Surface-treated cathode active material and lithium secondary battery using the same

The double-coating of metal oxide and PEDOT-PEG on cathode active materials addresses the stability and conductivity issues, enhancing the performance and lifespan of lithium secondary batteries.

DE102014223177B4Active Publication Date: 2024-12-05HYUNDAI MOTOR CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE102014223177
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2013-12-30
Filing Date
2014-11-13
Publication Date
2024-12-05
Estimated Expiration
2034-11-13

AI Technical Summary

Technical Problem

Existing surface treatments for cathode active materials in lithium secondary batteries face challenges in maintaining uniformity and stability, leading to reduced lithium ion mobility, electron conductivity, and thermal instability, which affect the battery's performance and lifespan.

Method used

A double-coating process is applied to the cathode active material, where a metal oxide is first coated followed by a conductive polymerized copolymer like PEDOT-PEG, which has both electron and ionic conductivity, to enhance electrochemical properties and thermal stability.

Benefits of technology

The double-coating process improves the electrochemical properties and thermal stability of the cathode active material, resulting in lithium secondary batteries with enhanced output characteristics and extended service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Surface-treated cathode active material which is double-coated by a primary coating of metal oxide on the surface of the cathode active material and a secondary coating of a polymerized copolymer having both electronic conductivity and ionic conductivity, thereby forming a double coating on the surface of the cathode active material, wherein the polymerized copolymer having both electronic conductivity and ionic conductivity is poly(3,4-ethylenedioxythiophene)-block-poly(ethylene glycol) (PEDOT-PEG), and wherein the metal oxide is coated in an amount of 0.1 to 2.0 wt.% based on the weight of the cathode active material.
Need to check novelty before this filing date? Find Prior Art

Description

BACKGROUND(a) TECHNICAL FIELD

[0001] The present disclosure relates to a surface-treated cathode active material and a lithium secondary battery using the same. More specifically, the present disclosure relates to a surface-treated cathode active material applicable to the manufacture of a lithium secondary battery with excellent output characteristics by performing double coating by primary coating a metal oxide on a surface of a cathode active material for the lithium secondary battery and secondary coating thereon a conductive polymerized copolymer having both ionic conductivity and electronic conductivity to improve the electrochemical properties and thermal stability of the cathode active material, and to a lithium secondary battery using the same. (b) TECHNICAL BACKGROUND

[0002] A lithium secondary battery is manufactured by using a material capable of intercalating and deintercalating lithium ions as a negative electrode and a positive electrode, and intercalating an organic electrolyte solution or a polymer electrolyte that allows lithium ions to move between the negative electrode and the positive electrode, and stores electrical energy by means of redox reactions depending on the intercalation and deintercalation of lithium ions in the positive electrode and the negative electrode.

[0003] In order to improve the electrochemical properties and safety of a lithium secondary battery as described above, studies on surface treatments of the cathode active material of the lithium secondary battery have been actively conducted.

[0004] In the case of the cathode active material for the lithium secondary battery, dissolving of HF formed in the electrolyte solution can be achieved by using metal oxide (Al 2 O 3 , ZrO 2 and La 2 O 3 ), metal phosphorus oxide (AlPO 4 and LiCoPO 4 ), carbon, halogen gas, metal hydroxide, a conductive polymer and the like to reduce direct reaction with the electrolyte by coating the positive electrode surface by several nm, and the stability of the crystal structure can be ensured by suppressing the elution of various transition metals.

[0005] However, there is a limitation that a disadvantage occurs when the movement of lithium ions and electrical conduction is interrupted in the case where a coating material such as a metal oxide, which is a non-conductor, is used, so that the mobility of lithium ions and electrons deteriorates. Furthermore, when coating with inorganic particles alone, it is difficult to ensure the uniformity of the coating. In particular, it is insufficient to ensure the structural stability of the cathode active material, and a side reaction with the electrolyte solution occurs due to the non-uniformity of the coating.

[0006] In the case of a polymer coating, it is possible to perform coating with an organic material as a related technique in terms of ensuring the uniformity of the coating, however, due to the thermal instability of the organic material and too large a thickness of the coating, ions cannot be easily transferred, so the performance deteriorates.

