RTB-based sintered magnet
By optimizing the distribution of Ce and another rare earth element in the R-T-B magnet's core and cladding sections, the magnet achieves enhanced adhesion and coercivity, overcoming peeling and corrosion challenges, and leveraging abundant Ce resources.
Patent Information
- Application Number
- DE102014105638
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2013-04-22
- Filing Date
- 2014-04-22
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2034-04-22
AI Technical Summary
Conventional R-T-B based magnets face issues with low adhesion strength between the magnetic body and protective films, leading to film peeling and corrosion, and have lower coercivity compared to Nd-Fe-B magnets, making them less suitable for replacement.
The R-T-B based magnet incorporates Ce and another rare earth element (R1) with a higher mass concentration in the cladding section than the core, enhancing adhesion strength to plated layers and maintaining high coercivity by optimizing the mass concentration ratio (B/A) between R1 and Ce in the core and cladding sections.
The modified R-T-B magnet achieves higher coercivity and improved adhesion strength to plated layers, addressing the peeling and corrosion issues, while effectively utilizing abundant Ce resources.
Abstract
Description
FIELD OF THE INVENTION
[0001] The present invention relates to a rare earth-based permanent magnet, in particular a rare earth-based permanent magnet, which is produced by selectively replacing part of the R in the RTB-based Permanent magnets are obtained by Ce. BACKGROUND
[0002] The RTB-based magnet (R is a rare earth element, T is Fe or Fe, part of which is replaced by Co, and B is boron) with a tetragonal compound RTB as the main phase is known to have excellent magnetic 2 14 properties and has been regarded as a representative permanent magnet with good functional properties since it was invented in 1982 (see Japanese Patent Laid-Open Publication No. JP S59 - 46 008 B2).
[0003] In particular, the RTB-based magnets in which the rare earth element R is selected from Nd, Pr, Dy, Ho or Tb high magnetic anisotropy fields Ha and have been widely used as permanent magnet materials. Of these, the Nd-Fe-B based magnet, which has Nd as the rare earth element R, is widely used in the household of People, in industry, in transport equipment and the like because it has a good balance between the saturation magnetization Is, the Curie temperature Tc and the magnetic anisotropy field Ha. Because in the However, in recent years, the uses of the R-Fe-B based magnet have been expanded and the consumption of Nd or Pr or the like has increased dramatically, it is essential that efficient use of Nd or Pr or the like as valuable resources and that the material costs of the R-Fe-B based magnet be reduced.
[0004] On the other hand, because the RTB-based magnet contains a rare earth element that oxidizes easily and iron as main component, its corrosion resistance is relatively low, so that its magnetic Properties would deteriorate due to oxidation. Therefore, various protective films are applied on the surface of the If the adhesive strength between the magnetic body and the protective film is low, the Peel off the protective film according to the conditions during use, which prevents corrosion of the magnet body Therefore, the adhesive strength between the magnetic body and the protective film must be improved The adhesive strength between the magnetic body and the protective film depends on both the physical and the chemical bonding force, but it depends largely on the chemical properties of the magnetic body and the protective film. This means that the adhesive properties are determined by the composition of the magnets is influenced. Patent documents Patent Document 1: Japanese Patent Publication No. JP H06 - 6 776 B2 Patent Document 2: Japanese Patent Publication No. JP H06 - 942 B2 Patent Document 3: Japanese Patent Publication No. JP H06 - 2 930 B2
[0005] Ce is known as a rare earth element R, which shows a high coercive force in rich resources. Patent Document 1 relates to a sintered magnet and a resin bonded magnet with low cost and good functional properties. This means that such a magnet has a composition of Ce-La-(didymium; a Nd- Pd alloy)-Fe, supplemented by a semimetal (semimetals), and has the formula Ce Pr Nd La (Fe M ) 1-xy -zxyz 1-mmn represented in the form of atomic ratios, where M consists of one or two or more elements selected from the group consisting of B, C, Si, Ge, P and S, x, y, z, t, m and n in the ranges 0.1 ≤ x ≤ 0.5, 0.1 ≤ y ≤ 0.85, 0 ≤ z ≤ 0.1, 0.02 ≤ m ≤ 0.1, 0 ≤ n ≤ 8.0 and 0 < 1 - x - y - z < 0.8. Here La is a essential component. With the properties of this type of magnet, the coercive force is 7.3 kOe (580.92 kA / m) or more.
