Electrode ink composition and fuel cell

The electrode ink composition with a platinum group metal catalyst and a secondary polymer that interacts via non-covalent bonding addresses the issue of dry cracking in fuel cell membranes, enhancing durability by accelerating the gel point and reinforcing the carbon microstructure.

DE102018104351B4Active Publication Date: 2024-11-28GM GLOBAL TECHNOLOGY OPERATIONS LLC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE102018104351
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-03-02
Filing Date
2018-02-26
Publication Date
2024-11-28
Estimated Expiration
2038-02-26

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Electrode ink composition, including: a solvent; a catalyst composition containing platinum group metals, dispersed in the solvent; a primary polymer dispersed in the solvent, wherein the primary polymer is an ionomer; and a secondary polymer dispersed in the solvent, wherein the secondary polymer interacts with the primary polymer via a non-covalent interaction; wherein the secondary polymer has an overlap concentration that is at least three times lower than the overlap concentration of the ionomer, wherein at the overlap concentration the polymer chains of the ionomer and the secondary polymer are just touching in solution.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present description concerns fuel cell membranes with improved durability and in particular fuel cell membranes in which drying cracks are mitigated and an electrode ink composition.

[0002] The electrode layer in proton exchange fuel cells (PEFCs) is typically applied using an ink containing a platinum or platinum alloy catalyst dispersed on a carbon black support, a perfluorosulfonic acid ionomer (PFSA), and an alcohol-water solvent. The carbon black support provides gas transport for reactants to the catalyst and product water to the flow channel, while the PFSA ionomer provides proton conduction to the catalyst and binding of the porous carbon network.

[0003] However, during the drying of the applied ink film, cracks can develop through the solvent, which directly affects the durability of the manufactured membrane electrode assembly (MEA) during fuel cell operation. 2 effects. As an example, it shows Fig. 1 the polymer flow and the resulting thickness reduction, which in a 25 µm thick NAFION ® -Membrane failure occurs when an electrode ruptures after a moisture cycle. Cell failure occurs as soon as a continuous rupture forms in the separator membrane due to reactant gas leakage between the anode and cathode layers.

[0004] The electrode layer has a high porosity of approximately 70 vol.% for optimal gas transport, which in turn results in low fracture toughness. Consequently, the coated ink film is prone to cracking through the layer during solvent drying. In addition to a uniform tensile stress derived from solvent capillary pressure within the consolidated carbon black mesopore volume, local tensile stress can also develop from uneven penetration of the ink ionomer solution into a porous coating substrate. Both stresses typically occur when the electrode ink is applied directly to gas diffusion media (CCDM or catalyst coating diffusion media), which then necessitate mechanical reinforcement of the fragile carbon microstructure to prevent cracking during solvent drying.

[0005] US 2013 / 0040222A1 describes a catalyst layer composition for a fuel cell comprising an ionomer cluster, a catalyst, and a solvent containing water and a polyhydric alcohol; and an electrode for a fuel cell comprising a catalyst layer comprising an ionomer cluster with a three-dimensional network-like structure and a catalyst, a method for producing an electrode for a fuel cell comprising a catalyst layer comprising an ionomer cluster with a three-dimensional network-like structure and a catalyst, and a membrane electrode assembly for a fuel cell comprising the electrode, and a fuel cell system comprising the membrane electrode assembly.

[0006] US 2008 / 0161429A1 describes a process for producing free-flowing and liquid-dispersible particles of a highly fluorinated ion-exchange polymer, in which a dispersion of a highly fluorinated ion-exchange polymer in a liquid consisting of at least 10 wt% of an organic liquid is provided, atomized to produce droplets, and released into an inert, heated gas. The dispersion droplets dry to produce free-flowing particles of highly fluorinated ion-exchange polymer with dry external surfaces and an internal residual moisture content of at least 4 wt%.

[0007] DE 10 2012 222 049 A1 describes an ink composition for the formation of a fuel cell electrode and, in particular, a fuel cell cathode layer. The ink composition comprises a first ionomer containing a protogenic group and having an equivalent weight of less than 800, an optional second ionomer containing a protogenic group and having an equivalent weight greater than 800, and a catalyst composition.

[0008] US 2015 / 0051064A1 describes electrocatalytic compositions comprising a platinum-based electrocatalyst and polyvinylpyrrolidone (PVP), wherein the PVP enhances certain properties of the platinum-based electrocatalyst. The electrolytic compositions described here are used in fuel cell technology.

[0009] Accordingly, there is a need for methods to improve fuel cell membranes by reducing electrode drying cracks.

[0010] The invention is defined by the independent claim.