[0007] Accordingly, depending on the specific inorganic material or polymer, the cathode active material has a limitation that cannot be overcome by improving the physical properties solely through surface modification.

[0008] For this reason, as a cathode active material surface modification technology for improving the high capacity, high output, and service life characteristics of the lithium secondary battery, a technology of coating manganese oxide with a conductive polymer or obtaining a coating by mixing two materials has been investigated, but there is only an intention to achieve performance improvement by simply increasing the content of the conductive material.

[0009] As an example of related art, Korean Patent Application Laid-Open No. KR 10 2007 0 008 115 A proposes sequentially coating a cathode active material with a first coating layer of oxide on a lithium transition metal oxide particle and a second coating layer of a conductive material on the first coating layer, as a technology having a double coating structure. However, the material used in the second coating layer is a purely electron-conductive material, and therefore, the movement of lithium ions during charging and discharging is not smooth.

[0010] Korean Patent Application Laid-Open No. KR 10 2011 0 023 067 A proposes a cathode active material for a lithium secondary battery, which sequentially includes a lithium metal oxide secondary particle core, a first shell formed by coating the surface of a portion of the secondary particle core with a plurality of barium titanate particles and a plurality of metal oxide particles, and a second shell formed by coating the surface of the first shell with a plurality of olivine-type lithium iron phosphate oxide particles and a plurality of conductive material particles. Furthermore, Korean Patent Application Laid-Open No.KR 10 2007 0 016 431 A proposes an active material for a lithium secondary battery comprising a core material and a surface treatment layer formed on the surface of the core material and including nano-sized inorganic particles and a conductive polymer.

[0011] However, according to the above-described technologies of the surface coating-treated cathode active material, although surface modification effect is improved compared with the existing technologies, conductivity and ion transfer effect are not fully achieved, and effects of improving performance such as electrochemical properties and thermal stability are small.

[0012] Japanese Patent Application Laid-Open No. JP 2005-524936 A proposes an electrode fabricated by extruding a conductive material and an ion-conductive polymer into an active material including a metal oxide through an extruder. However, the effects in improving performance, such as electrochemical properties and thermal stability, are not very good because the structure of the active material is unstable and non-uniform.

[0013] In addition to the technologies described above, there are some technologies that utilize a conductive polymer and a metal powder, such as a technology in which a cathode active material is coated with a polymer that exhibits both ionic conductivity and electrical conductivity, and a polymer film to which a conductive powder is added. However, this does not completely solve the existing problems in improving physical properties, such as maintaining a balance between conductivity and ion transfer effects.

[0014] WO 2013 / 169826 A1 describes particles of a cathode material for a lithium battery that are coated with polymers to prevent direct contact between the particles and the surrounding electrolyte. Prior to the polymer coating, the surfaces of the particles can be provided with a carbon or ceramic coating.

[0015] The information disclosed in this Background section above is intended only to enhance the understanding of the background of the invention and may therefore contain information that is not part of the prior art already known to a person skilled in the art in this country. SUMMARY OF REVELATION

[0016] The present disclosure has been made in an effort to solve the problems described above in connection with the related art.

[0017] As a result of intensive studies to solve the problems in the related art, it was found that when a cathode active material for a lithium secondary battery is double-coated, the electrochemical properties and thermal stability of the cathode active material are greatly improved by primarily coating an inorganic material on one surface of the cathode active material and then secondarily coating it with a conductive polymerized copolymer that exhibits both electronic conductivity and ionic conductivity. As a result, a lithium secondary battery with excellent output characteristics can be manufactured.

[0018] One aspect of the present disclosure provides a cathode active material double-coated with metal oxide and a polymerized copolymer having electronic conductivity and ionic conductivity on the surface of the cathode active material, wherein the polymerized copolymer having both electronic conductivity and ionic conductivity is poly(3,4-ethylenedioxythiophene)-block-poly(ethylene glycol) (PEDOT-PEG), and wherein the metal oxide is coated in an amount of up to 0.1 to 2.0 wt.% based on the weight of the cathode active material.

[0019] Another aspect of the present disclosure provides a cathode active material having a surface modified to greatly improve electrochemical properties and thermal stability.

