EROSION TESTING DEVICE, ACCELERATOR AND EROSION TESTING PROCEDURE
The erosion test device simulates real machine conditions to accurately assess thermal barrier coating erosion resistance using a combustion chamber and accelerator, addressing the limitations of existing devices.
Patent Information
- Application Number
- DE102015014407
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-11-11
- Filing Date
- 2015-11-06
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2035-11-06
AI Technical Summary
Existing erosion test devices for thermal barrier coatings in gas turbines fail to accurately evaluate erosion resistance under high-temperature, high-flow conditions without enlarging the device dimensions, as they cannot replicate the thermal and flow conditions of a real machine.
An erosion test device with a combustion chamber, erosion medium supply unit, accommodation unit, and accelerator that uses combustion gas as a carrier to simulate real machine conditions, allowing precise evaluation of thermal barrier coating erosion resistance.
The device enables precise evaluation of thermal barrier coating erosion resistance under conditions similar to a real machine, preventing device enlargement and ensuring accurate temperature and flow simulations.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to an erosion testing apparatus, an accelerator and an erosion testing method.
[0002] To improve the efficiency of a gas turbine, the temperature of a gas to be used may be set to a high value. That is, turbine elements (a turbine blade, a turbine vane, etc.) of the gas turbine are exposed to a high-temperature gas. For this reason, a thermal barrier coating (TBC) is applied to the surfaces of the turbine elements. The thermal barrier coating is formed by thermally spraying a flame-coating material, such as a ceramic-based material with low thermal conductivity, onto the surface of the turbine element serving as the flame-coating target. Since the turbine element is coated with the aforementioned thermal barrier coating, the thermal insulation properties and durability of the turbine element are improved.
[0003] The thickness of the thermal barrier coating decreases due to erosion caused by various particles contained in a fuel gas.
[0004] JP 2005-232590 A discloses a technology for improving the erosion resistance of a thermal barrier coating while maintaining low thermal conductivity. Specifically, as the thermal barrier coating, a zirconia lattice technology in the range of approximately 1.0117 to approximately 1.0148 is used, which comprises a zirconia-containing ceramic composition stabilized in a tetragonal crystal form using a metal oxide stabilizer of a stabilizing size, instead of only yttrium oxide, and has a transmittance of approximately 0.1 to 0.25.
[0005] For the above-mentioned thermal barrier coating, an evaluation test can be conducted using a test piece to confirm the above-mentioned erosion resistance.
[0006] In JP H08 - 62 114 A, in a testing apparatus for sandblasting a test piece with a powder carried by a carrier gas and measuring an abrasion loss of the test piece, a technology for heating the carrier gas to a desired temperature to perform sandblasting is proposed.
[0007] A generic erosion test device and a generic accelerator therefor are known from CN 1 03 063 563 A. In this device, the fuel gas with the accelerated erosion medium is introduced horizontally from a combustion chamber and via the connected accelerator into a housing for a test piece and blasted horizontally against the surface of the test piece arranged vertically in the housing.
[0008] US 2013 / 0 306 154 A1 describes a process and a suitable test device for generating a collision under controlled environmental conditions between an accelerated unidirectional horizontal gas / particle stream and a vertically arranged target object. Cooling of a test object carrier with cooling air is provided.
[0009] In the above-mentioned test apparatus disclosed in JP H08-62114 A, the carrier gas can be heated to approximately 800°C, which is approximately the melting temperature of a base material of the test piece. However, the carrier gas cannot be heated to a temperature exceeding the melting temperature of the base material. This is because a heat exchanger is used as the carrier gas heating unit. In the test apparatus disclosed in JP H08-62114 A, a flow rate of the carrier gas cannot be sufficiently increased because a gas cylinder is used as the carrier gas supply source.
[0010] For this reason, for example, when testing the thermal barrier coating of a high output gas turbine using a high flow rate fuel gas at a temperature of approximately 1500°C, the erosion resistance of the thermal barrier coating cannot be accurately evaluated because the thermal barrier coating cannot be tested under the same boundary conditions as a real machine.
