organic resin contains a lot of hydrogen and water; if an organic resin is above the Transistor 103 (in particular, above the oxide semiconductor film 111) is arranged, therefore, hydrogen and Water contained in the organic resin into the transistor 103 (in particular, into the oxide semiconductor film 111) and could degrade the electrical properties of the transistor 103. For this reason, it is preferable that the organic resin is at least not arranged in a region overlapping with the oxide semiconductor film 111. <Modifikationsbeispiel 3>
[0180] In each of the pixels 101 (m, n) in Fig. 5 and Fig. 6 and the pixels 101 (m, n) in Fig. 9, Fig. 10A, Fig. 10B, Fig. 11, Fig. 12, Fig. 13A and Fig. 13B, the shape of the transistor 103 is not limited to the shapes of the transistors in the above Drawings are limited and can be changed as needed. For example, as in pixel 101 (m, n) in Fig. 14 the transistor 103 may be a transistor 169 in which a region serving as a source electrode in the signal line 109 n a U-shape (or a C-shape, a square bracket shape or a horseshoe shape) to form a drain electrode serving area in the conductive film 113. With such a shape, a sufficient channel width can also in a transistor with a small area, and thus the amount of forward current (on- state current) of the transistor. It should be noted that other components of pixel 101 (m, n) in Fig. 14 are similar to those in Fig. 5. <Modifikationsbeispiel 4>
[0181] In each of the pixels 101 (m, n) in Fig. 5 and Fig. 6 and the pixels 101 (m, n) in Fig. 9, Fig. 10A, Fig. 10B, Fig. 11, Fig. 12, Fig. 13A and Fig. 13B, a channel-etched transistor is used as the transistor 103. The transistor 103 can be a channel protective transistor 183 in Fig. 15. The structure of the transistor 183 in Fig. 15 is the same as that of transistor 103 in Fig. 6, except that a channel-protecting film 182 is sandwiched between the oxide semiconductor film 111 and the signal line 109_n, which has a region serving as a source electrode and is arranged between the oxide semiconductor film 111 and the conductive film 113, which has a drain electrode serving area.
[0182] To form the transistor 183 in Fig. 15, the channel protecting film 182 is deposited over the oxide semiconductor film 111 formed, and then the signal line 109_n and the conductive film 113 are formed. The channel-protecting film 182 can be formed using a material for the insulating film 129 of the transistor 103. With a such a structure, an insulating film corresponding to the insulating film 129 of the transistor 103 does not need to be additionally formed in the Transistor 183 can be arranged. With the channel protecting film 182, the surface of the oxide semiconductor film 111 is not an etching solution or an etching gas used in the manufacturing process of the signal line 109_n and the conductive film 113 used, so that impurities between the oxide semiconductor film 111 and the channel protecting film 182 can be reduced. As a result, a leakage current that occurs between the signal line 109_n and the conductive Film 113 of the transistor 183 can be reduced. In addition, the channel-protecting film 182 can prevent that the oxide semiconductor film 111 (in particular a channel formation region) is damaged when the processing for forming the signal line 109_n and the conductive film 113. <Modifikationsbeispiel 5>
[0183] In each of the pixels 101 (m, n) in Fig. 5 and Fig. 6 and the pixels 101 (m, n) in Fig. 9, Fig. 10A, Fig. 10B, Fig. 11, Fig. 12, Fig. 13A and Fig. 13B, the oxide semiconductor film 111 of the transistor 103 is located between the gate insulating film 127 and the signal line 109_n, which has a region serving as a source electrode, and between the gate insulating film 127 and the conductive film 113, which has a region serving as a drain electrode. A transistor 190, in which as in Fig. 16 shows an oxide semiconductor film 195 between the insulating film 129 and the signal line 109_n, which has a source electrode, and between the insulating film 129 and the conductive film 113, which has a drain The area serving as the electrode can be used as the transistor 103. The structure of the transistor 190 in Fig. 16 is the same as that of transistor 103 in Fig. 6, except for the position of the oxide semiconductor film 195.
[0184] To form the transistor 190 in Fig. 16, the signal line 109_n and the conductive film 113 formed, and then the oxide semiconductor film 195 is formed. Therefore, a surface of the oxide semiconductor film 195 not an etching solution or an etching gas in the manufacturing process of the signal line 109_n and the conductive film 113 exposed so that impurities between the oxide semiconductor film 195 and the insulating film 129 are reduced As a result, a leakage current flowing between the signal line 109_n and the conductive film 113 of the transistor 190 flows, can be reduced. <Modifikationsbeispiel 6>
[0185] In each of the pixels 101 (m, n) in Fig. 5 and Fig. 6 and the pixels 101 (m, n) in Fig. 9, Fig. 10A, Fig. 10B, Fig. 11, Fig. 12, Fig. 13A and Fig. 13B, a transistor 185 having two facing gate electrodes as in Fig. 17 with the oxide semiconductor film 111 therebetween, instead of the transistor 103 with a single gate electrode can be used.
[0186] In the transistor 185, a conductive film 187 is formed over the insulating film 132 of one of the transistors 103, 104, 105, 106, 107, 108, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 160, 161, 162, 163, 164, 165, 166, 167, 168, 170, 179, 179, 180, 181, 182, 183, 184, 185, 190, 200, 200, 201, 203, 204, 207, 208, 209, 201, 202, 203, 204, 205, 206, 207, 208, 209, 209, 200, 203, 204 169, transistor 183 and transistor 190 described in this embodiment. The conductive film 187 overlaps at least with the channel formation region of the oxide semiconductor film 111. The width of the conductive film 187 in the channel length direction may, for example, be shorter than the distance between the signal line 109_n, which has a region serving as the source electrode of the transistor, and the region serving as the drain electrode conductive film 113. The conductive film 113 is preferably arranged to communicate with the channel formation region of the oxide semiconductor film 111, and the potential of the conductive film 187 is preferably the lowest potential of the image nals input to the signal line 109_n. Consequently, a current flowing in a region of the oxide semiconductor film 111 on the side of the conductive film 187 and between the source electrode and the drain electrode, controlled Thus, variations in the electrical properties between transistors in the pixel section 100 Furthermore, the conductive film 187 reduces an influence of a change in a surrounding electric field on the oxide semiconductor film 111, which leads to improving the reliability of the transistor.
[0187] Consequently, a semiconductor film is used as an electrode of a capacitor in the same process as a semiconductor film of a transistor, whereby a semiconductor device can be manufactured in which the aperture ratio and the capacitance of the capacitor is increased. In addition, an increase in the aperture ratio provide a semiconductor device with excellent display quality.
[0188] Furthermore, oxygen vacancies and impurities such as hydrogen and nitrogen in the semiconductor film (in particular the oxide semiconductor film) of the transistor, so that the semiconductor device of an embodiment the present invention has favorable electrical properties.
[0189] It should be noted that the structure and the like described in this embodiment may be changed as needed in combination with one of the structures in the other embodiments. (Embodiment 2)
[0190] In this embodiment, a semiconductor device of an embodiment of the present invention, which a different structure than those in the above embodiment, will be described with reference to drawings. In the In the semiconductor device described in this embodiment, the structure of a capacitor is different from that of the capacitor in the above embodiment. Regarding the components in the semiconductor device, this embodiment, which are similar to those of the semiconductor device in the above embodiment, to the above embodiment. <Struktur einer Halbleitervorrichtung>
[0191] Fig. 18 is a plan view of a pixel in this embodiment. The pixel 101 (m, n) in Fig. 18 has a structure in which a capacitor 205 is arranged instead of the capacitor 105 in the pixel 101(m, n) in Fig. 5. In the pixel 101(m, n) in Fig. 18, an insulating film 232 (not shown) is in contact with the oxide semiconductor film 119 in a region which is represented by dashed double-dot lines, in contrast to the pixel 101 (m, n) in Fig. 5. That is, that in the pixel 101 (m, n) in Fig. 18, an insulating film 229 (not shown) and an insulating film 231 (not shown) in the area shown by dashed double-dotted lines. This means that the capacitor 205 has the oxide semiconductor film 119 serving as one electrode, the pixel electrode 121 serving as the other electrode and the dielectric film serving as an insulating film 232 (not shown).
[0192] A cross-sectional view along the dash-dot line A1-A2 and the dash-dot line B1-B2 in Fig. 18 is shown in Fig. 19 shown.
[0193] The cross-sectional structure of the pixel 101 (m, n) in Fig. 18 is shown as follows. Above the substrate 102, the Scanning line 107_m, which has a region serving as a gate electrode, and the scanning line 107_m-1 are arranged. The gate insulating film 127 is disposed over the scanning line 107_m-1 and the scanning line 107_m. The oxide semiconductor film 111 is arranged over the gate insulating film 127 to overlap with the scanning line 107_m. The opening 123, which Scanning line 107_m-1 is arranged in a region of the gate insulating film 127 which is in contact with the Scanning line 107_m-1 is provided. The oxide semiconductor film 119 is formed over the gate insulating film 127 and in the opening 123 The signal line 109_n, which has a region serving as a source electrode, and the conductive film 113, which has a region serving as a drain electrode, are respectively formed over the oxide semiconductor film 111 and the gate Insulating film 127 is arranged. At least in a region that becomes the transistor 103, the insulating film 229, the Insulating film 231 and insulating film 232, which serve as protective insulating films of the transistor 103, over the gate insulating film 127, the signal line 109_n, the oxide semiconductor film 111 and the conductive film 113. Furthermore, at least in one Area that becomes the capacitor 205, the insulating film 232 is arranged over the oxide semiconductor film 119. The opening 117, which reaches the conductive film 113, is mounted in the insulating film 229, the insulating film 231 and the insulating film 232, and the pixel electrode 121 is above the Insulating film 231 and arranged in the opening 117. It should be noted that a base insulating film is arranged between the substrate 102, and the scanning lines 107_m-1 and 107_m and the gate insulating film 127.
[0194] The insulating film 229 is similar to the insulating film 129 described in Embodiment 1. The insulating film 231 is similar to the insulating film 131 described in Embodiment 1. The insulating film 232 is similar to the insulating film 131 described in Embodiment 1. 1 described insulating film 132.
[0195] When the insulating film 232 is used as a dielectric film between the oxide semiconductor film 119 serving as an electrode and the pixel electrode 121 serving as the other electrode as in the capacitor 205 in this embodiment the thickness of the dielectric film may be smaller than that of the dielectric film of the capacitor 105 in the Embodiment 1. Therefore, the capacitor 205 in this embodiment can have a higher capacitance per unit area than the capacitor 105 in Embodiment 1.
[0196] Since the capacitor 205 has a higher capacitance per unit area than the capacitor 105, the area of the oxide semiconductor film 119, which is necessary to obtain the capacitance equal to that of the capacitor 105, is small Consequently, a region on which the oxide semiconductor film 119 is not formed can be obtained in the pixel 101 (m, n). Thus, the light extraction efficiency (transmittance) of a light source such as a backlight in the semiconductor device of an embodiment of the present invention; as a result, the Display quality can be improved.
[0197] The insulating film 232 is preferably a nitride insulating film in a similar manner to the insulating film 132 in the Embodiment 1. When a nitride insulating film is formed by a plasma CVD method or a sputtering method as the insulating film 232 is formed, the oxide semiconductor film 119 is exposed to a plasma; therefore, oxygen vacancies in the oxide semiconductor film 119. Since the insulating film 232 is in contact with the oxide semiconductor film 119, Nitrogen and / or hydrogen in the nitride insulating film are also transferred to the oxide semiconductor film 119. When hydrogen in When the oxygen vacancies in the insulating film 232 are entered, electrons serving as charge carriers are generated. Alternatively a nitride insulating film is formed as the insulating film 232 and a heat treatment is carried out, wherein the Insulating film 232 is in contact with the oxide semiconductor film 119; therefore, nitrogen and / or hydrogen in the Nitride insulating film is transferred to the oxide semiconductor film 119. When hydrogen in the insulating film 232 enters the When oxygen vacancies occur, electrons are generated that serve as charge carriers. Consequently, the electrical The conductivity of the oxide semiconductor film 119 is increased, and the oxide semiconductor film 119 has N-type conductivity. In addition, the oxide semiconductor film 119 becomes a conductive film having a light-transmitting property and a Metal oxide film with conductive properties. The oxide semiconductor film 119 has a higher electrical conductivity than the oxide semiconductor film 111.
[0198] As described above, in the semiconductor device of this embodiment, the oxide semiconductor film 119 has a region that has a higher conductivity than the oxide semiconductor film 111. At least one region of the oxide semiconductor film 119, which is in contact with the insulating film 232, has N-type conductivity and a higher conductivity than a Region of the oxide semiconductor film 111 that is in contact with the insulating film 229.
[0199] It should be noted that it is preferable that the oxide semiconductor film 119 has a higher hydrogen concentration than the oxide semiconductor film 111. In the oxide semiconductor film 119, the hydrogen concentration caused by 19 3 Secondary ion mass spectrometry (SIMS) is higher than or equal to 8 × 10 atoms / cm , preferably higher than 20 3 20 3 or equal to 1 × 10 atoms / cm , more preferably higher than or equal to 5 × 10 atoms / cm . In the oxide semiconductor film 19 3 111, the hydrogen concentration measured by SIMS is lower than 5 × 10 atoms / cm , preferably lower 18 3 18 3 than 5 × 10 atoms / cm , more preferably lower than or equal to 1 × 10 atoms / cm , even more preferably lower 17 3 16 3 than or equal to 5 × 10 atoms / cm , even more preferably lower than or equal to 1 × 10 atoms / cm .
[0200] The specific resistance of the oxide semiconductor film 119 is lower than that of the oxide semiconductor film 111. The -8 specific resistance of the oxide semiconductor film 119 is preferably more than or equal to 1 × 10 times and less than or -1 equal to 1 × 10 times lower than the resistivity of the oxide semiconductor film 111. The resistivity of the -3 4 oxide semiconductor film 119 is typically higher than or equal to 1 × 10 Ωcm and lower than or equal to 1 × 10 - 3 -1 Ωcm, preferably higher than or equal to 1 × 10 Ωcm and lower than 1 × 10 Ωcm.
