Vehicle tires
A sulfur-crosslinkable rubber mixture for vehicle tire treads, comprising butadiene-acrylonitrile copolymer, plasticizer, and silica, addresses the conflict between wet braking and rolling resistance, enhancing both properties without compromising winter performance.
Patent Information
- Application Number
- DE102015214731
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2015-08-03
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2035-08-03
AI Technical Summary
Existing rubber compounds for vehicle tire treads face a conflict between improving wet braking and rolling resistance, with previous formulations either enhancing one property at the expense of the other, and there is a need for a formulation that maintains winter properties like traction on snow and dry braking behavior.
A sulfur-crosslinkable rubber mixture for vehicle tire treads containing 30 to 100 phr of butadiene-acrylonitrile copolymer, 35 to 70 phr of plasticizer, and 40 to 250 phr of silica, optimized to improve the trade-off between rolling resistance and wet grip without negatively affecting winter properties.
The rubber mixture achieves improved rolling resistance and wet grip performance while maintaining comparable traction on snow and dry braking behavior, with enhanced processability and reduced heat build-up.
Abstract
Description
[0001] The invention relates to a vehicle tire, in particular its tread.
[0002] The rubber composition of the tread largely determines the driving characteristics of a tire, especially a vehicle tire. Likewise, the rubber compounds used in belts, hoses and straps Used especially in areas subject to high mechanical stress, for stability and longevity of these Rubber products are essentially responsible for these rubber compounds. Therefore, these rubber compounds are used for vehicle tires, belts, Belts and hoses are subject to very high demands.
[0003] To influence the mixture and vulcanizate properties, the mixtures are given a wide variety of Aggregates are added and / or special polymers are used. Examples of aggregates include at this point fillers (e.g. carbon black), plasticizers, anti-aging agents and cross-linking systems made of sulfur, Accelerators and activators are called additives. If a property is improved by varying the mixture, this is often with a deterioration of another property, so that certain conflicting objectives exist. In the case of mixtures for In the case of vehicle tyre treads, such conflicting objectives exist, for example, with regard to abrasion behaviour and increased heat build-up, which results in poorer rebound elasticity and consequently poorer rolling resistance.
[0004] EP 0824567 B1 discloses a rubber mixture for treads of vehicle tires containing 10 phr nitrile Butadiene rubber (NBR) and carbon black as the main filler and silica as a further filler in quantities of 13.3 phr. Such a rubber compound shows an improvement in wet traction predictors at constant or deteriorated rolling resistance predictors.
[0005] DE 69213002 T2 discloses a rubber mixture containing 10 or 15 phr NBR and carbon black as filler. Such a rubber compound shows good physical properties, with an amount of 15 phr NBR and above the Rolling resistance predictors have deteriorated.
[0006] JP 2000-302915 A discloses a rubber mixture containing 20 or 30 phr NBR in combination with carbon black as Main filler to optimize abrasion properties at high hysteresis loss.
[0007] WO 2005056665 A1 discloses a rubber mixture containing 5, 10 or 15 phr of hydrogenated carboxylated NBR (HXNBR) and 80 phr silica or carbon black as filler. Such a rubber compound shows partially improved Wet grip indicators, partially improved rolling resistance indicators and partially improved abrasion behavior.
[0008] US 20130312892 A1 discloses a vehicle tire having a tread base plate comprising 100 phr NBR and 55 phr carbon black. Such a sub-plate is intended to prevent the migration of plasticizers from the tread into the inside the vehicle tire, while at the same time improving the handling behavior of the tire (road behavior) due to the higher stiffness and lower elongation of the sub-plate mixture.
[0009] DE 10 2006 016 915 A1 discloses rubber mixtures for tires containing an acrylonitrile-butadiene rubber, Silica and a plasticizer oil.
[0010] US 2013 / 0 312 892 A1 discloses rubber mixtures for tires containing acrylonitrile butadiene rubber and carbon black as a filler.
[0011] JP 2011-001535 A discloses cap rubber mixtures for treads containing a modified acrylonitrile Butadiene rubber and silica.
[0012] The present invention is based on the object of providing a sulfur-crosslinkable rubber mixture for Treads of vehicle tires, whose vulcanizate represents an improvement over the state of the art in With regard to the conflict of objectives between wet braking and rolling resistance, while the level of winter properties and dry braking performance is not significantly negatively affected.
