Bending resistance agent and laminate

A laminate with a bending-resistant layer using a resin-based agent maintains functional layer integrity before and after bending, addressing the deterioration issue in paper laminates.

JP7588264B1Active Publication Date: 2024-11-21SAKATA INX

Patent Information

Application Number
JP2024074909
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-12-20
Filing Date
2024-05-02
Publication Date
2024-11-21
Estimated Expiration
2044-05-02

AI Technical Summary

Technical Problem

The functionality of functional layers in paper laminates deteriorates due to bending, as seen in existing paper packaging materials with moisture-resistant properties.

Method used

A laminate configuration is developed with a paper base layer, a bending-resistant layer, and a functional layer, where the bending-resistant layer is formed using a resin-based agent with specific properties to prevent deterioration, including a resin content of 70-100% by mass and elongation and shape recovery criteria.

Benefits of technology

The laminate maintains the functionality of the functional layers before and after bending, enhancing moisture-proof, gas barrier, oil resistance, water resistance, and water repellency properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588264000001
    Figure 0007588264000001
  • Figure 0007588264000002
    Figure 0007588264000002
Patent Text Reader

Abstract

The present invention provides a folding resistance agent and a laminate in which various functional layers are provided on a paper base material, which makes it difficult for the functional layers to deteriorate before and after folding. [Solution] In a laminate in which a paper base layer, a folding-resistant layer, and a functional layer are laminated in this order, a folding-resistant agent for forming the folding-resistant layer satisfies the following conditions 1 to 3 (excluding the case where the folding-resistant agent is OKS-1009 and the functional layer is an active energy ray-curable ink composition layer). (Condition 1) The fold-resistant agent includes a resin and a medium, the resin including at least one resin selected from the group consisting of polyurethane-based resins, acrylic-based resins, polyester-based resins, polyvinyl alcohol-based resins, styrene-butadiene-based resins, and vinyl chloride-based resins, and the resin content (converted into solid content) in the fold-resistant agent is 70 to 100 mass %. (Condition 2) The bending-resistant layer has an elongation of 200% or more in a tensile test. (Condition 3) The shape recovery rate of the folding-resistant layer is 80% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a folding endurance agent and a laminate. More specifically, the present invention relates to a folding endurance agent and a laminate for preventing deterioration of the function of a functional layer before and after folding in a laminate having various functional layers provided on a paper base material. [Background technology]

[0002] In recent years, in order to respond to the demands of environmental friendliness and the SDGs (Sustainable Development Goals), there has been a demand for the food industry to move away from plastic and aluminum. In response to these demands, paper packaging materials with barrier properties (moisture resistance) have been considered (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-220494 A [Patent Document 2] JP 2009-155780 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when packaging materials are produced using the paper laminates described in Patent Documents 1 and 2, there is a problem in that the functionality of the functional layer (such as moisture resistance) is reduced by folding the package.

[0005] The present invention has been made in consideration of such conventional problems, and aims to provide a folding resistance agent and a laminate in which various functional layers are provided on a paper base material, which makes it less likely that the functionality of the functional layers will deteriorate before and after bending. [Means for solving the problem]

[0006] As a result of intensive research to solve the above problems, the inventors have found that the above problems can be solved by providing a folding-resistant layer between the paper base layer and the functional layer, and have completed the present invention. That is, the folding-resistant agent and laminate of the present invention that solve the above problems mainly include the following components.

[0007] (1) In a laminate in which a paper base layer, a folding-resistant layer, and a functional layer are laminated in this order, a folding-resistant agent for forming the folding-resistant layer, which satisfies the following conditions 1 to 3 (excluding the case where the folding-resistant agent is OKS-1009 and the functional layer is an active energy ray-curable ink composition layer). (Condition 1) The folding resistance agent includes a resin and a medium, the resin includes at least one selected from the group consisting of polyurethane resins, acrylic resins, polyester resins, polyvinyl alcohol resins, styrene-butadiene resins, and vinyl chloride resins; The content of the resin (calculated as solid content) in the folding endurance agent is 70 to 100% by mass. (Condition 2) The degree of elongation of the fold-resistant layer in a tensile test determined by the following formula is 200% or more. Elongation degree (%)=100×(Lb-L0) / L0 Here, Lb refers to the gauge length at break, and L0 refers to the gauge length before the tensile test. The tensile test is a tensile test performed in accordance with JIS K 6251. (Condition 3) The shape recovery rate of the folding-resistant layer, calculated by the following formula, is 80% or more. Shape restoration rate (%) = 100 × (L1-L2) / (L1-L0) Here, L0 refers to the gauge length before the tensile test. L1 refers to the gauge length at 100% elongation in the tensile test, and for those that cannot be elongated to 100%, it is the limit gauge length without breakage. L2 is the gauge length of the folding-resistant layer when the external force is removed after the tensile test, and the tensile test is conducted in accordance with JIS K 6251.

[0008] According to this configuration, the folding endurance agent is applied to a laminate having various functional layers provided on a paper base material so as to form a folding endurance layer between the paper base material and the functional layers, and the obtained laminate is less likely to have its function deteriorated before and after folding.

[0009] (2) The folding-resistant agent according to (1), wherein the functional layer includes at least one layer selected from the group consisting of a moisture-proof layer, a gas barrier layer, an oil-resistant layer, a water-resistant layer, and a water-repellent layer.

[0010] According to this configuration, the folding-resistant agent is applied to a laminate having various functional layers provided on a paper substrate so as to form a folding-resistant layer between the paper substrate and the functional layers. The obtained laminate is less likely to lose the functions (moisture resistance, gas barrier properties, oil resistance, water resistance, or water repellency) of the various functional layers before and after folding.

[0011] (3) A laminate comprising a paper base layer, a folding-resistant layer, and a functional layer laminated in this order, the folding-resistant layer being a layer formed by applying the folding-resistant agent described in (1) or (2).

[0012] With this configuration, the function of the functional layer in the obtained laminate is less likely to deteriorate before and after bending. Effect of the Invention

[0013] According to the present invention, it is possible to provide a folding resistance agent and a laminate in which various functional layers are provided on a paper base material, which makes it difficult for the functional layers to deteriorate before and after folding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] <Bending resistance agent> The folding-resistant agent of one embodiment of the present invention is a folding-resistant agent for forming a folding-resistant layer in a laminate in which a paper base layer, a folding-resistant layer, and a functional layer are laminated in this order, except when the folding-resistant agent is OKS-1009 and the functional layer is an active energy ray-curable ink composition layer. The folding-resistant agent satisfies the following conditions 1 to 3. Note that the folding-resistant agent of this embodiment only needs to have a configuration in which the paper base layer, the folding-resistant layer, and the functional layer are laminated in this order, and other layers may be provided before, after, or between them. (Condition 1) The fold-resistant agent includes a resin and a medium, the resin includes at least one resin selected from the group consisting of polyurethane-based resins, acrylic-based resins, polyester-based resins, polyvinyl alcohol-based resins, styrene-butadiene-based resins, and vinyl chloride-based resins, and the content of the resin (converted into solid content) in the fold-resistant agent is 70 to 100 mass %. (Condition 2) The degree of elongation of the fold-resistant layer in a tensile test determined by the following formula is 200% or more. Elongation degree (%)=100×(Lb-L0) / L0 Here, Lb refers to the gauge length at break, and L0 refers to the gauge length before the tensile test. The tensile test is a tensile test performed in accordance with JIS K 6251. (Condition 3) The shape recovery rate of the folding-resistant layer, calculated by the following formula, is 80% or more. Shape restoration rate (%) = 100 × (L1-L2) / (L1-L0) Here, L0 refers to the gauge length before the tensile test. L1 refers to the gauge length at 100% elongation in the tensile test, and for those that cannot be elongated to 100%, it is the limit gauge length without breakage. L2 is the gauge length of the folding-resistant layer when the external force is removed after the tensile test, and the tensile test is a tensile test conducted in accordance with JIS K 6251. Each of these is explained below.