[0011] In order to obtain a fuel gas with a high temperature and a high flow rate while taking into account the use of a combustion chamber of a real engine, the device would be enlarged in size.
[0012] The present invention is directed to providing an erosion testing apparatus, an accelerator, and an erosion testing method capable of accurately evaluating erosion resistance of a thermal barrier coating of a test piece while preventing an increase in the size of the apparatus.
[0013] According to the present invention, an erosion testing apparatus comprises the features of claim 1, including a combustion chamber configured to mix and combust compressed air and a fuel to obtain a fuel gas; and an erosion medium supply unit configured to supply an erosion medium to the fuel gas. The erosion testing apparatus further includes an accommodation storage unit configured to accommodate and store a test piece having a front surface coated with a thermal barrier coating; and an accelerator configured to accelerate the fuel gas with the erosion medium to collide with the test piece.
[0014] According to the above-mentioned configuration, the fuel gas of the combustion chamber can be used as a carrier gas of the erosion medium. For this reason, the temperature of the test piece is heated to the same temperature as that of the turbine element of the actual engine. Furthermore, the fuel gas comprising the erosion medium and burned by the combustion chamber can be accelerated by the accelerator and then collided with the test piece. Accordingly, the flow velocity of the fuel gas can be increased to the same flow velocity as that of the fuel gas of the actual engine by using the compact combustion chamber. That is, the boundary condition of the thermal barrier coating of the test piece can be the same as the boundary condition of the thermal barrier coating in the actual engine.
[0015] As a result, the erosion resistance of the thermal barrier coating of the test piece can be accurately evaluated while preventing any increase in dimensions.
[0016] According to the present invention, the erosion testing apparatus includes a cooling unit configured to blow a coolant to a rear surface of the test piece to cool the test piece.
[0017] According to the above-mentioned configuration, the base material of the test piece coated with the thermal barrier coating can be cooled. Therefore, the same temperature distribution as the temperature distribution in the thickness direction of the turbine element of the actual engine can be generated in the test piece.
[0018] According to the present invention, in the erosion test apparatus, the accelerator is connected to the combustion chamber. The erosion test apparatus further comprises a throttling section and a straight pipe section. The throttling section is tubular with a flow path cross-sectional area that gradually decreases downstream in the direction in which the fuel gas flows. The straight pipe section is tubular with a constant flow path cross-sectional area.
[0019] In this way, the flow velocity of the fuel gas can be increased evenly by gradually reducing the flow path cross-sectional area of the throttling section. Furthermore, the fuel gas can be rectified at an increased flow velocity by installing the straight pipe section to further accelerate the fuel gas. Therefore, the erosion medium can efficiently collide with the test piece while sufficiently increasing the flow velocity of the fuel gas.
[0020] According to a preferred embodiment of the present invention, in the erosion testing apparatus, the combustion chamber may comprise an air supply unit configured to supply air to a fuel gas for temperature adjustment.
[0021] According to the above-mentioned configuration, temperature-adjusting air can be supplied to the fuel gas to reduce the temperature of the fuel gas. Therefore, the temperature of the thermal barrier coating of the test piece can be easily adjusted to a desired temperature by increasing or decreasing the supply amount of temperature-adjusting air.
[0022] According to a preferred embodiment of the present invention, in the erosion testing apparatus, the accommodation storage unit may include an observation window in communication with an accommodation space configured to accommodate the test piece.
[0023] According to the above-mentioned configuration, a state of the test piece during the erosion test can be observed through the observation window. Therefore, the generation of a deviation between a boundary condition of the test piece and a boundary condition of the real machine can be suppressed.
[0024] According to the present invention, an accelerator comprises the features of claim 4, including, among others, a tubular throttling section having a flow path cross-sectional area that gradually decreases downstream; and a straight pipe section extending downstream in a straight pipe shape with a constant flow path cross-sectional area from a downstream end portion of the throttling section. An upstream end portion of the throttling section is connected to a combustion chamber configured to mix and combust compressed air and a fuel to obtain a fuel gas. A downstream end of the straight pipe section is connected to an accommodation storage unit configured to accommodate and store a test piece having a front surface coated with a thermal barrier coating.