[0201] In an operating method of the capacitor 205 in the semiconductor device of this embodiment, the potential of the oxide semiconductor film 119 (ie the potential of the scanning line 107_m-1) is lower than the potential of the pixel electrode 121 to be greater than or equal to the threshold voltage (Vth) of the capacitor 205 (MOS capacitor) in a Operating period of the capacitor 205, as in the operating method of the capacitor 105 in Embodiment 1. However, in the capacitor 205, the oxide semiconductor film 119 serving as an electrode has N-type conductivity and a high conductivity, so that the threshold voltage (Vth) in the negative direction as shown by a dashed line in Fig. 2. The potential of the oxide semiconductor film 119 (ie the potential of the scanning line 107_m-1) can according to the shift amount of the threshold voltage (Vth) of the capacitor 205 in the negative direction from lowest potential of the pixel electrode 121. Therefore, in the case where the threshold voltage of the capacitor 205 has a large negative value, the potential of the scanning line 107_m-1 is higher than the potential of the pixel electrode 121, as shown in Fig. 4B.
[0202] The oxide semiconductor film 119 serving as an electrode of the capacitor 205 is made to have a conductivity of the N-type and its electrical conductivity is increased as in this embodiment, so that the Threshold voltage shifts in a negative direction. Thus, the range of potential required to operate the capacitor 205 must be greater than the range of potential required to operate capacitor 105 at of the embodiment 1. Consequently, this embodiment is preferred because the capacitor 205 is constantly Stability in an operating period of the capacitor 205. <Verfahren zum Herstellen einer Halbleitervorrichtung>
[0203] Next, a method of manufacturing a semiconductor device of this embodiment will be described with reference to Fig. 20A, Fig. 20B and Fig. 21.
[0204] First, the scanning line 107_m-1 and the scanning line 107_m, each having a gate electrode serving area, is formed over the substrate 102. An insulating film which forms the gate insulating film 127 is formed to form the substrate 102, the scanning line 107_m-1 and the scanning line 107_m The opening 123 is formed in a region of the insulating film that is in contact with the scanning line 107_m-1. formed so that the gate insulating film 127 is formed. The oxide semiconductor film 111 is formed to be connected to the Scanning line 107_m to overlap. The oxide semiconductor film 119 is formed over the gate insulating film 127 and in the opening 123 formed to overlap with an area on which the pixel electrode 121 is to be formed. The signal line 109_n, which has a region serving as a source electrode, and the conductive film 113 which has a region serving as a drain electrode The insulating film 128 is formed over the gate insulating film 127, the signal line 109_n, the oxide semiconductor film 111, the conductive film 113, and the oxide semiconductor film 119. The insulating film 130 is formed over the insulating film 128 (see Fig. 20A). It should be noted that the above steps with respect to the Embodiment 1 can be carried out.
[0205] Then, a mask is formed over a portion of the insulating film 130 which is at least in contact with the oxide semiconductor film 111. The processing is carried out in such a way that an insulating film 228 and an insulating film 230 are formed using the mask and the oxide semiconductor film 119 is exposed. An insulating film 233 is formed over the exposed region and the insulating film 230 (see Fig. 20B). The mask can be a photoresist mask formed by a Photolithography process can be used, and the processing can be done by dry etching and / or Wet etching can be carried out. The insulating film 233 is similar to the insulating film 133 described in Embodiment 1 similar. It should be noted that heat treatment is preferably carried out while the insulating film 233 is in Contact with the oxide semiconductor film 119, e.g., after the insulating film 233 has been formed. The above steps can be carried out with respect to Embodiment 1.
[0206] When a nitride insulating film is formed by a plasma CVD method or a sputtering method as the insulating film 233 is formed, the oxide semiconductor film 119 is exposed to plasma; therefore, oxygen vacancies in the oxide semiconductor film 119 is formed. Since the insulating film 233, which is formed using a nitride insulating film, contact with the oxide semiconductor film 119, nitrogen and / or hydrogen are also transferred from the insulating film 233 to the oxide semiconductor film 119. When hydrogen enters the oxygen vacancies in the insulating film 233, Alternatively, a nitride insulating film is formed as the insulating film 232 and a Heat treatment is performed while the insulating film 232 is in contact with the oxide semiconductor film 119; therefore Nitrogen and / or hydrogen in the nitride insulating film are transferred to the oxide semiconductor film 119. This causes the electrical conductivity of the oxide semiconductor film 119 is increased, and the oxide semiconductor film 119 has a conductivity of N- Type. In addition, the oxide semiconductor film 119 becomes a conductive film with a light-transmitting property, which has a Metal oxide film with conductive properties. The oxide semiconductor film 119 has a higher electrical conductivity than the oxide semiconductor film 111.
[0207] Next, the opening 117 reaching the conductive film 113 is formed in the insulating films 228, 230 and 233 formed so that the insulating films 229, 231 and 232 are formed (see Fig. 21). Then, the pixel electrode 121, which is in contact with the conductive film 113 through the opening 117 (see Fig. 19). The above Steps may be performed with respect to Embodiment 1.
[0208] Through the above process, the semiconductor device according to this embodiment can be manufactured. <modifikationsbeispiel>
[0209] In the semiconductor device in this embodiment, the structure of a region where a capacitor provided, can be changed as needed. A concrete example is described using Fig. 22. The pixel 101 (m, n) in Fig. 22 has a capacitor 245 which includes the gate insulating film 127, the structure of which is different from that in Capacitor 105 of pixel 101 (m, n), which is shown in Fig. 5 and Fig. 6 in an area where the capacitor is provided.
[0210] The cross-sectional structure of the pixel 101 (m, n) in Fig. 22 is shown as follows. The gate insulating film 127 is a Stack of an insulating film 226 formed using a nitride insulating film and an insulating film 227, formed using an oxide insulating film, and only the insulating film 226 is provided in a region where at least the oxide semiconductor film 119 is provided. In such a structure, the nitride insulating film is Forming the insulating film 226 in contact with the base surface of the oxide semiconductor film 119 so that the oxide semiconductor film 119 which can exhibit N-type conductivity and higher conductivity. Regarding the top view according to Fig. 22 can be referred to Fig. 5. In this case, a dielectric film of the capacitor 245 forms the insulating films 129, 131 and 132. As the insulating films 226 and 227, the insulating films can be used as needed, which serve as the gate Insulating film 127 can be used, and the insulating film 227 can be made using an insulating film corresponding to the Insulating film 132 is similar. In addition, the insulating film 227 is formed as required with respect to the Embodiment 1 edited to obtain this structure.
[0211] In the structure in Fig. 22, the upward-facing surface of the oxide semiconductor film 119 can be in contact with the Insulating film 132. Namely, areas of the insulating films 129 and 131 in Fig. 22 that are in contact with the oxide semiconductor film 119 are removed. In this case, a dielectric film of the capacitor is the insulating film 132. When the upward-facing surface and the bottom surface of the oxide semiconductor film 119 are in contact with the Nitride insulating film, the oxide semiconductor film 119 can be made more efficient and sufficient so that it has N-type conductivity and higher conductivity than the oxide semiconductor film 119, in which only one of its surfaces in contact with the nitride insulating film.
[0212] With the structure in Fig. 22, a reduction in the thickness of the oxide semiconductor film 119 due to etching of the insulating film 129 and insulating film 131 can be prevented; thus, the yield of the semiconductor device is improved, compared to the semiconductor device in Fig. 18 and Fig. 19 .
[0213] Consequently, a semiconductor film is used as an electrode of a capacitor in the same process as a semiconductor film of a transistor, whereby a semiconductor device can be manufactured in which the aperture ratio is improved and the capacitance of the capacitor is increased. For example, if the pixel density of the semiconductor device in this embodiment is also about 300 ppi, the aperture ratio of the pixel is 50% or higher, 55% or higher, even 60% or higher. In addition, increasing the aperture ratio can Provide semiconductor device with excellent display quality.
[0214] Furthermore, oxygen vacancies and impurities such as hydrogen and nitrogen in the semiconductor film (in particular the oxide semiconductor film) of the transistor, so that the semiconductor device of an embodiment of the present invention has good electrical properties.
[0215] It should be noted that the structure and the like in this embodiment may be used in combination with any of the Structures and modification examples can be used in the other embodiments. (Embodiment 3)
[0216] In this embodiment, a semiconductor device of an embodiment of the present invention, which a different structure than that of the above embodiment will be described with reference to drawings. It should be noted that in this embodiment, a liquid crystal display device is used as an example of the semiconductor device an embodiment of the present invention. In the embodiment described in this Semiconductor device is a semiconductor film (especially an oxide semiconductor film) used as an electrode of a capacitor different from the one in the above embodiment. Regarding components of the Semiconductor device in this embodiment which is similar to that of the semiconductor device in the above embodiment are similar, refer to the above embodiment. <Struktur einer Halbleitervorrichtung>
[0217] Fig. 23 is a plan view of a pixel in this embodiment. The pixel 101 (m, n) in Fig. 23 includes a Capacitor 305. The capacitor 305 is arranged in a region separated from the scanning line 107_m, the Scanning line 107_m-1, signal line 109_n, and signal line 109_n+1. Capacitor 305 includes an oxide semiconductor film 319 having a higher electrical conductivity than the oxide semiconductor film 111 and a light-transmitting property, the pixel electrode 121 with a light-transmitting property and an insulating film (not in Fig. 23) having a light-transmitting property, which is included in the transistor 103 as a dielectric film. This means that the capacitor 305 has a light-transmitting property. In addition, since the oxide semiconductor film 319 through the opening 123 in contact with the scanning line 107_m-1, the capacitor 305 is electrically connected to the scanning line 107_m-1 connected.
[0218] The conductivity of the oxide semiconductor film 319 is higher than or equal to 10 S / cm and lower than or equal to 1000 S / cm, preferably higher than or equal to 100 S / cm and lower than or equal to 1000 S / cm. The oxide semiconductor film 319 has a such high conductivity and is therefore sufficient to serve as the electrode of the capacitor.
[0219] Since the capacitor 305 transmits light, the capacitor can be used in the entire operating range of the liquid crystal element, and thus the capacitor can be as large (in a large area) as possible in the pixel. As long as the capacity sufficient to operate the liquid crystal element is ensured can be increased, the pixel density can be increased to achieve high resolution.
[0220] Since the capacitor 305 has a higher capacitance per unit area than the capacitor 105 in the embodiment 1, the area of the oxide semiconductor film required to obtain the capacity can be that of the capacitor 105 is small. Consequently, an area on which the oxide semiconductor film 319 is not formed can in the pixel 101 (m, n) in Fig. 23. Thus, the light extraction efficiency (transmittance) of a Light source such as a backlight in the semiconductor device of an embodiment of the present invention can be improved; as a result, the display quality can be improved.
[0221] A cross-sectional view along the dash-dot line A1-A2 and the dash-dot line B1-B2 in Fig. 23 is shown in Fig. 24 shown.
[0222] A cross-sectional structure of the pixel 101 (m, n) in Fig. 23 is shown as follows. Above a substrate 102, the scanning line 107_m and the scanning line 107_m-1, each having a region serving as a gate electrode, The gate insulating film 127 is arranged over the scanning line 107_m-1 and the scanning line 107_m. Oxide semiconductor film 111 is disposed over the gate insulating film 127 to overlap with the scanning line 107_m. The Opening 123, which reaches the scanning line 107_m-1, is arranged in a region of the gate insulating film 127 which is in Contact with the scanning line 107_m-1. The oxide semiconductor film 319 is formed over the gate insulating film 127 and in the Opening 123. The signal line 109_n, which has a region serving as a source electrode, and the conductive film 113, which has a region serving as a drain electrode, are each formed over the oxide semiconductor film 111 and the Gate insulating film 127. An insulating film 129, an insulating film 131 and an insulating film 132, which serve as protective insulating films of the transistor 103 are provided over the gate insulating film 127, the signal line 109_n, the oxide semiconductor film 111, the conductive film 113 and the oxide semiconductor film 319. The opening 117 reaching the conductive film 113 is in the insulating film 129, the insulating film 131 and the insulating film 132, and the pixel electrode 121 is in the opening 117 and arranged over the insulating film 132. It should be noted that a base insulating film is arranged between the substrate 102, and the scanning lines 107 and the gate insulating film 127.
[0223] In the capacitor 305, the oxide semiconductor film 319 having N-type conductivity and a region with a higher electrical conductivity than the oxide semiconductor film 111, as one electrode of a pair of Electrodes, the pixel electrode 121 serves as the other of the pair of electrodes, and the insulating film 129, the insulating film 131 and the insulating film 132 serve as the dielectric film between the pair of electrodes.
[0224] For the oxide semiconductor film 319, an oxide semiconductor can be used which is suitable for the oxide semiconductor film 111 can be used. Since the oxide semiconductor film 319 is formed by applying the oxide semiconductor film manufacturing process 111, the oxide semiconductor film 319 contains a metal element of an oxide semiconductor which is present in the oxide semiconductor film 111. In addition, the oxide semiconductor film 319 includes a region with a higher electrical conductivity than the oxide semiconductor film 111, which means that the oxide semiconductor film 319 is an element (dopant) that increases the electrical conductivity. In particular, the oxide semiconductor film 319 contains as dopant one or more consisting of boron, nitrogen, fluorine, aluminum, phosphorus, arsenic, indium, tin, antimony and a noble gas element. The concentration of a dopant contained in the oxide semiconductor film 319, 19 3 22 3 is preferably higher than or equal to 1 × 10 atoms / cm and lower than or equal to 1 × 10 atoms / cm , in which If the conductivity of the oxide semiconductor film 319 is higher than or equal to 10 S / cm and lower than or equal to 1000 S / cm, preferably higher than or equal to 100 S / cm and lower than or equal to 1000 S / cm, so that the oxide semiconductor film 319 may be sufficient to serve as one electrode of the capacitor 305. It should be noted that the oxide semiconductor film 319 has N-type conductivity and high conductivity because it contains the above element (dopant); therefore the oxide semiconductor film 319 can be called conductive film.
[0225] Furthermore, in the semiconductor device of this embodiment, the oxide semiconductor film 319 serving as a Electrode of the capacitor 305, the N-type conductivity and a high electrical conductivity as in the Embodiment 2; therefore, the threshold voltage (Vth) shifts in the negative direction. Consequently, the Operating method of the capacitor 305 is similar to that in Embodiment 2. <Verfahren zum Herstellen einer Halbleitervorrichtung>
[0226] Next, a method of manufacturing a semiconductor device of this embodiment will be described with reference to Fig. 25A, Fig. 25B, Fig. 26A and Fig. 26B.