[0006] In addition, Patent Document 2 also relates to a sintered magnet and a resin-bonded magnet having low cost and high performance. It has a composition in which Ce-La-(didymium; a Nd-Pd alloy)-Fe-B is replaced by Co and the coercive force can be 7.9 kOe (628.66 kA / m).
[0007] Furthermore, Patent Document 3 also relates to a sintered magnet and a resin bonded magnet with low Cost and high performance. It has a composition of Ce-La-(didymium; a Nd- Pd alloy)-Fe is replaced by M and the coercive force can be 7.5 kOe (596.83 kA / m) or more.
[0008] The coercive force of each of these magnets is much lower than that of the Nd-TB based magnet, which is about 10 kOe (795.77 kA / m). Accordingly, it is difficult to use them to replace the conventional Nd-TB-based magnets to use.
[0009] Patent Document 4 (US 2013 / 0 009 503 A1) describes a sintered magnet, a motor, an automobile and a method for producing a sintered magnet. Patent Document 5 (US 2004 / 0 050 454 A1) describes a method for producing a permanent magnet. SUMMARY
[0010] The present invention is achieved by recognizing the above-mentioned situation. An object of The present invention is to provide a permanent magnet of an RTB-based magnet, wherein a Part of the R is selectively replaced by Ce, whereby compared to the conventional magnet an improvement in the Adhesion strength to a plated layer and the coercive force.
[0011] The RTB-based permanent magnet according to the present invention is an RTB-based sintered magnet (wherein R has Ce and R1 as essential components, R1 is at least one rare earth element other than Ce and T is at least one transition metal element containing Fe or the combination of Fe and Co as an essential component ), which has main phase grains with a core portion and a shell portion covering the core. If the mass concentration of R1 and Ce in the core section is set as αR1 and αCe, respectively, and the Mass concentration of R1 and Ce in the mantle section is defined as βR1 and βCe, respectively, the Mass concentration ratio (βR1 / βCe = B) between R1 and Ce in the mantle section is larger than that between R1 and Ce in the core section (αR1 / αCe = A). Here, B / A is 1.1 or more. With the above structure, the RTB-based sintered magnet can be obtained which has both high coercive force and high adhesive strength to the plated layer in the RTB-based sintered magnet.
[0012] The present invention has Ce and R1 as R, and Ce with rich resources can be effectively used In addition, Ce has the lowest melting point among the rare earth elements and has a high Moistenability for metals. By using Ce, the adhesion strength to the plated layer can be improved. In particular, Ce Ni and the like can be formed by Ce and Ni, and Ce accordingly has a high 3 compatibility with Ni. Therefore, the adhesion strength to the Ni-plated layer is high. On the other hand, there is the problem that the anisotropy field would be reduced. Therefore, in view of the great influence of the Anisotropy field of the crystal grain surface on the coercive force of the RTB-based magnet found that a high anisotropy field and a relatively high coercive force can be achieved by increasing the concentration of Ce at the crystal grain surface, namely in the shell section, is reduced compared to that in the core section. In this way, the present invention was achieved.
[0013] According to the present invention, the RTB-based magnet to which Ce has been added can have a higher coercivity than the RTB-based magnet, which has Ce as R, can be obtained by using Ce mainly in the core and R1, with the exception of Ce, is mainly distributed in the cladding. Because the adhesion strength to the plated film additionally compared to the conventional RTB-based magnets, where Nd, Pr, Dy, Ho and Tb are used as R can be improved, the plated film can be used in comparison with the conventional RTB-based magnets at in which Nd, Pr, Dy, Ho and Tb are used as R, are difficult to peel off. DETAILED DESCRIPTION OF EMBODIMENTS
[0014] The present invention will be described in detail based on the embodiments as follows. Furthermore, The present invention is not limited by the following embodiments and examples. In addition, The element components in the following embodiments and examples are those that are readily apparent to those skilled in the art. those that are essentially the same and those within an equivalent range. it is possible to use the following to suitably combine and select the element components disclosed in the embodiments and examples.