[0015] (Regarding condition 1) ·resin The resin includes at least one selected from the group consisting of polyurethane resin, acrylic resin, polyester resin, polyvinyl alcohol resin, styrene-butadiene resin, and vinyl chloride resin. From the viewpoint of solid content and viscosity, the resin is preferably an emulsion of polyurethane resin, acrylic resin, styrene-butadiene resin, or vinyl chloride resin. As a result, the folding resistance agent is applied to form a folding resistance layer containing the above resin between the paper base material and the functional layer in a laminate in which various functional layers are provided on the paper base material. The obtained laminate is less likely to have a function of the functional layer deteriorated before and after folding.

[0016] The polyurethane resin is not particularly limited, and an example thereof is a polyurethane resin obtained by reacting a diisocyanate compound with a diol compound, and optionally with a chain extender or a reaction terminator.

[0017] The diisocyanate compound is not particularly limited. Examples of the diisocyanate compound include aliphatic diisocyanate compounds such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate, alicyclic diisocyanate compounds such as isophorone diisocyanate and hydrogenated xylylene diisocyanate, and aromatic diisocyanate compounds such as xylylene diisocyanate, α,α,α',α'-tetramethylxylylene diisocyanate, toluylene diisocyanate, and diphenylmethane diisocyanate.

[0018] The diol compound is not particularly limited. For example, the diol compound may be a low molecular weight diol such as ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, or triethylene glycol; or a high molecular weight diol such as a polyester diol compound, a polyether diol compound, a polycarbonate diol compound, or a polybutadiene glycol compound.

[0019] The polyurethane resin may have various skeletons, for example, polyether polyurethane resin, polyester polyurethane resin, polyester-polyether polyurethane resin, polycarbonate polyurethane resin, etc.

[0020] The polyester resin is not particularly limited. For example, the polyester resin can be obtained by an esterification reaction of a polyvalent carboxylic acid and a polyhydric alcohol as raw material components.

[0021] The polycarboxylic acid is not particularly limited. Examples of the polycarboxylic acid include phthalic acid, isophthalic acid, tetrahydrophthalic acid, tetrahydroisophthalic acid, hexahydrophthalic acid, hexahydroterephthalic acid, trimellitic acid, adipic acid, sebacic acid, succinic acid, azelaic acid, fumaric acid, maleic acid, itaconic acid, pyromellitic acid, and the like, and acid anhydrides thereof.

[0022] The polyhydric alcohol is not particularly limited. For example, the polyhydric alcohol may be glycol or a polyhydric alcohol having a valence of 3 or more. Examples of glycols include ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, neopentyl glycol, hexylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-butyl-2-ethyl-1,3-propanediol, methylpropanediol, cyclohexanedimethanol, and 3,3-diethyl-1,5-pentanediol. Examples of polyhydric alcohols having a valence of 3 or more include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and dipentaerythritol.

[0023] The acrylic resin is not particularly limited. For example, the acrylic resin may be, for example, a polyester-modified acrylic resin, a polyurethane-modified acrylic resin, or a copolymer of versatic acid vinyl ester and an acrylic monomer, which is a copolymer of versatic acid vinyl ester and an acrylic monomer.

[0024] The polyvinyl alcohol-based resin is not particularly limited. For example, the polyvinyl alcohol-based resin may be polyvinyl alcohol, or a derivative or modified product of polyvinyl alcohol.

[0025] The degree of polymerization of the polyvinyl alcohol resin is preferably 100 to 5000, and more preferably 500 to 3000. When the degree of polymerization of the polyvinyl alcohol resin is within the above range, the folding endurance agent has excellent film strength and handling suitability.

[0026] The saponification degree of the polyvinyl alcohol resin is preferably 60 mol% or more, and more preferably 75 mol% or more. When the saponification degree of the polyvinyl alcohol resin is within the above range, the folding endurance agent has excellent film strength and water resistance.

[0027] The polyvinyl alcohol derivative is a polyvinyl alcohol derivative in which up to about 40 mol % of the hydroxyl groups are acetalized.

[0028] The modified polyvinyl alcohol includes those obtained by copolymerizing a carboxyl group-containing monomer, an amino group-containing monomer, a sulfone group-containing monomer, an acetoacetyl group-containing monomer, butenediol, and the like.

[0029] Polyvinyl alcohol resins include Poval and Exeval (both manufactured by Kuraray Co., Ltd.), Gohsenol, and Nichigo G-Polymer (both manufactured by Mitsubishi Chemical Co., Ltd.).

[0030] The styrene-butadiene resin is not particularly limited. For example, the styrene-butadiene resin is a resin emulsion obtained by emulsion polymerization or solution polymerization of a monomer composition containing a styrene monomer, butadiene, and, if necessary, other monomers copolymerizable with the styrene monomer and butadiene.

[0031] The styrene monomers include styrene, α-methylstyrene, β-methylstyrene, 2,4-dimethylstyrene, α-ethylstyrene, α-butylstyrene, 4-methoxystyrene, vinyltoluene, and divinylbenzene.

[0032] Other monomers copolymerizable with styrene monomers and butadiene include (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate and butyl (meth)acrylate; cyanide vinyl monomers such as acrylonitrile and methacrylonitrile; amide group-containing monomers such as (meth)acrylamide and N,N-dimethyl (meth)acrylamide; (meth)acrylic acid hydroxyalkyl ester monomers such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; carboxyl group-containing monomers such as itaconic acid, maleic acid, and (meth)acrylic acid. The styrene-butadiene resin emulsion is preferably a carboxy (carboxy group)-modified styrene-butadiene resin emulsion.

[0033] From the viewpoint of improving blocking and leveling properties, the glass transition temperature of the styrene-butadiene resin emulsion is preferably -20°C or higher, and more preferably -10°C or higher. The glass transition temperature is determined by differential scanning calorimetry (DSC) and is usually calculated from the midpoint of the temperature range where the glass transition occurs.

[0034] Styrene-butadiene resin emulsions include Nipol SX1105A, Nipol LX407S12, and Nipol LX435 (all manufactured by Zeon Corporation).

[0035] The vinyl chloride resin is not particularly limited. For example, the vinyl chloride resin may be a vinyl chloride homopolymer, a copolymer of vinyl chloride and a monomer copolymerizable with vinyl chloride, or a graft copolymer in which vinyl chloride is graft-copolymerized with a polymer other than the copolymer of vinyl chloride and a monomer copolymerizable with vinyl chloride. Among these, the vinyl chloride resin is preferably a vinyl chloride resin or a vinyl chloride resin emulsion.

[0036] The method for producing the vinyl chloride resin is not particularly limited. For example, the vinyl chloride resin can be produced by any known method, such as emulsion polymerization, suspension polymerization, solution polymerization, or bulk polymerization.

[0037] The monomer copolymerizable with vinyl chloride constituting the copolymer of vinyl chloride and a copolymerizable monomer is not particularly limited as long as it has a reactive double bond in the molecule. Such monomers include α-olefins such as ethylene, propylene, butylene, vinyl esters such as vinyl acetate and vinyl propionate, vinyl ethers such as butyl vinyl ether and cetyl vinyl ether, unsaturated carboxylic acids such as acrylic acid and methacrylic acid, esters of acrylic acid or methacrylic acid such as methyl acrylate, ethyl methacrylate, and phenyl methacrylate, aromatic vinyls such as styrene and α-methylstyrene, halogenated vinyls such as vinylidene chloride and vinyl fluoride, and N-substituted maleimides such as N-phenylmaleimide and N-cyclohexylmaleimide.

[0038] The polymer other than the vinyl chloride copolymer is not particularly limited as long as it can be graft-copolymerized with vinyl chloride.