[0011] The present invention solves one or more prior art problems by providing an electrode ink composition that forms fuel cell catalyst layers with reduced electrode dry cracking. The ink composition comprises a solvent, a catalyst composition containing platinum group metals dispersed in the solvent, a primary ionomer dispersed in the solvent, and a secondary polymer dispersed in the solvent, the secondary polymer interacting with the primary ionomer via a non-covalent interaction. The secondary polymer has an overlap concentration that is at least three times lower than the overlap concentration of the ionomer, and at this overlap concentration, the polymer chains of the ionomer and the secondary polymer are just in contact in solution.

[0012] According to an example, a fuel cell is provided which includes a catalyst layer formed from the ink composition described above. The fuel cell includes an anode catalyst layer, a cathode catalyst layer, a proton-conducting membrane arranged between the anode catalyst layer and the cathode catalyst layer, a first gas diffusion layer arranged above the anode catalyst layer, a second gas diffusion layer arranged above the cathode catalyst layer, an anode flow field plate arranged above the first gas diffusion layer, and a cathode flow field plate arranged above the second gas diffusion layer.Characteristically, at least one of the anode catalyst layer and the cathode catalyst layer includes a platinum group metal-containing catalyst composition, a primary ionomer, and a secondary polymer that interacts with the primary ionomer via a non-covalent interaction in solution.

[0013] As an example, a method for reducing electrode dry cracking in a fuel cell is provided. In this regard, the gel point of the ionomer solution in the electrode ink is manipulated to provide mechanical reinforcement. The gel point is accelerated by mixing the primary PFSA ionomer in solution with a secondary PFSA ionomer or another polymer that also provides strong chain association through either hydrogen or ionic bonding. The secondary ionomer or polymer accelerates the solidification or gel point of the ink solution during solvent drying. Both schemes have been shown to provide the necessary mechanical reinforcement of the fragile carbon microstructure to prevent cracking during the CCDM electrode fabrication process.

[0014] In one example, a secondary ionomer with significant chain expansion and extension is selected in a solution, which is then treated with NAFION. ® It is mixed to force strong chain association via hydrogen bonding (H-bonding) at its more accessible sulfonic acid sites. In one example, a high molecular weight polyvinyl-2-pyrrolidone (PVP) polymer is mixed with NAFION. ® , in order to effect a strong chain association via ionic bonding between the cationic ammonium and anionic sulfonate sites on each polymer. Fig. Figure 1 shows a scanning electron microscope image showing the polymer membrane flow during an electrode rupture after a moisture cycle. 2 . Fig. Figure 2 provides a schematic representation of a fuel cell containing catalyst layers with reduced dry cracking. Fig. 3A, Fig. 3B, Fig. 3C and Fig.3D illustrations depict the chemical structure of commercial polymers used in this invention: A. SSC-PFSA ionomer. B. MSC-PFSA ionomer. C. NAFION ® LSC-PFSA ionomer. D. PVP homopolymer. In Fig. 4 is the logarithmic dependence 10 plotted against the intrinsic viscosity of the molecular weight, measuring a consistent Mark-Houwink exponent over commercially available PFSA ionomer structures. Fig. Figure 5A shows a universal curve for the dependence of the normalized intrinsic viscosity on the equivalent weight, which is independent of the specific side chain structure of the sulfonate monomer. Fig. Figure 5B shows a universal curve for the how-conserved ionomer with increasing M. w at lower EW for the dependence of the measured intrinsic viscosity on the equivalent weight, which is independent of the specific side chain structure of the sulfonate monomer. Fig. Figure 6 shows the growth of the elastic modulus (G') for the drying of NAFION ® -Ionomer solutions. The rheometer used a cone-plate geometry of 60 mm (Ti, 1°) at a voltage amplitude of 0.2 Pa, 0.5 Hz and a time average of 100 s. Fig. Figure 7 shows Tan δ (or G'' / G') for drying NAFION ® -Ionomer solutions. Fig. 8. The alcohol-water composition for 6.0% NAFION ® The solution is monitored with proton NMR during the drying of the solvent. Fig. 9A and Fig. 9B. Recorded light micrographs show the significant reduction in cracking of the CCDM electrode at the same dry thickness (16 µm) after mixing the primary NAFION. ® -Ionomers with PVP polymer or SS700 ionomer in the electrode ink solution. A. I(NAFION) ® ) / C = 1.4 B. NAFION ® mixed with 2% PVP polymer or 25% SS700 ionomer.

[0015] Reference is now made in detail to currently preferred compositions, embodiments, and methods of the present invention, which represent the best ways of carrying out the invention currently known to the inventors. The figures are not necessarily to scale. It is understood, however, that the described embodiments are merely exemplary of the invention, which can be carried out in various and alternative forms. Therefore, the specific details described herein are not to be understood as limitations, but merely as a representative basis for the various aspects of the invention and / or as a representative basis for conveying the various application possibilities to those skilled in the field.