[0025] According to the above-mentioned configuration, the flow velocity of the fuel gas in the combustion chamber can be increased uniformly, and the fuel gas with the increased flow velocity can be rectified. Therefore, the erosion medium can efficiently collide with the test piece while sufficiently increasing the flow velocity of the fuel gas.
[0026] According to the present invention, an erosion test method comprises the features of claim 5, including, among others, supplying an erosion medium to a fuel gas obtained by mixing and burning compressed air and a fuel, accelerating a flow velocity of the fuel gas with the erosion medium by gradually reducing a flow path cross-sectional area, and then causing the fuel gas to collide with a test piece to which a thermal barrier coating is performed.
[0027] According to the above-mentioned configuration, the erosion test can be performed under the same conditions as the turbine element of the actual engine using a device that is sufficiently smaller than the actual gas turbine engine. Therefore, the evaluation of the thermal barrier coating can be performed easily and accurately.
[0028] According to the erosion test apparatus, accelerator and erosion test method, the thermal barrier coating of the gas turbine can be accurately evaluated using the fuel gas with a high temperature and a high flow rate while preventing an increase in the size of the apparatus. Fig. 1 is a partially cross-sectional perspective view of a test piece according to an embodiment of the present invention; Fig. 2 is a partial cross-sectional view showing a configuration of an erosion testing apparatus according to the embodiment of the present invention; Fig. 3 is an enlarged cross-sectional view of a bearing portion main body according to the embodiment of the present invention; Fig. 4 is a view for describing an example of a shape of an accelerator according to the embodiment of the present invention; and Fig. Figure 5 is a diagram in which a vertical axis represents a particle velocity (m / s) and a horizontal axis represents an acceleration distance (m).
[0029] Hereinafter, an erosion testing apparatus, an accelerator, and an erosion testing method according to an embodiment of the present invention will be described with reference to the accompanying drawings.
[0030] Fig. 1 is a partially cross-sectional perspective view of a test piece according to the embodiment of the present invention.
[0031] As in Fig. As shown in FIG. 1, a test piece 1 is formed by modeling a surface of a turbine blade of a gas turbine. The test piece 1 is formed from a base material 10 and a thermal barrier coating layer 11. The test piece 1 according to the embodiment is disk-shaped.
[0032] The base material 10 is formed of a heat-resistant alloy, such as a Ni (nickel)-based alloy or the like.
[0033] The thermal barrier coating layer 11 is formed on a surface of the base material 10. The thermal barrier coating layer 11 comprises a bond coating layer 12 and a top coating layer 13.
[0034] The bond coating layer 12 prevents the upper coating layer 13 from peeling off the base material 10. The bond coating layer 12 is a metal bond layer with good corrosion resistance and oxidation resistance. For example, the bond coating layer 12 is formed by thermally spraying a metal spray powder of an MCrAlY alloy, which serves as a flame coating material, on the surface of the base material 10. "M" of the MCrAlY alloy constituting the bond coating layer 12 represents a metal element. The metal element "M" is, for example, a single metal element or a combination of two or more elements, such as NiCo, Ni, Co, or the like.
[0035] The upper coating layer 13 is deposited on the surface of the bonding coating layer 12. The upper coating layer 13 is formed by spraying a flame coating material containing a ceramic onto the surface of the bonding coating layer 12. The upper coating layer 13 according to the embodiment is formed to have a permeability (a pore occupancy rate per unit volume) of, for example, approximately 8 to 15%. A zirconia-based ceramic can be used as the flame coating material when forming the upper coating layer 13. As the zirconia-based ceramic, yttria-stabilized zirconia (YSZ) and ytterbia-stabilized zirconia (YbSZ), which serves as zirconia (ZrO2) partially stabilized by ytterbium oxide (Yb2O3), or the like, are provided.In the test piece 1 according to the embodiment, the thermal barrier coating layer 11 is disposed on a front surface thereof, and the base material 10 is disposed on a rear surface thereof. That is, a metal constituting the base material 10 is exposed on the rear surface side of the test piece 1. For example, a thickness of the base material 10 according to the embodiment may be equal to a thickness of the base material of the turbine blade of the gas turbine, which is an actual engine.
