Composite thermal barrier coating
The composite thermal barrier coating with a bonding, insulating, and sealing layer addresses the inefficiencies of existing coatings by reducing heat transfer and maintaining engine efficiency through low thermal conductivity and reliable bonding.
Patent Information
- Application Number
- DE102017103229
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-02-15
- Filing Date
- 2017-02-16
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2037-02-16
AI Technical Summary
Existing thermal barrier coatings for internal combustion engines do not effectively balance low thermal conductivity and reliable bonding of multiple layers, leading to heat transfer losses and inefficiencies.
A composite thermal barrier coating comprising three layers: a bonding layer, an insulating layer made of sintered hollow microspheres with high porosity, and a sealing layer, designed to withstand high temperatures and prevent gas permeability, ensuring low thermal conductivity and low heat capacity.
The composite coating reduces heat transfer losses, maintains engine efficiency, and minimizes temperature fluctuations, enhancing catalyst activity and reducing knocking, while maintaining the engine's ability to breathe.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The disclosure generally relates to a composite thermal barrier coating. BACKGROUND
[0002] Internal combustion engines have multiple cylinders, multiple pistons, at least one intake port, and at least one exhaust port. The cylinders each have surfaces that define a combustion chamber. One or more surfaces of the internal combustion engine are coated with thermal barrier coatings to improve the heat transfer characteristics of the internal combustion engine.
[0003] EP 2 175 116 A1 describes a composite thermal barrier coating comprising a first, second, and third layer. The first layer is designed to be bonded to a substrate, while the second layer is bonded to the first layer and comprises a plurality of hollow microspheres bonded together. The third layer is bonded to the second layer and is impermeable to combustion gases such that the third layer forms a seal with the second layer.
[0004] DE 10 2006 039 756 A1 describes a similar composite thermal barrier coating.
[0005] US 8 356 482 B2 also describes a similar composite thermal barrier coating.
[0006] Furthermore, WO 2015 / 042 491 A1 also describes a similar composite thermal barrier coating in which hollow microspheres are coated with a nickel-based material.
[0007] US 2009 / 0 202 814 A1 describes a layer that is bonded to a substrate and comprises particles that in turn may consist of several layers.
[0008] CN 104 018 139 A describes hollow microbeads that have a coating of several layers.
[0009] EP 0 211 557 A2 describes a metal-ceramic multilayer system.
[0010] Furthermore, the entry “Cenosphere” in Wikipedia (URL: http: / / de.wikipedia.org / w / index.php) describes hollow microspheres made of aluminum or silicon oxide.
[0011] An object of the invention is to provide a composite thermal barrier coating having low thermal conductivity and reliable bonding of multiple layers. SUMMARY
[0012] This object is achieved by a thermal barrier coating having the features of claim 1.
[0013] The composite thermal barrier coating (TBC) can be applied to a surface of components in an internal combustion engine. The composite TBC is bonded to the engine components to provide insulation sealed against combustion gases with low thermal conductivity and low heat capacity.
[0014] The composite TBC comprises three layers bonded together: a first layer (bonding layer), a second layer (insulating layer), and a third layer (sealing layer). The insulating layer is sandwiched between the bonding layer and the sealing layer. The bonding layer is bonded to the component and to the insulating layer.
[0015] The insulation layer comprises hollow microspheres sintered together to form the insulation, which provides low effective thermal conductivity and low effective heat capacity.
[0016] The sealing layer is a thin film designed to withstand the high temperatures found in an engine. The sealing layer is impermeable to gases and has a smooth surface.
[0017] The composite TBC exhibits low thermal conductivity to reduce heat transfer losses and low heat capacity, allowing the surface temperature of the composite TBC to follow the gas temperature in the combustion chamber. Therefore, the composite TBC allows the component's surface temperatures to fluctuate with gas temperatures. This reduces heat transfer losses without compromising the engine's ventilation capability and without causing knocking. Furthermore, it reduces the heating of cold air entering the engine cylinder. Additionally, exhaust gas temperatures are increased, resulting in a shorter catalyst light-off time and improved catalyst activity.