[0016] Except as provided in the examples or where expressly stated, all numerical data concerning material quantities or reaction or usage conditions in this description are to be understood as being modified by the addition of "approximately" to describe the invention to the widest possible extent. Implementation within the specified numerical limits is generally preferred.Furthermore, unless expressly stated otherwise: percentages, "parts of," and ratios by weight; where a group or class of materials is described as suitable or preferred for a particular purpose in connection with the invention, this means that mixtures of two or more members of the group or class are equally suitable or preferred; the first definition of an acronym or other abbreviation applies to all subsequent uses of the same abbreviation and also applies accordingly to normal grammatical variations of the abbreviation initially defined. Finally, unless expressly stated otherwise, a property is measured using the same technique as previously or subsequently specified for the same property.

[0017] It is further understood that this invention is not limited to the specific embodiments and methods described below, as certain components or conditions may naturally vary. Furthermore, the terminology used here serves only to describe different embodiments of the present invention and is in no way to be understood as limiting.

[0018] It is further noted that, as used in the specification and the attached claims, the singular forms "ein / e" and "der / die / das" also include plural references, unless the context clearly indicates otherwise. For example, a singular reference to a component is intended to encompass a multitude of components.

[0019] The term "comprehensive" is synonymous with "including," "exhibiting," "containing," or "characterized by." These terms are to be interpreted inclusively and broadly, and do not exclude additional unspecified elements or procedural steps.

[0020] The phrase "consisting of" excludes any element, step, or component not specified in the claim. If this phrase appears in a section of the main body of a claim, rather than immediately following the introduction, it limits only the element described in that section; other elements are not excluded from the claim as a whole.

[0021] The phrase “essentially consisting of” limits the scope of a claim to the specified materials or steps, plus those which do not substantially affect the basic and novel feature(s) of the claimed subject matter.

[0022] The terms "comprising", "consisting of" and "essentially consisting of" may be used interchangeably. Where one of these three terms is used, the subject matter described and claimed herein may include the use of one of the other two terms.

[0023] Descriptions of the publications referenced in this application are deemed to be incorporated in full by reference into this application in order to more accurately describe the prior art to which this invention relates. Abbreviations:

[0024] "SSC" means short side chain. "MSC" means medium side chain. "LSC" means long side chain.

[0025] With reference to Fig.Figure 2 provides an idealized schematic cross-section of a fuel cell incorporating catalyst layers with reduced electrode dry cracking. The PEM fuel cell 10 includes a polymeric ion-conducting membrane 12 arranged between the cathode catalyst layer 14 and the anode catalyst layer 16. The fuel cell 10 also includes electrically conductive flow field plates 20, 22, which contain gas channels 24 and 26. The flow field plates 20, 22 are either bipolar plates (shown) or unipolar plates (i.e., end plates). In one embodiment, the flow field plates 20, 22 are formed from a metal plate (e.g., stainless steel) optionally coated with a noble metal, such as gold or platinum. In another embodiment, the flow field plates 20, 22 are formed from conductive polymers, which are also optionally coated with a noble metal.Furthermore, gas diffusion layers 32 and 34 are arranged between flow field plates and a catalyst layer. The catalyst layer of the cathode 14 and the catalyst layer of the anode 16 comprise carbon-supported catalysts prepared by the processes described below. Advantageously, at least one of the cathode catalyst layer 14 and the anode catalyst layer 16 is formed from the catalyst layer described below. In one refinement, the cathode catalyst layer 14 is formed from this ink composition. In another non-exclusive refinement, the anode catalyst layer 16 is formed from this ink composition.

[0026] In one embodiment, an electrode ink composition is provided that is suitable for forming the catalyst layers in a fuel cell with reduced electrode dry cracking. The ink composition comprises a solvent, a platinum group metal-containing catalyst composition dispersed in the solvent, a primary ionomer dispersed in the solvent, and a secondary polymer dispersed in the solvent. The platinum group metal-containing catalyst composition comprises a platinum group metal (e.g., Pt, Pd, Au, Ru, Ir, Rh, or Os) and, in particular, platinum. In a refinement, the platinum group metal-containing catalyst composition comprises an alloy of a platinum group metal and a transition metal (e.g., Co and / or Ni). Typically, the platinum group metal-containing catalyst composition includes a support (e.g.,Carbon particles) on which the platinum group metal is arranged. In one refinement, the ink composition includes the platinum group-containing catalyst composition in an amount of 1% to 10% by weight of the total ink composition. In another refinement, the primary ionomer and the secondary polymer are each present independently in an amount of approximately 1% to approximately 20% by weight of the total ink composition. In yet another refinement, the primary ionomer and the secondary polymer are each present independently in an amount of approximately 2% to approximately 10% by weight of the total ink composition. In some refinements, the amounts of the primary ionomer and the secondary polymer are approximately equal.In a further refinement, the ink composition includes the solvent in an amount of approximately 70% to approximately 97% by weight of the total ink composition. Usable solvents include, but are not limited to, water, alcohols (e.g., ethanol, propanol), combinations of water and alcohols, and the like. Characteristically, the secondary polymer interacts with the primary ionomer via a non-covalent interaction.