[0013] This task is solved by a vehicle tire, the tread of which at least in the cap is a vulcanizate at least one sulfur-crosslinkable rubber mixture containing: - 30 to 100 phr of at least one butadiene-acrylonitrile copolymer and - At least one silica and - 35 to 70 phr of at least one plasticizer.
[0014] Surprisingly, it was found that with a comparatively high amount of the butadiene-acrylonitrile Copolymers, in a vulcanizate produced from the rubber mixture an improvement with regard to the conflict of objectives from rolling resistance and wet grip, while the other properties are not negatively affected. In particular, the winter properties properties, especially traction on snow, as well as dry braking performance remain at a comparable Level.
[0015] The components of the sulfur-curable rubber mixture are described in more detail below. Statements apply to the vehicle tire according to the invention.
[0016] The term phr (parts per hundred parts of rubber by weight) used in this document is the term used in the The dosage of the parts by weight of the individual In this document, substances are calculated as 100 parts by weight of the total mass of all substances present in the mixture. high molecular weight (weight average molecular weight Mw according to GPC from 250000 to 5000000 g / mol) and thus made of solid rubber.
[0017] The rubber mixture contains 30 to 100 phr of at least one butadiene-acrylonitrile copolymer. Butadiene-acrylonitrile- Copolymers are also called acrylonitrile butadiene rubber or nitrile butadiene rubber (NBR).
[0018] According to a preferred embodiment, the rubber mixture contains 55 to 100 phr, particularly preferably 70 to 100 phr, most preferably 85 to 100 phr, of at least one butadiene-acrylonitrile copolymer.
[0019] According to a particularly preferred embodiment, the rubber mixture contains 100 phr of at least one Butadiene-acrylonitrile copolymer (NBR) and therefore no other high-molecular rubber, which as a polymer in the 100 parts of rubber would be lost. ®
[0020] Butadiene-acrylonitrile copolymers are known to the person skilled in the art and are available, for example, under the trade names KRYNAC from Lanxess. Within the scope of the present invention, the butadiene-acrylonitrile copolymers are also NBR for short.
[0021] The NBR contained in the rubber mixture can also be carboxylated NBR (XNBR) and / or hydrogenated NBR (HNBR) and / or hydrogenated carboxylated NBR (HXNBR), as described for example in WO 2005056665 A1. A mixture of NBR and / or XNBR and / or HNBR and / or HXNBR is also conceivable.
[0022] However, the NBR contained in the rubber mixture is preferably not modified, so that it is preferably unmodified NBR.
[0023] The NBR preferably has an acrylonitrile content according to ISO 24698-1 of 15 to 50 wt.%, particularly preferably 25 to 40 wt.%, most preferably 30 to 37 wt.%.
[0024] The NBR preferably has a Mooney viscosity ML (1+4) at 100 °C (without pretreatment) according to ISO289 / ASTM D 1646 from 20 to 80 MU (mooney units ME), particularly preferably 20 to 60 MU, especially preferably 30 to 50 MU.
[0025] With an NBR with the mentioned preferred embodiments concerning acrylonitrile content and Mooney viscosity, the rubber compound shows optimized processability, especially good miscibility and a ® good extrusion properties. One such NBR is available, for example, under the trade name KRYNAC 3345 F from Available from Lanxess.
[0026] In the event that the rubber mixture contains less than 100 phr of butadiene-acrylonitrile copolymers, ie 30 to 99.9 phr, contains at least one other diene rubber.
[0027] Diene rubbers are rubbers obtained by polymerization or copolymerization of dienes and / or cycloalkenes and thus C=C double bonds either in the main chain or in the side groups have.
[0028] The further diene rubber may be natural polyisoprene and / or synthetic polyisoprene and / or epoxidized polyisoprene and / or styrene-butadiene rubber (SBR) and / or butadiene rubber (BR, polybutadiene) and / or styrene-isoprene rubber and / or halobutyl rubber and / or polynorbornene and / or isoprene-isobutylene Copolymer and / or ethylene-propylene-diene rubber and / or chloroprene rubber and / or acrylate rubber and / or Fluororubber and / or silicone rubber and / or polysulfide rubber and / or epichlorohydrin rubber and / or Styrene-isoprene-butadiene terpolymer and / or hydrogenated styrene-butadiene rubber and / or butadiene-isoprene rubber act.