[0020] Another aspect of the present disclosure provides a lithium secondary battery having a long service life and excellent output characteristics by employing a cathode active material having electrochemical properties and thermal stability greatly improved due to surface modification.

[0021] According to an exemplary embodiment of the present disclosure, a surface-treated cathode active material is double-coated by primarily coating a metal oxide on the surface of a cathode active material and secondarily coating a polymerized copolymer having both electronic conductivity and ionic conductivity, thereby forming a double coating on the surface of the cathode active material, wherein the polymerized copolymer having both electronic conductivity and ionic conductivity is poly(3,4-ethylenedioxythiophene)-block-poly(ethylene glycol) (PEDOT-PEG), and wherein the metal oxide is coated in an amount of up to 0.1 to 2.0 wt.% based on the weight of the cathode active material.

[0022] In another aspect of the present disclosure, a lithium secondary battery comprising the surface-treated cathode active material is provided.

[0023] The surface-treated cathode active material according to the present disclosure is a cathode active material in which the electrochemical properties of a positive electrode material for a lithium secondary battery are greatly improved by the above-described double coating treatment with metal oxide and an electron- and ion-conducting copolymerized polymer (PEDOT-PEG).

[0024] In particular, it is possible to improve the high voltage and service life characteristics as well as the structural and thermal stability by surface modification of the cathode active material by secondarily and uniformly coating the polymer PEDOT-PEG, which has both electronic conductivity and ionic conductivity, on a primary coated inorganic material, compared to electrode materials coated only with the inorganic material.

[0025] It is also possible to manufacture a lithium secondary battery having better output characteristics than existing electrodes coated with an inorganic material by using a polymer material having electronic conductivity and ionic conductivity to improve the movement of lithium ions and the electronic conductivity of the electrode.

[0026] Other aspects and embodiments of the invention are discussed below.

[0027] It is understood that the term "vehicle" or "vehicular" or other similar terms, as used herein, includes motor vehicles generally; for example, passenger cars including sport utility vehicles (SUVs); buses; trucks; various commercial vehicles; watercraft, including various boats and ships; aircraft and the like; and hybrid vehicles; electric vehicles; plug-in hybrid-electric vehicles; hydrogen-powered vehicles; and other alternative fuel vehicles (e.g., fuel derived from resources other than petroleum). As used herein, a hybrid vehicle is a vehicle that has two or more power sources, for example, vehicles that are both gasoline-powered and electric-powered.

[0028] The above and other features of the invention are discussed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The above and other features of the present disclosure will now be described in detail with reference to certain exemplary embodiments thereof illustrated in the accompanying drawings set forth below, by way of illustration only, and are therefore not limitative of the present disclosure. Fig. 1 is a schematic view illustrating a structure in which a surface-treated cathode active material according to the present disclosure is double-coated. Fig. 2 is a conceptual view of a coating process schematically illustrating a double coating process of the surface-treated cathode active material according to the present disclosure. Fig. 3(a) to 3(d) are photographs comparing differently coated cathode active materials, including a scanning electron microscope (SEM) photograph of LiNi 0,6 Co0,2 Mn 0,2 O 2 , which is double-coated with an inorganic material and a conductive polymer, and an SEM photograph of untreated LiNi 0,6 Co 0,2 Mn 0,2 O 2 . Figs 4(a) to 4(d) are transmission electron microscopy (TEM) comparison photographs of LiNi 0,6 Co 0,2 Mn 0,2 O 2 before and after coating with each component according to the present disclosure. Fig. 5A and Fig. 5B are graphs showing the cycle characteristics of a LiNi o , 6 Co 0 , 2 Mn 0 , 2 0 2 -Electrode as a function of the charging voltage for the cathode active material, in which polyethylenedioxythiophene (PEDOT, reference example) or polyethylenedioxythiophene-polyethylene glycol (PEDOT-PEG, according to the invention) are used as coating materials and compared with each other. In Fig. 5A the charging voltage is 4.3 V and in Fig. 5B the charging voltage is 4.6 V. Fig. Figure 6 is a graph comparing the cycle characteristics for each thickness of a double coating by double-coating the cathode active material, with charging and discharging performed 50 times at a charging voltage of 4.6 V. Fig. 7A and Fig. 7B are graphs showing the cycle characteristics of the LiNi 0,6 Co 0,2 Mn 0,2 O 2 electrode as a function of the charging voltage for the cathode active material, where Al 2 O 3 or an Al 2 O 3 +PEDOT-PEG double coating are used as coating materials and compared with each other. Fig. 7A the charging voltage is 4.3 V and Fig. 7B the charging voltage is 4.6 V. Fig. Figure 8 is a graph showing the improvements in the cycle characteristics of the LiNi0,6 Co 0,2 Mn 0,2 O 2 electrode at high temperature (55°C) depending on the coating of the cathode active material. Fig. 9 is a graph showing the discharge capacities of the LiNi 0,6 Co 0,2 Mn 0,2 O 2 electrode as a function of the discharge rate (C-rate) of the cathode active material. Fig. 10 is a graph showing the improvements in thermal stability of the LiNi 0,6 Co 0,2 Mn 0,2 O 2 -electrode depending on the coating of the cathode active material. Fig. 11A and Fig. 11B are graphs comparing the cycle characteristics of a lithium secondary battery versus charging voltage for the lithium secondary battery in which the cathode active material is used. In Fig. 11A the charging voltage is 4.3 V and in Fig.11B the charging voltage is 4.6 V. Fig. Figure 12 is a graph comparing the cycle characteristics of a lithium secondary battery at high temperature (55°C) for the lithium secondary battery using the cathode active material.