[0027] In one variant, the secondary polymer interacts with the primary ionomer via hydrogen bonding. In another variant, the secondary polymer interacts with the primary polymer via ionic bonding. Specifically, both variants utilize hydrogen or ionic bonding of a primary NAFION. ®-Ionomers with a secondary polymer. This mixing scheme can be extended to other secondary polymers that have a sufficient molecular weight (M w > 250 kD), low overlap concentration (c * < 0.20 wt.% in ethanol : water : 1 wt.%) and effective sites for association with the sulfonate anion on a primary PFSA ionomer such as NAFION ® .

[0028] In most refinements, the primary polymer is a perfluorosulfonic acid polymer (PFSA). A particularly suitable primary polymer is provided by formulas I or II: where n averages between 1 and 10; m is 1, 2, or 3; o averages from about 30 to 800; and p is 1, 2, or 3. In one refinement, n is approximately 5; m is 1; and o averages from about 300 to 700.

[0029] Regarding the variation that utilizes a hydrogen bond interaction, secondary PFSA ionomers with a high chain expansion coefficient in an alcohol-water solution and a long chain length are particularly useful in this application because they are stable in the fuel cell operating condition and contribute to the primary ionomer functions: namely, proton conduction to the Pt catalyst and bonding in the electrode layer. Table 1 lists other commercially available PFSA ionomers for mixing into the electrode ink solution, while the Fig. 3A-3C illustrate their chemical composition. For the Fig. In 3A-C, n is on average between 1 and 10 and m is 1, 2, or 3. In commercially available examples of Fig. 3A has an equivalent weight of 720 g / mol with n = 4.4 and m = 1, or an equivalent weight of 830 g / mol with n = 5.5 and m = 1. In commercially available examples of Fig.3B has an equivalent weight of 825 g / mol with n = 4.5 and m = 1, or an equivalent weight of 980 g / mol with n = 6.0 and m = 1. In commercially available examples of Fig. 3C has an equivalent weight of 950 g / mol with n = 5.1 and m = 1 or an equivalent weight of 1050 with n = 6.1 and m = 1.

[0030] The primary and secondary polymers are characterized by their equivalent weights and molecular weights. The ionomer equivalent weight (EW) is defined as the polymer weight per mole of sulfonic acid and is expressed in units of g / mol. The EW measurement involves releasing the acidic hydrogen ion in 1 N NaCl solution formulated in a 400 M excess, which is then titrated with 10.0 ± 0.1 mN NaOH solution using a Mettler-Toledo DL15 autotitrator instrument. The weight-mean molecular weight of the ionomer (M) w ) and the intrinsic viscosity (η) are measured by size exclusion chromatography (SEC). 10An Agilent 1100 series instrument was equipped with an isocratic pump, an autosampler, and a dual-wavelength spectrophotometric detector, an Agilent PD2020 dual-angle LS (light scattering) detector, a Malvern Model 270 DV (viscosity detector), and a Waters Corporation Model 410 DRI (refractive index detector). The DV and DRI were positioned in parallel after the spectrophotometric and LS detectors. Three Agilent Olexis 7.5 × 300 mm columns at 35.0 °C were used with N,N-dimethylformamide (DMF) containing 0.1 M LiNO₃. The eluent was pre-filtered using 0.22 µm Millipore GS filters. The columns were calibrated using 15 Agilent polymethyl methacrylate (PMMA) narrow standards with a molar mass between 0.58 and 1400 kDa. The injection volumes were 100 µL, and the optimal injected sample concentration was 0.5–2.0 mg / mL. The wavelength of the LS detector laser diode was 680 nm.The specific refractive increment (dn / dc) of PMMA at 680 nm was estimated to be 0.062 ml / g. The peak area reaction factor of the DRI detector was calculated from narrow PMMA standards, and the dn / dc values ​​of the perfluorinated ionomers were then estimated from their integrated DRI detector reactions. The LS detector was calibrated using isotropically scattering PMMA standards of known molar mass.