[0029] In particular chloroprene rubber, butyl rubber, halobutyl rubber or ethylene-propylene-diene rubber are used in combination with nitrile rubber and / or hydrogenated acrylonitrile butadiene rubber in the production of technical rubber articles such as belts, straps and hoses, and / or shoe soles.
[0030] Preferably, the further diene rubber is selected from the group consisting of natural Polyisoprene (NR), synthetic polyisoprene (IR), styrene-butadiene rubber (SBR) and butadiene rubber (BR).
[0031] The natural and / or synthetic polyisoprene of all embodiments can be either cis- 1,4-polyisoprene as well as 3,4-polyisoprene. However, the use of cis-1,4-polyisoprene with a cis 1,4 content > 90 wt.%. On the one hand, such a polyisoprene can be prepared by stereospecific polymerization in solution with Ziegler-Natta catalysts or using finely divided lithium alkyls. Natural rubber (NR) is such a cis-1,4 polyisoprene, the cis-1,4 content in natural rubber is larger 99% by weight.
[0032] Furthermore, a mixture of one or more natural polyisoprenes with one or more synthetic Polyisoprene(s) are conceivable.
[0033] The butadiene rubber (= BR, polybutadiene) can be any type known to the person skilled in the art. These include the so-called high-cis and low-cis types, whereby polybutadiene with a cis content greater than or equal to 90 wt.% is referred to as high-cis type and polybutadiene with a cis content of less than 90 wt.% is referred to as low-cis type A low-cis polybutadiene is, for example, Li-BR (lithium-catalyzed butadiene rubber) with a cis content of 20 to 50 % by weight. With a high-cis BR, particularly good abrasion properties and low hysteresis of the rubber mixture.
[0034] The polybutadiene(s) used can be modified and functionalized end-group modified and / or functionalized along the polymer chains. The modification can be those with hydroxy groups and / or ethoxy groups and / or epoxy groups and / or siloxane groups and / or amino- Groups and / or aminosiloxane and / or carboxy groups and / or phthalocyanine groups and / or silane sulfide groups However, there are also other modifications known to the expert, also known as functionalizations Metal atoms can be a component of such functionalizations.
[0035] In the event that styrene-butadiene rubber (styrene-butadiene copolymer) is contained in the rubber mixture, It can be either solution-polymerized styrene-butadiene rubber (SSBR) or emulsion-polymerized Styrene-butadiene rubber (ESBR), although a mixture of at least one SSBR and at least one ESBR can be used. The terms ´´styrene-butadiene rubber´´ and ´´styrene-butadiene copolymer´´ are used in used synonymously in the context of the present invention.
[0036] The styrene-butadiene copolymer used can be modified with the modifications mentioned above for polybutadiene and Functionalizations can be end-group modified and / or functionalized along the polymer chains.
[0037] The rubber mixture contains at least one silica.
[0038] The terms ´´silicic acid´´ and ´´silica´´ are used in the context of the present invention, as well as in the professional world common, used synonymously.
[0039] According to a particularly preferred embodiment, the rubber mixture contains 40 to 250 phr, preferably 40 to 160 phr, particularly preferably 40 to 120 phr, of at least one silicic acid.
[0040] According to a preferred embodiment, the rubber mixture contains 40 to 70 phr, particularly preferably 50 up to 70 phr, at least one silica. This is used in the tread of vehicle tires to Improvement in rolling resistance, wet braking and dry braking achieved.
[0041] According to a further preferred embodiment, the rubber mixture contains 40 to 100 phr, especially preferably 70 to 100 phr, most preferably 75 to 87 phr, of at least one silicic acid. Use in the tread of vehicle tires improves the conflict between rolling resistance and wet braking An improvement has been achieved, with wet braking in particular being significantly improved. In the case of silicas, are the silicas known to the person skilled in the art which are suitable as fillers for tyre rubber mixtures, However, it is particularly preferred if a finely divided, precipitated silica is used, which has a 2 Nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) from 35 to 350 m / g, preferably from 60 to 2 2 2 260 m / g, particularly preferably from 120 to 230 m / g, and a CTAB surface area (according to ASTM D 3765) of 30 to 400 m 2 2 / g, preferably from 60 to 250 m / g, particularly preferably from 120 to 230 m / g.