[0227] The scanning lines 107_m-1 and 107_m, each serving as a gate electrode, are formed over the substrate 102 An insulating film to be processed into the gate insulating film 127 is formed around the substrate 102, the Scanning line 107_m-1 and the scanning line 107_m. The opening 123 is formed in a region of the insulating film, which is in contact with the scanning line 107_m-1, so that the gate insulating film 127 is formed. The Oxide semiconductor film 111 is formed to overlap with the scanning line 107_m. The oxide semiconductor film 119 is formed over the gate insulating film 127 and in the opening 123 to form a region on which the pixel electrode 121 to be formed (see Fig. 25A). It should be noted that the above steps are related to the Embodiment 1 can be carried out.
[0228] Next, a dopant is added to the oxide semiconductor film 119 to form the oxide semiconductor film 319 and then the signal line 109_n, which has a region serving as a source electrode, and the conductive film 113 having a region serving as a drain electrode is formed (see Fig. 25B).
[0229] A method for adding a dopant to the oxide semiconductor film 119 is described as follows: a mask is provided in a region other than the oxide semiconductor film 119 and one or more dopants selected from boron, Nitrogen, fluorine, aluminum, phosphorus, arsenic, indium, tin, antimony and a noble gas element are added to the oxide semiconductor film 119 by an ion implantation method, a ion doping process or the like. Alternatively, the oxide semiconductor film 119 may be exposed to a plasma containing the dopant to add the dopant to the oxide semiconductor film 119, instead of a Ion implantation or ion doping is used. It should be noted that a Heat treatment can be performed after the dopant has been added to the oxide semiconductor film 119. The heat treatment can be carried out as required with regard to the details of the heat treatment for removing water or hydrogen of the oxide semiconductor film 111 and the oxide semiconductor film 119 in Embodiment 1.
[0230] The step of adding the dopant may be performed after forming the signal line 109_n and the conductive film 113 are carried out.
[0231] Next, the insulating film 128 is formed over the gate insulating film 127, the signal line 109_n, the oxide semiconductor film 111, the conductive film 113 and the oxide semiconductor film 319. The insulating film 130 is formed over the insulating film 128 formed, and the insulating film 133 is formed over the insulating film 130 (see Fig. 26A). The above steps can with respect to Embodiment 1.
[0232] Next, the opening 117 reaching the conductive film 113 is formed in the insulating films 128, 130 and 133, formed so that the insulating films 129, 131 and 132 are formed (see Fig. 26B). The pixel electrode 121, which is Contact with the conductive film 113 through the opening 117 is formed (see Fig. 24). The above steps can be carried out with respect to Embodiment 1.
[0233] By the above process, the semiconductor device in this embodiment can be manufactured.
[0234] Consequently, a semiconductor film is used as an electrode of a capacitor in the same process as a semiconductor film of a transistor, whereby a semiconductor device can be manufactured in which the aperture ratio is improved and the capacitance of the capacitor is increased. For example, if the pixel density of the semiconductor device is also about 300 ppi, the aperture ratio of the pixel 50% or higher, 55% or higher, even 60 % or higher in this embodiment. In addition, increasing the aperture ratio can Provide semiconductor device with excellent display quality.
[0235] Furthermore, oxygen vacancies and impurities such as hydrogen and nitrogen in the semiconductor film (in particular the oxide semiconductor film) of the transistor, so that the semiconductor device of an embodiment of the present invention has good electrical properties.
[0236] It should be noted that the structure and the like in this embodiment are appropriate in combination with one of the structures of the other embodiments. (Embodiment 4)
[0237] In this embodiment, an embodiment suitable for an oxide semiconductor film having a Semiconductor film is in the transistor and the capacitor which are included in the semiconductor device which is in the above embodiment is applicable.
[0238] The oxide semiconductor film is preferably formed using one of an amorphous oxide semiconductor, a single-crystalline oxide semiconductor, a polycrystalline oxide semiconductor and an oxide semiconductor having a crystal region (a crystalline oxide semiconductor with alignment with respect to the c-axis or c-axis aligned crystalline oxide semiconductor (CAAC-OS)).
[0239] A crystal region in the CAAC-OS fits into a cube with an edge length of less than 100 nm. In a observation image obtained with a transmission electron microscope (TEM), in the CAAC-OS a limit between crystal regions is not clear. Furthermore, no grain boundary was found in the CAAC-OS by TEM. Consequently, in the CAAC-OS, a reduction in electron mobility attributed to the grain boundary is suppressed.
[0240] In each of the crystal regions contained in the CAAC-OS, a c-axis is oriented in a direction which parallel to a normal vector of a surface where the CAAC-OS is formed, or to a normal vector of a surface of the CAAC-OS is a triangular or hexagonal atom arrangement is formed, which is viewed from the direction perpendicular to the ab-plane, and metal atoms are in a arranged in a layered manner or metal atoms and oxygen atoms are arranged in a layered manner, when viewed from the direction perpendicular to the c-axis. It should be noted that for crystal regions the directions of the a-axis and the b-axis of one crystal region from those of another crystal region may vary. In this description, the term "perpendicular" covers a range of 85° to 95°. In addition, the term ´´parallel´´ covers a range from -5° to 5°. A part of the oxygen of the oxide semiconductor can be replaced by nitrogen.
[0241] In the CAAC-OS, the distribution of the crystal regions is not necessarily uniform. For example, in the Formation process of the CAAC-OS in the case where the crystal growth from one surface side of the oxide semiconductor film, the proportion of crystal regions near the surface of the oxide semiconductor film in In some cases, it is higher than that near the surface where the oxide semiconductor film is formed. When an impurity is added to the CAAC-OS, the crystallinity of the crystal region in a range to which the impurity is added, in some cases reduced. Consequently, if the concentration of the Impurities (typically silicon or carbon) in the CAAC-OS lower than or equal to 1 atomic%, preferably is less than or equal to 0.6 atom%, a CAAC-OS with high crystallinity can be formed.
[0242] Since the c-axes of the crystal regions contained in the CAAC-OS are aligned in the direction parallel to a normal vector of a surface where the CAAC-OS is formed, or to a normal vector of a surface of the CAAC-OS can be determined depending on the shape of the CAAC-OS (the cross-sectional shape of the surface where the CAAC- OS is formed, or the cross-sectional shape of the surface of the CAAC-OS) the directions of the c-axes are It should be noted that when the CAAC-OS is formed, the direction of the c-axis of the crystal region is such a direction that is parallel to a normal vector of the surface where the CAAC-OS is formed or to a normal vector of the surface of the CAAC-OS. The crystal area is determined by the film formation or formed by a crystal formation treatment, such as a heat treatment after film formation.
[0243] There are three methods for forming a CAAC-OS.
[0244] In the first method, an oxide semiconductor film is formed at a temperature higher than or equal to 100 °C and lower than or equal to 450 °C, resulting in crystal regions in which the c-axes are aligned in the direction which are parallel to a normal vector of a surface where the oxide semiconductor film is formed or to a Normal vector of a surface of the oxide semiconductor film in which oxide semiconductor film is formed.
[0245] In the second method, an oxide semiconductor film is formed with a small thickness, and then it is a temperature higher than or equal to 200 °C and lower than or equal to 700 °C, whereby crystal regions, in which the c-axes are aligned in the direction parallel to a normal vector of a surface where the oxide semiconductor film, or to a normal vector of a surface of the oxide semiconductor film, in which oxide semiconductor film can be formed.
[0246] In the third method, a first oxide semiconductor film is formed with a small thickness, then it is a temperature higher than or equal to 200 °C and lower than or equal to 700 °C, and a second Oxide semiconductor film is formed, whereby crystal regions in which the c-axes are aligned in the direction, the parallel to a normal vector of a surface where the oxide semiconductor film is formed, or to a Normal vector of a surface of the oxide semiconductor film in which oxide semiconductor film is formed.
[0247] In a transistor using the CAAC-OS for an oxide semiconductor film, the change in the electrical The transistor's properties are small when exposed to visible or UV light. Consequently, the transistor, which which uses CAAC-OS for the oxide semiconductor film, has a high reliability.
[0248] For example, the CAAC-OS is preferably formed by a sputtering process using a polycrystalline When ions collide with the sputtering target, a layer of oxide in the sputtering target The crystal region contained in the sputtered layer can be separated from the target along an ab-plane. In other words: a sputtered Particles with a plane parallel to the ab-plane (flat plate-shaped sputtered particle or pellet-shaped sputtered particle) can fall off the sputtering target. In In this case, the flat plate-shaped or pellet-shaped sputtered particle reaches a surface where the CAAC-OS while maintaining its crystalline state. This allows the CAAC-OS to be deposited.
[0249] The following conditions are preferably used for the deposition of the CAAC-OS.
[0250] By reducing the amount of contaminants entering the CAAC-OS during deposition, it can prevent the crystal state from being spoiled by the impurities. For example, the Concentration of impurities present in the deposition chamber (e.g. hydrogen, water, carbon dioxide or nitrogen). In addition, the concentration of impurities in a deposition gas In particular, a deposition gas is used whose dew point is lower than or equal to -80 ° C, preferably lower than or equal to -100 °C.
[0251] By increasing the heating temperature of the surface during deposition where the CAAC-OS is formed (e.g. the temperature at which the substrate is heated), migration of a sputtered particle after the sputtered particle has reached the surface where the CAAC-OS is formed. In In particular, the temperature of the surface during deposition where the CAAC-OS is formed is higher than or equal to 100 °C and lower than or equal to 740 °C, preferably higher than or equal to 150 °C and lower than or equal to 500 °C. By increasing the temperature of the surface during deposition where the CAAC-OS is formed, when the flat plate-shaped or pellet-shaped sputtered particle reaches the surface where the CAAC-OS is formed, a migration on the surface where the CAAC-OS is formed, so that a flat surface of the sputtered particle adheres to the surface where the CAAC-OS is formed.
[0252] Furthermore, it is preferable that the oxygen content of the deposition gas is increased and the power optimized to reduce plasma damage during deposition. The oxygen content of the deposition gas is higher than or equal to 30 vol%, preferably 100 vol%.
[0253] As an example of the sputtering target, a target made of an In-Ga-Zn-O compound is described below.
[0254] The In-Ga-Zn based polycrystalline metal oxide target is prepared by mixing InO powder, GaO - XY Powder and ZnO powder in a predetermined molar ratio, applying pressure and performing a Z Heat treatment at a temperature higher than or equal to 1000 °C and lower than or equal to 1500 °C This pressure treatment can be carried out during cooling or heating. It should be noted that X, Y and Z are predetermined positive numbers. Here, the predetermined molar ratio of InO - X Powder to GaO powder and ZnO powder, for example 2:2:1, 8:4:3, 3:1:1, 1:1:1, 4:2:3 or 3:1:2. The powder types and the YZ The molar ratio in which the powders are mixed can be adjusted as required depending on the desired sputtering target be determined.
[0255] The oxide semiconductor film may further have a structure in which a plurality of oxide semiconductor films are stacked. For example, the oxide semiconductor film may have a stacked layer structure of a first oxide semiconductor film and a second oxide semiconductor film formed using metal oxides with different compositions For example, the first oxide semiconductor film can be formed using one of two types of metals-containing oxide, an oxide containing three types of metals and an oxide containing four types of metals containing oxide, and the second oxide semiconductor film may be formed using one of the above oxides which is different from the one used for the first oxide semiconductor film.
[0256] Alternatively, the oxide semiconductor film may have a two-layer structure of the first oxide semiconductor film and the second oxide semiconductor film, the constituent elements of which are the same and the atomic ratios of the Constituent elements of the first oxide semiconductor film and the second oxide semiconductor film are different. For example, the first oxide semiconductor film contains In, Ga and Zn with an atomic ratio of 3:1:2, and the second oxide semiconductor film may contain In, Ga and Zn with an atomic ratio of 1:1:1. Alternatively, the first oxide semiconductor film may contain In, Ga and Zn with an atomic ratio of 2:1:3, and the second oxide semiconductor film may contain In, Ga and Zn with a atomic ratio of 1:3:2. It should be noted that a portion of each atom in the atomic ratio of the oxide semiconductor film varies within an error range of ±20%.
[0257] Here, in one of the first oxide semiconductor film and the second oxide semiconductor film which is closer to the gate electrode (on the channel side), the atomic ratio of In to Ga preferably has the relationship In ≥ Ga. In the another oxide semiconductor film facing away from the gate electrode (on the back channel side), the atomic ratio of In to Ga preferably satisfies the relationship In ≤ Ga. With a stacked layer structure of this A transistor with high field-effect mobility can be fabricated using oxide semiconductor films. In contrast, the atomic ratio of In to Ga in the oxide semiconductor film closer to the gate electrode (the oxide semiconductor film on the channel side), the relationship In < Ga, and the atomic ratio of In to Ga in the Oxide semiconductor film on the back channel side satisfies the relationship In ≥ Ga, which reduces the amount of change in Threshold voltage of a transistor reduced as a result of a change over time or a reliability test can be.
[0258] The first oxide semiconductor film containing In, Ga and Zn with an atomic ratio of 1:3:2 may be formed by a Sputtering process using an oxide target with an atomic ratio of 1:3:2 under conditions where the substrate temperature is room temperature and a sputtering gas argon or a mixture of argon and oxygen. The second oxide semiconductor film, which contains In, Ga and Zn with an atomic ratio of 3:1:2, can be a sputtering process using an oxide target with an atomic ratio of 3:1:2 in a similar manner to the first oxide semiconductor film is formed.
[0259] Furthermore, the oxide semiconductor film may have a three-layer structure of a first oxide semiconductor film, a second oxide semiconductor film and a third oxide semiconductor film in which the constituent elements are the same, wherein the Atomic ratios of the constituent elements of the first oxide semiconductor film, the second oxide semiconductor film and the third oxide semiconductor film are made differently. The case where the oxide semiconductor film has a three-layer structure, is described in Fig. 27.