[0031] Regarding the variation that uses ionic bonding, the secondary polymers are hydrocarbon polymers with functional groups that can accept a proton (e.g., amino polymers or inimine-containing polymers). Therefore, hydrocarbon polymers in this ionic bonding class acquire a cation charge in a typical ink solution with pH(e) < 2. This is achieved when the basic functional group has a pKa > 5. A particularly useful secondary polymer that interacts with the primary polymer via ionic bonding is a high molecular weight polyvinyl-2-pyrrolidone (PVP). A structure for PVP is given in Fig.3D is provided, where n averages 5000 to 15000. A particularly useful weight-average molecular weight for PVP is about 1000 kDa. Specific additional examples of the second polymer interacting via ionic bonding include, but are not limited to, polyamides, polyamide-amines, poly(2-ethyl-2-oxazoline), poly(alkyl- and / or -aryl-substituted oxazolines), poly(hydroxyalkyl acrylates), poly(hydroxyalkyl methacrylates), poly(hydroxyalkyl ethyleneimines), polyacrylamides, poly(dimethylaminoalkyl acrylates), poly(dimethylaminoalkyl methacrylates), poly(diallyldimethylammonium chloride), poly(aminophosphazenes), poly(alkylaminophosphazenes), and combinations thereof. In some refinements, secondary polymers interacting via ionic bonds are characterized by having a high weight-average molecular weight.In particular, the weight-mean molecular weight of the secondary polymer in this number of variations is equal to or greater than or equal to, in ascending order of preference, 400 kDa, 500 kDa, 600 kDa, or 700 kDa. In a further refinement, the weight-mean molecular weight of the secondary polymer is equal to or less than or equal to, in descending order of preference, 1200 kDa, 1100 kDa, 1000 kDa, or 800 kDa. In some refinements, the equivalent weight of the secondary polymer using ionic bonding is approximately 50 to 500 g / mol. In other refinements, the equivalent weight of the secondary polymer using ionic bonding is approximately 100 to 300 g / mol.

[0032] The primary ionomer and the secondary polymer are characterized by their respective limiting viscosity and overlap concentration, which measure chain expansion in solution. For a spherical particle in suspension or polymer chain conformation in solution, the Einstein equation (1) gives the solution viscosity (η) at dilute concentration for a given solvent viscosity (η). s ) and volume fraction (ϕ). A more expanded chain conformation increases the volume fraction occupied by the polymer (ϕ), which in turn increases the solution viscosity (η). η−ηsηs=2.5φ

[0033] The transition between dilution and semidilute occurs at the overlap concentration (c*) at which the polymer chains in solution just touch. For uncharged polymers, the inverse viscosity [η] converges to a plateau value with decreasing concentration; unloaded* is then simply determined in equation (2) by the reciprocal of [η], where η sp = specific viscosity. limc→0η−ηsηsc=limc→0ηspc=[η] cungeladene*=1[η]

[0034] In contrast, ionic polymer chains change their solution conformation below the dilute limit or in the presence of free salt by counterionizing the native charge density along their backbone. As a result, the chain extension of ionic polymers is measured by the intrinsic viscosity at a consistent free salt concentration above the concentration of the ionic monomer in solution, or by the overlap concentration in the absence of any free salt concentration.

[0035] The marginal viscosity of commercially available PFSA ionomers is compared in Table 1 with their corresponding equivalents and weight-mean molecular weights. The SEC method 10An ionomer solution was autoclaved at 230 °C in 0.1 wt% n-propanol (nPrOH): water (H₂O)₄: 1 wt% solution, diluted to 0.075 wt% with dimethylformamide (DMF), and then concentrated to 0.20 wt% by slow nitrogen drying. The elution solvent was DMF with a 100 mM LiNO₃ salt, which is significantly higher than the ionic monomer concentration (1–2 mM) in solution. Table 1. Ionomer properties Company Side chain (type) Product type EW (g / mol) M w kD) Side chain (molar-%) n:m (mol / M ol) # ) #) EC[η ] dl / g) SEC[ŋ] (300kD , dl / g) Dupont LSC (NAFION® ) 2021 1 050 20 1 6,5 % 6 .1 ,081 0 ,077 Dupont LSC (NAFION® ) 2020 9 50 20 1 6,5 % 5 .1 ,095 0 ,091 Supplier A SSC S700 7 20 20 1 9,2 % 4 .4 ,260 0 ,177 Supplier B SSC 83-20 8 30 20 1 5,3% 5 ,5 ,200 0 ,136 Supplier C MS C - 8 25 60 1 8,3°% 4 ,5 ,150 0 ,132 Supplier C MS C - 9 80 30 1 4,3 % 6 ,0 ,095 0 ,089