[0042] According to a preferred development, the rubber mixture contains 1 to 20 phr, preferably 1 to 10 phr, particularly preferably 1 to 7 phr of at least one carbon black. Within the scope of the present invention, all those skilled in the art known types of carbon black are conceivable. However, a carbon black with an iodine adsorption number according to ASTM D 1510 is preferred. from 20 to 180 g / kg, particularly preferably 30 to 140 kg / g, and a DBP number according to ASTM D 2414 of 30 to 200 ml / 100 g, preferably 90 to 180 ml / 100 g, especially preferably 90 to 150 ml / 100g. A particularly suitable carbon black in the context of the present invention is For example, a carbon black of ASTM type N339 with an iodine adsorption number of 90 g / kg and a DBP number of 120 ml / 100g. This provides particularly good properties for use in vehicle tires, especially in the tread. with regard to the technical task.
[0043] The rubber mixture may contain, preferably in the smallest possible amounts, ie preferably 0 to 2 phr, further fillers Other (non-reinforcing) fillers in the context of the present invention include aluminosilicates, Kaolin, chalk, starch, magnesium oxide, titanium dioxide or rubber gels as well as fibers (such as aramid fibers, glass fibers, carbon fibers, cellulose fibers).
[0044] Further reinforcing fillers are, for example, carbon nanotubes (CNT) including discrete CNTs, so-called hollow carbon fibers (HCF) and modified CNTs containing one or more functional groups, such as Hydroxy, carboxy and carbonyl groups), graphite and graphene and so-called ´´carbon-silica dual-phase filler´´.
[0045] Zinc oxide is not one of the fillers in the context of the present invention.
[0046] The rubber mixture contains at least one plasticizer, the total amount of plasticizer being 35 to 70 Surprisingly, a comparatively high amount of 35 to 70 phr also produces very good Properties of the rubber compound with regard to the conflicting objectives of rolling resistance and wet grip.
[0047] This results in a particularly good Processability of the rubber compound, especially of the extrudates before crosslinking, with good Rolling resistance and good (and therefore low) heat build-up.
[0048] The plasticizers used in the present invention include all those known to the person skilled in the art Plasticizers such as synthetic plasticizers based on esters or ethers or aromatic, naphthenic or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate) or RAE (Residual Aromatic Extract) or TDAE (treated distillate aromatic extract), or rubber-to-liquid oils (RTL) or biomass-to-liquid oils (BTL) preferably with a Polycyclic aromatics content of less than 3% by weight according to method IP 346 or rapeseed oil or factice or resins, such as rosin or coumarone-indene resins or adhesive resins such as Koresin, or liquid polymers whose average Molecular weight (determination by GPC = gel permeation chromatography, based on BS ISO 11344:2004) between 500 and 20000 g / mol. If additional liquid polymers are used as plasticizers in the rubber mixture, These are not included as rubber in the calculation of the composition of the polymer matrix.
[0049] However, naphthenic or paraffinic mineral oil plasticizers are not suitable for use in the automotive industry due to their low compatibility with NBR is preferably contained only in small quantities of 0 to 5 phr.
[0050] Preferably, a synthetic plasticizer based on ester or ether is used. Such plasticizers are ® ® ® ® Available under the trade names Vulkanol 81, Vulkanol 85, Vulkanol 88, Vulkanol 90 from Lanxess. ®
[0051] The plasticizer is thus preferably selected from the group consisting of ether thioethers (e.g. Vulkanol ® 85), mixtures of thio- and carboxylic acid esters (e.g. Vulkanol 81), methylene-bis-thioglycolic acid butyl ester (e.g. Vulkanol ® ® 88), thiodiglycolic acid di-2-ethylhexyl ester (e.g. Vulkanol 90), aromatic polyethers and polyglycol ethers, where Methylenebis-thioglycolic acid butyl ester is particularly preferred. According to a preferred embodiment of the invention the amount of methylene-bis-thioglycolic acid butyl ester is 35 to 70 phr. Surprisingly, with a comparatively high amount of 35 to 70 phr also very good properties of the rubber compound with regard to the conflicting objectives of rolling resistance and wet grip.
[0052] The plasticizer(s) are preferably used in the production of the rubber mixture in at least one Basic mixing stage added.