[0018] The foregoing features and advantages, as well as other features and advantages of the present teachings, will be readily apparent from the following detailed description of the best modes for carrying out the present teachings when taken in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a schematic diagram of a vehicle illustrating a side view of a single-cylinder internal combustion engine having a composite thermal barrier coating disposed on multiple components. Fig. Figure 2 is a schematic cross-sectional side view of the composite thermal barrier coating disposed on the component. Fig. 3 is a schematic cross-sectional side view of another embodiment of the composite thermal barrier coating disposed on the component. Fig. Figure 4 is a schematic cross-sectional side view of a portion of hollow microspheres each having a first and a second metallic cover layer. Fig. Figure 5 is a schematic cross-sectional side view of the hollow microspheres section of Fig. 4, wherein the first and second metallic covering layers are sintered together; Fig. Figure 6 is a schematic cross-sectional side view of the hollow microspheres section of Fig. 5, wherein the first and second metallic covering layers are bonded together by diffusion to form a metal alloy. DETAILED DESCRIPTION
[0019] Those skilled in the art will recognize that terms such as "above," "below," "upward," "downward," "at the top," "at the bottom," etc., are used to describe the figures and are not limitations on the scope of the disclosure as defined by the appended claims.
[0020] Referring to the drawings, in which like reference numerals refer to like components throughout the views, Fig. 1 illustrates a portion of an exemplary vehicle 10. The vehicle 10 may include an engine 13 with a component 12. The component 12 has a composite (multi-layer) thermal barrier coating (TBC) 14 of the type disclosed herein applied thereto.
[0021] Although the vehicle 10 and the engine 13 of Fig. 1 illustrates a typical example application suitable for the composite TBC 14 disclosed herein, the present design is not limited to vehicle and / or engine applications. Any stationary or mobile machine or article of manufacture in which a component is subject to heat may benefit from the use of the present design. For consistency of illustration, the vehicle 10 and engine 13 are described below as an example system, without limiting the use of the composite TBC 14 to such an embodiment.
[0022] Fig. 1 illustrates an engine 13 defining a single cylinder 26. However, those skilled in the art will recognize that the present disclosure may also be applied to components 12 of engines 13 having multiple cylinders 26. Each cylinder 26 defines a combustion chamber 30. The engine 13 is configured to provide power for propelling the vehicle 10. The engine 13 may be, but is not limited to, a diesel engine or a gasoline engine.
[0023] The engine 13 further includes an intake assembly 36 and an exhaust manifold 38, each in fluid communication with the combustion chamber 30. The engine 13 includes a reciprocating piston 28 that is slidably movable within the cylinder 26.
[0024] The combustion chamber 30 is configured to combust an air / fuel mixture to provide energy for propulsion of the vehicle 10. Air may enter the combustion chamber 30 of the engine 13 by passing through the intake assembly 36, in which airflow from the intake manifold into the internal combustion engine 30 is controlled by at least one intake valve 32. Fuel is injected into the combustion chamber 30 to be mixed with the air or is introduced through the intake valve(s) 32, thereby providing an air / fuel mixture. The air / fuel mixture is ignited in the combustion chamber 30. Combustion of the air / fuel mixture produces exhaust gas, which exits the combustion chamber 30 and is drawn into the exhaust manifold 38. More specifically, an air flow (exhaust gas flow) from the combustion chamber 30 is controlled by at least one exhaust valve 34.