[0036] Fig. Figure 4 shows the dependence of the ionomer limiting viscosity on the molecular weight in nPrOH:H2O:DMF solvent with 100 mM LiNO3. The Mark-Houwink equation (3) describes the intrinsic viscosity dependence for a polymer solution with a molecular weight (M). The exponent (a MH The value ranges from 0.5 (theta limit or poor solvent quality) to 0.8 (good solvent quality) for flexible polymers. All commercial PFSA ionomers in Table 1 show a consistent value.MH = 0.70, which allows for a simple prediction of the influence of molecular weight on ionomer chain expansion. [η]=K∗Ma

[0037] Similarly, it shows Fig. 5. The dependence of the ionomer marginal viscosity on the equivalent weight in the SEC solvent system. In this case, there is a single universal curve to predict the equivalent weight influence on the ionomer chain expansion.

[0038] The overlap concentration for ionic polymers is also measured in the absence of free salt, which reduces the counterion screening of the native charge density along its backbone. This represents a limiting case that more closely approximates the elongation of the native ionomer chain in an electrode ink, since the concentration of the free salt is typically far below that of the ionic monomer. The overlap concentration (c*) is measured in a dilution series where the solution viscosity only doubles the native solvent viscosity (η). s ). η(cgeladene*)=2∗ηs

[0039] Table 2 shows the relative chain expansion for SS700 (EW720) compared to NAFION. ®(EW950) ionomer in H₂O versus ethanol (EtOH):H₂O:1:1 wt% solution. The ionomer chains are compressed in poor solvent (water only), as shown by an overlap concentration at 2–3 wt% solution. However, the SS700 ionomer opens significantly more than the Nafion. ® -Ionomer in EtOH:H₂O::1:1 wt% solvent, as indicated by overlap concentrations of 0.060% versus 0.63% wt% solution. The relative chain expansion between the two ionomer types is four times higher in the overlap than in the intrinsic viscosity measurement due to the counterion screening of the free salt present in the latter case. Table 2. Ionomer chain expansion Ionomer EW SEC[η] c** (wt% solution) (Type) (g / mol) (dl / g) (H2O) (EtOH:H2 O::1:1) LSC (NAFION®) 950 0,095 2,7 % 0,63 % SSC (SS700) 720 % 0,260 2,1 % 0,060 %

[0040] In one variation, the primary polymer for the system, which uses hydrogen bonds, is a long side-chain polymer with an equivalent weight of 850 to 1050 g / mol and a weight-average molecular weight of 250 to 500 kDa. In one refinement, the secondary polymer is a short side-chain polymer with an equivalent weight of 500 to 850 g / mol and a weight-average molecular weight of 300 to 2000 kDa. In another refinement, the secondary polymer is a long-sided chain polymer with an equivalent weight of 550 to 850 g / mol and a weight-average molecular weight of 500 to 1500 kDa.

[0041] In a variation of the present embodiment, the secondary polymer requires a significantly higher intrinsic viscosity, or equivalently, a lower overlap concentration, than the primary ionomer. Typically, the secondary polymer exhibits an overlap concentration that is at least three times lower than that of the primary polymer. If the secondary polymer has a chemical PFSA structure, the equivalent and molecular weight are selected in combination to achieve this intrinsic overlap concentration.

[0042] In another refinement, the secondary polymer has an overlap concentration that is at least 5 times lower than the overlap concentration of the primary polymer. In yet another refinement, the secondary polymer has an overlap concentration that is at least 10 times lower than the overlap concentration of the primary polymer. In further refinements, the secondary polymer has an overlap concentration that is at most 15 to 20 times lower than the overlap concentration of the primary polymer. In some refinements, the secondary polymer has an overlap concentration that is 5 to 20 times lower than the overlap concentration of the primary polymer. Although the relationship regarding the overlap concentration applies to both variations of the secondary polymer (i.e.,(Ionic bonding and hydrogen bonding) is applicable, it is most useful for the examples that use hydrogen bonding.

[0043] The following examples illustrate the different embodiments of the present invention. Those skilled in the art will recognize many variations within the present invention and the scope of the claims.

[0044] An electrode ink is prepared using a 30% PtCo alloy catalyst nanoparticle carried on Ketjen Black and reacted with NAFION in n-propanol-water solvent (nPrOH: H2O::3:1 wt%). ® The primary ionomer is dispersed. This represents a typical cathode ink composition for the fabrication of PEFC cells. The ink is then applied directly to commercial diffusion media (catalyst-coated diffusion medium, CCDM), which can lead to uneven permeation of the ionomer solution into its porous structure.