[0015] The RTB-based sintered magnet according to the present embodiment contains 11 - 18 at% of the Rare earth element (R). The R according to the present invention has Ce and R1 as essential components, and R1 is at least one rare earth element with the exception of Ce. If the R content is less than 11 at%, the formation of RT 2 14 B-phase as the main phase in RTB-based sintered magnet is not sufficient, α-Fe and the like precipitate with soft magnetic properties and the coercive force is significantly reduced. On the other hand, if the R component is larger than 18 at%, the volume ratio of RT B phase as the main phase is reduced and the residual flux density 2 14 In addition, the R-rich phase, which is effective in the formation of the coercive force, is reduced, resulting in a Reduction of the coercive force, corresponding to the fact that R reacts with oxygen and the proportion of contained oxygen increases.
[0016] According to the present embodiment, the rare earth element (R) contains Ce and R1. R1 is at least one Rare earth element except Ce. Like R1, it can contain other components in the form of impurities from the raw materials or impurities introduced during the manufacturing process. Furthermore, assumed that for obtaining a high magnetic anisotropy field R1 is preferably Nd, Pr, Dy, Ho and Tb. In addition, R1 is preferred Nd in terms of raw material price and corrosion resistance. Content ratio between R1 and Ce in the rare earth element (R) is 50 : 50 ∼ 90 : 10. Because Ce is among the rare earth elements, it has a high hydratability. Accordingly, the The adhesion strength to the plated layer can be improved by adding Ce. However, if the Ce content exceeds 50% the residual flux density and coercive force tend to decrease. On the other hand, if the Ce content is less than 10%, the effect of improving the adhesion strength to the plated layer usually becomes smaller.
[0017] The RTB-based sintered magnet according to the present embodiment contains 5 - 8 at% boron (B). When the If the B content is less than 5 at%, a high coercive force cannot be achieved. On the other hand, if the B content is greater than 8 at%, the residual magnetic density tends to decrease. Accordingly, the upper limit for B is set at 8 at%.
[0018] The RTB-based sintered magnet according to the present embodiment may contain 4.0 at% Co or less Co forms the same phase as Fe, but has an impact on the increase of the Curie temperature as well as the Increasing the corrosion resistance of the grain boundary phases. In addition, the according to the present invention RTB-based sintered magnets used contain Al and / or Cu in the range of 0.01 - 1.2 at%. Due to the fact that Al and / or Cu is contained in such an area, high coercive force, high corrosion resistance and the Improvement of the temperature properties of the obtained sintered magnet can be realized.
[0019] The RTB-based sintered magnet according to the present embodiment may also contain other elements For example, elements such as Zr, Ti, Bi, Sn, Ga, Nb, Ta, Si, V, Ag, Ge and the like may be suitably On the other hand, impurity elements such as oxygen, nitrogen, carbon and the like, preferably reduced as much as possible. In particular, the oxygen content, which reduces the magnetic properties are impaired, preferably 5000 ppm or less, more preferably 3000 ppm or less. The reason for this is that if the oxygen content is high, the rare earth oxide phase acts as the non-magnetic component increases, resulting in reduced magnetic properties.