[0025] With reference to Fig. 1 and Fig. 2, the composite TBC 14 may be disposed on a face or surface of one or more of the components 12 of the engine 13, i.e., the piston 28, the intake valve 32, the exhaust valve 34, internal walls of the exhaust manifold 38, the combustion dome 39, and the like. The composite TBC 14 is bonded to the component 12 to form an insulator configured to reduce heat transfer losses, improve efficiency, and increase the exhaust gas temperature during operation of the engine 13. The composite TBC 14 is configured to provide low thermal conductivity and low heat capacity. Thus, the low thermal conductivity reduces heat transfer losses, and the low heat capacity means that the surface of the composite TBC 14 follows the temperature of the gas during temperature fluctuations and that the heating of cold air entering the cylinder is minimized.
[0026] With reference to Fig. 2, each component 12 includes a substrate 16 having a surface 18, and the composite TBC 14 is bonded to the surface 18 of the substrate 16. The composite TBC 14 may include three layers: a first layer (bonding layer) 20, a second layer (insulating layer) 22, and a third layer (sealing layer) 24. However, depending on the material involved, it should be appreciated that in certain embodiments, the TBC 14 may not include the first bonding layer 20, as an outer portion of the insulating layer 22 may be configured to bond directly to the substrate 16. For example, if the first bonding layer 20 comprises nickel (Ni) and the substrate 16 comprises iron (Fe), the first layer 20 may not be required. However, the composite TBC 14 may include more than three layers, as explained in more detail below.
[0027] The insulation layer 22 comprises a plurality of hollow microspheres 40 sintered together to create a layer with extremely high porosity. Preferably, the porosity of the insulation layer 22 is at least 80%. More preferably, the porosity of the insulation layer 22 is at least 95%. The high porosity ensures that a corresponding volume of air and / or gases is contained therein, thereby providing the desired insulation properties of low effective thermal conductivity and low effective heat capacity. The thickness T2 of the insulation layer 22 is between 100 micrometers (µm) and 1 millimeter (mm). More preferably, the thickness T2 of the insulation layer 22 is between 100 and 500 µm. Even more preferably, the thickness T2 of the insulation layer 22 is between 100 and 300 µm. The insulation layer 22 is designed to withstand pressures of at least 80 bar.More preferably, the insulation layer 22 is configured to withstand pressures of at least 100 bar. Even more preferably, the insulation layer 22 is configured to withstand pressures of at least 150 bar. Additionally, the insulation layer 22 is temperature-configured to withstand surface temperatures of at least 300 degrees Celsius (°C). More preferably, the insulation layer 22 is configured to withstand temperatures of at least 500°C. Even more preferably, the insulation layer 22 is configured to withstand temperatures of at least 1100°C. The heat capacity of the TBC 14 is configured to ensure that the surface of the substrate 16 is not heated above 500°C.
[0028] The hollow microspheres 40 may be comprised of hollow polymer, metal, glass, and / or ceramic spheres 45. The hollow spheres 45 are coated with metal, such as nickel or iron alloys. In one non-limiting embodiment, the hollow microspheres 40 are comprised of metal, such as nickel, nickel alloy compounds, and the like. At least one metallic capping layer 44 may be disposed on an outer surface of each sphere 45. The metallic capping layer 44 may comprise nickel (Ni). The metallic capping layer 44 may be disposed on the outer surface of the microspheres 40 by electroplating, flame spraying, painting, electroless plating, vapor deposition, and the like.It will be appreciated that the hollow spheres 45, which are composed of a polymer, a metal, and a glass with a melting temperature lower than that of the metallic cover layer 44, may melt or otherwise dissolve during the bonding or sintering of the metallic-coated microspheres to become part of the metallic cover layer 44, or may melt and transform into a lump of material within the hollow microsphere 40. However, if the melting temperature of the hollow sphere 45 is higher than the melting temperature of the material of the metallic cover layer 44, such as when the hollow sphere 45 is formed from a ceramic material, the hollow sphere 45 remains intact and does not dissolve or become absorbed. The metallic cover layer 44 may comprise nickel, iron, and the like. The hollow microspheres 40 may have a diameter D1 between 5 and 100 µm.More preferably, the microspheres 40 may have a diameter D1 between 20 and 100 µm. Even more preferably, the microspheres 40 may have a diameter D1 between 20-40 µm. It will be appreciated that the microspheres do not necessarily have the same diameter, as a mixture of diameters may be formed to provide a desired open porosity, i.e., packing density, to deliver a desired amount of strength to the insulating layer. Several of the hollow microspheres 40 may be molded or sintered at a sintering temperature under pressure for a molding time until bonds are formed between the cover layers 44 of adjacent hollow microspheres 40 forming the insulating layer 22. The sintering temperature may approach the melting temperature of the metallic cover layer 44.However, in the case where the hollow balls 45 are made of a ceramic material, the sintering temperature is not below the melting temperature of the metal-coated balls 45.