[0039] Examples of polyvinyl chloride resins include Vinyblan (manufactured by Nisshin Chemical Industry Co., Ltd.) and Sumikaflex (manufactured by Sumika Chemtex Co., Ltd.).

[0040] The resin content in the solid content of the fold-resistant agent (solid content equivalent) is not particularly limited. For example, the resin content in the fold-resistant agent may be 70% by mass or more, and preferably 80% by mass or more. The resin content in the fold-resistant agent may be 100% by mass or less. By having the resin content within the above range, the fold-resistant agent can achieve both coating suitability and coating film properties.

[0041] ·Medium The medium is not particularly limited as long as it satisfies conditions 1 to 3. For example, when the folding-resistant agent is aqueous, the medium may be only water, or may be an aqueous medium in which water and a water-miscible organic solvent are mixed. The water-miscible organic solvent is not particularly limited. For example, the water-miscible organic solvent is alcohols such as methanol, ethanol, and propanol, polyhydric alcohols such as ethylene glycol and propylene glycol, and alkyl ether derivatives thereof, esters such as ethyl formate, methyl acetate, and ethyl acetate, and ketones such as acetone.

[0042] In addition, when the folding-resistant agent is a solvent, the medium may be an alcohol-based solvent such as methanol, ethanol, isopropyl alcohol, normal propanol, butanol, isobutanol, or tert-butanol; an aromatic hydrocarbon-based solvent such as toluene or xylene; an aliphatic hydrocarbon-based solvent such as hexane, cyclohexane, methylcyclohexane, or ethylcyclohexane; a ketone-based solvent such as acetone, methyl ethyl ketone, methyl isobutyl ketone, or cyclohexanone; an ester-based solvent such as ethyl acetate, n-propyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, or tert-butyl acetate; an ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, or ethylene glycol monoethyl ether.

[0043] Glycol solvents such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, and esters thereof, and the esters thereof are preferably those which have been mainly acetated, and examples of the esters include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate.

[0043] When the folding-resistant agent is solvent-based, from an environmental perspective, the medium is preferably a mixed solvent of an ester-based organic solvent, an alcohol-based organic solvent, and a ketone-based organic solvent, or a mixed solvent of an ester-based organic solvent and an alcohol-based organic solvent which is more environmentally friendly.

[0044] The content of the medium is not particularly limited. For example, the content of the medium in the fold-resistant agent is preferably 40% by mass or more, more preferably 45% by mass or more. The content of the medium in the fold-resistant agent is preferably 80% by mass or less. By having the content of the medium within the above range, the fold-resistant agent can optimize storage stability, printability, and application amount.

[0045] ·Optional ingredients The folding endurance agent of the present embodiment may contain optional components in addition to the above resin and medium. The optional components are not particularly limited. Examples of the optional components include wax, defoaming agent, inorganic filler, release agent, thickener, surface conditioner, surfactant, plasticizer, polymerization inhibitor, ultraviolet absorber, light stabilizer, antioxidant, etc.

[0046] (Regarding condition 2) The folding-resistant agent of the present embodiment is a folding-resistant agent for forming a folding-resistant layer in a laminate in which a paper base layer, a folding-resistant layer, and a functional layer are laminated in this order.

[0047] Regarding condition 2, the degree of elongation in a tensile test of the fold-resistant layer obtained by using the fold-resistant agent of this embodiment is 200% or more. The degree of elongation is expressed by the following formula. Elongation degree (%)=100×(Lb-L0) / L0 Here, Lb refers to the gauge length at break, and L0 refers to the gauge length before the tensile test. The tensile test is a tensile test performed in accordance with JIS K 6251.

[0048] The degree of elongation of the folding-resistant layer is sufficient to be 200% or more, and is preferably 250% or more. If the degree of elongation of the folding-resistant layer is less than 200%, the folding-resistant layer is unlikely to maintain the function of the functional layer before and after folding the laminate, and the function is likely to deteriorate. In this embodiment, the degree of elongation of the folding-resistant layer can be measured by the following method.

[0049] -Measuring method for elongation of folding-resistant layer A folding resistance agent is applied to a substrate of your choice such as glass, dried, and peeled off to prepare a JIS K 6251 tensile No. 3 dumbbell-shaped test piece (film thickness 300 μm). Then, under the following conditions, using the following testing machine, the elongation of each test piece is measured when it is pulled to the point of breaking. Tensile testing machine: AGS-X, manufactured by Shimadzu Corporation Stretching speed: 300mm / min Temperature: 23℃ Humidity: 50%

[0050] (Regarding condition 3) Regarding condition 3, the shape restoration degree of the fold-resistant layer is 80% or more. The shape restoration degree may be 80% or more, preferably 90% or more, and more preferably 95% or more. If the shape restoration degree is less than 80%, the fold-resistant layer has difficulty in maintaining the function of the functional layer.

[0051] In this embodiment, the degree of shape recovery can be evaluated by carrying out a tensile test carried out in accordance with JIS K 6251. The tensile test for evaluating the degree of shape recovery can be carried out under the following conditions using the following testing machine.

[0052] - Method for evaluating the degree of shape restoration of the folding-resistant layer A folding resistance agent is applied to a substrate such as glass, dried, and peeled off to obtain a test specimen. Using the obtained test specimen, a JIS K 6251 tensile No. 3 dumbbell shape (film thickness 300 μm) is prepared. Next, each test specimen is stretched using the following test machine under the following conditions and held in that state for 5 minutes. After that, the test specimen is removed from the test machine, and the length of the test specimen is measured after 3 hours. Tensile testing machine: AGS-X, manufactured by Shimadzu Corporation Stretching speed: 50mm / min Temperature: 23℃ Humidity: 50% The degree of shape restoration is calculated by the following formula. Shape restoration rate (%) = 100 × (L1-L2) / (L1-L0 ) Here, L0 refers to the gauge length before the tensile test. L1 refers to the gauge length at 100% elongation in the tensile test, and for those that cannot be elongated to 100%, it is the limit gauge length without breakage. L2 is the gauge length when the external force is removed after the tensile test.

[0053] Returning to the explanation of the folding endurance agent as a whole, the laminate to which the folding endurance agent is applied is a laminate in which a paper base layer, a folding endurance layer, and a functional layer are laminated in this order.

[0054] (Paper base layer) The paper base layer is not particularly limited. For example, the paper constituting the paper base layer is not particularly limited. For example, the paper may be any paper that is generally used and contains plant-derived pulp as the main component, such as bleached or unbleached kraft paper, fine paper, paperboard, liner paper, coated paper, one-sided gloss paper, glassine paper, graphene paper, etc. Among these, the paper is preferably paper that contains pulp as the main component, which is easily dispersible in water by mechanical disintegration.

[0055] The basis weight and thickness of the paper base layer are not particularly limited. For example, the basis weight of the paper base layer is 30 g / m 2 It is preferable that the thickness is 50 g / m or more. 2 More preferably, the thickness of the paper base layer is 300 g / m or more. 2 It is preferable that the thickness is less than 250 g / m 2 When the thickness and basis weight of the paper base layer are within the above ranges, the folding endurance agent can easily maintain the function of the functional layer.

[0056] (bending resistant layer) The folding-resistant layer is a layer formed by applying the folding-resistant agent of this embodiment.

[0057] The method of applying the fold resistance agent to the paper substrate is not particularly limited. For example, the application method may be a method using a blade coater, a bar coater, an air knife coater, a slit die coater, a gravure coater, a gravure reverse coater, a microgravure coater, a gate roll coater, or the like.

[0058] The applied fold-resistant agent is dried. The drying method for drying the fold-resistant agent is not particularly limited. For example, the drying method may use known drying equipment, such as a hot air dryer, an infrared ray dryer, a gas burner, a hot plate, etc.