[0053] To improve the processability and to bind the silica and other polar Silane coupling agents can be used in rubber compounds by adding fillers to the diene rubber. One or more different silane coupling agents can be used in combination. Rubber compounds can therefore contain a mixture of different silanes. The silane coupling agents react with the surface silanol groups of the silica or other polar groups during mixing of the rubber or the rubber mixture (in situ) or even before the addition of the filler to the rubber in the sense of a Pretreatment (premodification). Silane coupling agents that can be used are all Silane coupling agents known to those skilled in the art for use in rubber compounds can be used. Coupling agents known in the art are bifunctional organosilanes which contain at least have an alkoxy, cycloalkoxy or phenoxy group as a leaving group and which have as other functionality a group which, after cleavage, may enter into a chemical reaction with the double bonds of the polymer The latter group can include, for example, the following chemical groups: -SCN, -SH, -NH or -S - (with x = 2 to 8). 2 x
[0054] Thus, as silane coupling agents, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl)polysulfides with 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfide (TESPD) or mixtures of the sulfides with 1 to 8 sulfur atoms with different contents of the various sulphides. TESPT can also be used as Mixture with carbon black (trade name X50S® from Evonik) can be added. A silane mixture is preferred. which contains 40 to 100 wt.% disulfides, particularly preferably 55 to 85 wt.% disulfides and especially preferably contains 60 to 80 wt.% disulfides. Such a mixture is available, for example, under the trade name Si 261® from Evonik, which is described in DE 102006004062 A1. Blocked mercaptosilanes, such as those from WO 99 / 09036 can be used as silane coupling agents. Silanes, such as those described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1 and WO 2008 / 083244 A1 can For example, silanes known under the name NXT (e.g. 3-(octanoylthio)-1-propyl-triethoxysilane) in various versions from Momentive, USA, or those sold under the name VP Si 363® by distributed by Evonik Industries.
[0055] Furthermore, the rubber mixture may contain further activators and / or agents for the binding of fillers, especially carbon black. This can be, for example, the compound S- disclosed in EP 2589619 A1. (3-Aminopropyl)thiosulphuric acid and / or its metal salts, which, especially when combined with at least one carbon black as a filler results in very good physical properties of the rubber mixture.
[0056] The silanes and activators mentioned for binding fillers are used in the production of Rubber mixture preferably added in at least one basic mixing stage.
[0057] Furthermore, the rubber mixture may contain conventional additives in conventional parts by weight, which Production preferably in at least one basic mixing stage. These additives include a) Anti-aging agents such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl- p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) Activators, such as zinc oxide and fatty acids (e.g. stearic acid) or zinc complexes such as Zinc ethylhexanoate c) waxes, d) mastication aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD) and e) processing aids, such as fatty acid salts, such as zinc soaps, and fatty acid esters and their derivatives.
[0058] The proportion of the total amount of further additives is 3 to 150 phr, preferably 3 to 100 phr and particularly preferably 5 to 80 phr.
[0059] The total amount of the other additives contains 0.1 to 10 phr, preferably 1 to 8 phr, especially preferably 1.5 to 4 phr, zinc oxide (ZnO).
[0060] This can be any type of zinc oxide known to the person skilled in the art, such as ZnO granules or - 2 Powder. The zinc oxide commonly used typically has a BET surface area of less than 10 m / g. 2 However, it can also be a zinc oxide with a BET surface area of 10 to 100 m / g, such as so-called ´´nano-zinc oxides´´, be used.
[0061] It is common practice to add zinc oxide as a vulcanization accelerator to a rubber mixture for sulfur crosslinking. The activator is usually added in combination with fatty acids (e.g. stearic acid). The sulfur is then Complex formation activated for vulcanization.
[0062] The vulcanization of the sulfur-crosslinkable rubber mixture is carried out in the presence of sulfur and / or Sulphur donors with the help of vulcanization accelerators, whereby some vulcanization accelerators can also act as a sulfur donor. The accelerator is selected from the group consisting of Thiazole accelerators and / or mercapto accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or thiuram accelerators and / or thiophosphate accelerators and / or Thiourea accelerators and / or xanthate accelerators and / or guanidine accelerators.
[0063] Preference is given to using a sulfenamide accelerator selected from the group consisting of N- Cyclohexyl-2-benzothiazolesufenamide (CBS) and / or N,N-Dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or Benzothiazyl-2-sulfenemorpholide (MBS) and / or N-tert-butyl-2-benzothiazylsulfenamide (TBBS).