[0029] According to another embodiment described in Fig. 4 - 6, the insulation layer 22 may be formed from hollow microspheres 40 that initially have two metallic cover layers 44A, 44B. First, Fig. 4, the hollow microsphere 40 initially has a first (inner) metallic covering layer 44A coated with a second (outer) metallic covering layer 44B. The inner metallic covering layer 44A comprises nickel (Ni), which is subsequently coated with the outer metallic covering layer 44B comprising copper (Cu or Cu-Zn). The outer metallic coating 44B of Cu or Cu-Zn is applied to the inner metallic covering layer 44A by electroplating, flame spraying, painting, electroless plating, vapor deposition, and the like to form the outer metallic covering layer 44B. A thickness of the outer metallic covering layer 44B should be thinner than a thickness of the inner metallic covering layer 44A. Furthermore, a weight of the metallic material (i.e., the Cu or Cu-Zn) of the outer metallic covering layer 44B cannot be much greater than a weight of the metal (i.e.,of the Ni) of the inner metallic cap layer 44A. Thus, the weight of the Cu material of the second metallic cap layer 44B is not much greater than the weight of the Ni of the inner metallic cap layer 44A. Preferably, the weight of the Cu material of the outer metallic cap layer 44B is less than the weight of the inner metallic cap layer 44A for a maximum temperature. It is important to maintain a low amount of Cu because too much Cu lowers the melting temperature of the resulting alloy material.
[0030] With reference to Fig. 2 and Fig. 3, the coated microspheres 40 are arranged in a desired layer having a desired thickness T2. Referring to Fig. 5, the microspheres 40 are heated to a temperature approximately equal to or above the melting temperature of the outer metallic cover layer 44B. Thus, the temperature is sufficient to cause soldering or melting of the second cover layer. Referring to Fig. 6, the temperature is next reduced below the solidus temperature. The temperature is maintained for a period of time below the solidus temperature, but at a temperature sufficient for diffusion to occur between the copper (Cu or Cu-Zn) of the outer metallic capping layer 44B and the nickel (Ni) of the first metallic capping layer 44A. Thus, solid-state diffusion occurs between the respective inner and outer metallic capping layers 44A, 44B to form a metallic alloy capping layer 44C. Therefore, the resulting insulating layer 22 includes a nickel-copper alloy (Ni-Cu or Ni-Cu-Zn alloy) layer 44C surrounding the hollow microspheres 40. The amount of diffusion that occurs between the inner and outer metallic capping layers 44A, 44B is a function of the temperature and time used for the microspheres 40.Additionally, diffusion bonding can be performed at an elevated pressure to equalize pressure in each of the microspheres and the atmosphere.
[0031] Additionally, when the hollow microspheres 40 are formed from a ceramic and heated to promote bonding between adjacent microspheres 40, the spheres 45 upon which the inner metallic cover layer 44A is disposed may melt. In cases where the hollow spheres 45 are formed from a polymer, a metal, and glass, the hollow spheres 45 may melt as a function of the material properties of the hollow spheres 45 and the sintering temperature applied to the microspheres 40. When melting of the hollow spheres 45 occurs, the inner metallic cover layer 44A is no longer a "coating," but instead becomes an inner wall 46 of the microsphere 40.