[0036] Fig. 2 is a partial cross-sectional view showing a configuration of an erosion testing apparatus according to the embodiment of the present invention.
[0037] As in Fig. As shown in Figure 2, an erosion test apparatus 20 includes a combustion chamber 21, an erosion medium supply unit 22, a storage unit 23, and an accelerator 24. The erosion test apparatus 20 is a device for causing an erosion medium (powder) carried by a carrier gas to collide with the aforementioned test piece 1. A user can evaluate erosion characteristics of the thermal barrier coating layer 11 by measuring abrasion losses of the test piece 1 tested by the erosion test apparatus 20.
[0038] The combustion chamber 21 mixes a fuel with the air compressed by a compressor (not shown) and burns the mixed fuel. A fuel gas G burned by the combustion chamber 21 becomes a carrier gas of the erosion medium. The combustion chamber 21 includes an air supply unit 25 that can supply the compressed air from the outside to the fuel gas G. The air supply unit 25 can precisely adjust the air content supplied to the fuel gas G using an electromagnetic valve or the like. According to the air supply unit 25, for example, a temperature of the fuel gas G can be reduced because the air content supplied to the fuel gas G is increased.
[0039] The combustion chamber 21 is arranged above the storage unit 23 by a frame 26. The combustion chamber 21 is mounted on the frame 26 by an inlet port 21a directed downward so that the fuel gas G is directed downward in a vertical direction. The combustion chamber 21 includes a container 21b with good thermal insulation, and thermal energy of the fuel gas G is prevented from being released to the outside via the container 21b.
[0040] The erosion medium supply unit 22 supplies the erosion medium to the fuel gas G. The erosion medium supply unit 22 is mounted on the combustion chamber 21. The erosion medium supply unit 22 connects the erosion medium to the fuel gas G by quantitatively supplying the erosion medium housed in a container (not shown) or the like. For example, the erosion medium can be indirectly supplied to the fuel gas G by combining the erosion medium with compressed air before combustion. For example, quartz sand, alumina, fly ash, or the like can be used as the erosion medium.
[0041] The accommodation storage unit 23 accommodates the test piece 1 having a surface covered by the thermal barrier coating layer 11 in a state in which the test piece 1 is stored from below. The accommodation storage unit 23 includes a chamber 27 and a storage section main body 28.
[0042] The chamber 27 forms an accommodation space S configured to accommodate the test piece 1. Wall portions 29 forming the chamber 27 are formed of the same material with good thermal insulation as the container 21b of the aforementioned combustion chamber 21. That is, the chamber 27 can keep the accommodation space S warm by thermally insulating the wall portion 29. The wall portion 29 and the container 21b ensure thermal insulation by forming the wall portion 29 and the container 21b using a heat-insulating material or by attaching a heat-insulating material to a frame (not shown).
[0043] Fig. 3 is an enlarged cross-sectional view of the bearing portion main body according to the embodiment of the present invention.
[0044] As in Fig. 2 and Fig. As shown in Figure 3, the support section main body 28 cools the base material 10 exposed on the rear surface side of the test piece 1 while supporting the test piece 1 from below. The support section main body 28 includes a cooling air supply unit 31 and a support ring section 32.
[0045] The cooling air supply unit 31 blows the cooling air supplied from the outside against the base material 10. The cooling air supply unit 31 comprises an air supply pipe 33 and a box body 34.
[0046] The air supply pipe 33 runs through a side wall 27a (see Fig. 2) of the chamber 27. The air supply pipe 33 is tubular and extends toward a center of the accommodation space S in a horizontal direction. The cooling air supplied from the outside to the center of the accommodation space S flows through the air supply pipe 33. One end portion of the air supply pipe 33 is connected to the side wall of the box body 34.