[0064] As a sulphur-donating substance, all sulphur-donating substances known to the person skilled in the art If the rubber mixture contains a sulfur-donating substance, this is preferably selected from the group containing e.g. thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD) and / or Tetramethylthiuram disulfide (TMTD) and / or tetraethylthiuram disulfide (TETD), and / or thiuram tetrasulfides, such as Dipentamethylenethiuram tetrasulfide (DPTT), and / or dithiophosphates, such as DipDis (bis-(diisopropyl)thiophosphoryl disulfide) and / or bis(O,O-2-ethylhexylthiophosphoryl)polysulfide (e.g. Rhenocure SDT 50®, Rheinchemie GmbH) and / or zinc dichloryldithiophosphate (e.g. Rhenocure ZDT / S®, Rheinchemie GmbH) and / or zinc alkyl dithiophosphate, and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and / or Diarylpolysulfides and / or dialkylpolysulfides.
[0066] Other network-forming systems, such as those sold under the trade names Vulkuren®, Duralink® or Perkalink®, or network-forming systems as described in WO 2010 / 049216 A2, can be used in the rubber compound. This system contains a vulcanizing agent which is Functionality greater than four and at least one vulcanization accelerator. The vulcanizing agent, which is a functionality of greater than four has, for example, the general formula A): G[CH -CH -SY] A) where G is a a 2a 2 bc polyvalent cyclic hydrocarbon group and / or a polyvalent heterohydrocarbon group and / or a polyvalent siloxane group containing 1 to 100 atoms; wherein each Y is independently selected from a rubber-active group, sulfur-containing functionalities; and where a, b and c are integers for which Independently: a equals 0 to 6; b equals 0 to 8; and c equals 3 to 5.
[0067] The rubber-active group is preferably selected from a thiosulfonate group, a dithiocarbamate group, a thiocarbonyl group, a mercapto group, a hydrocarbon group and a sodium thiosulfonate group (Bunte salt group). This results in very good abrasion and tear properties of the rubber compound. The present invention uses sulfur and sulfur donors, including sulfur-donating silanes such as TESPT, and Vulcanization accelerators as described above and vulcanizing agents with a functionality greater than four crosslinking, as described in WO 2010 / 049216 A2, such as a vulcanizing agent of formula A), as well as the above The systems Vulkuren®, Duralink® and Perkalink® are conceptually summarized as vulcanizing agents.
[0068] During the production of the rubber mixture, at least one vulcanizing agent is preferably selected from the group containing, particularly preferably consisting of, sulfur and / or sulfur donors and / or Vulcanization accelerators and / or vulcanizing agents that crosslink with a functionality greater than four, in the This allows the mixed ready mix to be vulcanized into a produce sulfur-cured rubber compounds, particularly for use in vehicle tires.
[0069] The use of the accelerators TBBS and / or CBS and / or diphenylguanidine (DPG) is particularly preferred.
[0070] In addition, vulcanization retarders may be present in the rubber mixture.
[0071] The terms ´´vulcanized´´ and ´´crosslinked´´ are used synonymously in the context of the present invention.
[0072] According to a preferred embodiment of the invention, in the production of the sulfur-crosslinkable Several accelerators are added to the rubber mixture in the final mixing stage.
[0073] The sulphur-crosslinkable rubber mixture is produced according to the process customary in the rubber industry Process in which a basic mixture with all components except the Vulcanization system (sulfur and vulcanization-influencing substances). By adding the The final mixing stage produces the finished mixture. The finished mixture is produced, for example, by an extrusion process or calendering and brought into the appropriate shape.
[0074] The subsequent processing is carried out by vulcanisation, whereby due to the scope of the present Invention added vulcanization system, sulfur crosslinking takes place.
[0075] The rubber mixture described above is particularly suitable for use in vehicle tires, in particular In principle, the application in all tire components is conceivable, especially in a Tread, especially in the cap of a tread with cap / base construction.
[0076] The cap is the part of the tread of the vehicle tire that comes into contact with the road surface, while the base is the radially underlying inner part of the tread that is not in contact with the road surface comes.
[0077] For use in vehicle tires, the mixture is preferably prepared as a ready-mix before vulcanization in the form a tread and applied as known during the production of the green vehicle tire.
[0078] The production of the rubber mixture for use as a body mixture in vehicle tires is carried out as already The difference lies in the shaping after the extrusion process or calendering of the mixture. The resulting shapes of the unvulcanized rubber mixture for one or more different body Mixtures are then used to build a green tire.