[0059] The thickness of the folding-resistant layer is not particularly limited. For example, the thickness of the folding-resistant layer is preferably 1 μm or more, more preferably 3 μm or more. The thickness of the folding-resistant layer is preferably 30 μm or less, more preferably 20 μm or less. By having the thickness of the folding-resistant layer within the above range, the function of the functional layer in the obtained laminate is unlikely to deteriorate before and after folding.

[0060] (Functional layer) The functional layer is a layer for imparting various functions to the paper substrate. The laminate of the present embodiment includes a folding-resistant layer formed by applying the folding-resistant agent described above. As a result, the laminate is less likely to lose the functions imparted by the functional layer before and after folding.

[0061] The functional layer is not particularly limited. The functional layer can be appropriately selected depending on the desired application. Specifically, the functional layer preferably includes at least one layer selected from among a moisture-proof layer, a gas barrier layer, an oil-resistant layer, a water-resistant layer, and a water-repellent layer. This makes it difficult for the functions of the various functional layers (moisture-proof property, gas barrier property, oil resistance, water resistance, or water repellency) of the obtained laminate to decrease before and after folding.

[0062] When the functional layer is a moisture-proof layer The moisture-proof layer is provided by applying a moisture-proof coating agent, which, for example, contains an anionic binder resin, an inorganic layered compound, and an aqueous medium.

[0063] The anionic binder resin is not particularly limited. For example, the anionic binder resin may be a styrene-butadiene copolymer, a styrene-acrylic copolymer, a methacrylate-butadiene copolymer, an acrylonitrile-butadiene copolymer, an olefin-unsaturated carboxylic acid copolymer, an acrylic ester polymer, or the like. Among these, the anionic binder resin is preferably at least one selected from the group consisting of a styrene-butadiene copolymer, a styrene-acrylic copolymer, and an olefin-unsaturated carboxylic acid copolymer, and more preferably an olefin-unsaturated carboxylic acid copolymer, in view of good water resistance, good elongation, and resistance to cracking of the functional layer due to folding.

[0064] Styrene-butadiene copolymers are copolymers obtained by emulsion polymerization of monomers consisting of aromatic vinyl compounds such as styrene, α-methylstyrene, vinyltoluene, pt-butylstyrene, and chlorostyrene, conjugated diene compounds such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene, and other compounds copolymerizable with these. The aromatic vinyl compound is preferably styrene, etc. The conjugated diene compound is preferably 1,3-butadiene.

[0065] Styrene-acrylic copolymers are copolymers obtained by emulsion polymerization of aromatic vinyl compounds such as styrene, α-methylstyrene, vinyltoluene, pt-butylstyrene, and chlorostyrene with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, and butene tricarboxylic acid, unsaturated polycarboxylic acid alkyl esters having at least one carboxyl group such as itaconic acid monoethyl ester, fumaric acid monobutyl ester, and maleic acid monobutyl ester, unsaturated sulfonic acid monomers or their salts such as acrylamidopropanesulfonic acid, acrylic acid sulfoethyl sodium salt, and methacrylic acid sulfopropyl sodium salt, and other compounds copolymerizable with these monomers. The aromatic vinyl compound is preferably styrene, etc. The unsaturated carboxylic acid monomers and unsaturated sulfonic acid monomers or their salts are preferably acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and the like.

[0066] The olefin-unsaturated carboxylic acid copolymer is a copolymer obtained by emulsion polymerization of an olefin, particularly an α-olefin such as ethylene or propylene, with an unsaturated carboxylic acid such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, butene tricarboxylic acid, an unsaturated polycarboxylic acid alkyl ester having at least one carboxyl group such as itaconic acid monoethyl ester, fumaric acid monobutyl ester, and maleic acid monobutyl ester, an unsaturated sulfonic acid monomer or its salt such as acrylamidopropanesulfonic acid, acrylic acid sulfoethyl sodium salt, and methacrylic acid sulfopropyl sodium salt, and other compounds copolymerizable with these monomers. The olefin is preferably an α-olefin, particularly ethylene. The unsaturated carboxylic acid monomer and the unsaturated sulfonic acid monomer or their salt are preferably acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and the like. As a specific example of an olefin-unsaturated carboxylic acid copolymer, an aqueous dispersion of ammonium salt of ethylene-acrylic acid copolymer is commercially available as ZAIXXEN AC, ZAIXXEN A, etc. (manufactured by Sumitomo Seika Chemicals Co., Ltd.), and can be easily obtained and used.

[0067] The content of the anionic binder resin is not particularly limited. For example, the content of the anionic binder resin is preferably 20% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on the total solid content of the moisture-proof coating agent. The content of the anionic binder resin is preferably 95% by mass or less, more preferably 85% by mass or less, based on the total solid content of the moisture-proof coating agent. When the content of the anionic binder resin is within the above range, the resulting functional layer (moisture-proof layer) can exhibit high moisture resistance.

[0068] The inorganic layered compound is not particularly limited. For example, the inorganic layered compound may be either a natural product or a synthetic product, or may be a mixture of these. Natural products include smectite clay minerals such as montmorillonite, kaolinite (kaolin mineral), pyrophyllite, talc, beidellite, nontronite, saponite, hectorite, sauconite, and stevensite, and mica clay minerals such as bentonite, pure mica, and brittle mica. Synthetic products include synthetic hectorite (sodium magnesium silicate), synthetic bentonite, synthetic saponite, and synthetic mica. Among these, from the viewpoint of improving dispersibility, the inorganic layered compound is preferably at least one selected from the group consisting of water-swellable montmorillonite, bentonite, and synthetic mica, synthetic hectorite, and synthetic bentonite. In addition, from the viewpoint of improving barrier properties, the inorganic layered compound is more preferably montmorillonite, synthetic mica, or synthetic hectorite. The inorganic layered compounds may be used in combination.

[0069] The content of the inorganic layered compound is not particularly limited. For example, the content of the inorganic layered compound is preferably 80% by mass or less, more preferably 70% by mass or less, even more preferably 30% by mass or less, and particularly preferably 20% by mass or less, based on the total solid content in the moisture-proof coating agent. On the other hand, the content of the inorganic layered compound is preferably 1% by mass or more, more preferably 2% by mass or more, based on the total solid content in the moisture-proof coating agent. By having the content of the inorganic layered compound within the above range, the obtained functional layer (moisture-proof layer) can exhibit high moisture resistance.

[0070] The aqueous medium is not particularly limited. For example, the aqueous medium may be water alone, or may be a mixture of water and a water-miscible organic solvent such as an alcohol such as methanol, ethanol, or propanol, a polyhydric alcohol such as ethylene glycol or propylene glycol, an alkyl ether derivative thereof, an ester such as ethyl formate, methyl acetate, or ethyl acetate, or a ketone such as acetone.

[0071] The moisture-proof coating agent may contain at least one selected from amino acids and cationic resins in order to further improve moisture-proofing. The amino acids and cationic resins are not particularly limited. For example, the amino acids include glycine, alanine, leucine, valine, phenylalanine, proline, serine, threonine, lysine, arginine, aspartic acid, glutamic acid, polylysine, polyglutamic acid, polyglutamic acid, and other amino acids, amino acid polymers, and amino acid derivatives. The amino acids may be copolymers of amino acids. The amino acids are preferably copolymers or polymers of amino acids in terms of better moisture-proofing.

[0072] Examples of the cationic resin include polyalkylene polyamines, polyamide compounds, polyamidoamine-epihalohydrin or formaldehyde condensation reaction products, polyamine-epihalohydrin or formaldehyde condensation reaction products, polyamide polyurea-epihalohydrin or formaldehyde condensation reaction products, polyamine polyurea-epihalohydrin or formaldehyde condensation reaction products, polyamidoamine polyurea-epihalohydrin or formaldehyde condensation reaction products, polyamide polyurea compounds, polyamine polyurea compounds, polyamidoamine polyurea compounds, polyamidoamine compounds, polyethyleneimine, polyvinylpyridine, amino-modified acrylamide compounds, polyvinylamine, and polydiallyldimethylammonium chloride.