[0020] The RTB-based sintered magnet according to the present embodiment has main phase grains having a core section and a mantle section covering the core. If the mass concentration of R1 and Ce in the core section is defined as αR1 and αCe respectively and the mass concentration of R1 and Ce in the mantle section is defined as βR1 or βCe, the ratio (B / A) between the mass concentration ratio between R1 and Ce in the mantle (βR1 / βCe = B) and the mass concentration ratio between R1 and Ce in the Core section (αR1 / αCe = A) 1.1 or more. As mentioned above, the coercive force of the RTB based magnets are strongly influenced by the anisotropy field of the crystal grain surface. Because Ce (cerium) and R1 than R and the concentration of Ce at the crystal grain surface, ie in the mantle section, is reduced, in the RTB-based sintered magnet according to the present embodiment, a higher coercive force is obtained than the conventional Ce-TB-based magnet. In view of the above point, B / A is preferably 1.4 or more. In addition, R1 is preferably at least one selected from the group consisting of Nd, Pr, Dy, Ho and Tb. Group.
[0021] In the RTB-based sintered magnet according to the present embodiment, the protective film is formed on the surface of the body of the sintered magnet.
[0022] The protective film according to the present embodiment is not particularly limited, but the one formed by The protective film obtained by electrolytic plating is particularly preferred for use. As materials in Electrolytic plating can use any of Ni, Ni-P, Cu, Zn, Cr, Sn and Al, and it can also other materials can be used. In particular, Ce Ni and the like can be formed by Ce and Ni, so 3 that Ce has a high compatibility with Ni. Therefore, Ni is best suited for the plated film. In addition, A multilayer of these materials can also be formed to cover the magnet. The magnet is formed by electrolytic Plating is a typical embodiment of the present invention, while the protective film obtained by The protective film obtained by other methods can also be provided. Protective film can be any of the films produced by non-electrolytic plating, chemical Conversion treatment, of which a chromate treatment is a representative example, resin coating or a combination of these. It is necessary to select the thickness of the protective film depending on the size of the rare earth-based sintered magnetic body, the level of desired corrosion resistance and the like The thickness can be set in the range of 1 - 100 µm. The thickness of the protective film is preferably 1 ∼ 50 µm.
[0023] The preferred example of the manufacturing method according to the present invention is described below During the manufacture of the RTB-based magnet according to the present embodiment, first the raw material alloys for obtaining the RTB-based magnet with the desired composition The alloys can be melted by strip casting or other known melting processes in vacuum or an inert gas atmosphere, preferably an Ar atmosphere. In the strip casting process, the the raw material in the non-oxidizing atmosphere such as an Ar gas atmosphere and the like, and the The resulting molten solution is then sprayed onto the surface of the rotating roller. The quenched molten solution is rapidly solidified to form a layer or flake (squama). Rapidly solidified alloys have a homogeneous organization with a grain diameter of 1 - 50 µm. There is no restriction on obtaining the raw material alloys by the strip casting process. The alloys can by a melting process such as high frequency induction melting and the like. Furthermore, the solution can be applied to a water-cooled copper plate after melting to prevent segregation cast to solidify them. Apart from that, the materials obtained by a reduction-diffusion process Alloys can also be used as raw materials.
[0024] In obtaining the RTB-based sintered magnet according to the present invention, essentially the so-called single alloy process is used, where an alloy is used as raw material to sintered magnets. The so-called mixing process can also be used, using a mixture consisting mainly of RT 2 B-crystal grains (low-R alloy) and a more R than the low-R alloy 14 containing alloy (high-R alloy).
[0025] The raw alloys are fed to the pulverization step. If the mixing process is used, the low-R alloy and the high-R alloy are pulverized separately or together. The pulverization step has a coarse pulverization step and a fine pulverization step. First, the raw alloys are pulverized, until a particle diameter of about a few hundred µm is obtained. The coarse pulverization is preferably carried out under Use of a stamp mill, a jaw crusher, a brown mill and the like in an inert gas atmosphere Before coarse pulverization, it is effective that hydrogen is absorbed in the raw alloy and the Hydrogen is then released to perform pulverization. The purpose of the hydrogen release treatment is to reduce the hydrogen, which is the impurity in the rare earth-based sintered magnet. Maintained heating temperature for absorbing hydrogen is set at 200 °C or more, preferably 350 °C or more. Although the holding time varies depending on the relationship with the holding temperature, the Thickness of the raw alloy and the like may change, it is set to at least 30 minutes or more, preferably 1 hour or more. The hydrogen release treatment is carried out in a vacuum or in an Ar air stream. Furthermore, the hydrogen absorbers treatment and hydrogen release treatment are not essential treatments. Hydrogen pulverization can also than coarse pulverization to avoid mechanical coarse pulverization.