[0260] In a transistor 297 in Fig. 27, a first oxide semiconductor film 299a, a second oxide semiconductor film 299b and a third oxide semiconductor film 299c is stacked in this order from the side of the gate insulating film 127. As material of the first oxide semiconductor film 299a and the third oxide semiconductor film 299c, a material consisting of InM1 Zn (x x yOz ≥ 1, y > 1, z > 0, M1 is Ga, Hf or the like). It should be noted that in the case where a material of each of the first oxide semiconductor film 299a and the third oxide semiconductor film 299c contains Ga, a material having a large proportion of Ga, in particular a material that can be represented by InM1 Zn O, where x is greater than 10 xyz is unsuitable because a powder could be generated during deposition. It should be noted that the structure of the Transistor 297 is the same as that of the transistors in the above embodiments (e.g., transistor 103 in the Embodiment 1), except that the first oxide semiconductor film 299a, the second oxide semiconductor film 299b and the third oxide semiconductor film 299c.
[0261] As the material of the second oxide semiconductor film 299b, a material represented by InM2 Zn O (x ≥ 1, y ≥ 1, z > 0, xy2 M2 is Ga, Sn or the like).
[0262] Materials of the first oxide semiconductor film 299a, the second oxide semiconductor film 299b and the third Oxide semiconductor film 299c are selected as needed so that a well structure is formed in which the conduction band of the second oxide semiconductor film 299b is deeper, with respect to the vacuum level, than the conduction bands of the first oxide semiconductor film 299a and the third oxide semiconductor film 299c.
[0263] As described in Embodiment 1, silicon or carbon belonging to the group 14, in the oxide semiconductor film generation of electrons serving as charge carriers, which leads to an increase in An oxide semiconductor film becomes an N-type due to the presence of silicon or carbon in it. Oxide semiconductor film. Therefore, the concentration of silicon in oxide semiconductor films and the concentration of carbon 13 3 17 3 in oxide semiconductor films each lower than or equal to 3 × 10 / cm , preferably lower than or equal to 3 × 10 / cm . It It is particularly preferable to use a structure in which the first oxide semiconductor film 299a and the third Oxide semiconductor film 299c surrounds or encloses the second oxide semiconductor film 299b, which serves as a charge carrier path, so that not many group 14 elements enter the second oxide semiconductor film 299b. In other words, the first Oxide semiconductor film 299a and the third oxide semiconductor film 299c can also be called barrier films that prevent that group 14 elements such as silicon and carbon enter the second oxide semiconductor film 299b.
[0264] For example, the first oxide semiconductor film 299a may contain In, Ga and Zn with an atomic ratio of 1:3:2, the second oxide semiconductor film 299b may contain In, Ga and Zn with an atomic ratio of 3:1:2 and the third oxide semiconductor film 299c may contain In, Ga and Zn with an atomic ratio of 1:1:1. noted that the third oxide semiconductor film 299c is formed by a sputtering method using an oxide target containing In, Ga and Zn with an atomic ratio of 1:1:1.
[0265] Alternatively, a three-layer structure may be used in which the first oxide semiconductor film 299a contains In, Ga and Zn with an atomic ratio of 1:3:2, the second oxide semiconductor film 299b contains In, Ga and Zn with an atomic ratio of 1:1:1 or 1:3:2, and the third oxide semiconductor film 299c contains In, Ga and Zn with an atomic ratio of 1:3:2.
[0266] Since the constituent elements of the first oxide semiconductor film 299a, the second oxide semiconductor film 299b and the third oxide semiconductor film 299c are the same, the second oxide semiconductor film 299b has fewer defect states (trap levels) at the interface with the first oxide semiconductor film 299a. In particular, the defect states (trap levels) less than the defect states at the interface between the gate insulating film 127 and the first oxide semiconductor film 299a. For this reason, when the oxide semiconductor films are stacked in the above manner, the size of the Change in the threshold voltage of a transistor due to a change over time or a Reliability testing can be reduced.
[0267] Further, when materials of the first oxide semiconductor film 299a, the second oxide semiconductor film 299b and the third oxide semiconductor film 299c can be selected as required so that a well structure is formed, in which the conduction band of the second oxide semiconductor film 299b is lower, from the vacuum level, than the conduction bands of the first oxide semiconductor film 299a and the third oxide semiconductor film 299c, the field-effect mobility (field-effect mobility) of the transistor and the magnitude of the change in the threshold voltage of the transistor as a result a change over time or a reliability test can be reduced.
[0268] In addition, the first oxide semiconductor film 299a, the second oxide semiconductor film 299b and the third oxide semiconductor film 299c using oxide semiconductors with different degrees of crystallization. With other In other words, the oxide semiconductor film can be formed as required with a combination of any of a single-crystal oxide semiconductor, a polycrystalline oxide semiconductor, an amorphous oxide semiconductor and a CAAC-OS When an amorphous oxide semiconductor is used as one of the first oxide semiconductor film 299a, the second oxide semiconductor film 299b and the third oxide semiconductor film 299c, an internal voltage or external voltage of the oxide semiconductor film can be facilitated, fluctuations in the electrical properties of the transistors can be reduced and the magnitude of the change in the threshold voltage of the transistor due to a change over time or a reliability check can be reduced.
[0269] At least the second oxide semiconductor film 299b, which can serve as a channel formation region, is preferably a CAAC OS film. An oxide semiconductor film on the rear channel side, ie the third oxide semiconductor film 299c in this Embodiment, is preferably an amorphous oxide semiconductor film or a CAAC-OS film. With such a structure can measure the magnitude of the change in the threshold voltage of a transistor as a result of a change over time or a reliability check.
[0270] It should be noted that the structure and the like in this embodiment may be used in combination with one of the structures of the other embodiments. (Embodiment 5)
[0271] A semiconductor device having a display function (also referred to as a display device) may be Using the transistor and the capacitor, for the examples in the above embodiments have been described. In addition, some or all of the driver circuits that support the transistor, formed over a substrate where a pixel portion is formed, thereby forming a system on the display panel (system on panel). In this embodiment, an example of a Display device using the transistor, examples of which are described in the above embodiments described with reference to the drawings. Fig. 29 is a cross-sectional view showing a cross-sectional structure along the dot-dash line X1-X2 in Fig. 28B. It should be noted that in Fig. 29 only a part of the structure of a pixel section is shown.
[0272] In Fig. 28A, a sealing material 905 is arranged such that it forms a layer arranged over a first substrate 901. pixel portion 902, wherein the pixel portion 902 is sealed with a second substrate 906. In Fig. 28A, a signal line driver circuit 903 and a scan line driver circuit 904 each using a single-crystalline semiconductor or a polycrystalline semiconductor over a separately prepared substrate, and in an area different from the area surrounded by the sealing material 905, above the first substrate 901. Furthermore, various signals and potentials are applied to the Signal line driver circuit 903, scanning line driver circuit 904 and pixel section 902 of a flexible printed circuit (flexible printed circuit: FPC) 918.
[0273] In Fig. 28B and Fig. 28C, the sealing material 905 is arranged such that it covers the pixel portion 902 and the Scan line driver circuit 904 arranged above the first substrate 901. The second substrate 906 is arranged above the pixel section 902 and the scan line driver circuit 904. As a result, the pixel section 902 and the scanning line driver circuit 904 together with a display element through the first substrate 901, the Sealing material 905 and the second substrate 906 are sealed. In Fig. 28B and Fig. 28C, a Signal line driver circuit 903 constructed using a single-crystal semiconductor or a polycrystalline semiconductor over a separately prepared substrate, in a region which is different from that of the Sealing material 905 is different, mounted over the first substrate 901. In Fig. 28B and Fig. 28C shows various signals and potentials to the signal line driver circuit 903, the scan line driver circuit 904 and the pixel section 902 from an FPC 918.
[0274] Although Fig. 28B and Fig. 28C each illustrate an example in which the signal line driver circuit 903 formed separately and mounted on the first substrate 901 is an embodiment of the present invention not limited to this structure. The scanning line driver circuit can be formed separately and then assembled or only part of the signal line driver circuit or part of the scan line driver circuit be designed separately and then assembled.
[0275] It should be noted that a connection method of a separately formed driver circuit does not require a special restrictions, and a chip on glass (COG) process, a wire bonding process (wire bonding method), an automatic bonding using a tape (tape automated bonding: TAB) method or the like can be used. Fig. 28A shows an example in which the signal line driver circuit 903 and the Scan line driver circuit 904 are assembled by a COG method. Fig. 28B shows an example in which the Signal line driver circuit 903 is mounted by a COG method. Fig. 28C shows an example in which the Signal line driver circuit 903 is mounted by a TAB method.
[0276] The display device includes in its category a display panel in which a display element is sealed, and a module in which an integrated circuit (IC) containing a regulator or the like is connected to mounted on the display panel.
[0277] A display device in this specification refers to an image display device, a display device or a light source (including an illumination device). The display device further comprises Category also includes the following modules: a module to which a connector such as an FPC or a Tape Carrier Package (TCP); a module with a TCP whose end is provided with a printed circuit board; and a module, in which an integrated circuit (IC) is mounted directly on a display element by a COG process.
[0278] The pixel section 902 and the scanning line driver circuit 904 provided over the first substrate 901 include a plurality of transistors, and one of the transistors used in the above embodiments described can be applied.
[0279] As a display element arranged in the display device, a liquid crystal element (also known as liquid crystal display element) or a light-emitting element (also called a light-emitting display element A light-emitting element includes in its category an element whose Luminance is controlled by a current or a voltage, and in particular an organic electroluminescent (EL) element, an inorganic EL element, etc. In addition, a display medium whose contrast is changed by an electrical effect, such as electronic ink. An example of a Liquid crystal display device using a liquid crystal element as a display element is shown in Fig. 29 shown.
[0280] The liquid crystal display device in Fig. 29 is a vertical electric field mode display device. A liquid crystal display device includes a connection terminal electrode 915 and a terminal electrode 916. The connection terminal electrode 915 and the connection electrode 916 are electrically connected to a terminal formed in the FPC 918 is connected by an anisotropic conductive material 919.
[0281] The connection terminal electrode 915 is formed using the same conductive film as a first Electrode 930 is formed, and the terminal electrode 916 is formed using the same conductive film as a A source electrode and a drain electrode of each of a transistor 910 and a transistor 911 are formed.
[0282] The pixel section 902 and the scanning line driver circuit 904 arranged above the first substrate 901 each include a plurality of transistors. Transistor 910 is included in pixel section 902 and the Transistor 911 is included in the scan line driver circuit 904. An insulating film 924, which is connected to the insulating films 129, 131 and 132 described in Embodiment 1 is formed over oxide semiconductor films of the transistors 910 and 911. Note that an insulating film 923 is an insulating film serving as a base film.
[0283] In this embodiment, each of the transistors described in the above embodiments have been used as the transistors 910 and 911. A capacitor 926 is connected using a oxide semiconductor film 927, the insulating film 924 and the first electrode 930. It should be noted that the Oxide semiconductor film 927 is electrically connected through an opening formed in a gate insulating film 922 with a Scanning line 929, which serves as a capacitor line. The scanning line 929 is connected using the same conductive film such as scanning lines having regions serving as gate electrodes of the transistors 910 and 911. Although a capacitor having the structure described in Embodiment 1 is used here in the Drawing as the capacitor 926, a capacitor having the structure shown in each of the other embodiments described may be used as required.
[0284] In addition, an example is shown in which a conductive film 917 is formed in a region of the insulating film 924 in the Transistor 911 included in the scanning line driver circuit 904 is provided such that the conductive film 917 overlaps with a channel formation region of the oxide semiconductor film. The conductive film 917 can have a potential and serve as the gate electrode of transistor 911. This means that transistor 911 is a double-gate transistor (dual gate transistor). It should be noted that the conductive film 917 is formed using the same conductive film as the first electrode 930 may be formed. In addition, the width of the conductive film 917 in the direction of Channel length should be shorter than the distance between the source electrode and the drain electrode of transistor 911.
[0285] Thanks to the conductive film 917, a fluctuation of the gate voltage (rising gate voltage) in which a Forward current begins to flow at different drain voltages in the transistor 911, which is in the scan line driver circuit 904. With the conductive film 917, a current can be further controlled in a region of the oxide semiconductor film on the side of the conductive film 917 and between the source electrode and the drain electrode of transistor 911. Consequently, fluctuations in the electrical Characteristics between a plurality of transistors included in the scan line driver circuit 904, In addition, if the potential of the conductive film 917 is equal to the minimum potential of the Scan line driver circuit 904 of transistor 911 is equal or substantially equal, a fluctuation of the Threshold voltage of the transistor 911 can be reduced; thus, the reliability of the transistor 911 can be improved It should be noted that the minimum potential of the scan line driver circuit 904 is the lowest potential of the Potentials supplied to operate the scan line driver circuit 904. In the case where the potential the source electrode of transistor 911 is used as a reference point of the potential required to operate the scan line driver circuit 904, the potential of the source electrode (Vss) is, for example, the minimum Potential.
[0286] In addition, the conductive film 917 has a function of blocking an external electric field. With other In other words, the conductive film 917 has a function to prevent an external electric field from affecting the interior (a circuit section including the transistor) (especially a function to avoid static Electricity). The static electricity prevention function of the conductive film 917 can prevent fluctuations in electrical properties of the transistor 911 due to the influence of an external electric field such as suppress static electricity; thus the Reliability of the transistor 911 can be improved. Although the transistor used in the scan line driver circuit shown in Fig. 29, a transistor included in a signal line driver circuit can also be a Double-gate transistor similar to the transistor 911. In the case where a double-gate transistor is used as a transistor used in the signal line driver circuit, the transistor has an effect similar to that of transistor 911.
[0287] Consequently, the semiconductor device (display device) of one embodiment of the present invention has a high reliability.
[0288] Here, a structure of a transistor used in the semiconductor device (display device) of a embodiment of the present invention, for example, a plurality of transistors included in the Scan line driver circuit 904 are included, in which a line containing a gate electrode and a line containing a source electrode or a drain electrode, electrically connected to each other via a conductive film Fig. 30A shows a plan view of the structure and Fig. 30B shows a cross-sectional view along the dash-dot line Line Y1-Y2 and the dash-dot line Z1-Z2 in Fig. 30A.
[0289] As shown in Fig. 30A, a line 950 containing the gate electrode of the transistor 911 and a Line 952 containing the source electrode or the drain electrode of the transistor 911 in contact with a conductive Film 958 disposed in an opening 954 and an opening 956.