[0073] The moisture-proof coating agent may be appropriately blended with additives as necessary. The additives are not particularly limited. Examples of additives include dispersants, surfactants, defoamers, wetting agents, dyes, color adjusters, thickeners, etc.

[0074] The method for producing the moisture-proof coating agent is not particularly limited. For example, the moisture-proof coating agent can be prepared by mixing an anionic binder resin, an inorganic layered compound, an aqueous medium, and optionally amino acids, a cationic resin, and additives, and thoroughly stirring and mixing the mixture at room temperature.

[0075] When the functional layer is a moisture-proof layer, the thickness of the moisture-proof layer is not particularly limited. For example, the thickness of the moisture-proof layer is preferably 3 μm or more, more preferably 5 μm or more. The thickness of the moisture-proof layer is preferably 30 μm or less, more preferably 20 μm or less. When the thickness of the moisture-proof layer is within the above range, the obtained laminate has excellent moisture resistance.

[0076] When the functional layer is a gas barrier layer The gas barrier layer is provided by applying a gas barrier coating agent, for example, a water-based polymer, an inorganic layered compound, or an aqueous medium.

[0077] The aqueous polymer is not particularly limited. For example, the aqueous polymer may be polyvinyl alcohol, modified polyvinyl alcohol, starch and its derivatives, cellulose derivatives, polyvinylpyrrolidone, polyacrylonitrile resins, polyamide resins, polyester resins, urethane resins, polyacrylic acid and its salts, casein, polyethyleneimine, etc. Among these, the aqueous polymer is preferably a fully saponified or partially saponified polyvinyl alcohol or a modified polyvinyl alcohol, from the viewpoint of imparting a better gas barrier property. Examples of the modified polyvinyl alcohol include ethylene modified polyvinyl alcohol, carboxy modified polyvinyl alcohol, silicon modified polyvinyl alcohol, acetoacetyl modified polyvinyl alcohol, diacetone modified polyvinyl alcohol, etc.

[0078] The content of the aqueous polymer is not particularly limited. For example, the content of the aqueous polymer is preferably 50% by mass or more, and more preferably 70% by mass or more, of the total solid content of the gas barrier coating agent.

[0079] The inorganic layered compound is the same as the inorganic layered compound described above in relation to the moisture-proof layer. From the viewpoint of improving the gas barrier property, the inorganic layered compound is preferably at least one selected from the group consisting of mica, bentonite and kaolin.

[0080] The content of the inorganic layered compound is not particularly limited. For example, the content of the inorganic layered compound is preferably 1 part by mass or more, more preferably 30 parts by mass or more, relative to 100 parts by mass of the aqueous polymer of the gas barrier coating agent. The content of the inorganic layered compound is preferably 20 parts by mass or less, more preferably 50 parts by mass or less, relative to 100 parts by mass of the aqueous polymer of the gas barrier coating agent. By the content of the inorganic layered compound being within the above range, the obtained functional layer (gas barrier layer) has excellent gas barrier properties under high humidity.

[0081] The aqueous medium may be water alone, or may be an aqueous medium obtained by mixing water with a water-miscible organic solvent such as an alcohol, such as methanol, ethanol, or propanol; a polyhydric alcohol, such as ethylene glycol or propylene glycol, or an alkyl ether derivative thereof; an ester, such as ethyl formate, methyl acetate, or ethyl acetate; or a ketone, such as acetone.

[0082] The method for producing the gas barrier coating agent is not particularly limited. For example, the gas barrier coating agent can be prepared by mixing an aqueous polymer, an inorganic layered compound, and an aqueous medium, and thoroughly stirring and mixing the mixture at room temperature.

[0083] When the functional layer is a gas barrier layer, the thickness of the gas barrier layer is not particularly limited. For example, the thickness of the gas barrier layer is preferably 0.1 μm or more, more preferably 0.5 μm or more. The thickness of the gas barrier layer is preferably 10 μm or less, more preferably 5 μm or less. When the thickness of the gas barrier layer is within the above range, the obtained laminate has excellent gas barrier properties.

[0084] When the functional layer is an oil-resistant layer The oil-resistant layer is provided by applying an oil-resistant coating agent. For example, the oil-resistant coating agent may be an oil-resistant coating agent containing a pigment, a styrene-butadiene copolymer, polyvinyl alcohol, and an aqueous medium, or an oil-resistant coating agent containing a styrene-acrylic copolymer, wax, and an aqueous medium.

[0085] An oil-resistant coating agent containing pigment, styrene-butadiene copolymer, polyvinyl alcohol, and an aqueous medium is described.

[0086] The pigment is not particularly limited. For example, the pigment may be various pigments such as inorganic pigments and organic pigments. Inorganic pigments include kaolins such as kaolin, structural kaolin, delaminated kaolin, and calcined kaolin, synthetic mica, heavy calcium carbonate, light calcium carbonate, talc, calcium sulfate, barium sulfate, titanium dioxide, zinc oxide, alumina, aluminum hydroxide, magnesium carbonate, magnesium oxide, silica, magnesium aluminosilicate, calcium silicate, white carbon, bentonite, zeolite, sericite, smectite, and other minerals. Among these, kaolin is preferred because it can impart excellent oil resistance and water resistance. In addition, kaolin has excellent transparency and gloss when the density of the greaseproof paper is increased.

[0087] When the pigment is kaolin, the average particle size of the kaolin is preferably 0.5 μm or more, more preferably 1 μm or more. Also, the average particle size of the kaolin is preferably 20 μm or less, more preferably 10 μm or less. When the average particle size of the kaolin is within the above range, the obtained functional layer (oil-resistant layer) has excellent oil resistance.

[0088] Examples of organic pigments include solid, hollow, or through-hole type particles of polydienes such as polyisoprene, polyneoprene, and polybutadiene; polyalkenes such as polybutene, polyisobutylene, and polypropylene; polymers or copolymers of vinyl monomers such as vinyl acetate, styrene, (meth)acrylic acid, (meth)acrylic acid alkyl esters, (meth)acrylamide, and methyl vinyl ether; polyurethane resins, polyester resins, polyamide resins, urea resins, melamine resins, and benzoguanamine resins.

[0089] The pigment content is not particularly limited. For example, the pigment content is preferably 20% by mass or more, more preferably 40% by mass or more, based on the total solid content of the oil-resistant coating agent. The pigment content is preferably 70% by mass or less, more preferably 65% ​​by mass or less, based on the total solid content of the oil-resistant coating agent. By having the pigment content within the above range, the obtained oil-resistant layer has excellent oil resistance and water resistance.

[0090] The styrene-butadiene copolymer is blended to impart excellent water resistance (water repellency) to the functional layer. The styrene-butadiene copolymer is obtained by copolymerizing styrene and butadiene as monomers. When a water-insoluble copolymer is used, the copolymer may be used in the form of a latex. The styrene-butadiene copolymer of this embodiment is not particularly limited. For example, the styrene-butadiene copolymer is "A6160" commercially available from Asahi Kasei Corporation.

[0091] The glass transition temperature (Tg) of the styrene-butadiene copolymer is preferably 30°C or lower, more preferably 20°C or lower, and even more preferably 0°C or lower. The Tg of the styrene-butadiene copolymer is preferably -40°C or higher, more preferably -30°C or higher, and even more preferably -20°C or higher. When the Tg of the styrene-butadiene copolymer is within the above range, the obtained oil-resistant layer can exhibit excellent film-forming ability and excellent water-repellency and oil-resistance.

[0092] The average particle size of the styrene-butadiene copolymer is preferably 0.01 μm or more, more preferably 0.03 μm or more. The average particle size of the styrene-butadiene copolymer is preferably 1.0 μm or less, more preferably 0.5 μm or less. When the average particle size of the styrene-butadiene copolymer is within the above range, the styrene-butadiene copolymer has excellent water dispersibility.