[0030] It should be understood that the accompanying drawings are not necessarily to scale and are a somewhat simplified representation of various features illustrating the basic principles of the invention. The specific design features of the present invention as disclosed herein include, for example, specific dimensions, orientations, locations, and shapes, which will be determined in part by the precise intended use and environment of use.

[0031] In the figures, reference numerals refer to the same or equivalent parts of the present invention throughout the various figures of the drawings. DETAILED DESCRIPTION

[0032] Reference will now be made in detail to various embodiments of the present disclosure, examples of which are illustrated in the accompanying drawings and described below. While the invention will be described in connection with exemplary embodiments, it is to be understood that the present description is not intended to limit the invention to those exemplary embodiments. On the contrary, the invention is intended to cover not only the exemplary embodiments, but also various alternatives, modifications, equivalents, and other embodiments included within the spirit and scope of the invention as defined by the appended claims.

[0033] An exemplary embodiment of the present disclosure will now be described in detail as follows.

[0034] The present disclosure relates to a surface-treated cathode active material in which metal oxide and PEDOT-PEG as a polymerized copolymer having both electronic conductivity and ionic conductivity are sequentially coated on the surface of the cathode active material as a double coating.

[0035] According to the present disclosure, cathode active materials that can be used are those selected from lithium transition metal oxides and sulfur compounds. Specific examples of the cathode active material that can be used in the present disclosure include LiNiCoO 2 , LiNi x Co y Mn z O 2 (0≤x≤1.0≤y≤1.0≤1≤z), LiNi 0,5 Mn 1,5 O 4 , LiMn 2 O 4 , LiFePO 4 , sulfur and the like.

[0036] As an example of the metal oxide first applied to the surface of the cathode active material of the present disclosure, it is possible to use one or more selected from the group consisting of Al 2 O 3 , SiO 2 , TiO 2 , SnO 2 , CEO 2 ZrO 2 , BaTiO 3 and Y 2 O 3 Metal oxides that can be used have an average particle diameter of 1 nm to 100 nm.

[0037] According to the present disclosure, the metal oxide is applied in an amount of up to 0.1 to 2.0 wt.% based on the weight of the cathode active material.

[0038] According to the present disclosure, the metal oxide is first coated in a small thickness on the surface of the cathode active material, and then secondly a polymerized copolymer having both electrode conductivity and ionic conductivity is coated thereon.

[0039] According to the present disclosure, poly(3,4-ethylenedioxythiophene)-block-poly(ethylene glycol) (PEDOT-PEG) is used as the polymerized copolymer having both electronic conductivity and ionic conductivity.