[0290] As in the cross-sectional structure in Fig. 30B, the insulating film 923 is disposed over the first substrate 901, which Gate insulating film 922 is arranged over the line 950 and the insulating film 923, the line 952 is arranged over the gate Insulating film 922 is arranged and the insulating film 924 is arranged over the gate insulating film 922 and the line 952. Furthermore In a region along the dash-dot line Y1-Y2, the opening 954 reaching the line 950 is in the gate Insulating film 922 and insulating film 924. In an area along the dash-dot line Z1-Z2, the opening 956, which reaches the line 952, is arranged in the insulating film 924. Furthermore, the conductive film 958 is arranged over the insulating film 924 and arranged in the opening 954 and the opening 956.
[0291] According to the above, the line 950 containing the gate electrode and the line 952 containing the source electrode or the drain electrode are electrically connected to each other via the conductive film 958.
[0292] The conductive film 958 can be formed by applying the manufacturing process of the conductive film 917 of the transistor 911 be trained.
[0293] The opening 954 and the opening 956 may be formed simultaneously. The details are as follows. Insulating film to be processed into the gate insulating film 922 is formed over the line 950, the line 952 is formed over the insulating film and an insulating film to be processed into the insulating film 924 is formed over the line 952 formed. Thereafter, a mask is formed over the insulating film 924, and the insulating films are the mask to form the opening 954 and the opening 956. A photoresist mask can be used as a mask The insulating films can be processed by dry etching. If the line 950 is processed using a metal material or the like, the selectivity ratio of the line 950 and the gate insulating film 922 with respect to the line 950; thus, the opening 954 and the opening 956 are formed simultaneously by dry etching.
[0294] The transistor 910 in the pixel section 902 is electrically connected to a display element.
[0295] A liquid crystal element 913, which is a display element, includes the first electrode 930, a second electrode 931 and a liquid crystal 908. It should be noted that an insulating film 932 and an insulating film 933 serving as an alignment film are arranged such that the liquid crystal 908 is located therebetween. The second electrode 931 is on the side of the second substrate 906. The second electrode 931 overlaps with the first electrode 930, wherein the Liquid crystal 908 is located therebetween. Regarding the liquid crystal element 913, one can refer to the description of liquid crystal element 108 in Embodiment 1. The first electrode 930 corresponds to the pixel electrode 121 in the embodiment 1, the second electrode 931 corresponds to the counter electrode 154 in the embodiment 1, the Liquid crystal 908 corresponds to the liquid crystal 160 in the embodiment 1, the insulating film 932 corresponds to the Alignment film 158 in Embodiment 1, and the insulating film 933 corresponds to the alignment film 156 in the Embodiment 1.
[0296] The first electrode 930 and the second electrode 931 (each of them is also called a pixel electrode, common electrode, counter electrode or the like) for applying a voltage to the display element can have translucent properties or light-reflecting properties, which depend on the direction in which light extracted, the position where the electrodes are arranged, and the pattern structure of the electrodes depend.
[0297] The first electrode 930 and the second electrode 931 may be formed as needed using a material that similar to that of the pixel electrode 121 and the counter electrode 154 in Embodiment 1.
[0298] A spacer 935 is a columnar spacer obtained by selectively etching an insulating film and is provided to determine the distance between the first electrode 930 and the second electrode 931 (a Cell gap. Alternatively, a spherical spacer can be used.
[0299] The first substrate 901 and the second substrate 906 are fixed in place by a sealing material 905. As the Sealing material 905 may be an organic resin such as a thermosetting resin or a photocuring resin be used. Furthermore, the sealing material 905 is in contact with the insulating film 924.
[0300] In the semiconductor device (display device) of one embodiment of the present invention, a opaque film (black matrix), an optical component (an optical substrate), such as a polarization component, a retardation component (retardation member) or an antireflection component, and etc. are provided as required. For example, circular polarization can be achieved by using a polarization substrate and a retardation substrate. Furthermore, a backlight, a Side lighting or the like can be used as a light source.
[0301] Since the transistor is easily broken due to static electricity or the like, it is preferable to Protection circuit is provided to protect the driver circuit. The protection circuit is preferably Using a non-linear element.
[0302] Fig. 31A to Fig. 31C show an example of the display device in Fig. 28A to Fig. 28C and Fig. 29, in which has a portion (contact portion) for common electrical connection with the second electrode 931 formed on the second substrate 906 is arranged, is formed over the first substrate 901.
[0303] The joint connection portion is provided at a location provided with the sealing material for bonding the first substrate 901 to the second substrate 906 overlapped, provided and is electrically connected to the second electrode 931 via conductive particles in the sealing material. Alternatively, the section is connected to the a position that does not overlap with the sealing material (except the pixel portion), and a paste including conductive particles is provided separately from the sealing material to be connected to the section for common connection, whereby the common connection section is electrically connected to the second Electrode 931 is connected.
[0304] Fig. 31A is a cross-sectional view of the common connection portion taken along line IJ in the Top view in Fig. 31B.
[0305] A common potential line 975 is arranged over a gate insulating film 922 and is formed using of the same material and by the same steps as a source electrode 971 or a drain electrode 973 of the Transistor 910 in Fig. 31A to Fig. 31C.
[0306] Further, the common potential line 975 is covered with the insulating film 924, and the insulating film 924 has a A plurality of openings at a location that overlaps with the common potential line 975. These openings are formed by the same steps as a contact hole connecting the first electrode 930 and one of the source electrodes 971 and the drain electrode 973 of the transistor 910.
[0307] Furthermore, the common potential line 975 is connected to a common electrode 977 through the openings. common electrode 977 is arranged over the insulating film 924 and is formed using the same material and by the same steps as the connection terminal electrode 915 and the first electrode 930 in the pixel section trained.
[0308] In this way, the joint connection section can be manufactured by the same manufacturing process as the switching element may be formed in the pixel portion 902.
[0309] The common electrode 977 is an electrode that is in contact with the conductive particles in the Sealing material, and is electrically connected to the second electrode 931 of the second substrate 906.
[0310] Alternatively, as shown in Fig. 31C, a common potential line 985 can be formed using the same material and by the same steps as the gate electrode of transistor 910.
[0311] In the common connection section in Fig. 31C, the common potential line 985 is under the gate insulating film 922 and the insulating film 924; and the gate insulating film 922 and the insulating film 924 have a plurality of openings at a location that overlaps with the common potential line 985. These openings are Etching the insulating film 924 through the same steps as a contact hole connecting the first electrode 930 and one of the source Electrode 971 and the drain electrode 973 of the transistor 910, and by further selective etching of the gate Insulating film 922 is formed.
[0312] Furthermore, the common potential line 985 is connected to a common electrode 987 through the openings The common electrode 987 is arranged over the insulating film 924 and is connected using the the same material and through the same steps as the connecting terminal electrode 915 and the first electrode 930 formed in the pixel section.
[0313] Consequently, a semiconductor film is used as an electrode of a capacitor in the same process as a semiconductor film of a transistor, whereby a semiconductor device can be manufactured in which the aperture ratio is improved and the capacitance of the capacitor is increased. For example, if the pixel density of the semiconductor device is also about 300 ppi, the aperture ratio of the pixel 50% or higher, 55% or higher, even 60 % or higher in this embodiment. In addition, increasing the aperture ratio can Provide semiconductor device with excellent display quality.
[0314] Furthermore, oxygen vacancies and impurities such as hydrogen and nitrogen in the semiconductor film (in particular the oxide semiconductor film) of the transistor, so that the semiconductor device of an embodiment of the present invention has good electrical properties.
[0315] It should be noted that the structure and the like in this embodiment may be used in combination with one of the structures of the other embodiments. (Embodiment 6)
[0316] The semiconductor device of one embodiment of the present invention may be used in any of various electronic devices (including gaming machines). Examples of electronic devices include Television sets (also called TVs or TV receivers), computer monitors, cameras, such as Digital cameras or digital video cameras, digital photo frames, mobile phones, portable game consoles, portable Information terminals, audio playback devices, gaming machines (e.g. pachinko machines or Gaming machines), gaming machine housings, and the like. Examples of these electronic devices are shown in Fig. 32A to Fig. 32C.
[0317] Fig. 32A shows a table 9000 with a display section. In the table 9000, a display section 9003 installed in a housing 9001, and an image can be displayed on the display section 9003. It should be noted, that the housing 9001 is carried by four leg sections 9002. Furthermore, a power cable 9005 for supplying a Power provided to the chassis 9001.
[0318] The semiconductor device described in any of the above embodiments can be used in the display section 9003. Thus, the display quality of the display section 9003 can be improved.
[0319] The display section 9003 has a touch-sensitive input function. When a user presses displayed buttons 9004 displayed on the display section 9003 of the table 9000, with his finger or the like, The user can operate the screen and enter information. In addition, if the table 9000 is equipped with communicate with household appliances or control the household appliances, the table 9000 as a control device that Household appliances can be controlled by actions on the screen. For example, using a Semiconductor device with an image sensor function, the display section 9003 has a touch-sensitive input function have.
[0320] Furthermore, the screen of the display section 9003 can be hinged in the housing 9001 perpendicular to a floor; therefore, the table 9000 can also be used as a television. If a If a TV with a large screen is placed in a small room, a free space is reduced; if a However, since the display section is built into a table, a space in the room can be used efficiently.
[0321] Fig. 32B illustrates a television set 9100. In the television set 9100, a display section 9103 is arranged in a Housing 9101 and an image can be displayed on the display section 9103. It should be noted that here the housing 9101 is supported by a foot 9105.
[0322] The television set 9100 can be controlled by means of an operating switch of the housing 9101 or a separate Remote control 9110. With a control button 9109 of the remote control 9110, the television channels and the volume are controlled so that an image displayed on the display section 9103 can be controlled Furthermore, the remote control 9110 may have a display section 9107 for displaying data obtained from the Remote control 9110.
[0323] The television set 9100 in Fig. 32B is provided with a receiver, a modem, and the like. The TV set 9100 can receive general TV broadcasts. Furthermore, if the Television 9100 is connected to a communications network either wired or wirelessly via the modem, a unidirectional (from a sender to a receiver) or bidirectional (between a sender and a Recipients or between recipients) information transfer may be carried out.
[0324] The semiconductor device described in any of the above embodiments can be used in the display sections 9103 and 9107. This can improve the display quality of the television become.
[0325] Fig. 32C illustrates a computer 9200. The computer 9200 includes a main body 9201, a housing 9202, a display section 9203, a keyboard 9204, an external connection terminal 9205, a pointing device 9206 and the like.
[0326] The semiconductor device described in any of the above embodiments can be used for Display section 9203 can be used. This can improve the display quality of the computer.
[0327] Fig. 33A and Fig. 33B show a foldable tablet computer. In Fig. 33A the tablet computer is open and includes a housing 9630, a display section 9631a, a display section 9631b, a button for switching the display mode 9034, an on / off switch 9035, a button for switching the power saving mode 9036, a clasp 9033 and a button for operation 9038.
[0328] The semiconductor device described in any of the above embodiments can be used for display section 9631a and the display section 9631b. Thus, the display quality of the tablet Computers can be improved.
[0329] A part of the display section 9631a may be a touch screen area 9632a, and data may be displayed by touching displayed operation keys 9638. It should be noted that Fig. 33A shows as an example that half Area of the display section 9631a has only a display function and the other half area has a touchscreen function However, the structure of the display section 9631a is not limited to these. The entire area of the display section 9631a can have a touchscreen function. For example, the entire display section 9631a can display keyboard buttons and serve as a touch screen, while the Display section 9631b can be used as a display screen.
[0330] In the display section 9631b, as in the display section 9631a, a part of the display section 9631b may be a Touch screen area 9632b. When a finger, a pen or the like touches the place where a button 9639 for Switching to a keyboard display mode is displayed on the touchscreen, keyboard buttons on the Display section 9631b.
[0331] Touch input can be performed on the touchscreen areas 9632a and 9632b simultaneously become.
[0332] The button for switching the display mode 9034 allows switching, for example, between a Portrait and landscape format and between monochrome and color display. With the button to switch the Power saving mode 9036 to switch to a power saving mode, the display luminance can be adjusted according to the amount of Outside light, which is detected by an optical sensor in the tablet computer, when using the tablet The tablet computer can be optimized for other detection devices such as a sensor for Detecting the inclination (such as a gyroscope or an accelerometer) in addition to the optical sensor.
[0333] Although the display section 9631a and the display section 9631b have the same display area in Fig. 33A An embodiment of the present invention is not limited to this example. The display section 9631a and the display section 9631b may have different areas or different display quality. For example, one of them may be a display panel that displays images with higher resolution than the other display panel can display.
[0334] Fig. 33B shows the folded tablet computer, which includes the housing 9630, a solar cell 9633 and a charge / discharge control circuit 9634. It should be noted that Fig. 33B shows an example in which the charge / Discharge control circuit 9634 includes a battery 9635 and a DC-DC converter 9636.
[0335] Since the tablet computer can be foldable, the housing 9630 can be closed when the tablet computer is not in use. Thus, the display sections 9631a and 9631b can be protected. Therefore, a Tablet computer that has high durability and high reliability in terms of long-term use, be provided.
[0336] The tablet computer in Fig. 33A and Fig. 33B may have a function for displaying various types of data (e.g. B. a still image, a moving image and a text image), a function for displaying a calendar, a Date, time or the like on the display section, a function for inputting by touch for operation or modification of the data displayed by entering it by touch on the display section, a Have the function of controlling processing by means of various types of software (programs) and the like.
[0337] The solar cell 9633, which is attached to the surface of the tablet computer, supplies energy to a touchscreen, a display section, an image signal processing section, and the like. It should be noted that the solar cell 9633 may be arranged on one or both surfaces of the housing 9630 so that the battery 9635 can be charged efficiently When a lithium-ion battery is used as the 9635 battery, there is an advantage of Reduction or the like.
[0338] The structure and operation of the charge / discharge control circuit 9634 shown in Fig. 33B are described using a block diagram in Fig. 33C. The solar cell 9633, the battery 9635, the DC-DC converter 9636, a converter 9637, switches SW1, SW2 and SW3 and the display section 9631 are shown in Fig. 33C, and the Battery 9635, DC-DC converter 9636, converter 9637 and switches SW1 to SW3 correspond to the charging / discharge control circuit 9634 in Fig. 33B .