[0093] The content of the styrene-butadiene copolymer is not particularly limited. For example, the content of the styrene-butadiene copolymer is preferably 20% by mass or more, more preferably 25% by mass or more, based on the total solid content of the oil-resistant coating agent. The content of the styrene-butadiene copolymer is preferably 50% by mass or less, more preferably 45% by mass or less, based on the total solid content of the oil-resistant coating agent. By having the content of the styrene-butadiene copolymer within the above range, the oil-resistant coating agent can form an oil-resistant layer on the paper substrate that is excellent in water resistance (water repellency) in addition to oil resistance.

[0094] The polyvinyl alcohol is not particularly limited. For example, the polyvinyl alcohol is a polyvinyl alcohol-based resin such as unmodified fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, or modified polyvinyl alcohol. The modified polyvinyl alcohol is ethylene-modified polyvinyl alcohol, carboxy-modified polyvinyl alcohol, silicon-modified polyvinyl alcohol, acetoacetyl group-modified polyvinyl alcohol, diacetone group-modified polyvinyl alcohol, or the like. Among these, unmodified fully saponified polyvinyl alcohol, ethylene-modified polyvinyl alcohol, and carboxy-modified polyvinyl alcohol are preferred because they can impart excellent oil resistance. Furthermore, ethylene-modified polyvinyl alcohol can suppress the thickening of the oil-resistant coating agent. This makes the oil-resistant coating agent excellent in coating suitability. In addition, the oil-resistant layer obtained has an excellent coated surface condition.

[0095] The content of the polyvinyl alcohol-based resin is not particularly limited. For example, the content of the polyvinyl alcohol-based resin is preferably 0.5% by mass or more, more preferably 3% by mass or more, based on the total solid content of the oil-resistant coating agent. The content of the polyvinyl alcohol-based resin is preferably 20% by mass or less, more preferably 10% by mass or less, based on the total solid content of the oil-resistant coating agent. When the content of the polyvinyl alcohol-based resin is within the above range, the oil-resistant layer obtained can exhibit better oil resistance. Furthermore, the polyvinyl alcohol-based resin can suppress thickening of the oil-resistant coating agent. This allows the oil-resistant coating agent to suppress the occurrence of coating defects.

[0096] The aqueous medium may be water alone, or may be an aqueous medium obtained by mixing water with a water-miscible organic solvent such as an alcohol, such as methanol, ethanol, or propanol; a polyhydric alcohol, such as ethylene glycol or propylene glycol, or an alkyl ether derivative thereof; an ester, such as ethyl formate, methyl acetate, or ethyl acetate; or a ketone, such as acetone.

[0097] Next, we will explain an oil-resistant coating agent that contains a styrene-acrylic copolymer, wax, and an aqueous medium.

[0098] Examples of the styrene-acrylic copolymer include styrene-acrylic copolymers obtained by copolymerizing styrene or a styrene derivative with acrylic acid (methacrylic acid) and alkyl acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate, and alkyl methacrylates such as methyl methacrylate, and the like. A styrene-acrylic copolymer emulsion is preferred.

[0099] Examples of the wax include polyolefin waxes such as paraffin wax, carboxyl group-containing paraffin wax, microcrystalline wax, polyethylene wax, carboxyl group-containing polyethylene wax, polypropylene wax, and ethylene-propylene copolymer wax, candelilla wax, rice wax, montan wax, fatty acids such as stearic acid, fatty acid amides such as stearic acid amide, stearic acid bisamide, oleic acid amide, and palmitic acid amide, and fatty acid metal salts such as zinc stearate and calcium stearate. The wax content is preferably 1.5 to 20 mass% of the total solid content of the oil-resistant coating agent.

[0100] The aqueous medium may be water alone, or may be an aqueous medium obtained by mixing water with a water-miscible organic solvent such as an alcohol, such as methanol, ethanol, or propanol; a polyhydric alcohol, such as ethylene glycol or propylene glycol, or an alkyl ether derivative thereof; an ester, such as ethyl formate, methyl acetate, or ethyl acetate; or a ketone, such as acetone.

[0101] The method for producing the oil-resistant coating agent is not particularly limited. For example, the oil-resistant coating agent can be prepared by mixing a pigment, a styrene-butadiene copolymer, polyvinyl alcohol and an aqueous medium, or by mixing a styrene-acrylic copolymer, a wax and an aqueous medium, and thoroughly stirring and mixing the mixture at room temperature.

[0102] When the functional layer is an oil-resistant layer, the thickness of the oil-resistant layer is not particularly limited. For example, the thickness of the oil-resistant layer is preferably 1 μm or more, more preferably 3 μm or more. The thickness of the oil-resistant layer is preferably 20 μm or less, more preferably 10 μm or less. When the thickness of the oil-resistant layer is within the above range, the obtained laminate has excellent oil resistance.

[0103] When the functional layer is a water-resistant layer The water-resistant layer is provided by applying a water-resistant coating agent. The water-resistant coating agent is not particularly limited. For example, the water-resistant coating agent may be a water-resistant coating agent containing a styrene-acrylic copolymer, a wax, and an aqueous medium.

[0104] The styrene-acrylic copolymer is not particularly limited. For example, the styrene-acrylic copolymer is a styrene-acrylic copolymer obtained by copolymerizing styrene and a styrene derivative with acrylic acid (methacrylic acid) and alkyl acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate, or alkyl methacrylates such as methyl methacrylate, etc. Among these, the styrene-acrylic copolymer is preferably a styrene-acrylic copolymer emulsion.

[0105] The wax is not particularly limited. For example, the wax may be paraffin wax, carboxyl group-containing paraffin wax, microcrystalline wax, polyethylene wax, carboxyl group-containing polyethylene wax, polypropylene wax, ethylene-propylene copolymer wax, or other polyolefin wax, candelilla wax, rice wax, montan wax, fatty acid such as stearic acid, fatty acid amide such as stearic acid amide, stearic acid bisamide, oleic acid amide, palmitic acid amide, or other fatty acid metal salt such as zinc stearate or calcium stearate. The wax content is preferably 1.5 to 20 mass% of the total solid content of the water-resistant coating agent.

[0106] The aqueous medium may be water alone, or may be an aqueous medium obtained by mixing water with a water-miscible organic solvent such as an alcohol, such as methanol, ethanol, or propanol; a polyhydric alcohol, such as ethylene glycol or propylene glycol, or an alkyl ether derivative thereof; an ester, such as ethyl formate, methyl acetate, or ethyl acetate; or a ketone, such as acetone.

[0107] The method for producing the water-resistant coating agent is not particularly limited. For example, the water-resistant coating agent can be prepared by mixing a styrene-acrylic copolymer, a wax, and an aqueous medium, and thoroughly stirring and mixing the mixture at room temperature.

[0108] When the functional layer is a water-resistant layer, the thickness of the water-resistant layer is not particularly limited. For example, the thickness of the water-resistant layer is preferably 1 μm or more, more preferably 3 μm or more. The thickness of the water-resistant layer is preferably 20 μm or less, more preferably 10 μm or less. When the thickness of the water-resistant layer is within the above range, the obtained laminate has excellent water resistance.

[0109] When the functional layer is a water-repellent layer The water-repellent layer is provided by applying a water-repellent coating agent. For example, the water-repellent coating agent contains a water repellent agent, an aqueous medium, and, if necessary, an inorganic pigment.

[0110] The water repellent is not particularly limited. For example, the water repellent is a water-based coating agent containing paraffin-based hydrocarbons (e.g., Brightone FC-350 manufactured by Sakata Inx Corporation), a wax-based water repellent (e.g., Celestial 40R manufactured by Lion Specialty Chemicals Corporation), etc. The water repellent is not limited to paraffin-based. The water repellent may contain modified wax components such as microcrystalline wax, polyethylene wax, and maleic petroleum resin. The wax-based component may contain rosin-based resin or unsaturated higher alcohol, etc.