[0040] According to the present disclosure, the cathode active material sequentially double-coated with the metal oxide and the polymerized copolymer as described above may have a total coating thickness of 5 to 500 nm. In certain embodiments, the total coating thickness may be 10 to 100 nm. If the coating is too thin, it is difficult to expect an improvement in performance, and if the coating is too thick, the resistance encountered in the transfer of ions and electrons is increased, making it difficult to achieve high capacity.

[0041] Fig. 1 is a schematic view illustrating a structure in which a surface-treated cathode active material according to the present disclosure is double-coated.

[0042] According to the present disclosure, disadvantages of each of the inorganic material and the polymer can be compensated by a double coating method that uses both inorganic material and polymer instead of the inorganic material or the polymer alone.

[0043] First, a metal oxide, which is the inorganic material applied as a primary coating to the cathode active material, is primarily coated on the surface of the cathode active material to ensure the thermal stability of the metal oxide and improve its service life characteristics. A polymerized copolymer, which exhibits both electronic conductivity and ionic conductivity, is then secondarily coated to overcome the non-uniformity of the primarily coated inorganic material and simultaneously improve the electronic conductivity and ionic conductivity of the cathode active material. In particular, the polymerized copolymer, which exhibits both electronic conductivity and ionic conductivity, significantly improves the reduction in electronic and ionic conductivity caused by coating with the primary metal oxide, which is a non-conductor.When the polymerized copolymer having electronic conductivity and ion conductivity is applied to the cathode active material, it exhibits facilitated ion transfer and electron conduction in the intercalation and deintercalation reactions of lithium compared to other polymers, and thus the capacity and output characteristics are greatly improved.

[0044] When the cathode active material according to the present disclosure, which is surface-treated with the polymerized copolymer having electronic conductivity and ionic conductivity used in the present disclosure, such as PEDOT-PEG polymer, is used in a lithium secondary battery, a coating can be stably maintained during charge and discharge cycles because the coating does not dissolve in ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and the like used in an electrolyte solution for the lithium secondary battery. Accordingly, the structural stability of the cathode active material can be maintained, and a side reaction with the electrolyte solution can be reduced. In particular, the effects of the coating are maximized at high voltage and high temperature, where decomposition of the electrolyte solution occurs.Furthermore, since the polymer is used as the final coating, the present disclosure has the additional effect of increasing the adhesion force with a polymer material used as a binder for the lithium secondary battery. This effect according to the present disclosure is demonstrated in the following examples.

[0045] As described above, the present disclosure can improve the electrochemical characteristics and thermal stability of the cathode active material for a lithium secondary battery by dual-coating the metal oxide coating and the electron- and ion-conductive polymerized copolymer. Specifically, it is possible to improve the high-voltage and service life characteristics, as well as the structural and thermal stability, by modifying the surface by first thinly coating the metal oxide on the surface of the cathode active material and secondarily uniformly coating a polymer having both electron conductivity and ion conductivity on the primary coating, compared to electron materials coated only with the inorganic material.

[0046] According to the present disclosure, it is possible to provide a lithium secondary battery having better output characteristics than a battery employing an existing electrode coated with inorganic material by using a polymer having electron conductivity and ion conductivity to improve the movement of lithium ions and electron conductivity of the electrode, as described above.

[0047] Accordingly, the present disclosure provides a lithium secondary battery employing a surface-treated cathode active material as described above.

[0048] The lithium secondary battery manufactured by using the surface-treated cathode active material according to the present disclosure has excellent output characteristics and improvement in long service life compared with existing lithium secondary batteries.

[0049] The lithium secondary battery manufactured using the surface-treated cathode active material according to the present disclosure can be used not only in small-sized secondary batteries used in portable electronic devices such as mobile phones, laptop computers, and digital cameras, but also in medium- to large-sized energy storage devices and the like used in electric vehicles, energy storage systems, and the like. In particular, the lithium secondary battery can be used for an electric vehicle that consumes a relatively large amount of energy and is used extensively for a long period of time.