[0339] First, an example of operation in the case where power is supplied from the solar cell 9633 using from outside light. The voltage of the energy generated by the solar cell 9633 is determined by the DC-DC converter 9636 increases or decreases so that a voltage for charging the battery 9635 is obtained. When the display section 9631 is operated with the energy from the solar cell 9633, the switch SW1 is turned on, and the voltage of the energy is transferred from the wall ler 9637 to a voltage required to operate the display section 9631. In addition, when no display is performed on the display section 9631, the switch SW1 off, and the switch SW2 is turned on so that charging of the battery 9635 can be carried out.
[0340] Although the solar cell 9633 is shown here as an example of an energy generating device, there is no special limitation to a means for charging the battery 9635, and the battery 9635 can be charged by means of another Energy generating means such as a piezoelectric element or a thermoelectric converter element (Peltier element). For example, the 9635 battery can be charged using a contactless Energy transfer module capable of wireless (contactless) transmission and reception of energy, or another means of charging can be used in combination with it.
[0341] It should be noted that the structure and the like in this embodiment are used in combination with one of the Structures and the like may be used in the other embodiments as needed. [Example 1]
[0342] In this example, the resistances of an oxide semiconductor film and a multilayer film are measured using Fig. 34A to Fig. 34D and Fig. 35.
[0343] First, the structure of a sample is described using Fig. 34A to Fig. 34D.
[0344] Fig. 34A is a plan view of a sample 1, a sample 2, a sample 3 and a sample 4, and Fig. 34B to Fig. 34D are cross-sectional views along the dash-dot line A1-A2 in Fig. 34A. It should be noted that the top views of the Samples 1 to 4 are the same, and their cross-sectional views are different because the stacked layer structures of the Cross-sections are different. The cross-sectional views of Sample 1, Sample 2, and Samples 3 and 4 are shown in Fig. 34B, Fig. 34C and Fig. 34D respectively.
[0345] Regarding Sample 1, an insulating film 1903 is formed over a glass substrate 1901, an insulating film 1904 is formed over the insulating film 1903, and an oxide semiconductor film 1905 is formed over the insulating film 1904. The two End regions of the oxide semiconductor film 1905 are provided with a conductive film 1907 and a conductive film 1909, each of which is electrode, and the oxide semiconductor film 1905 and the conductive films 1907 and 1909 are covered with a Insulating film 1910 and an insulating film 1911. It should be noted that an opening 1913 and an opening 1915 in the insulating films 1910 and 1911, and that the conductive film 1907 and the conductive film 1909 are Opening 1913 and opening 1915 are exposed.
[0346] Regarding Sample 2, the insulating film 1903 is formed over the glass substrate 1901, the insulating film 1904 is formed over the insulating film 1903, and the oxide semiconductor film 1905 is formed over the insulating film 1904. The two End regions of the oxide semiconductor film 1905 are connected to the conductive films 1907 and 1909, each serving as an electrode. covered, and the oxide semiconductor film 1905 and the conductive films 1907 and 1909 are covered with the insulating film 1911. It It should be noted that an opening 1917 and an opening 1919 are arranged in the insulating film 1911, and that the conductive film 1907 and the conductive film 1909 are exposed through the opening 1917 and the opening 1919 respectively.
[0347] With respect to each of Samples 3 and 4, the insulating film 1903 is formed over the glass substrate 1901, the insulating film 1904 is formed over the insulating film 1903, and a multilayer film 1906 is formed over the insulating film 1904 The two end regions of the multilayer film 1906 are connected to the conductive films 1907 and 1909, which each serve as an electrode, and the multilayer film 1906 and the conductive films 1907 and 1909 are covered with the insulating film 1911. It should be noted that the openings 1917 and 1919 are arranged in the insulating film 1911 and that the conductive film 1907 and the conductive film 1909 were exposed through the opening 1917 and the opening 1919 respectively are.
[0348] As described above, the structures of the insulating films in contact with the upwardly facing Surface of the oxide semiconductor film 1905 or the multilayer film 1906, in samples 1 to 4. In In Sample 1, the oxide semiconductor film 1905 and the insulating film 1910 are in contact with each other; in Sample 2, the Oxide semiconductor film 1905 and the insulating film 1911 in contact with each other; and in Samples 3 and 4, the multilayer film 1906 and the insulating film 1911 are in contact with each other.
[0349] Next, methods for preparing the samples will be described.
[0350] First, a method for forming Sample 1 will be described.
[0351] A 400 nm thick silicon nitride film was deposited as the insulating film 1903 over the glass substrate 1901 by a plasma CVD process.
[0352] Next, a 50 nm thick silicon oxynitride film was formed as the insulating film 1904 over the insulating film 1903 by a plasma CVD process.
[0353] Then, a 35 nm thick IGZO film was deposited as the oxide semiconductor film 1905 over the insulating film 1904 by a Sputtering process using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1: 1:1. After that, an etching treatment was performed on the IGZO film with a mask formed by a Photolithography process was carried out, so that the oxide semiconductor film was formed in 1905.
[0354] Next, the conductive films 1907 and 1909 were deposited over the insulating film 1904 and the oxide semiconductor film 1905 designed in such a way that a 50 nm thick tungsten film, a 400 nm thick aluminum film and a 100 nm thick titanium film in in this order by a sputtering process and then subjected to an etching treatment with a mask formed by a photolithography process.
[0355] Subsequently, a 450 nm thick silicon oxynitride film was deposited as the insulating film 1910 over the insulating film 1904, the oxide semiconductor film 1905, the conductive film 1907 and the conductive film 1909 by a plasma CVD process formed, and then a heat treatment was carried out for one hour at 350 °C in a mixture atmosphere of Nitrogen and oxygen.
[0356] Next, a 50 nm thick silicon nitride film was formed as the insulating film 1911 over the insulating film 1910 by a Plasma CVD process.
[0357] Then, a mask is formed over the insulating film 1911 by a photolithography process, and then an etching treatment is carried out on the insulating film 1911 so that the openings 1913 and 1915 in the insulating films 1910 and were trained in 1911.
[0358] Through the above process, Sample 1 was formed.
[0359] Next, a method for forming the sample 2 will be described.
[0360] Next, a 450 nm thick silicon oxynitride film was deposited as the insulating film 1910 over the insulating film 1904, the oxide semiconductor film 1905, the conductive film 1907 and the conductive film 1909 of Sample 1 by a plasma CVD process, and then a heat treatment was carried out for one hour at 350 °C in a mixture atmosphere of nitrogen and oxygen. The insulating film was then removed in 1910.
[0361] Next, a 50 nm thick silicon nitride film was deposited as the insulating film 1911 over the insulating film 1904, the oxide semiconductor film 1905, the conductive film 1907 and the conductive film 1909 by a plasma CVD process trained.
[0362] Then, a mask is formed over the insulating film 1911 by a photolithography process, and then an etching treatment is carried out on the insulating film 1911 so that the openings 1917 and 1919 in the insulating film 1911 were trained.
[0363] Through the above process, Sample 2 was formed.
[0364] Next, a method for forming the sample 3 will be described.
[0365] Regarding Sample 3, the multilayer film 1906 was used instead of the oxide semiconductor film 1905 of Sample 2. The multilayer film 1906 was formed over the insulating film 1904 in such a way that a 10 nm thick IGZO film was a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:3:2, a 10 nm thick IGZO Film using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1, and then a 10 nm thick IGZO film using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:3: 2, were successively formed by a sputtering process. Subsequently, an etching treatment was applied to the stacked IGZO films with a mask formed by a photolithography process, so that the multi-layered film was developed in 1906.
[0366] Through the above process, Sample 3 was formed.
[0367] Next, a method for forming the sample 4 will be described.
[0368] Regarding Sample 4, the multilayer film 1906 was used instead of the oxide semiconductor film 1905 of Sample 2 The multilayer film 1906 was formed over the insulating film 1904 in such a way that a 20 nm thick IGZO Film using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:3:2, a 15 nm thick IGZO film using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1, and then a 10 nm thick IGZO film using a target made of a metal oxide containing In, Ga and Zn with a atomic ratio of 1:3:2, were successively formed by a sputtering process. Subsequently, a Etching treatment on the stacked IGZO films with a mask formed by a photolithography process was carried out, so that the multi-layer film was formed in 1906.
[0369] Through the above process, Sample 4 was formed.
[0370] Next, the sheet resistance of the oxide semiconductor film 1905 in each of Samples 1 and 2 and the Sheet resistance of the multilayer film 1906 was measured in each of samples 3 and 4. In sample 1, a sensor brought into contact with the openings 1913 and 1915 to measure the sheet resistance of the oxide semiconductor film 1905. In each of the samples 2 to 4, a sensor was brought into contact with the openings 1917 and 1919 to measure the To measure the sheet resistance of the oxide semiconductor film 1905 or the multilayer film 1906. It should be noted that in the oxide semiconductor film 1905 in each of Samples 1 and 2 and in the multilayer film 1906 in each of Samples 3 and 4 the widths of the conductive films 1907 and 1909 facing each other were 1 mm each and the distance between the conductive films 1907 and 1909 was 10 µm. In addition, in each of the samples 1 to 4, the potential of the conductive film 1907, and 1 V was applied to the conductive film 1909.
[0371] Fig. 35 shows the sheet resistance of samples 1 to 4. 11
[0372] The sheet resistance of Sample 1 was about 1 × 10 Ω. The sheet resistance of Sample 2 was about 2620 Ω. The sheet resistance of sample 3 was about 4410 Ω. The sheet resistance of sample 4 was about 2930 Ω.
[0373] In the above manner, the oxide semiconductor films 1905 and the multilayer films 1906 have different Sheet resistances because the insulating films in contact with the oxide semiconductor film 1905 and the insulating films in contact with the multilayer film in 1906 were different.
[0374] It should be noted that when the above sheet resistances of Samples 1 to 4 are converted into specific resistances 5 were converted, the resistivities of Sample 1, Sample 2, Sample 3 and Sample 4 were 3.9 × 10 Ω. -3 -2 -2 cm, 9.3 × 10 Ωcm, 1.3 × 10 Ωcm and 1.3 × 10 Ωcm, respectively.
[0375] In Sample 1, the silicon oxynitride film used as the insulating film 1910 was in contact with the top surface of the oxide semiconductor film 1905 and was separated from the silicon nitride film, which was the Insulating film used in 1911. In contrast, in sample 2, the silicon nitride film used as the Insulating film used in 1911, in contact with the upward-facing surface of the oxide semiconductor film in 1905 and was in contact with the upward-facing surface of the multilayer film 1906. When the oxide semiconductor film 1905 or the multilayer film 1906 is formed as in The above is provided in contact with the silicon nitride film used as the insulating film 1911, Defects such as oxygen vacancies are generated in the oxide semiconductor film 1905 or the multilayer film 1906, and What hydrogen in the silicon nitride film is transferred to the oxide semiconductor film 1905 or the multilayer film 1906 or in it diffuses. Consequently, the conductivity of the oxide semiconductor film 1905 or the multilayer film 1906 is improved.
[0376] For example, in the case where an oxide semiconductor film is used for a channel formation region of a transistor used, it is preferable to use a structure in which a silicon oxynitride film is in contact with the oxide semiconductor film as in Sample 1. In addition, it is preferable to use as a light-transmitting conductive film for an electrode of a capacitor to use a structure in which a silicon nitride film is in contact with a oxide semiconductor film or a multilayer film as in Samples 2 to 4. With such a structure can then, even if an oxide semiconductor film or a multilayer film used for a channel formation region of a transistor, and an oxide semiconductor film or a multilayer film used for an electrode of a capacitor is used, are formed by the same process, the specific resistance of the oxide semiconductor film and the resistivity of the multilayer film can be made different.
[0377] Next, the values of the sheet resistances of samples 2 and 3, which were tested in an environment at a high temperature and high humidity. The conditions of the samples used here are described below. It should be noted that the conditions here are partly different from those of Samples 2 and 3 are different. Therefore, samples that have the same structure as samples 2 and 3 and are subject to trained under different training conditions are referred to as Sample 2a and Sample 3a.
[0378] First, a method for forming the sample 2a will be described.
[0379] The insulating film 1903 and the insulating film 1904 were formed over the glass substrate 1901.
[0380] Then, a 35 nm thick IGZO film was deposited as the oxide semiconductor film 1905 over the insulating film 1904 by a Sputtering process using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1: 1:1. After that, an etching treatment was performed on the IGZO film with a mask formed by a Photolithography process is carried out, and a heat treatment was then carried out at 350 °C or 450 °C carried out so that the oxide semiconductor film was formed in 1905.
[0381] Next, the conductive film 1907 and the conductive film 1909 were deposited over the insulating film 1904 and the Oxide semiconductor film 1905 is formed such that a 50 nm thick tungsten film and a 400 nm thick copper film are formed in this order by a sputtering process and then subjected to an etching treatment with a mask formed by a photolithography process.
[0382] Subsequently, a 450 nm thick silicon oxynitride film was deposited as the insulating film 1910 over the insulating film 1904, the oxide semiconductor film 1905, the conductive film 1907 and the conductive film 1909 by a plasma CVD process formed and a heat treatment was then carried out for one hour at 350 °C in a mixture atmosphere of Nitrogen and oxygen.
[0383] Next, a 50 nm thick silicon nitride film was deposited as the insulating film 1911 over the insulating film 1904, the oxide semiconductor film 1905, the conductive film 1907 and the conductive film 1909 by a plasma CVD process It should be noted that the temperature during formation of the silicon nitride film was 220 °C or 350 °C.
[0384] Then, a mask is formed over the insulating film 1911 by a photolithography process, and a Etching treatment was then carried out on the insulating film 1911 so that the openings 1913 and 1915 in the insulating films were trained in 1910 and 1911.
[0385] Through the above process, Sample 2a was formed.
[0386] Next, a method for forming the sample 3a will be described.
[0387] Regarding Sample 3a, the multilayer film 1906 was used instead of the oxide semiconductor film 1905 of Sample 2a The multilayer film 1906 was formed over the insulating film 1904 such that a 10 nm thick IGZO Film using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1, and a 10 nm thick IGZO film using a metal oxide target, containing In, Ga and Zn with an atomic ratio of 1:3:2, were successively formed by a sputtering process. Subsequently, an etching treatment was performed on the stacked IGZO films using a mask formed by a Photolithography process was carried out, and a heat treatment was then carried out at 350 °C or 450 °C carried out, so that the multi-layer film was formed in 1906.