[0026] After coarse pulverization, fine pulverization is carried out. During fine pulverization, mainly a jet mill is used to grind the coarsely pulverized powder with a particle diameter of about a few hundred µm to a finely pulverized powder with a particle diameter of 2.5 - 6 µm, preferably 3 - 5 µm. The jet mill releases inert gas from a narrow nozzle at high pressure and creates a fast air flow. The coarsely pulverized powder is accelerated by the fast air flow, which creates a Collision between coarsely pulverized powders with each other or a collision between coarsely pulverized powders and a target or a container wall and the pulverization is carried out.
[0027] Wet pulverization can also be used for fine pulverization. In wet pulverization, a ball mill, a wet attrition mill or the like may be used to grind the coarsely pulverized powder with a Particle diameter of about a few hundred µm to a finely pulverized powder with a particle diameter of 1.5 - 5 µm, preferably 2 - 4.5 µm. In wet pulverization, the fine powder can be pulverized with a low Oxygen concentration can be obtained because the pulverization can take place without magnetic powder containing oxygen by choosing a suitable dispersing medium.
[0028] During fine pulverization, a fatty acid or a derivative of the fatty acid or a hydrocarbon, such as zinc stearate, calcium stearate, aluminum stearate, stearinamide, oleinamide, ethylenebis-isostearinamide as stearic acid based compounds or oleic acid-based compounds, paraffin, naphthalene as hydrocarbons and the like in a range of about 0.01 ∼ 0.3 wt.% to improve lubrication and To improve orientation when forming.
[0029] The fine powder is formed in the magnetic field. 2
[0030] The forming pressure when forming in a magnetic field can be in the range of 0.3 ∼ 3 ton / cm (30 ∼ 300 MPa) The forming pressure can be constant from start to finish, and it can also be gradually increased or reduced, or it can be changed randomly. The lower the forming pressure, the better the Orientation. However, if the forming pressure is too low, handling problems arise due to the insufficient stability of the formed body. From this point of view, the forming pressure from the above The resulting relative density of the formed body obtained in the magnetic field is usually 40 ∼ 60%.
[0031] The magnetic field is applied in the range of approximately 10 - 20 kOe (960 - 1600 kA / m). The applied magnetic field is not limited to a magnetostatic field, and it can also be a pulsed magnetic field. In addition, a magnetostatic field and a pulsed magnetic field can also be used together.
[0032] Then, the formed body is sintered in a vacuum or an inert gas atmosphere. The sintering temperature must be according to the conditions in the type of composition, the pulverization process, the difference the average particle diameter and particle size distribution and the like. The formed body is sintered at 1000 ∼ 1200 °C for 8 to 50 hours. This is because the diffusion of Ce from the shell section to the core section is insufficient and the structure in which the mass concentration of R1 and Ce in the core section and the cladding section is controlled, cannot be obtained if the sintering time is shorter than 8 hours, and grain growth progresses considerably and in particular has a bad effect on the coercive force if the sintering time is 50 hours or more.
[0033] After sintering, the resulting sintered body can be subjected to an aging treatment. The step is an important step for controlling the coercive force. If the aging treatment is divided into two stages, It is effective to keep them at about 800 °C and about 600 °C for a given time. If the heat treatment at about 800 °C after sintering, the coercive force increases, so that it is particularly suitable for the mixing process Because the coercive force is significantly increased during heat treatment at about 600 °C, the Aging treatment is preferably carried out at 600 °C if the aging treatment is carried out in one stage is executed.
[0034] The embodiments for preferred implementation of the present invention have been described above, and the Structure of the present invention can be obtained by increasing the R1 content in the shell. In this case, the Grain boundary diffusion method can also be used by the R1-containing or an R1-containing layer forming powder is attached to the surface of the sintered body and heating is carried out.