[0111] The aqueous medium may be water alone, or may be an aqueous medium obtained by mixing water with a water-miscible organic solvent such as an alcohol, such as methanol, ethanol, or propanol; a polyhydric alcohol, such as ethylene glycol or propylene glycol, or an alkyl ether derivative thereof; an ester, such as ethyl formate, methyl acetate, or ethyl acetate; or a ketone, such as acetone.

[0112] There is no particular limitation on the method for producing the water-repellent coating agent. As an example, the water-repellent coating agent can be prepared by mixing the water-repellent agent and an aqueous medium, and thoroughly stirring and mixing the mixture at room temperature.

[0113] When the functional layer is a water-repellent layer, the thickness of the water-repellent layer is not particularly limited. For example, the thickness of the water-repellent layer is preferably 1 μm or more, more preferably 3 μm or more. The thickness of the water-repellent layer is preferably 20 μm or less, more preferably 10 μm or less. When the thickness of the water-repellent layer is within the above range, the obtained laminate has excellent water repellency.

[0114] Returning to the explanation of the folding endurance agent, the folding endurance agent of the present embodiment is applied to a laminate in which various functional layers are provided on a paper substrate, so as to form a folding endurance layer between the paper substrate and the functional layer. In the obtained laminate, the function of the functional layer is unlikely to deteriorate before and after folding.

[0115] <Laminate and method for producing the laminate> The laminate according to one embodiment of the present invention is a laminate in which a paper base layer, a folding-resistant layer, and a functional layer are laminated in this order. The folding-resistant layer is a layer formed by applying the above-mentioned folding-resistant agent.

[0116] The paper base layer, the folding-resistant layer and the functional layer that constitute the laminate are as described above in relation to the embodiment of the folding-resistant agent.

[0117] The method of manufacturing the laminate is not particularly limited. For example, the laminate can be produced by applying a folding resistance agent to a paper base layer, and then applying various functional coating agents (moisture-proof coating agent, gas barrier coating agent, oil-resistant coating agent, water-resistant coating agent, water-repellent coating agent). The folding resistance agent and the functional coating agent applied may be dried after each application, or may be dried together after both applications.

[0118] The coating weight of the folding-resistant layer (solid content equivalent) is 1g / m 2 It is preferable that the content is 3 g / m or more. 2The coating amount of the folding-resistant layer (solid content equivalent) is preferably 30 g / m or more. 2 It is preferable that the thickness is less than 20 g / m 2 When the coating amount of the fold-resistant layer is within the above range, the obtained laminate exhibits excellent fold resistance.

[0119] When the functional layer is a moisture-proof layer, the coating amount of the moisture-proof coating agent (converted into solid content) is 1 g / m 2 It is preferable that the content is 3 g / m or more. 2 It is more preferable that the coating amount of the moisture-proof coating agent (converted into solid content) is 30 g / m or more. 2 It is preferable that the thickness is less than 20 g / m 2 When the coating amount of the moisture-proof coating agent is within the above range, the laminate exhibits excellent moisture proofness.

[0120] When the functional layer is a gas barrier layer, the coating amount of the gas barrier coating agent (converted into solid content) is 0.1 g / m 2 It is preferable that the content is 0.5 g / m or more. 2 It is more preferable that the coating amount of the gas barrier coating agent (converted into solid content) is 10 g / m or more. 2 It is preferable that the thickness is less than 5 g / m 2 When the coating amount of the gas barrier coating agent is within the above range, the laminate exhibits excellent gas barrier properties.

[0121] When the functional layer is an oil-resistant layer, the coating amount of the oil-resistant coating agent (converted into solid content) is 1 g / m 2 It is preferable that the content is 3 g / m or more. 2 It is more preferable that the coating amount of the oil-resistant coating agent (converted into solid content) is 20 g / m or more. 2 It is preferable that the thickness is less than 10 g / m 2 When the coating amount of the oil-resistant coating agent is within the above range, the laminate exhibits excellent oil resistance.

[0122] When the functional layer is a water-resistant layer, the coating amount of the water-resistant coating agent (converted into solid content) is 1 g / m 2 It is preferable that the content is 3 g / m or more. 2 It is more preferable that the coating amount of the water-resistant coating agent (converted into solid content) is 20 g / m or more. 2 It is preferable that the thickness is less than 10 g / m 2 When the coating amount of the water-resistant coating agent is within the above range, the laminate exhibits excellent water resistance.

[0123] When the functional layer is a water-repellent layer, the coating amount of the water-repellent coating agent (converted into solid content) is 1 g / m 2 It is preferable that the content is 3 g / m or more. 2 It is more preferable that the coating amount of the water-repellent coating agent (converted into solid content) is 20 g / m or more. 2 It is preferable that the thickness is less than 10 g / m 2 When the coating amount of the water-repellent coating agent is within the above range, the laminate exhibits excellent water repellency.

[0124] As described above, according to the present embodiment, in a laminate in which various functional layers are provided on a paper base material, a fold-resistant layer containing the above-mentioned fold-resistant agent is formed between the paper base material and the functional layer, so that the function of the functional layer in the obtained laminate is unlikely to deteriorate before and after folding. EXAMPLES

[0125] The present invention will be described in more detail below with reference to the following examples. The present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass". The figures for the amounts of each material in the tables are "parts by mass".

[0126] The raw materials used are shown below. <Paper base material> OK Blizzard (grammage 70g / m 2 (manufactured by Oji Materia Co., Ltd.)

[0127] <Damp-proof coating agent> To 60.0 parts of anionic binder (Zaixen A, solids content 25%, manufactured by Sumitomo Seika Chemicals Co., Ltd.), 25.0 parts of an inorganic layered compound (Somasif ME300B-4T, solids content 8%, manufactured by Katakura Co-op Agri Co., Ltd.) was added under stirring, and 2.0 parts of a modified amide resin (Sumirez (registered trademark) Resin SPI-203 (50) H, manufactured by Taoka Chemical Co., Ltd.) as a dispersant and 13 parts of ion-exchanged water were further added and stirred to obtain a moisture-proof coating agent.

[0128] <Oil-resistant coating agent> The oil-resistant coating agent used was INXKote WB FLEXO FDA GREASE RES AC4551.

[0129] <Bending resistance agent> Polyurethane resin 1 (Superflex 460S, Daiichi Kogyo Seiyaku Co., Ltd.) Polyurethane resin 2 (Superflex 210, Daiichi Kogyo Seiyaku Co., Ltd.) Acrylic resin 1 (DXA.4081, manufactured by VANORA) Acrylic resin 2 (Neocryl A-1125, manufactured by Covestro) Polyvinyl alcohol resin 1 (OKS-1009, manufactured by Mitsubishi Chemical Corporation) Polyvinyl alcohol resin 2 (BVE8049Q, manufactured by Mitsubishi Chemical Corporation) Polyvinyl alcohol resin 3 (OKS-8118, manufactured by Mitsubishi Chemical Corporation) Styrene-butadiene resin 1 (Smartex VA-1015, Nippon A&L Co., Ltd.) Styrene-butadiene resin 2 (Nipol LX407S12, Zeon Corporation)

[0130] <Manufacturing method of folding resistance agent> As shown in Table 1, polyurethane resins 1 and 2, acrylic resin 1, and styrene-butadiene resins 1 and 2 were diluted with a medium (ion-exchanged water) to a solid content of 30%, to obtain folding-resistant agents 1-3, 8, and 9. For acrylic resin 2, the original solution was used as folding-resistant agent 4. In addition, polyvinyl alcohol resins 1-3 were dissolved in a solvent (ion-exchanged water) to obtain solutions with a solid content of 10%, to obtain folding-resistant agents 5-7.