[0388] Through the above process, Sample 3a was formed.
[0389] Then, the sheet resistance of the oxide semiconductor film 1905 in Sample 2a and the sheet resistance of the multilayer film 1906 in sample 3a. In each of samples 2a and 3a, a sensor is placed in contact with the Openings 1917 and 1919 to measure the sheet resistance of the oxide semiconductor film 1905 or the multilayer Film 1906. It should be noted that in the oxide semiconductor film 1905 in Sample 2a and in the multilayer Film 1906 in sample 3a, the widths of the conductive films 1907 and 1909 facing each other are 1.5 mm each and the distance between the conductive films 1907 and 1909 was 10 µm. In addition, in each of the samples 2a and 3a the potential of the conductive film 1907 was an earth potential, and 1 V was applied to the conductive film 1909. The values The sheet resistances of samples 2a and 3a were measured after samples 2a and 3a had been heated for 60 hours and 130 hours at 60 °C in an atmosphere with a humidity of 95%.
[0390] Fig. 39 shows the values of the sheet resistances of samples 2a and 3a. It should be noted that in Fig. 39 the Temperature for forming the silicon nitride film as the insulating film 1911 in each sample 220 °C (a solid line) or 350 °C (a dashed line). Furthermore, a black circle and a black triangle represent the samples that after forming the oxide semiconductor film 1905 or the multilayer film 1906, a heat treatment at 350 °C, and a white circle and a white triangle represent the samples which were subjected to the Forming the oxide semiconductor film 1905 or the multilayer film 1906 by heat treatment at 450 °C The black and white circles represent the samples including the oxide semiconductor film 1905, namely sample 2a, and the white triangle represents the sample including the multilayer film 1906, ie the Sample 3a. It should be noted that the measurement result of Sample 3a, which was obtained after forming the multilayer film 1906 was subjected to a heat treatment at 350 °C (represented by a black triangle), not in Fig. 39 is shown.
[0391] Fig. 39 shows that samples 2a and 3a had small values of sheet resistance and a preferred value of the surface resistance for one electrode of a capacitor, which is 0.2 MΩ, and that the size of the The change over time in the sheet resistance values of samples 2a and 3a was small. As described above, the Size of change in the value of the sheet resistance of the oxide semiconductor film or the multilayer film in Contact with the silicon nitride film is small in a high temperature and high humidity environment. Therefore The oxide semiconductor film or the multilayer film can be used as a light-transmitting conductive film used for an electrode of a capacitor is used.
[0392] Next, the values of the sheet resistances of samples 2a and 3a at a substrate temperature of 25 ° C, 60 °C or 150 °C, and the measurement results are shown in Fig. 40. It should be noted that here each of the Samples 2a and 3a were used, which contained the silicon nitride film formed as the insulating film 1911 at 220 °C and after forming the oxide semiconductor film 1905 or the multilayer film 1906 of a heat treatment at 350 °C. In addition, in Fig. 40, a black circle represents the measurement result of the Sample 2a and a black triangle represents the measurement result of sample 3a.
[0393] Fig. 40 shows that the sheet resistance values of the oxide semiconductor film 1905 and the multilayer film 1906, even when the substrate temperature was increased. In other words, the oxide semiconductor film or the multilayer film in contact with the silicon nitride film is a degenerate semiconductor. The size of the Change in the value of the sheet resistance of the oxide semiconductor film or the multilayer film in contact with the silicon nitride film was small even when the substrate temperature was changed; therefore, the oxide semiconductor film or the multilayer film as a light-transmitting conductive film used for an electrode of a capacitor will be used.
[0394] It should be noted that the structure in this example may be used in combination with one of the structures of other embodiments and examples. [Example 2]
[0395] In this example, analysis of impurities in an oxide semiconductor film and an insulating film over the Oxide semiconductor film is described using Fig. 36A and Fig. 36B.
[0396] In this example, two kinds of samples (hereinafter referred to as Sample 5 and Sample 6) were used as samples for trained in contamination analysis.
[0397] First, a method for forming the sample 5 will be described below.
[0398] Regarding Sample 5, an IGZO film was formed over a glass substrate, and a silicon nitride film was formed above it. After that, a heat treatment was carried out for one hour at 450 °C in a nitrogen atmosphere and then a heat treatment for one hour at 450 °C in a mixed gas atmosphere of nitrogen and oxygen (the proportion of nitrogen was 80% and the proportion of oxygen was 20%) was carried out successively.
[0399] It should be noted that as the IGZO film, a 100 nm thick IGZO film was formed by a sputtering method using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1, under the following conditions: the flow rate of Ar gas was 100 sccm and the flow rate of O gas was 2 100 sccm (the proportion of O gas was 50%); the pressure was 0.6 Pa; the power for forming a film was 5000 W; 2 and the substrate temperature was 170 °C.
[0400] In addition, a 100 nm thick silicon nitride film was deposited by a PE-CVD method under the following conditions: the flow rate of SiH gas was 50 sccm, the flow rate of N gas was 4 2 5000 sccm and the flow rate of NH gas was 100 sccm; the pressure was 100 Pa; the power to form the 3 Film was 1000 W; and the substrate temperature was 220 °C.
[0401] Next, a method for forming the sample 6 will be described below.
[0402] An IGZO film was formed over a glass substrate, and a silicon oxynitride film and a silicon nitride film were stacked on top. They were then heat treated for one hour at 450 °C in a nitrogen atmosphere and then a heat treatment for one hour at 450 °C in a mixture atmosphere of Nitrogen and oxygen (the proportion of nitrogen was 80% and the proportion of oxygen was 20%) successively carried out.
[0403] It should be noted that the conditions for forming the IGZO film and the silicon nitride film are similar to those of were similar to sample 5. In addition, a 50 nm thick silicon oxynitride film was grown by PE-CVD Process under the following conditions: the flow rate of SiH gas was 30 sccm and the 4 The flow rate of N O gas was 4000 sccm; the pressure was 40 Pa; the film forming power was 150 W. 2 and the substrate temperature was 220 °C. Then, a 400 nm thick silicon oxynitride film was deposited by a PE-CVD process under the following conditions: the flow rate of SiH gas was 160 sccm and the flow rate 4 of N O gas was 4000 sccm; the pressure was 200 Pa; the power to form a film was 1500 W; and the 2 Substrate temperature was 220 °C.
[0404] Figures 36A and 36B show the results of the impurity analysis of samples 5 and 6.
[0405] It should be noted that the impurity analysis in the direction of the arrow in each of Fig. 36A and Fig. 36B is carried out by Secondary ion mass spectrometry (SIMS) was used. In other words, the measurement was taken from the side of the glass substrate.
[0406] Fig. 36A shows the concentration profile of hydrogen (H) obtained by measuring sample 5. Fig. Figure 36B shows the concentration profile of hydrogen (H) obtained by measuring sample 6. 20 3
[0407] Fig. 36A shows that the concentration of hydrogen (H) in the IGZO film was 1.0 × 10 atoms / cm, and that 23 3 the concentration of hydrogen (H) in the silicon nitride film was 1.0 × 10 atoms / cm. In addition, Fig. 36B shows that the 19 3 Concentration of hydrogen (H) in the IGZO film was 5.0 × 10 atoms / cm, and that the concentration of 21 3 Hydrogen (H) in the silicon oxynitride film was 3.0 × 10 atoms / cm.
[0408] It is known that it is fundamentally difficult to obtain precise data in the vicinity of a sample surface or in Proximity to an interface between stacked films of different materials using the SIMS analysis. Therefore, in the case where the distribution of the concentration of hydrogen (H) in the film in a thickness direction using SIMS, an average value as the concentration of Hydrogen (H) used from an area where the film is provided, the value does not change much and a Essentially constant strength can be maintained.
[0409] A difference between the IGZO films in the concentration of hydrogen (H) was determined in this way by Change in the structure of the insulating film in contact with the IGZO film was found.
[0410] For example, in the case where one of the above IGZO films is used in a channel formation region of a transistor is formed, it is preferable to use a structure in which a silicon oxynitride film is in contact with the IGZO film as arranged in Sample 6. It is preferable to use as a light-transmitting conductive film for an electrode of a capacitor to use a structure in which a silicon nitride film is in contact with the IGZO film as in sample 5 With such a structure, even if an IGZO film used for a channel formation region of a transistor, and an IGZO film used for an electrode of a capacitor, through which the same process, the hydrogen concentrations of the IGZO films are made different from each other become. [Example 3]
[0411] In this example, the amounts of defects in an oxide semiconductor film and a multilayer film described in Fig. 37A to Fig. 37C and Fig. 38.
[0412] First, the structure of a sample is described.
[0413] A sample 7 includes a 35 nm thick oxide semiconductor film over a quartz substrate and a 100 nm thick Nitride insulating film over the oxide semiconductor film.
[0414] A sample 8 and a sample 9 each comprise a 30 nm thick multilayer film over a quartz substrate and a 100 nm thick nitride insulating film over the multilayer film. It should be noted that in the multilayer film of Sample 8, a 10 nm thick first oxide film, a 10 nm thick oxide semiconductor film and a 10 nm thick second oxide film are stacked in this order. In the multilayer film of sample 9, a 20 nm thick first oxide film, a 15 nm thick oxide semiconductor film and a 10 nm thick second oxide film are stacked in this order. Samples 8 and 9 differ from sample 7 in that the multilayer film instead of the oxide semiconductor film is included.
[0415] A sample 10 includes a 100 nm thick oxide semiconductor film over a quartz substrate, a 250 nm thick Oxide insulating film over the oxide semiconductor film and a 100 nm thick nitride insulating film over the oxide insulating film. The difference between sample 10 and samples 7 to 9 is that the oxide semiconductor film is not in contact with the Nitride insulating film, but is in contact with the oxide insulating film.
[0416] Next, methods for forming the samples will be described.
[0417] First, a method for forming the sample 7 will be described.
[0418] A 35 nm thick IGZO film was formed as the oxide semiconductor film over the quartz substrate. IGZO film, the 35 nm thick IGZO film was deposited by a sputtering process using a target made of a Metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1, formed under the following conditions: the flow rate of Ar gas was 100 sccm and the flow rate of O gas was 100 sccm (the proportion of O - 2 2 gas was 50%); the pressure was 0.6 Pa; the power to form a film was 5000 W; and the substrate temperature was 170 °C.
[0419] Then, as a first heat treatment, a heat treatment for one hour at 450 °C in a nitrogen atmosphere and then a heat treatment for one hour at 450 °C in a mixed gas atmosphere of Nitrogen and oxygen (the proportion of nitrogen was 80% and the proportion of oxygen was 20%) successively carried out.
[0420] Next, a 100 nm thick silicon nitride film was formed as the nitride insulating film over the oxide semiconductor film. Regarding the silicon nitride film, a 100 nm thick silicon nitride film was deposited by a PE-CVD process under the following conditions: the flow rate of SiH gas was 50 sccm, the flow rate of N gas was 4 2 5000 sccm and the flow rate of NH gas was 100 sccm; the pressure was 100 Pa; the power to form a 3 Film was 1000 W; and the substrate temperature was 350 °C.
[0421] Thereafter, as a second heat treatment, a heat treatment was carried out for one hour at 250 °C in a nitrogen atmosphere.
[0422] Through the above process, Sample 7 was formed.
[0423] Next, a method for forming the sample 8 will be described.
[0424] Regarding Sample 8, the multilayer film was formed instead of the oxide semiconductor film of Sample 7. Regarding the multilayer film, the 10 nm thick first oxide film was formed by a sputtering method using a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:3:2, under the following Conditions: the flow rate of Ar gas was 180 sccm and the flow rate of O gas was 20 2 sccm (the proportion of O gas was 10%); the pressure was 0.6 Pa; the power to form a film was 5000 W; and 2 The substrate temperature was 25 °C. Then, the 10 nm thick oxide semiconductor film was deposited by a sputtering process under Use of a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:1:1, under the following conditions: the flow rate of Ar gas was 100 sccm and the flow rate of O gas 2 was 100 sccm (the proportion of O gas was 50%); the pressure was 0.6 Pa; the power to form a film was 5000 2 W; and the substrate temperature was 170 °C. Then, the 10 nm thick second oxide film was deposited by a sputtering process under Use of a target made of a metal oxide containing In, Ga and Zn with an atomic ratio of 1:3:2, under the following conditions: the flow rate of Ar gas was 180 sccm and the flow rate of O gas 2 was 20 sccm (the proportion of O gas was 10%); the pressure was 0.6 Pa; the power for forming a film was 5000 W; 2 and the substrate temperature was 25 °C.
[0425] Other steps are similar to those of Sample 7. Sample 8 was formed by the above process.
[0426] Next, a method for forming the sample 9 will be described.
[0427] Regarding Sample 9, the multilayer film was formed instead of the oxide semiconductor film of Sample 7. Regarding the multilayer film, the 20 nm thick first oxide film was deposited over the quartz substrate under the same conditions as the first oxide film of Sample 8. Then, the 15 nm thick oxide semiconductor film was sputtering process under the same conditions as the oxide semiconductor film of Sample 8. Then, the 10 nm thick second oxide film was formed under the same conditions as the second oxide film of Sample 8.
[0428] Other steps are similar to those of Sample 7. Sample 9 was formed by the above process.
[0429] Next, a method for forming the sample 10 will be described.
[0430] Regarding Sample 10, the 100 nm thick oxide semiconductor film over the quartz substrate was deposited under the same Conditions as in sample 7.
[0431] Then, a first heat treatment was carried out under conditions similar to those of Sample 7, carried out.
[0432] Next, as the oxide insulating film, a 50 nm thick first silicon oxynitride film and a 200 nm thick second silicon oxynitride film stacked over the oxide semiconductor film. Here, the 50 nm thick first silicon oxynitride film formed by a PE-CVD process under the following conditions: the flow rate of SiH gas was 30 sccm 4 and the flow rate of N O gas was 4000 sccm; the pressure was 40 Pa; the film forming power was 2 150 W; and the substrate temperature was 220 °C. Then, the 200 nm thick second silicon oxynitride film was replaced by a PE CVD process under the following conditions: the flow rate of SiH gas was 160 sccm and the flow rate of N O gas 4 2 was 4000 sccm; the pressure was 200 Pa; the power to form a film was 1500 W; and the substrate temperature was 220 °C. It should be noted that the second silicon oxynitride film is a film containing oxygen at a higher ratio than Contains oxygen in the stoichiometric composition.