[0035] The sintered body is cut into predetermined sizes and shapes after the above treatment. Although the processing method for the surface of the sintered body is not particularly limited, Machining is defined as grinding treatment under Using a grindstone and the like.
[0036] Next, the protective film is formed. The formation of the protective film can be carried out by the known method according to the species of the protective film. For example, in the case of electroplating, a conventional process, such as degreasing, washing with water, etching (e.g. with nitric acid), washing with Water, film formation using electroplating, washing with water, drying, etc. The Degreasing and chemical etching using acids can be carried out, and the surface of the sintered body is cleaned.
[0037] The plating bath used in electroplating Ni may be a Watt bath without nickel chloride (ie under Using nickel sulfate and boric acid as main components), an amidosulfonic acid bath, a fluoborate bath, a Nickel bromide bath and the like. In this case, however, to reduce the dissolution of the anode Preferably nickel ions are added to the bath solution. Nickel ions are preferably added in the form of a nickel sulfate or Nickel bromide solution added. EXAMPLES
[0038] The invention will be described in detail below using the examples and comparative examples which However, the present invention is not limited to the following examples. (Example 1)
[0039] The composition of the raw alloy was 14.9 mol% R - 6.43 mol% B - 0.57 mol% Co - 0.06 mol% Cu - 0.44 mol% Al - Fe Rest. R was set in terms of the molar ratio to R1 : Ce = 100 : 0 ∼ 10 : 90. The metals or Alloys as the raw materials were formulated to have the above composition. Raw alloy layers were melted and cast by strip casting.
[0040] The obtained raw alloy sheets were pulverized by hydrogen to obtain a coarsely pulverized powder. Oleinamide in a proportion of 0.1 wt.% was added to the coarsely pulverized powder as a lubricant. Then, fine pulverization was carried out under high pressure in a nitrogen gas atmosphere using a Jet mill to obtain a finely pulverized powder.
[0041] Subsequently, the resulting finely pulverized powder was shaped in a magnetic field. In particular, the Forms were carried out in a magnetic field of 15 kOe (1193.66 kA / m) under a pressure of 140 MPa, and a shaped body with a size of 20 mm x 18 mm x 13 mm was obtained. The direction of the magnetic field was Pressing direction perpendicular direction. In addition, the resulting molded body was heated at 1030 °C for 1 to 48 hours sintered. The diffusion of Ce toward the grain boundary phase could be further enhanced by extending the sintering time. Next, an aging treatment was carried out at 800°C for one hour and at 500°C for one hour carried out to obtain the sintered body.
[0042] A BH tracer was used to measure the coercive force of the obtained sintered body. The results are shown in Table 1.
[0043] Subsequently, each sintered body was electroplated with Ni. The film thickness of the Ni- plated layer is 10 µm. After the formation of the Ni-plated layer, the adhesion strength of the Ni film, ie the The results are shown in Table 1. Furthermore, the adhesion strength was measured by the test method defined in JIS- H8504 2000-02-29. Methods of adhesion test for metallic coatings.
[0044] In addition, the resulting sintered body was covered with an epoxy resin and its cross-section was ground. Commercially available sandpaper was used for sanding. The sanding was carried out while the Sandpaper with a low roughness was changed to one with a high roughness. Finally, a Leather and diamond abrasive grains were used for grinding. At that time, grinding was done without water and The components in the grain boundary phase would be corroded if water were used.
[0045] The composition distribution of the samples after grinding was investigated using EPMA. The core section, the shell section, the triple point and the like in the main phase grains were Viewing backscattered electron images and EPMA images of an electron microscope. Regarding the Points, a quantitative analysis was carried out on the basis of at least 30 points each to determine the Mass concentration to obtain the assumed average composition. The mass concentrations of R1 and Ce in the core section were designated as αR1 and αCe, respectively, and the mass concentrations of R1 and Ce in the Shell section of the crystal grains were designated as βR1 and βCe, respectively. The mass concentration ratio between R1 and Ce in the mantle section, ie βR1 / βCe, was designated as B, and the Mass concentration ratio between R1 and Ce in the core section, i.e. αR1 / αCe, was designated as A. The Measured αR1, αCe, βR1, βCe and the calculated A, B and B / A are shown in Table 1.