[0045] Fig. Figure 6 shows the relative growth of the solid-like or elastic modulus (G') of four NAFION ® -Ionomer solutions during solvent evaporation at 25 °C. The comparison example uses only NAFION. ® The ionomer is formulated with a 5.0 wt% solution in nPrOH: H₂O::3:1 wt%. This primary ionomer solution shows no increase in the solution elasticity modulus up to the last measurement at 20% solids content, whereas both preferred embodiments show an increasing solid-like modulus, reaching 0.20 Pa at 16% solids. These embodiments blend either the secondary PFSA-SSC ionomer or PVP polycation while maintaining the initial polymer concentration at 5.0 wt% solution.

[0046] In the ionic bond variation, PVP homopolymer exhibits a very low equivalent weight of 110 g / mol, coupled with a high M wat 960 kD. Since this secondary polymer is highly charged by the available PFSA ionomer present in a typical electrode ink, the polycation chain elongates in solution and strongly bonds to the NAFION through ionic bonding of the ammonium and sulfonate sites on each polymer. ® -Polyanion.

[0047] The NAFION ® The SS700 PFSA ionomer mixture is formulated at a 3:1 wt% ratio, with the hydrogen bonding of the more readily accessible sulfonic acid groups on the SSC ionomer being responsible for the faster growth of the solid-state modulus upon solvent evaporation. The ionic compound with the extended PVP polymer exhibits an even greater growth in the elastic modulus at the lower relative loading of 1 or 5 wt% NAFION. ® .

[0048] The solidification or gel point of the ink ionomer solution occurs when the elastic modulus (G') reaches and then crosses the viscous (G') modulus. Fig. 7 shows tan δ (or G'' / G') for the same four NAFION ® -Solutions during solvent evaporation. The modulus of elasticity is minimal at the beginning of solvent evaporation, which is reflected in the measured G'' / G' > 7, since the polymer solutions are more liquid than solid at this stage of the solvent drying process.

[0049] The comparison example with NAFION present only in the ink solution ® The -ionomer does indeed show a further increase in tan δ upon solvent evaporation. That is, the viscosity modulus continues to increase with the primary ionomer concentration, but the elastic modulus does not, as in Fig. Figure 6 shows the preferred embodiments, which incorporate the more expanded SS700 ionomer or a more extended PVP polycation chain with NAFION. ®-Ionomer mixing, a significantly decreasing tan δ, approaching a consolidation point (G'' / G' = 1) for the polymer solution with solvent drying.

[0050] The PtCo alloy catalyst ink is applied directly to commercially available diffusion media (catalyst coating-on-diffusion-media, CCDM). For the comparison example, the (NAFION) ® (The carbon ratio of the ink is formulated at I / C = 1.40) and is applied with a Mayer rod to achieve a target deposition of 0.20 mg Pt and 0.48 mg carbon. 2 The substrate is then dried under an IR lamp at 60 °C. The CCDM ink I / C is intentionally formulated above the optimized cathode power (near I / C = 1.00) due to the permeation of the ink solution into the porous substrate. The resulting electrode thickness is measured at ~16 mm, implying a porosity of ~70 vol.%.

[0051] Table 3 shows the calculated composition of the applied paint film in three stages of the drying process: namely after permeation of the paint solution into the porous coating substrate, upon saturation of the solvent of the consolidated carbon microstructure and after completion of the solvent drying process. Table 3. Ink compositions Electrode composition Electrode ink solution at saturation moist wt.% dry Vol.% solvent density 0 ,854 / cc Ketjet Black 5,0 % 14,7 % Ionomer loading = solvent loading = 2 9,7 % ew.- % PtCo 2,3 % 0,7 % 3 9,4 % ew.- % NAFION ® 7,0 % 20,6 °% H2O wt% solvent = 3 6,0 % ew.- % solvent 85,7 % 0,0 % nPrOH wt% solvent = 6 4,0 % ew.- % invalid 0,0 % 64,0 %

[0052] After permeation of the applied ink solution into the diffusion medium substrate, approximately 30% of the ionomer solution is removed from the wet electrode layer, increasing the carbon loading from 3.00% to 4.13 wt% ink. At saturation, the remaining ionomer solution just fills the consolidated carbon microstructure, resulting in an ionomer loading of approximately 25 wt% ink at this stage with an 85% solvent loss. Mechanical reinforcement of a gelling ionomer solution is required at or shortly before this point in the electrode drying process to prevent breakage of the fragile carbon microstructure.

[0053] The water content of the ink solution also increases at saturation due to the higher vapor pressure of the nPrOH solvent, which drives a higher tensile stress in conjunction with the higher surface tension of the liquid. 1 NMR application in Fig.Figure 8 shows an increase from 25 to 55 wt% solvent during carbon solidification.