[0050] In the following, the present disclosure will be described in detail with reference to examples, but it is not limited by the examples. EXAMPLES

[0051] The following examples illustrate the invention and are not intended to limit it. EXAMPLE 1. Surface treatment of the cathode active material

[0052] A schematic surface coating process of the active material is shown in Fig. 2. The coating was applied as shown in Fig. 2. A cathode active material can be used for all metal oxide materials, and in the present example it was used for the Li[Ni 0,6 Co 0,2 Mn 0,2 ]O 2 material (hereinafter NMC 622). A dry coating was applied to the NMC 622 surface using aluminum oxide (Al 2 O 3, Aldrich), which has a size of 2 to 9 nm, and a deposited amount of 0.5 wt.% was used for dry coating. A state-of-the-art ball milling method was used for dry coating, and the dry coating was carried out at a speed of 300 rpm for 6 hours.

[0053] The cathode active material subjected to dry coating was placed in a nitromethane solution in which a PEDOT-PEG polymer was dissolved, and the resulting solution was stirred at 60°C for 6 hours. After stirring, a solid was obtained by filtration, and the double coating on the surface of the cathode active material was completed by vacuum drying the solid at 110°C. EXAMPLE 2. Morphology analysis of the cathode active material

[0054] The morphology of the cathode active material that had undergone coating was confirmed. To confirm the degree of dispersion of the coating material on the surface of the electrode that had undergone coating, imaging results of various elements were analyzed using a scanning electron microscope and recorded in the Fig. 3(a) to 3(d) are illustrated.

[0055] As a result of comparison with the cathode active material (untreated positive electrode) that was not coated, aluminum (Al) and sulfur (S) present in the inorganic material and the conductive polymer were detected for the case of the double-coated cathode active material, and it could be seen that the elements were uniformly deposited on the surface of the cathode active material. The photographs observed using TEM in the Fig.Figures 4(a) to 4(d) show, respectively, (a) the surface of the active material before coating, (b) the surface of the active material after coating with the electron- and ion-conductive polymer, (c) the surface of the active material after primary coating with metal oxide, and (d) the surface of the active material that has undergone double coating with the inorganic material and the electron- and ion-conductive polymer. It can be seen that coating uniformity can be ensured by secondary coating of the conductive polymer on the surface of the primary-coated inorganic material. EXAMPLE 3. Preparation of an electrode and a cell using the coated cathode active material

[0056] After poly(vinylidene fluoride) (PVdF), used as a binder to prepare a positive electrode, was completely dissolved in N-methylpyrrolidone, super-P carbon as a conductive material and double-coated LiNi 0,6 Co 0,2 Mn 0,2 O 2 was measured and added to the resulting mixed solution, and the resulting mixture was stirred. In this case, the weight ratio of the cathode active material, the conductive material, and the binder was adjusted to 85:7.5:7.5.

[0057] The fully mixed slurry solution was applied to aluminum foil, dried, and subjected to a lamination process using a roller press. This was done to increase the mutual bonding force of the active material, the conductive material, and the binder and to effectively bond the materials to the current collector.

[0058] After the compression process, an electrode of appropriate size was prepared by a cutting process and dried at 110°C in a vacuum oven for 24 hours. A button cell was fabricated using the prepared positive electrode.

[0059] Lithium metal was laminated onto a copper foil, and the resulting laminate was used as the negative electrode. A 1 M LiPF 6 A solution prepared in a mixed solvent of ethylene carbonate / dimethyl carbonate (50 / 50 by volume) was used as the electrolyte solution, and a polyethylene separator film was used as the separator film. All electrodes were fabricated in a dry room, and battery fabrication was carried out in a glove box in which an argon atmosphere was maintained.

[0060] For the manufactured cell, charge and discharge cycles were carried out in a range of 2.6 to 4.3 V or 2.6 to 4.6 V with a current density of 0.5 C. EXAMPLE 4. Evaluation of the characteristics of the lithium secondary battery

[0061] The service life characteristics of cells undergoing a formation process were evaluated for each charging voltage (4.3 V and 4.6 V) using a positive electrode (untreated) that had not been coated, a positive electrode (modified NCM PEDOT) coated only with an electron-conductive polymer, and a positive electrode (modified NCM PEDOT-PEG) coated with a polymer exhibiting both ionic and electronic conductivity. The charging and discharging results, as shown in the Fig. 5A and Fig.5B were obtained by repeating charging and discharging 50 times at a current density of 0.5 C at room temperature. As a result, it can be seen that the highest capacity and best service life characteristics were obtained for the case of coating with PEDOT-PEG, which is an ion-conductive and electron-conductive copolymerized polymer.