[0433] Next, a 100 nm thick silicon nitride film was deposited over the oxide insulating film under the same conditions as in sample 7.
[0434] Then, a second heat treatment was carried out under conditions similar to those of Sample 7, carried out.
[0435] Through the above process, Sample 10 was formed.
[0436] Next, samples 7 to 10 were measured by ESR. In the ESR measurement at a predetermined Temperature becomes a value of a magnetic field (H ) in which a microwave is absorbed, for an equation g = hn 0 / bH is used, so that a parameter, namely the g-factor, can be obtained. It should be noted that the frequency 0 of the microwave is represented by v, and that Planck's constant and Bohr's magneton are represented by h and β, which are both constants.
[0437] The ESR measurement was carried out under the following conditions. The temperature during the measurement was room temperature (25 °C), the high frequency power (microwave power) of 8.92 GHz was 20 mW, and the Direction of a magnetic field was parallel to a surface of each sample.
[0438] Fig. 37A shows a first derivative curve obtained by the ESR measurement of the oxide semiconductor film of Sample 7; and Fig. 37B and Fig. 37C show curves of first derivatives (first derivative curves) obtained by ESR measurement of the multilayer films of samples 8 and 9. Fig. 37A shows the measurement result of sample 7, Fig. 37B shows the measurement result of sample 8, and Fig. 37C shows the measurement result of Sample 9.
[0439] Fig. 38 shows a first derivative curve obtained by ESR measurement of the oxide semiconductor film of Sample 10.
[0440] In Fig. 37A to Fig. 37C, Sample 7 has a signal symmetry due to a defect in the oxide semiconductor film, when a g-factor is 1.93. Samples 8 and 9 each have a signal symmetry due to a defect in the multilayer film when a g-factor is 1.95. Regarding sample 7, the spin density at the time when a g- 19 3 Factor 1.93 was 2.5 × 10 spins / cm , in sample 8 the total spin densities at the time when g-factors 19 3 1.93 and 1.95 were 1.6 × 10 spins / cm , and in sample 9 the total spin densities at the time when g- 19 3 Factors were 1.93 and 1.95, 2.3 × 10 spins / cm . In other words, it is found that the oxide semiconductor film and the multilayer film may have defects. It should be noted that an oxygen vacancy is an example of the defect in the oxide semiconductor film and the multilayer film.
[0441] Although in Fig. 38 the thickness of the oxide semiconductor film of Sample 10 is larger than that of Sample 7 and those of multilayer films of samples 8 and 9, signal symmetry due to a defect was not detected, ie, the 16 Number of defects was less than or equal to the lower detection limit (here the lower detection limit was 3.7 × 10 3 spins / cm ). Consequently, it is found that the number of defects in the oxide semiconductor film cannot be determined.
[0442] It is found that when a nitride insulating film, here the silicon nitride film formed by a PE-CVD method is formed, is in contact with an oxide semiconductor film or a multilayer film, defects such as Oxygen vacancies are generated in the oxide semiconductor film or the multilayer film. In contrast, when an oxide insulating film, here the silicon oxynitride film, is provided over an oxide semiconductor film, excess oxygen in the silicon oxynitride film, ie oxygen whose proportion is higher than that of oxygen in of the stoichiometric composition, diffuses into the oxide semiconductor film and thus the number of defects in the oxide semiconductor film is not increased.
[0443] As described above, as in Samples 7 to 9, the oxide semiconductor film or the multilayer film formed in Contact with the nitride insulating film, many defects, such as oxygen vacancies, and has a high conductivity and can thus be used as an electrode of a capacitor. In contrast, as in sample 10, a Oxide semiconductor film in contact with the oxide insulating film, few oxygen vacancies and low conductivity and can therefore be used as a channel formation region of a transistor.
[0444] Now, the cause of a reduction in the resistivity of the oxide semiconductor film or the multilayer film in contact with the nitride insulating film is described below. <Energie und Stabilität zwischen Existenzformen von Wasserstoff (H)>
[0445] First, the energy difference and stability in a form of H ions encapsulated in an oxide semiconductor film exists, with calculated results. Here, InGaZnO was used as the oxide semiconductor film. 4
[0446] The structure used for the calculation is based on an 84-atom body model in which the doubled Number of a hexagonal unit cell of InGaZnO arranged along the a-axis and b-axis. 4
[0447] As the body model, a model was prepared in which an O atom bonded to three In atoms and one Zn atom bonded is replaced by an H atom. This is called VoH (see Fig. 41A).
[0448] In the body model, an O atom bonded to three In atoms and one Zn atom is removed, resulting in a Oxygen vacancy Vo is formed. A model was prepared in which in the vicinity of the oxygen vacancy Vo a H atom is bonded to an O atom, to which a Ga atom and two Zn atoms are bonded on the ab face. The is referred to as Vo+H (see Fig. 41B).
[0449] An optimization calculation was carried out on the above two models using a fixed lattice constant to calculate of the total energy. It should be noted that the smaller the value of the total energy, the more stable the structure becomes.
[0450] The calculation was carried out using a first-principles calculation software VASP (The Vienna Ab initio Simulation Package). The calculation conditions are shown in Table 1. [Table 1] VASP software Pseudopotential PAW Function GGA / PBE Cut-off energy 500 eV K-point 4×4×1
[0451] As a pseudopotential calculation of the electron states, a potential was used that was augmented by a ´´projector wave´´- (PAW-) method was used, and the function was ´´generalized-gradient-approximation / Perdew- Burke-Ernzerhof: (GGA / PBE)´´ used.
[0452] In addition, the total energy of the two models obtained by the calculations is shown in Table 2 shown. [Table 2] Model Total Energy VoH -456,084eV Vo+H -455,304eV
[0453] According to Table 2, the total energy of VoH is lower than that of Vo+H by 0.78 eV. Therefore, VoH more stable than Vo+H. Consequently, when a H atom approaches an oxygen vacancy (Vo), the H atom could easily the oxygen vacancy (Vo) instead of being bound to an O atom. <Thermodynamischer Zustand von VoH>
[0454] Next, the formation energy and the charge state of VoH, which is determined by a oxygen vacancy (Vo) is generated, described with calculated results. The The formation energy of VoH varies depending on the charge state and also on the Fermi energy. Therefore, the + stable charge state of VoH depending on the Fermi energy. Here (VoH) means a state in which an electron - is released from VoH, (VoH) means a state in which an electron is captured by VoH, and (VoH)° + - means a state in which an electron is not transferred. The formation energies of (VoH) , (VoH) and (VoH)° were calculated.
[0455] The calculation was carried out using the first-principles calculation software VASP. Calculation conditions are shown in Table 3. [Table 3] VASP software Pseudopotential PAW Function HSE06 Cut-off energy 800 eV Number of K-point sampling 2×2×1 (Opt.) 4×4×1 (Single) Spin polarization as set up Shielding parameter 0.2 Share of nonlocal Fock exchange- 0.25 Number of atoms 84
[0456] As a pseudopotential calculation of electron states, a potential was used which was generated by a ´´projector augmented wave (PAW) method was generated, and the function was ´´Heyd-Scuseria-Ernzerhof (HSE) DFT Hybrid- Factor (HSE06)'' is used.
[0457] It should be noted that the formation energy of an oxygen vacancy was calculated as follows: a Dilution limit of the concentration of oxygen vacancies was assumed, and excessive spread of electrons and holes to the conduction band and the valence band was corrected. In addition, a shift of the valence band due to the defect structure is corrected by the average electrostatic potential, whereby the Upper limit of the valence band of a complete crystal served as the zero point for the energy. + -
[0458] Fig. 42A shows the formation energies of (VoH) , (VoH) and (VoH)°. The horizontal axis represents the Fermi level + and the vertical axis represents the formation energy. The solid line represents the formation energy of (VoH) the dash-dot line represents the formation energy of (VoH)°, and the dashed line represents the formation energy of - (VoH). In addition, the transition level from a positive VoH charge to a negative VoH charge above 0 is determined by ε (+ / -) is displayed.
[0459] Fig. 42B shows a thermodynamic transition level of VoH. According to the calculation result, the Energy gap of InGaZnO 2.739 eV. Furthermore, when the energy of the valence band is 0 eV, the 4 transition level (ε (+ / -)) 2.62 eV, which exists just below the conduction band. This shows that InGaZnO is 4 Capture of an H atom in an oxygen vacancy Vo is of N-type.
[0460] When an oxide semiconductor film is exposed to a plasma, the oxide semiconductor film is damaged and defects such as cracks are formed. B. Oxygen vacancies are created in the oxide semiconductor film. In addition, when a nitride insulating film is in contact with an oxide semiconductor film, hydrogen contained in the nitride insulating film is transferred to the oxide semiconductor film. As a result, VoH in an oxide semiconductor film is transferred by the entry of Hydrogen is formed into an oxygen vacancy in the oxide semiconductor film, so that the oxide semiconductor film becomes an N-type oxide semiconductor film and its resistivity is reduced. As described above, the oxide semiconductor film, which is in contact with the nitride insulating film can be used as an electrode of a capacitor.
[0461] This application is based on Japanese Patent Application Serial No. 2012-188010 filed with Japanese Patent Office on August 28, 2012, and Japanese patent application serial no. 2013-053989, filed with the Japanese Patent Office on March 15, 2013, the entire contents of which are hereby incorporated by reference into this disclosure.< / modifikationsbeispiel>
Claims
1. A semiconductor device comprising: a signal line (109_n); a first scanning line (107_m); a second scanning line (107_m-1); a first transistor (103) comprising a source, a drain and a gate; a second transistor comprising a source, a drain and a gate; a pixel electrode (121); and a capacitor (105) comprising an electrode (119) and the pixel electrode (121) above the electrode (119), wherein the source or drain of the first transistor (103) is electrically connected to the pixel electrode (121), wherein the first scanning line (107_m) is electrically connected to the gate of the first transistor (103), wherein the signal line (109_n) is electrically connected to the other of the source and drain of the first transistor (103) and the source or drain of the second transistor, wherein the second scanning line (107_m-1) is electrically connected to the gate of the second transistor and the electrode of the capacitor (105), and wherein the electrode (119) of the capacitor (105) comprises an oxide film comprising indium and zinc.
2. A semiconductor device according to claim 1, wherein the first transistor comprises an oxide semiconductor film over the gate of the first transistor.
3. A semiconductor device according to claim 2, wherein the oxide semiconductor film comprises indium and zinc.
4. A semiconductor device according to claim 2, further comprising an insulating film over the oxide semiconductor film, wherein the source and the drain of the first transistor lie above the insulating film.
5. A semiconductor device according to claim 2, wherein the electrode of the capacitor has a higher conductivity than the oxide semiconductor film.
6. A semiconductor device according to claim 2, wherein the electrode of the capacitor and the oxide semiconductor film of the first transistor are provided on a same insulating surface.
7. A semiconductor device according to claim 1, comprising an insulating film over the first scanning line and the second scanning line includes, wherein the source and drain of the first transistor are above the insulating film, wherein the insulating film comprises an opening, and wherein the electrode of the capacitor is in contact with the second scanning line in the opening of the insulating film.
8. A semiconductor device according to claim 1, comprising a nitride insulating film in contact with an upwardly facing surface the electrode of the capacitor.
9. A semiconductor device according to claim 1, comprising a nitride insulating film in contact with a base surface of the electrode of the capacitor.
10. A semiconductor device according to claim 1, wherein the electrode of the capacitor comprises an impurity which is at least one selected from the group consisting of boron, nitrogen, fluorine, aluminum, phosphorus, arsenic, indium, tin, antimony and a noble gas element.
11. A semiconductor device according to claim 1, further comprising a liquid crystal over the pixel electrode (121).
12. A semiconductor device comprising: a substrate (102); a first scan line (107_m) and a second scan line (107_m-1) above the substrate (102); a first insulating film (127) over the first scanning line (107_m) and the second scanning line (107_m-1); a first oxide film (111), a second oxide film (119) and a third oxide film, each formed over the first insulating film lie (127); a signal line (109_n) overlying the first oxide film (111) and the third oxide film and electrically connected to the first oxide film (111) and the third oxide film; a conductive film (113) overlying the first oxide film (111) and electrically connected to the first oxide film (111) is connected; a second insulating film (131) over the signal line (109_n), the conductive film (113) and the second oxide film (119); and a pixel electrode (121) overlying the second insulating film (131) and electrically connected to the conductive film (113) is connected, wherein each of the first oxide film (111), the second oxide film (119) and the third oxide film comprises indium and zinc, wherein the first oxide film (111) overlaps with the first scanning line (107_m), wherein the second oxide film (119) overlaps with the pixel electrode (121), wherein the third oxide film overlaps with the second scanning line (107_m-1), and wherein the second oxide film (119) is electrically connected to the second scanning line (107_m-1).
13. A semiconductor device according to claim 12, wherein the second oxide film has a higher conductivity than the first oxide film and the third oxide film.
14. A semiconductor device according to claim 12, wherein the first insulating film is a nitride film and is in contact with the second oxide film.
15. A semiconductor device according to claim 12, wherein the second insulating film is a nitride film and is in contact with the second oxide film.
16. A semiconductor device according to claim 12, wherein the second oxide film comprises an impurity containing at least one selected from the group consisting of boron, nitrogen, fluorine, aluminum, phosphorus, arsenic, indium, tin, antimony and a noble gas element.
17. A semiconductor device according to claim 12, wherein the first insulating film is an oxide film and is in contact with the first oxide film and the third oxide film.
18. A semiconductor device according to claim 12, wherein the second insulating film is an oxide film and is in contact with the first oxide film and the third oxide film.
19. A semiconductor device according to claim 12, further comprising a third insulating film between the second insulating film and the signal line, wherein the second insulating film is in contact with the second oxide film.
20. The semiconductor device of claim 12, further comprising a liquid crystal over the pixel electrode.
Citation Information
Patent Citations
Semiconductor device and method for manufacturing the same
JP2007096055A
Semiconductor device and its manufacturing method
JP2007123861A
Clip mounting seat and interior material
JP2012188010A
Correlation detection circuit, correlation detection method and program
JP2013053989A
JP0000S6210619A