[0079] The body mixture is the rubber mixture for the other external and internal components of a Tire refers to, as essentially squeegee, sidewall, inner liner (inner layer), core profile, belt, shoulder, Belt profile, carcass, bead reinforcement, bead profile, horn profile and bandage.
[0080] For the use of the rubber mixture in belts and straps, especially in conveyor belts, the extruded The unvulcanised mixture is brought into the appropriate shape and is often reinforced with reinforcements, e.g. B. synthetic fibers or steel cords. This usually results in a multi-layer structure consisting of one and / or several layers of rubber mixture, one and / or several layers of the same and / or different Strengthening member and one and / or more further layers of the like and / or another rubber mixture.
[0081] The subject of the present invention is a vehicle tire which has at least one component Vulcanizate of at least one sulfur-crosslinkable rubber mixture with the above-mentioned features.
[0082] The vehicle tire comprises at least one vulcanizate of at least one sulfur-crosslinkable rubber mixture with above-mentioned features at least in the tread.
[0083] The vehicle tire with a tread has a cap / base construction and the tread contains the Rubber compound at least in the cap.
[0084] Vehicle tires containing the rubber compound at least in the tread show an improvement in Conflict of objectives between wet braking and rolling resistance, while maintaining the same level of winter properties, especially the Traction on snow, as well as dry braking behavior.
[0085] In the context of the present invention, vehicle tires are understood to mean pneumatic vehicle tires and solid rubber tires, including tires for industrial and construction vehicles, truck, car and two-wheel tires.
[0086] The rubber mixture is also suitable for other components of vehicle tires, such as in particular Sidewall, tread pattern and internal tire components.
[0087] The rubber compound is also suitable for other technical rubber articles, such as bellows, conveyor belts, air springs, Belts, straps or hoses, as well as shoe soles, whereby due to the requirement profile they are particularly suitable for suitable for conveyor belts.
[0088] The subject of the present invention is a vehicle tire as described above.
[0089] Preferably, the sulfur-crosslinkable rubber mixture of the tread of the inventive Vehicle tire contains 40 to 250 phr of at least one silica. The sulfur-crosslinkable Rubber mixture of the tread of the vehicle tire according to the invention 55 to 100 phr of at least one butadiene Acrylonitrile copolymer.
[0090] The sulfur-crosslinkable rubber mixture of the tread of the vehicle tire according to the invention contains 35 up to 70 phr of at least one plasticizer.
[0091] For all other components and further quantities including preferred embodiments for butadiene Acrylonitrile copolymer, silica, plasticizer and all other ingredients are subject to the above sulfur crosslinked bare rubber mixture.
[0092] The invention will now be explained with reference to comparative and exemplary embodiments, which are summarized in Table 1 are explained in more detail.
[0093] The comparison mixtures are designated V, the mixtures for vehicle tires according to the invention are designated E marked.
[0094] The mixture was prepared according to the usual procedure in the rubber industry under usual Conditions in three stages in a laboratory mixer in which initially in the first mixing stage (basic mixing stage) all Components other than the vulcanization system (sulfur and vulcanization-influencing substances) were mixed. In the second mixing stage, the base mixture was mixed again. By adding the vulcanization system in In the third stage (finished mixing stage) the finished mixture was produced, mixing at 90 to 120 °C.
[0095] Test specimens were prepared from all mixtures by vulcanization after 20 minutes under pressure at 160°C manufactured and with these test specimens, material properties typical for the rubber industry were determined with the following specified test procedures. • Mooney viscosity ML 1+3 at 100 °C (Mooney units ME) ASTM D1646 • Shore A hardness at room temperature (RT) according to DIN ISO 7619-1 • Rebound resilience at room temperature and 70°C according to ISO 4662 or ASTM D 1054 • Elongation at break and stress value at 300% elongation (module 300, M300) at room temperature according to DIN 53,504 • dynamic storage modulus E' and maximum (max) loss factor tan δ (tan delta, TanD) at 55 ° C and an elongation of 8% from dynamic mechanical measurement based on DIN 53 513, Strain sweep at a pre-compression of 20% and a frequency of 10 Hz.