[0032] With reference to Fig. 2, the bonding layer 20 is configured to bond to the surface 18 of the substrate 16 and to the insulating layer 22 such that the insulating layer 22 is secured to the substrate 16. According to one non-limiting embodiment, the bonding layer 20 is configured to diffuse into the surface 18 of the substrate 16 and into the insulating layer 22 to form interconnections therebetween. According to one non-limiting embodiment, the substrate 16 comprises aluminum, the insulating layer 22 comprises nickel-coated microspheres 40, and the bonding layer 20 comprises brass, i.e., a copper-zinc (Cu-Zn) alloy material. The Cu-Zn content is determined to produce optimal bond strength, optimal thermal expansion properties, optimal heat treatment operations, optimal fatigue resistance, and the like.Copper and zinc exhibit good solid-state solubility in aluminum, nickel, and iron, while iron and nickel exhibit very low solid-state solubility in aluminum. Therefore, the bond layer 20 comprising copper and zinc combinations provides a structural interlayer that enhances the diffusion bond between the adjacent aluminum substrate 16 and the adjacent nickel or iron insulation layer 22. However, it should be understood that the substrate 16, insulation layer 22, and bond layer 20 are not limited to aluminum, nickel, and brass, but may include other materials.
[0033] One side of the bonding layer 20 may be disposed over the surface 18 of the substrate 16, such that the bonding layer 20 is disposed between the substrate 16 and the insulating layer 22. A compressive force may be applied to the insulating layer 22 and the substrate 16 at a bonding temperature for at least a minimum application time. The melting temperature of the material of the bonding layer 20 is lower than the melting temperature of each of the substrate 16 and the material of the insulating layer 22. According to another embodiment, the melting temperature of the material of the bonding layer 20 is between the melting temperature of each of the substrate 16 and the material of the insulating layer 22.Furthermore, the required bonding temperature may be lower than the melting temperature of the material of the substrate 16 and the material of the insulating layer 22, but sufficiently high enough to cause diffusion bonding to occur between the metallic material of the substrate 16 and the metallic material of the bonding layer 20, as well as between the metallic material of the substrate 16 and the metallic material of the insulating layer 22.
[0034] With reference to Fig. 2, it can be seen that the interconnect layer 20 may be bonded to an inner surface of the insulation layer 22 before the interconnect layer 20 is bonded to the surface 18 of the substrate 16.
[0035] Additionally, the bonding layer 20 is not limited to being bonded to the surface 18 of the substrate 16 and / or the insulating layer 22 by means of solid state diffusion, as other methods of adhesion may also be used, such as wetting, soldering, and combinations thereof.
[0036] Now on Fig. 3, the insulating layer 22 may comprise more than one layer. More specifically, the insulating layer 22 may comprise a microstructured layer 22A and a transition layer 22B. The microstructured layer 22A is a layer comprising the plurality of hollow microspheres 40 bonded together as described above. The transition layer 22B may comprise nickel or iron. More specifically, the metallic material of the transition layer 22B and the coating of the microspheres 40 of the microstructured layer 22A are identical to assist in the bonding between the layers 22A, 22B. Thus, the microspheres 40 in a peripheral region of the microstructured layer 22A are bonded to the transition layer 22B when the microstructured layer 22A and the transition layer 22B are heated to a temperature sufficient to bond the microsphere layer (i.e., the insulating layer 22) to the transition layer 22B of the metallic material (i.e.,Nickel, iron, and the like). The microstructure layer 22A is formed to have a thickness T2 between 100 µm and 1 mm. More preferably, the thickness T2 of the microstructure layer 22A is between 100 and 500 µm. Even more preferably, the thickness T2 of the microstructure layer 22A is between 100 and 300 µm. The microstructure layer 22A is designed to withstand pressures of at least 150 bar and surface temperatures of at least 1100°C.