[0062] The cathode active material was double coated primarily with alumina and secondarily with a PEDOT-PEG copolymer, which exhibits electronic conductivity and ionic conductivity, and the cycling characteristics were evaluated for each coating thickness and are shown in Fig.6. As a result, it can be seen that when the coating thickness was as thin as 8 nm, the initial capacity was high, but the service life characteristics deteriorated rapidly. When the coating thickness was as thick as 180 nm, the coating acted as a resistor, resulting in a low discharge capacity value in the initial stage. In contrast, a positive electrode material double-coated with a thickness of 30 nm showed excellent service life characteristics along with high discharge capacity in the initial stage.

[0063] The service life characteristics were evaluated for each charging voltage (4.3 V and 4.6 V) for the case where the cathode active material was coated only with aluminum oxide and the case where the cathode active material was double-coated with aluminum oxide and the polymer exhibiting electronic and ionic conductivity. The results, as shown in the Fig. 7A and Fig. 7B were obtained by repeating charging and discharging 50 times at a current density of 0.5 C at room temperature.

[0064] Regarding the Fig. 7A and Fig. 7B, the two cathode active materials coated with aluminum oxide showed improved lifetime characteristics at both 4.3 V ( Fig. 7A) and at 4.6 V ( Fig.7B) compared to the uncoated cathode active material. However, non-uniformity of the coating caused a side reaction with some of the electrolyte solution. Therefore, the double coating compensated for the coating with the inorganic oxide material layer, which still has some disadvantages. The coating problem was overcome by introducing an electron- and ion-conductive copolymerized polymer. The double-coated cathode active material showed the best performance and service life characteristics, and it was confirmed that the double-coated cathode active material showed excellent performance even under different charging voltages.

[0065] The service life characteristics were compared under high temperature conditions of 55°C, and results are shown in Fig. 8. With regard to Fig.8 it can be seen that, since the internal resistance of the cells decreases at high temperature, a higher capacity is achieved at high temperature than at room temperature (see Fig. 7A). In contrast, it can be seen that the uncoated positive electrode material exhibits relatively poor service life characteristics, while structural collapse of the cathode active material and side reactions with the electrolyte solution still occur rapidly. However, it can be seen that an electrode double-coated with alumina and a conductive polymer exhibits high capacity and excellent service life characteristics. This is because the double coating of metal oxide and polymer layer effectively suppresses side reactions with the electrolyte solution. EXAMPLE 5. Evaluation of high-rate characteristics

[0066] The charge and discharge evaluation was performed three times at each current density, while increasing the current density from a low rate to a high rate. This test confirms the capacity characteristics of the cathode active material under conditions of rapid charge and discharge. It is a technique that evaluates the characteristics by successively applying high current, unlike the evaluation of service life characteristics using a constant current density.

[0067] The results of the evaluation of the charging capacity will be presented in Fig. 9. The results in Fig.9 show that the double-coated electrode exhibits high capacity at a high rate, which requires high output power. Specifically, the capacity recovery rate of the cathode active material is confirmed by changing the current density from a low rate to a high rate, and the structural stability can be indirectly confirmed. For the double-coated electrode, as shown in Fig. As illustrated in Figure 6, a high capacity recovery rate of 99.8% was obtained. EXAMPLE 6. Evaluation of thermal stability after evaluation of service life characteristics

[0068] After evaluating the service life characteristics of the lithium secondary battery, the battery was disassembled in the charged state, the thermal stability of the cathode active material was analyzed using a differential scanning calorimeter (DSC) and is shown in Fig.10, and the results are summarized in Table 1 below.

[0069] For the coated electrode, it can be seen that the exothermic peak shifted toward the high-temperature region, and the amount of heat released decreased rapidly. It can be seen that the coating, composed of the metal oxide and the polymer, suppressed the exothermic reaction of the cathode active material with the electrolyte solution, thus improving thermal stability.