[0096] Furthermore, tire tests were carried out, namely in the comparative example V1 and in the inventive Examples E1 and E2, each with the compound as a tread cap. The following test methods were applied: • Wet braking: ABS braking, braking distance from 80 km / h, wet asphalt, low µ (low µ) • Dry braking: ABS braking, braking distance from 100 km / h, dry asphalt, high µ (high µ) • Rolling resistance: according to ISO 28580 • Traction - Snow: Acceleration on snow and determination of traction force.
[0097] The determined values were converted into performance, whereby the comparison mixture V1 was used for each tested property was standardized to 100% performance. All other compound performances refer to this Comparison mixture V1. Values < 100% mean a deterioration in the properties, while values > 100% represents an improvement. Table 1 Components Unit V1 E1 E2 NR TSR phr 20 - - a) B phr 50 - - R b) phr 30 - - SBR c) phr - 100 100 NBR Soot N339 phr 14 2 2 d) phr 85 58 83 Silica TDAE phr 29 - - e) phr - 20 45 plasticizers f) phr 8 5 8 Silane G) phr 11.7 8 8 additives h) phr 5 - - Process aids i) phr 3.8 3.8 3.8 accelerator Sulfur phr 2.1 2.2 2.2 Physical properties Mooney ME 71 49 32 Shore hardness A Shore A 63 66 66 Rebound RT % 34 35 31 Rebound 70 °C % 45 51 45 Diff. Rebound 11 16 14 Elongation at break % 581 465 414 M300 MPa 5.7 9.1 9.6 E' (8%) MPa 4.7 6.2 5.7 TanD (max.) 0.209 0.202 0.242 Tire results Rolling resistance % 100 102 100 Wet braking % 100 103 105 Traction - Snow % 100 99 100 Substances used: a) BR: Nd-BR, Buna CB 25, Lanxess b) SBR: oil-extended SSBR: 72.7 wt% SSBR, 27.3 wt% TDAE, DSSK 2560, Sibur c) ® NBR: KRYNAC 3345, Lanxess, Mooney viscosity ML (1+4) 100 °C without Pretreatment 45 ± 5 MU, acrylonitrile content 33 ± 1.0 wt.% d) Silica VN3, Evonik e) ® Plasticizer: Vulkanol 88, Lanxess f) ® Silane: 75% by weight S-silane, Si75, Evonik 2 G) Additives: Anti-aging agents: 6PPD, DTPD, ozone protection wax; zinc oxide, stearic acid h) Processing aids: fatty acid esters and zinc soaps i) Vulcanization accelerators: CBS, MBT (2-mercaptobenzothiazole) and DPG
[0098] As can be seen from Table 1, the rubber mixtures E1 and E2 for tires according to the invention and containing 100 phr NBR compared to a rubber compound with a polymer system for treads from the State of the art V1 shows an improvement in the conflict of objectives between rolling resistance and wet grip indicators, which is due to the increased differences in rebound elasticity (rebound 70 °C minus rebound RT). At the same time, a Vehicle tyres containing the rubber compounds E1 and E2 in the tread, an improvement in the conflict of objectives of Rolling resistance and wet braking, as can be seen from the tire results.
[0099] At the same time, the level of the other properties and requirements, such as in particular dry braking and traction on snow is not significantly negatively affected.
Claims
1. Vehicle tyres, the tread of which contains at least in the cap a vulcanizate of at least one sulphur-curable Rubber mixture containing the following components: - 35 to 100 phr of at least one butadiene-acrylonitrile copolymer and - at least one silica and - 35 to 70 phr of at least one plasticizer.
2. Vehicle tyre according to claim 1, characterised in that the sulphur-crosslinkable rubber mixture contains 40 to 250 phr of at least one silicic acid.
3. Vehicle tyre according to one of the preceding claims, characterized in that the sulphur-crosslinkable Rubber mixture containing 55 to 100 phr of at least one butadiene-acrylonitrile copolymer.
Citation Information
Patent Citations
rubber compounds
DE102006004062A1
Run-flat radial tyres for vehicles, with a sidewall reinforcement of crescent-shaped cross-section made from a rubber mixture containing acrylonitrile-butadiene rubber with a certain range of nitrile content
DE102006016915A1
TIRE TREAD COMPOSITIONS 1. Field of the Invention
DE69213002T2
Tire tread composition
EP0824567B1
Method for using s-(3-aminopropyl)thiosulfuric acid and / or metal salt thereof
EP2589619A1