[0054] Fig. Figure 9 shows that ionomer consolidation can only occur prior to carbon solidification of the electrode ink if either aSS700 PFSA ionomer or a PVP polycation is combined with the NAFION ® -Primary ionomer is mixed in the ink solution. The growth of the elastic modulus in Fig. 7 is only observed for the preferred ink solutions (16% polymer) prior to carbon solidification (25% polymer or carbon solids).

Claims

[1] An electrode ink composition comprising: a solvent; a platinum group metal-containing catalyst composition dispersed in the solvent; a primary polymer dispersed in the solvent, wherein the primary polymer is an ionomer; and a secondary polymer dispersed in the solvent, wherein the secondary polymer interacts with the primary polymer via a non-covalent interaction; wherein the secondary polymer has an overlap concentration that is at least three times lower than the overlap concentration of the ionomer, wherein at the overlap concentration polymer chains of the ionomer and the secondary polymer just touch in solution. [2] The electrode ink composition according to claim 1, wherein the primary polymer is described by the formulas I or II:wherein: n is 1 to 10; m is 1, 2 or 3; o is about 30 to 800; and p is 1, 2 or 3. [3] The electrode ink composition according to claim 2, wherein the non-covalent interaction is a hydrogen bond. [4] The electrode ink composition according to claim 3, wherein the secondary polymer is described by formula III:wherein: n is 1 to 10; and m is 1, 2 or 3. [5] The electrode ink composition according to claim 3, wherein the primary polymer is a long side chain polymer having an equivalent weight of 850 to 1050 g / mol and a weight average molecular weight of 250 to 500 kDa, and the secondary polymer is a short side chain polymer having an equivalent weight of 500 to 850 g / mol and a weight average molecular weight of 300 to 2000 kDa, or a long side chain polymer having an equivalent weight of 550 to 850 g / mol and a weight average molecular weight of 500 to 1500 kDa. [6] The electrode ink composition according to claim 1, wherein the non-covalent interaction is by ionic bonding. [7] The electrode ink composition of claim 6, wherein the secondary polymer is a high molecular weight polyvinyl-2-pyrrolidone having a weight average molecular weight greater than or equal to 400 kDa. [8] The electrode ink composition of claim 6, wherein the secondary polymer is selected from the group comprising: polyamides, polyamide-amines, poly(2-ethyl-2-oxazoline), poly(alkyl- and / or -aryl-substituted oxazolines), poly(hydroxyalkyl acrylates), poly(hydroxyalkyl methacrylates), poly(hydroxyalkylethyleneimines), polyacrylamides, poly(dimethylaminoalkyl acrylates), poly(dimethylaminoalkyl methacrylates), poly(diallyldimethylammonium chloride), poly(aminophosphazenes), poly(alkylaminophosphazenes), and combinations thereof. [9] Fuel cell (10), comprising: an anode catalyst layer (16); a cathode catalyst layer (14); an ion-conducting membrane (12) arranged between the anode catalyst layer (16) and the cathode catalyst layer (14); a first gas diffusion layer (32) disposed over the anode catalyst layer (16); a second gas diffusion layer (34) disposed over the cathode catalyst layer (14); an anode flow field plate (20) disposed above the first gas diffusion layer (32); and a cathode flow field plate (22) disposed over the second gas diffusion layer (34), wherein at least one of the anode catalyst layer (16) and the cathode catalyst layer (14) includes a platinum group metal-containing catalyst composition, a primary polymer that is an ionomer, and a secondary polymer, wherein the secondary polymer interacts with the primary polymer via a non-covalent interaction when the primary polymer and the secondary polymer are dispersed in a solvent; and wherein the secondary polymer has an overlap concentration that is at least three times lower than the overlap concentration of the ionomer, wherein at the overlap concentration polymer chains of the ionomer and the secondary polymer just touch in solution. [10] Fuel cell (10) according to claim 9, wherein the primary polymer is described by formula I:wherein: n is 1 to 10; m is 1, 2 or 3; o is about 30 to 800; and p is 1, 2 or 3.

Citation Information

Patent Citations

  • Improved electrode with reduced shrinkage cracking due to mixed equivalent weight ionomers

    DE102012222049A1

  • Process for producing re-dispersable particles of highly fluorinated polymer

    US20080161429A1

  • Catalyst layer composition for fuel cell, electrode for fuel cell, method of preparing electrode for fuel cell, membrane-electrode assembly for fuel cell, and fuel cell system using the membrane-electrode assembly

    US20130040222A1

  • Polyvinylpyrrolidone (PVP) for enhancing the activity and stability of platinum-based electrocatalysts