[0070] The following Table 1 compares the thermal DSC characteristics of the cathode active material in the charged state after charging and discharging. [Table 1] electrode Exothermic peak temperature (°C) Amount of heat released (J / g) untreated positive electrode 281, 0 587,5 aluminum oxide coated positive electrode 286, 9 320, 1 Double coated positive electrode 287,4 198,5 EXAMPLE 7. Evaluation of the performance of the lithium secondary battery

[0071] A lithium secondary battery was fabricated using graphite-based mesocarbon microbeads (MCMB) as the negative electrode, and the characteristics for each condition were evaluated. After fabrication of the lithium secondary battery, the service life characteristics of cells formed according to the present disclosure were evaluated for each charging voltage (4.3 V and 4.6 V). The charging and discharging results, as described in Fig. 11A and Fig. 11B, were obtained by repeating charging and discharging 50 times at a current density of 0.5 C at room temperature. When the charging voltage was 4.3 V, the positive electrode double-coated with alumina and a PEDOT-PEG polymer, which exhibits electronic and ionic conductivity, showed the highest initial capacity and excellent service life characteristics, as shown in Fig. 11A shown. Fig.Figure 11B illustrates the service life characteristics for high-voltage charging (4.6 V). It can be seen that the service life characteristics are significantly improved by a double coating of alumina and PEDOT-PEG as the charging voltage is increased.

[0072] For a lithium secondary battery using the double-coated cathode active material, cycle characteristics at high temperature were evaluated and are shown in Fig. 12. In the graph of Fig.12, coated active materials exhibit better service life characteristics at high temperatures (55°C) than the case where an uncoated cathode active material is used. In particular, due to the suppression of the destruction effects of the crystal structure in the cathode active material, combined with the decomposition of the electrolyte solution, the double coating of alumina and the PEDOT-PEG polymer exhibits improved service life characteristics compared to the existing cathode active material.

[0073] The surface-treated cathode active material according to the present disclosure can be used in small and medium-sized to large-sized lithium secondary batteries. In particular, the surface-treated cathode active material according to the present disclosure can be used for lithium secondary batteries used in various mobile electronic devices, electric vehicles, and energy storage systems.

[0074] The invention has been described in detail with reference to embodiments thereof. However, it will be understood by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

[1] Surface-treated cathode active material which is double-coated by a primary coating of metal oxide on the surface of the cathode active material and a secondary coating of a polymerized copolymer having both electronic conductivity and ionic conductivity, thereby forming a double coating on the surface of the cathode active material, wherein the polymerized copolymer having both electronic conductivity and ionic conductivity is poly(3,4-ethylenedioxythiophene)-block-poly(ethylene glycol) (PEDOT-PEG), and wherein the metal oxide is coated in an amount of 0.1 to 2.0 wt.% based on the weight of the cathode active material. [2] The surface-treated cathode active material according to claim 1, wherein the cathode active material is selected from lithium transition metal oxides and sulfur compounds. [3] The surface-treated cathode active material according to claim 1, wherein the metal oxide is one or more selected from the group consisting of Al 2 O 3 , SiO 2 TiO 2 , SnO 2 , CEO 2 , ZrO 2 , BaTiO 3 and Y 2 0 3 is. [4] The surface-treated cathode active material according to claim 1, wherein the particles of the metal oxide have an average particle diameter of 1 to 100 nm. [5] The surface-treated cathode active material according to claim 1, wherein the total thickness of the double coating is 10 to 100 nm. [6] A lithium secondary battery comprising the surface-treated cathode active material according to claim 1. [7] Use of the lithium secondary battery according to claim 6 as a battery for mobile electronics or as a battery for an electric vehicle. [8] A lithium secondary battery comprising the surface-treated cathode active material according to claim 2. [9] A lithium secondary battery comprising the surface-treated cathode active material according to claim 3. [10] A lithium secondary battery comprising the surface-treated cathode active material according to claim 5.

Citation Information

Patent Citations

  • Electrode manufacturing method

    JP2005524936A

  • Cathode Active Material for Lithium Secondary Batterywith Improved Cycle Life and Safety

    KR1020070008115A

  • Active material for lithium secondary battery,preparing method for the same and secondary batterywith the same

    KR1020070016431A

  • Cathode active materials for lithium secondary batteries, method of preparing for the same and lithium secondary batteries comprising the same

    KR1020110023067A

  • Coated particles for lithium battery cathodes

    WO2013169826A1