[0047] The box body 34 changes the direction of the cooling air supplied through the air supply pipe 33 to the rear surface of the test piece 1. In the box body 34 according to the embodiment, only one upper wall 34a is formed from a stamped metal, a mesh, or the like with a plurality of holes. Accordingly, the cooling air flowing into the box body 34 from the air supply pipe 33 is discharged upward through the holes in the upper wall 34a.
[0048] The bearing ring portion 32 is formed in a ring shape and protrudes upward from an upper wall peripheral edge of the box body 34 of the cooling air supply unit 31. The test piece 1 is held by the bearing ring portion 32. Bolt coupling, welding, or the like is used as a holding method of the test piece 1. Accordingly, the test piece 1 is supported by the bearing ring portion 32 from below in a posture parallel to the upper wall 34a, while the test piece 1 is spaced a predetermined distance from the upper wall 34a of the box body 34. The cooling air supply unit 31 may include a temperature detection unit, such as a thermocouple or the like, installed in a flow path through which the cooling air flows. Accordingly, a flow rate of the cooling air can be adjusted according to the temperature of the cooling air detected by the temperature detection unit to control a temperature distribution in a thickness direction of the test piece 1.
[0049] The air supply pipe 33, the box body 34 and the bearing ring portion 32 constituting the above-mentioned bearing portion main body 28 have not only a function as a duct configured to supply the cooling air, but also a function as a hinge support configured to support the test piece 1 from below.
[0050] The accommodation storage unit 23 includes an observation window portion 35 communicating with the accommodation space S in which the test piece 1 is accommodated. The observation window portion 35 extends in a radial direction around the test piece 1, which is supported by the storage portion main body 28. A thermal viewer TV (“thermo viewer”) capable of detecting the temperature distribution of the test piece 1 is attached to the observation window portion 35 according to the embodiment. In the embodiment, the case in which only one observation window portion 35 is formed on the accommodation storage unit 23 is exemplified. However, a plurality of observation window portions 35 may be formed with respect to the accommodation storage unit 23.
[0051] An observation device other than the thermal viewer TV may be attached to the observation window portion 35.
[0052] In Fig. 3, the above-mentioned bearing ring portion 32 includes, for example, a notch (not shown) or the like, such that the cooling air colliding with the rear surface of the test piece 1 is discharged into the accommodation space S. An erosion medium discharge mechanism (not shown) configured to discharge the erosion medium blown to the test piece 1 is installed on the accommodation bearing unit 23. The erosion medium blown to the test piece 1 is sucked to be discharged to the outside of the chamber 27 by the erosion medium discharge mechanism.
[0053] The accelerator 24 accelerates a flow velocity of the fuel gas G with the erosion medium to cause the fuel gas G to collide with the test piece 1. As shown in Fig. 2, the accelerator 24 includes a throttling section 36 and a straight pipe section 37.
[0054] In the throttling portion 36, an upstream end portion in a direction in which the fuel gas G flows is connected to the combustion chamber 21. The throttling portion 36 is tubularly formed with a flow path cross-sectional area that gradually decreases downstream in a direction in which the fuel gas G flows. In the throttling portion 36 according to the embodiment, the flow path cross-sectional area is reduced at a constant inclination angle.
[0055] The straight tube section 37 is formed in a straight tube shape with a constant flow path cross-sectional area. The straight tube section 37 connects a downstream end section 36a of the throttling section 36 and the accommodation storage unit 23. Specifically, the straight tube section 37 extends from the downstream end section 36a of the throttling section 36 into the interior of the accommodation space S of the accommodation storage unit 23. A downstream end section 37a of the straight tube section 37 is disposed directly above the test piece 1. The straight tube section 37 is disposed such that an axis O1 thereof is perpendicular to the front surface of the test piece 1 housed in the accommodation storage unit 23. That is, the accelerator 24 brings an interior space S1 of the combustion chamber 21 into communication with the accommodation space S of the accommodation storage unit 23.