[0037] The transition layer 22B is bonded to the coating 44 of the individual microspheres 40 at contact points 46. The transition layer 22B provides a support structure or backbone for the microsphere layer 22A, thereby imparting strength and rigidity to the insulating layer 22. Thus, the strength and rigidity of the insulating layer 22 are a function of a thickness of the transition layer 22B. Additionally, the transition layer 22B is bonded to the interconnect layer 20 opposite the microstructure layer 22A, such that the interconnect layer 20 is disposed between the substrate 16 and the transition layer 22B of the insulating layer 22. Thus, the transition layer 22B is disposed in a facing contact relationship with the interconnect layer 20.Upon exposure of the transition layer and the bond layer to heat for a sufficient period of time, metal diffusion occurs between the bond layer 20 and the substrate 16, and between the bond layer 20 and the transition layer 22B of the insulation layer 22. The transition layer 22B provides a larger surface contact area for the bond layer 20 to support a larger area for diffusion bonding than when the transition layer 22B is not used, and the microspheres 40 of the microstructure layer 22A are directly bonded to the bond layer 20 by diffusion (as shown in FIG. Fig. 2 is shown).
[0038] It will be appreciated that any desired number of interconnect layers 20 may be deposited having the desired properties as long as the interconnect layer 20 is bonded to the insulating layer 22 and the substrate 16.
[0039] With further reference to Fig. 2, the sealing layer 24 is disposed over the insulating layer 22 such that the insulating layer 22 is disposed between the sealing layer 24 and the connecting layer 20. The sealing layer 24 is a high-temperature thin film. More specifically, the sealing layer 24 comprises a material designed to withstand temperatures of at least 1100°C. The sealing layer 24 is designed to be thin, i.e., to have a thickness T3 of no more than 20 µm. More preferably, the sealing layer 24 is designed to have a thickness T3 of no more than 5 µm. The sealing layer 24 is impermeable to combustion gases, thus creating a seal between the sealing layer 24 and the insulating layer 22.Such sealing prevents contaminants from combustion gases, such as unburned hydrocarbons, soot, partially reacted fuel, liquid fuel, and the like, from entering the porous structure defined by the hollow microspheres 40. If such contaminants were allowed to enter the porous structure, the air contained within the porous structure would ultimately be displaced by the contaminants, and the insulating properties of the insulating layer 22 would be reduced or eliminated.
[0040] The sealing layer 24 may be formed to have an outer surface 42 that is smooth. The presence of a smooth sealing layer 24 may be important to prevent the generation of turbulent airflow as air flows over the outer surface 42 of the sealing layer 24. Furthermore, the presence of a sealing layer 24 with a smooth surface prevents an increased heat transfer coefficient. According to one non-limiting example, the sealing layer 24 may be applied to the insulating layer 22 by electroplating or vapor deposition. According to another non-limiting example, the sealing layer 24 may be applied to the insulating layer 22 simultaneously with the sintering of the insulating layer 22.
[0041] The sealing layer 24 is designed to be sufficiently elastic to resist rupture or cracking during exposure to combustion gases, thermal fatigue, or contaminants. Furthermore, the sealing layer 24 is designed to be sufficiently elastic to resist expansion and / or contraction of the underlying insulation layer 22.
[0042] With further reference to Fig.3, the sealing layer 24 may comprise more than one layer. More specifically, the sealing layer 24 may comprise a first barrier layer 24A and a second barrier layer 24B. The first barrier layer 24A may be disposed on the insulating layer 22, and the second barrier layer 22B may be disposed on the first barrier layer 24A, such that the first barrier layer 24A is disposed between the second barrier layer 24B and the insulating layer 22. The second barrier layer 24B may be formed to have the outer surface 42 that is smooth. The first barrier layer 24A and the second barrier layer 24B may be stacked to provide desired properties, such as extremely high temperature resistance and corrosion resistance.By way of non-limiting example, the second barrier layer 24B provides corrosion resistance and extremely high temperature resistance, while the first barrier layer 24A provides a seal against the underlying insulation layer 22 to prevent contaminants from entering open spaces defined between the microspheres 40 of the underlying insulation layer 22. It will be appreciated that any desired number of sealing layers 24 may be applied, providing the desired properties, as long as the sealing layer 24 provides a seal against the underlying insulation layer 22 to prevent contaminants or gases from entering the open spaces defined by the microspheres 40. In addition, a thickness T3 of the sealing layer 24 is preferably no greater than 20 µm, regardless of the number of individual barrier layers.More preferably, the thickness T3 of the sealing layer 24 is formed to have a thickness T3 of not more than 5 µm.