[0131] [Table 1]

[0132] <Example 1> On one side of the paper base material, the bending resistance agent 1 is applied in an amount of 3 g / m2 after drying. 2 After coating with a bar coater, the layer was dried with a dryer at 60°C to form a folding-resistant layer. An oil-resistant agent was then applied on top of the layer so that the coating amount after drying was 6 g / m 2 After coating with a bar coater so as to obtain the above composition, the coating was dried with air from a dryer at 60° C. to form an oil-resistant layer, thereby preparing a laminate for evaluating oil resistance of Example 1.

[0133] <Examples 2 to 8> Laminates for evaluating oil resistance and laminates for evaluating moisture proofness were prepared in the same manner as in Example 1, except that folding resistance agents 1, 3, 5, and 6 were used for the oil resistant layer and the moisture proof layer in the combinations shown in Table 2 below.

[0134] <Comparative Examples 1 and 2> Each functional layer was applied to one side of the paper substrate with a coating weight of 6 g / m2 after drying. 2 After coating with a bar coater so as to obtain the above composition, the coating was dried with air from a dryer at 60° C. to form an oil-resistant layer, thereby preparing a laminate for evaluating oil resistance or a laminate for evaluating moisture proofness of Comparative Examples 1 and 2.

[0135] <Comparative Examples 3 to 10> Laminates for evaluating oil resistance and laminates for evaluating moisture proofness were prepared in the same manner as in Example 1, except that folding resistance agents 2, 4, 7, and 9 were used for the oil resistant layer and the moisture proof layer in the combinations shown in Table 2 below.

[0136] The degree of elongation and the degree of shape restoration of the fold-resistant layer were evaluated by the following evaluation methods. The results are shown in Table 2.

[0137] The obtained laminate was evaluated for moisture resistance and oil resistance according to the type of functional layer. These evaluations were performed before and after bending as described below. The results are shown in Table 2.

[0138] (Method for measuring the elongation of the folding-resistant layer) A folding resistance agent was applied to a glass substrate, dried, and peeled off to prepare a JIS K 6251 tensile No. 3 dumbbell-shaped test piece (film thickness 300 μm). Next, the elongation of each test piece was measured when it was pulled to breakage using the following test machine under the following conditions. Tensile testing machine: AGS-X, manufactured by Shimadzu Corporation Stretching speed: 300mm / min Temperature: 23℃ Humidity: 50% The degree of elongation is calculated by the following formula: Elongation degree (%)=100×(Lb-L0) / L0 Here, Lb refers to the gauge length at break, and L0 refers to the gauge length before the tensile test. The tensile test is a tensile test performed in accordance with JIS K 6251.

[0139] (Method for evaluating shape recovery of folding-resistant agent) The degree of shape recovery was evaluated by carrying out a tensile test according to JIS K 6251. The tensile test for evaluating the degree of shape recovery was carried out using the following test machine under the following conditions. A folding resistance agent was applied to a glass substrate, dried, and peeled off to prepare a JIS K 6251 tensile type 3 dumbbell-shaped test piece (film thickness 300 μm). Next, each test piece was stretched using the following test machine under the following conditions and held in that state for 5 minutes. Thereafter, the test piece was removed from the test machine, and the length of the test piece after 3 hours was measured. Tensile testing machine: AGS-X, manufactured by Shimadzu Corporation Stretching speed: 50mm / min Temperature: 23℃ Humidity: 50% The degree of shape restoration is calculated by the following formula. Shape restoration rate (%) = 100 × (L1-L2) / (L1-L0) Here, L0 refers to the gauge length before the tensile test. L1 refers to the gauge length at 100% elongation in the tensile test, and for those that cannot be elongated to 100%, it is the limit gauge length without breakage. L2 is the gauge length when the external force is removed after the tensile test.

[0140] (How to fold) A 4000g roller was rolled at a speed of 30cm / sec and passed over the laminate 10 times to make the first crease in the laminate. The laminate with the crease was opened, and a second crease was made in the same manner as the first crease, perpendicular to the first crease. The laminate was folded so that the side coated with the coating agent was on the inside.

[0141] (Oil resistance) 0.03 g of salad oil was dropped onto the coated surface of the laminate (on the intersection of the fold for the folded sample). After 90 minutes, the area of ​​the salad oil seeping through to the back side was measured, and the extent to which the stain area had been reduced was evaluated compared to when no folding-resistant layer was provided. Note that when no folding-resistant layer was provided (Comparative Example 1), the stain area was 12.4 cm 2 In addition, in all of the Examples and Comparative Examples, when no creases were made in the laminate, there was absolutely no bleeding to the back surface.

[0142] (Moisture resistance) The laminate obtained above was measured for water vapor transmission rate (WVTR value, g / m2) in accordance with JIS Z 0208-1976. 2 / day) was measured. The temperature and humidity conditions were a temperature of 40±0.5°C and a relative humidity of 90±2%. The deterioration value of the water vapor transmission rate was calculated before and after folding, and the extent to which the deterioration value had been reduced was evaluated compared to when no folding-resistant layer was provided. Note that when no folding-resistant layer was provided (Comparative Example 2), the water vapor transmission rate before folding was 25.6 g / m 2 / day, water vapor transmission rate after folding is 56.6g / m 2 / day, and the degradation value is 31.0g / m 2 It was / day.

[0143] [Table 2]

[0144] As shown in Table 2, it was found that the laminates obtained using the folding endurance agents of Examples 1 to 8 of the present invention were less susceptible to deterioration in the function of the functional layer before and after folding.

Claims

1. A laminate in which a paper base layer, a folding-resistant layer, and a functional layer are laminated in this order, The following conditions 1 to 3 are met: A folding-resistant agent for forming the folding-resistant layer (excluding the case where the folding-resistant agent is OKS-1009 and the functional layer is an active energy ray-curable ink composition layer). (Condition 1) The folding resistance agent includes a resin and a medium, the resin includes at least one selected from the group consisting of a polyurethane resin, an acrylic resin, a polyester resin, a polyvinyl alcohol resin, a styrene-butadiene resin, and a vinyl chloride resin; The content of the resin (calculated as solid content) in the folding endurance agent is 70 to 100% by mass. (Condition 2) The degree of elongation of the fold-resistant layer in a tensile test determined by the following formula is 200% or more. Elongation degree (%) = 100 x (Lb-L0) / L0 Here, Lb indicates the gauge length at break, and L0 indicates the gauge length before the tensile test. The tensile test is a tensile test performed in accordance with JIS K 6251. (Condition 3) The shape recovery rate of the folding-resistant layer, calculated by the following formula, is 80% or more. Shape restoration rate (%) = 100 × (L1 - L2) / (L1 - L0) Here, L0 refers to the gauge length before the tensile test. L1 refers to the gauge length at 100% elongation in the tensile test, and for those that cannot be elongated to 100%, it is the limit gauge length at which the material does not break. L2 is the gauge length of the fold-resistant layer when the external force is removed after the tensile test, and the tensile test is a tensile test performed in accordance with JIS K 6251.

2. The folding endurance agent according to claim 1 , wherein the functional layer includes at least one layer selected from the group consisting of a moisture-proof layer, a gas barrier layer, an oil-resistant layer, a water-resistant layer, and a water-repellent layer.

3. A paper base layer, a folding-resistant layer, and a functional layer are laminated in this order, 3. A laminate, wherein the folding-resistant layer is a layer formed by applying the folding-resistant agent according to claim 1 or 2.

Citation Information

Patent Citations

  • Resin composition, water-proof and moistureproof paper using the same, and its production method

    JP2002220494A

  • Water-based emulsion adhesive

    JP2009057490A

  • Method for producing moisture-proof paper

    JP2009155780A

  • Base paper for paper container

    JP2014077212A

  • Migration-preventing coating agent

    JP2023007353A

Cited By

  • Laminate and method for manufacturing a laminate

    JP2026165657A

  • Bending-resistant materials and laminates

    JP7716559B1