[0056] Fig. 4 is a view for describing an example of a shape of the accelerator according to the embodiment of the present invention. Fig. Figure 5 is a diagram in which a vertical axis represents a particle velocity (m / s) and a horizontal axis represents an acceleration distance (m).
[0057] As in Fig. As shown in Figure 4, an inclination angle θ of the throttling portion 36 according to the embodiment is designed to be larger than an angle of repose of the erosion medium. Here, the inclination angle θ is an angle with respect to a horizontal plane perpendicular to the axis O1.
[0058] An inner diameter D2 of the straight pipe section 37 is set to a large value based on an amount of exhaust gas from the combustion chamber 21 such that a flow velocity in an outlet port of the straight pipe section 37 is smaller than a speed of sound. For example, assuming that the amount of exhaust gas “Q” (m 3 / s) and the sound speed of the exhaust gas “Vc” (m / s), when a load of the combustion chamber 21 is 100%, the inner diameter D2 can be obtained by the following equation (1). D2=(Q / Vc×4 / π)0.5
[0059] The straight pipe section 37 is designed to have a length L such that a particle velocity of the erosion medium reaches a desired value.
[0060] For example, in the case where a gas flow velocity of the straight pipe section 37 is 600 m / s and a particle diameter of the erosion medium is 100 µm, when a target value of the particle velocity of the erosion medium is set to 200 m / s, the length L (= acceleration distance) of the straight pipe section 37 is preferably about 0.5 m, as shown in Fig. 5 is shown.
[0061] When a gas flow velocity of the throttling portion 36 is “V1” and a gas flow velocity of the straight pipe portion 37 is “V2”, the following equation (2) is satisfied. V1 / V2=D2 / D1
[0062] As shown in the diagram in Fig.As shown in Figure 5, in a region where an acceleration distance approaches "0" (e.g., a range from 0 to 1 m), the acceleration distance is increased to suddenly increase the particle velocity of the erosion medium. In other words, in the region where the acceleration distance approaches "0", an increase rate of the particle velocity is increased. However, in the environment where the acceleration distance exceeds 1 m, the increase rate of the particle velocity is suddenly reduced, while a deviation of the particle diameter occurs. In other words, when the acceleration distance exceeds 1 m, the particle velocity cannot be easily increased even if the acceleration distance is increased. That is,, in the range of acceleration distance in which the rate of increase of the particle velocity is large, if the length L of the straight pipe section 37 is adjusted, the particle velocity can be efficiently increased while preventing elongation of the straight pipe section 37.
[0063] Next, an erosion test method by the erosion test apparatus 20 according to the embodiment will be described.
[0064] First, the test piece 1 is prepared with the thermal barrier coating layer 11 on or on the front surface of the base material 10.
[0065] Further, the test piece 1 is adjusted with respect to the bearing section main body 28.
[0066] Thereafter, the erosion medium having a desired particle diameter is placed in the container of the erosion medium supply unit 22 in advance.
[0067] Then, the erosion test device 20 is driven. Then, the compressed air and fuel are combusted in a mixed state in the combustion chamber 21, and high-temperature fuel gas G serving as a carrier gas (i.e., high-temperature fuel gas) is generated. Further, the compressed air is supplied to the high-temperature fuel gas G via the air supply unit 25 to adjust its temperature, and the erosion medium is quantitatively supplied.
[0068] The cooling air is blown from the rear surface to the test piece 1 arranged in the accommodation space S of the accommodation storage unit 23 via the cooling air supply unit 31. Accordingly, cooling of the base material 10 is continued.
[0069] In this state, the fuel gas G containing a certain amount of the erosion medium flows into the accelerator 24 to be accelerated to a flow rate at which the erosion medium reaches a target speed. The erosion medium accelerated to the target speed by the accelerator 24 sequentially collides with the thermal barrier coating layer 11 of the test piece 1 held by the accommodation space S, particularly the upper coating layer 13. Here, the temperature adjustment of the fuel gas G and the temperature adjustment of the test piece 1 by the cooling air are performed such that the temperature distribution of the test piece 1 is observed through the thermal observer TV by a user, so that the same temperature distribution as that of the actual machine is achieved.