[0043] Furthermore, the bonding layer 20, the insulating layer 22 and the sealing layer 24 are each formed to have suitable thermal expansion coefficient properties to withstand thermal fatigue.
[0044] It is understood that the composite TBC 14 can be applied to components other than those found in an internal combustion engine. More specifically, the composite TBC 14 can be applied to components of aircraft, rockets, injection molds, and the like.
[0045] Although the best modes for carrying out many aspects of the present teachings have been described in detail, those skilled in the art to which these teachings apply will recognize various alternative aspects for practicing the present teachings that are within the scope of the appended claims.
Claims
[1] A composite thermal barrier coating (14) comprising: a first layer (20) configured to be bonded to a substrate (16); a second layer (22) connected to the first layer (20); wherein the second layer (22) comprises a plurality of hollow microspheres (40) bonded together; and a third layer (24) connected to the second layer (22); wherein the third layer (24) is impermeable to combustion gases such that the third layer (24) seals off the second layer (22); wherein the first layer (20) is configured to be bonded to a substrate (16) comprising a metal; wherein each of the plurality of hollow microspheres (40) has a metallic coating (44) such that adjacent microspheres (40) of the plurality of hollow microspheres (40) are bonded together at the respective coatings (44); wherein the second layer (22) comprises a microstructure layer (22A) and a transition layer (22B); wherein the transition layer (22B) is connected to the first layer (20) by diffusion and the transition layer (22B) is connected to the microstructure layer (22A); wherein the first layer (20) comprises a copper-based material, a zinc-based material and / or an alloy comprising copper and zinc; wherein the coating (44) of each of the plurality of hollow microspheres (40) comprises a nickel-based material and / or an iron-based material; and wherein the transition layer (22B) comprises a nickel-based material and / or an iron-based material, such that the transition layer (22B) is bonded to the first layer (20) by diffusion and the transition layer (22B) is sintered to the coating (44) of the adjacent hollow microspheres (40) of the plurality of microspheres (40). [2] The composite thermal barrier coating (14) of claim 1, wherein the coating (44) further comprises a copper-based material and / or an alloy comprising copper and nickel. [3] The composite thermal barrier coating (14) of claim 1, wherein the second layer (22) has a porosity of at least 80%. [4] The composite thermal barrier coating (14) of claim 3, wherein the second layer (22) has a porosity of at least 95%. [5] The composite thermal barrier coating (14) of claim 1, wherein a thickness (T3) of the third layer (24) is not greater than 20 µm. [6] The composite thermal barrier coating (14) of claim 5, wherein a thickness (T3) of the third layer (24) is not greater than 5 µm. [7] Composite thermal barrier coating (14) according to claim 6, wherein the third layer (24) comprises a first barrier layer (24A) and a second barrier layer (24B); wherein the first barrier layer (24A) is connected to the second layer (22) and the second barrier layer (24B) is connected to the first barrier layer (24A) such that the first barrier layer (24A) is arranged between the second barrier layer (24B) and the second layer (22).
Citation Information
Patent Citations
Hollow microsphere / Ni-Fe-P / Cu composite coating and preparation method thereof
CN104018139A
shielding component, in particular a heat shield
DE102006039756A1
Metal-ceramics jointed articles
EP0211557A2