[0046] Compared with the samples obtained with a sintering time of one hour, the samples with a longer sintering time In the samples obtained, the R1 fraction in the shell section is greater than that of R1 in the core section, regardless of the Ratio R1 : Ce in the raw material composition. The reason given was the development of heat treatment induced interdiffusion between Ce in the main phase grains and Nd is considered as R1 of the grain boundary. If Example 5, Comparative Example 2, Examples 6 and 7 were compared with the same raw material composition, there was a slight difference between the R1 fraction in the mantle section and that in the core section when the Firing time in Comparative Example 2 was one hour, and B / A became larger as the sintering time became longer. Accordingly, based on these results, it could be stated that interdiffusion developed and that B / A increased if the heat treatment time was increased.
[0047] By comparing Comparative Example 3, in which the sintering time was one hour, with Comparative Example 4 and Comparative Example 2, it was found that the coercive force decreased if the Ce content was increased, it However, only a slight deterioration of the coercive force was found in the examples where the sintering time was increased to 8 hours and 48 hours and the ratio between Ce in the core section and that in the mantle section However, the reduction in coercive force was significant in the compositions with a significant Ce content increased considerably. Furthermore, in the samples sintered for 48 hours with R1 : Ce = 100 : 0, the Coercivity compared to the samples fired for a shorter time, assuming that this was due to the abnormal growth of the crystal grains. Accordingly, the composition was due to the Surface of the grains closer to R1-Fe-B than to (R1·Ce)-Fe-B, which is determined based on the raw material composition was accepted.
[0048] There was no big difference in the A / B values compared to Example 5, where the ratio between R1 and Ce was 50 : 50 and Nd was used as R1, and Examples 9 and 10, where Pr and Dy were added as R1, The coercivity in Example 11 was high because Dy was added with a high anisotropy.
[0049] The coercive force induction mechanisms of the RTB-based sintered magnet were classified as nucleation type and the coercivity was controlled by the composition on the surface of the grains. Therefore, assumed that a higher coercive force, closer to that of R1-Fe-B and greater than that was achieved as assumed based on the raw material composition.
[0050] As shown in Table 1, regardless of the sintering time, the adhesion strength with a plated film improved if the Ce concentration was increased. It was assumed that the reason for this was the better chemical Adhesion between the Ce and the plated film than between Nd and the plated film. To increase the Adhesive strength is preferably added Ce.
Claims
1. RTB-based sintered permanent magnet, comprising: Main phase grains with a core section and a mantle section covering the core, where, if the mass concentration of R1 and Ce in the core section is denoted as αR1 and αCe respectively and the Mass concentration of R1 and Ce in the mantle section is designated as βR1 and βCe, respectively, the ratio (B / A) between the mass concentration ratio between R1 and Ce in the mantle section (βR1 / βCe = B) and that between R1 and Ce in the core section (αR1 / αCe = A) is 1.1 or more, where R has Ce and R1 as essential components, R1 is at least one rare earth element other than Ce and T is at least one transition metal element containing Fe or the combination of Fe and Co as an essential component has where the content ratio between R1 and Ce in the rare earth element R is 50 : 50 - 90 :
10.
2. The RTB-based sintered permanent magnet according to claim 1, wherein B / A is 1.4 or more.
3. RTB-based sintered permanent magnet according to claim 1, wherein R1 is at least one element selected from the group consisting of Group consisting of Nd, Pr, Dy, Ho and Tb.
Citation Information
Patent Citations
Permanent magnet
JP1984046008A
Printing machine
JP1994000942A
Air conditioner
JP1994002930A
Thermal AGC system bi-directional amplifier
JP1994006776A
Method for preparation of permanent magnet
US20040050454A1