[0070] After this state has been continued for a predetermined time, the user stops the erosion testing device 20, extracts the test piece 1 from the accommodation storage unit 23, and evaluates an abrasion state or the like generated due to the upper coating layer 13 or the like.
[0071] Accordingly, according to the above-mentioned embodiment, the fuel gas G of the combustion chamber 21 can be used as the carrier gas of the erosion medium. For this reason, the temperature of the test piece 1 can be heated to the same temperature as that of the turbine element of the actual engine. The fuel gas G containing the erosion medium can collide with the test piece 1 after being accelerated by the accelerator 24. Accordingly, the flow velocity of the fuel gas G containing the erosion medium can be increased to the same flow velocity as that of the fuel gas of the actual engine by using the compact combustion chamber 21. That is, a boundary condition of the thermal barrier coating layer 11 of the test piece 1 can be equal to a boundary condition of the thermal barrier coating in the actual engine.Accordingly, the erosion resistance of the thermal barrier coating layer 11 of the test piece 1 can be accurately evaluated while preventing an increase in the size of the device.
[0072] Furthermore, since the cooling air supply unit 31 is provided, the base material 10 of the test piece 1 coated with the thermal barrier coating layer 11 can be cooled. Therefore, the same temperature distribution as the temperature distribution in the thickness direction of the turbine element of the actual engine can be generated in the test piece 1. Consequently, the erosion resistance of the test piece 1 with respect to the thermal barrier coating layer 1 can be more accurately evaluated.
[0073] Furthermore, in the accelerator 24, the flow velocity of the fuel gas can be increased uniformly because the flow path cross-sectional area of the throttling portion 36 is gradually reduced. Furthermore, because the straight pipe portion 37 is installed, the fuel gas G can be rectified with the flow velocity increased by the throttling portion 36 to further accelerate the fuel gas G. Consequently, the erosion medium can efficiently collide with the test piece 1 while sufficiently increasing the flow velocity of the fuel gas G.
[0074] Furthermore, the temperature adjustment air may be supplied to the fuel gas G to reduce the temperature of the fuel gas G. For this reason, since the supply amount of the temperature adjustment air is increased or decreased, the temperature of the thermal barrier coating layer 11 of the test piece 1 can be easily adjusted to a desired temperature.
[0075] Furthermore, a state of the test piece 1 during the erosion test can be observed through the observation window section 35. For this reason, generation of a deviation between the boundary condition of the test piece 1 and the boundary condition of the real machine can be suppressed.
[0076] The present invention is not limited to the above-mentioned embodiment, but various modifications may be added to the above-mentioned embodiment.
[0077] For example, in the above-mentioned embodiment, the case where the support portion main body 28 functions as the cooling unit configured to cool the test piece 1 has been described. However, the embodiment is not limited to the above-mentioned configuration, but, for example, a mechanism configured to hold the test piece 1 and a mechanism configured to supply the cooling air may be installed separately from each other.
[0078] Furthermore, in the above-mentioned embodiment, the case where the cooling air supply unit includes the air supply pipe 33 and the box body 34 has been described. However, the air supply pipe 33 may be curved such that the opening portion of the air supply pipe 33 is directed toward the test piece 1, and the cooling air may be blown from the air supply pipe 33 toward the test piece 1.
[0079] The present invention can be applied to the erosion test apparatus, the accelerator and the erosion test method, and the erosion resistance of the thermal barrier coating of the test piece can be accurately evaluated while preventing an increase in the size of the apparatus. List of reference symbols 1 test piece 10 Basic material 11 thermal barrier coating layer 12 Compound coating layer 13 upper coating layer 20 Erosion test device 21 Combustion chamber 21a Inlet connection 21b Container 22 Erosion medium supply unit 23 Accommodation Storage Unit 24 accelerators 25 Air supply unit 26 frames 27 Chamber 27a side wall 28 Bearing section main body 29 wall section 31 Cooling air supply unit 32 bearing ring section 33 Air supply pipe 34 box bodies 34a upper wall 35 observation window section 36 throttling section 36a downstream end section 37 Straight pipe section 37a downstream end section S accommodation room S1 interior G Fuel gas O1 axis TV thermal viewer
Claims
[1] Erosion test device (20), comprising: a combustion chamber (21) configured to mix and burn compressed air and a fuel to obtain a fuel gas (G), an erosion medium supply unit (22) configured to supply an erosion medium to the fuel gas (G), an accommodation storage unit (23) configured to accommodate and store a test piece (1) having a front surface coated by a thermal barrier coating (11), an accelerator (24) configured to accelerate the fuel gas (G) with the erosion medium to collide it with the test piece (1), and a cooling unit configured to cool the test piece (1), wherein the accelerator (24) comprises: a tubular throttling portion (36) connected to the combustion chamber (21) and having a flow path cross-sectional area that gradually decreases downstream in a direction in which the fuel gas (G) flows, and a straight pipe section (37) which is formed in a straight pipe shape with a constant flow path cross-sectional area and connects a downstream end section (36a) of the throttling section (36) and the accommodation bearing unit (23), wherein the straight pipe section (37) extends from the downstream end section (36a) of the throttling section (36) into the interior of an accommodation space (S) of the accommodation storage unit (23), characterized by , that the cooling unit is configured to blow a coolant upwards to a rear surface of the test piece (1), and a downstream end portion (37a) of the straight pipe portion (37) is arranged directly above the test piece (1). [2] The erosion testing apparatus (20) according to claim 1, wherein the combustion chamber (21) comprises an air supply unit (25) configured to supply air to the fuel gas (G) for temperature adjustment. [3] The erosion testing apparatus (20) according to claim 1 or 2, wherein the accommodation storage unit (23) has an observation window (35) communicating with the accommodation space (S) configured to accommodate the test piece (1). [4] Accelerator (24), comprising: a tubular throttling section (36) having a flow path cross-sectional area that gradually decreases downstream, and a straight pipe section (37) extending in a straight pipe shape with a constant flow path cross-sectional area downstream from a downstream end section (36a) of the throttling section (36), wherein an upstream end portion of the throttling portion (36) is connected to a combustion chamber (21) configured to mix and burn compressed air and a fuel to obtain a fuel gas (G), and a downstream end of the straight pipe section (37) is connected to an accommodation storage unit (23) configured to accommodate and store a test piece (1) having a front surface coated by a thermal barrier coating (11), wherein the straight pipe section (37) extends from the downstream end section (36a) of the throttling section (36) into the interior of an accommodation space (S) of the accommodation storage unit (23), characterized by, that a downstream end portion (37a) of the straight pipe portion (37) is arranged directly above the test piece (1). [5] Erosion test method, comprising: Supplying an erosion medium to a fuel gas (G) obtained by mixing and burning compressed air and a fuel, Blowing a coolant upwards to a rear surface of a test piece (1) on which a thermal barrier coating (11) is formed to cool the test piece (1), Accelerating a flow velocity of the fuel gas (G) with the erosion medium by gradually reducing a flow path cross-sectional area, and Causing the fuel gas (G) with the accelerated erosion medium to collide with the test piece (1) on which the thermal barrier coating (11) is formed, wherein the fuel gas (G) with the accelerated erosion medium passes through a straight pipe section (37) which is formed in a straight pipe shape with a constant flow path cross-sectional area, and a downstream end section (37a) of the straight pipe section (37) is arranged directly above the test piece (1).
Citation Information
Patent Citations
Testing device for simulation and real-time detection of high-temperature deposition corrosion of thermal barrier coatings
CN103063563A
High temperaure blast erosion test equipment
JP1996062114A
Thermal barrier coating with improved impact and erosion resistance
JP2005232590A
Process to Create a Collision Between a Stream of Gas and Particles and a Target
US20130306154A1