Procedure and structure

The method addresses out-diffusion issues in barrier-free conductive structures by using low-temperature annealing and anchor points to minimize cobalt diffusion, enhancing electrical performance and stability.

DE102020119831B4Active Publication Date: 2024-11-14TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
DE102020119831
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-22
Filing Date
2020-07-28
Publication Date
2024-11-14
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

Conductive structures without barrier or coating layers, such as ruthenium-filled structures over cobalt, face challenges in preventing out-diffusion of cobalt atoms during annealing or temperature cycling, leading to performance degradation and electrical interruptions.

Method used

A method involving low-temperature annealing and the formation of anchor points within the cobalt structures to minimize cobalt diffusion, combined with a ruthenium deposition process that forms a ruthenium oxide interface layer to enhance adhesion and prevent metal pullout during planarization.

Benefits of technology

The method reduces contact resistance and prevents out-diffusion of cobalt, maintaining electrical integrity and reducing void formation in conductive structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Procedure, comprehensive: Applying an etch stop layer (150) to a cobalt contact (105) arranged on a substrate (125); Application of a dielectric (155) to the etch stop layer (150); Etching of the dielectric (155) and the etch stop layer (150) to form an opening (600) to expose an upper surface of the cobalt contact (105); Etching the exposed upper surface of the cobalt contact (105) to form a depression in the cobalt contact (105), wherein the depression extends laterally under the etch stop layer (150); Applying a ruthenium metal (110) to substantially fill the depression and opening (600); Tempering of the ruthenium metal (110) to form an oxide layer between the ruthenium metal (110) and the dielectric (155); Planarizing the ruthenium metal (110) to essentially planarize the surfaces of the ruthenium metal (110) and the dielectric (155) together; and Applying a metal oxide etch stop layer (1200) over the entire surface of the planarized ruthenium metal (110) and the dielectric (155).
Need to check novelty before this filing date? Find Prior Art

Description

STATE OF THE ART

[0001] In an integrated circuit, conductive structures (e.g., metal contacts, vias, and lines) are electrically connected to transistor regions, such as the gate electrode and the source / drain regions, and are designed to conduct electrical signals to and from the transistors. Depending on the complexity of the integrated circuit, the conductive structures can form one or more layers of metallic traces.

[0002] US 2019 / 0 287 851 A1 discloses exemplary embodiments relating to conductive features such as metal contacts, vias, lines, etc., and methods for forming these conductive features. US 2014 / 0 183 738 A1 discloses a metal compound containing cobalt and a method for forming a metal compound containing cobalt. DE 10 2017 127 206 A1 describes a method for manufacturing a semiconductor device. US 6 713 373 B1 discloses a method for conductive copper lines in a semiconductor device. US 2009 / 0 304 914 A1 discloses a thin and conformal barrier layer and a copper layer in the copper interconnect. US 6 506 668 B1 discloses a method for forming interconnect elements on a semiconductor chip. The invention is defined by the independent claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0003] Aspects of the present disclosure are best understood by reference to the following detailed description when taken in conjunction with the accompanying drawings. It should be noted that, in accordance with industry practice, various features are not drawn to scale. Indeed, the dimensions of various features may be arbitrarily exaggerated or reduced for clarity of illustration. Fig. 1A is an isometric view of a barrier-free or overcoat-free conductive structure formed on conductive cobalt structures in accordance with some embodiments. Fig. 1B and Fig. 1C are cross-sectional views of barrier-free or coating-free conductive structures formed on conductive cobalt structures in accordance with some embodiments. Fig. 2A and Fig. 2B are flow diagrams of a method describing the formation of barrier-free or overcoat-free conductive structures in accordance with some embodiments. Fig. 3A / B - 7A / B are cross-sectional views of various manufacturing processes during the formation of barrier-free or overcoat-free conductive structures on conductive cobalt structures in accordance with some embodiments. Fig. 8A is an enlarged cross-sectional view of a contact opening on a conductive cobalt structure in accordance with some embodiments. Fig. 8B is an enlarged top view of a contact opening on a conductive cobalt structure in accordance with some embodiments. Fig. 9-11 are enlarged cross-sectional views of various manufacturing operations during the formation of a barrier-free or overcoat-free conductive structure on a conductive cobalt structure in accordance with some embodiments. Fig. 12A and Fig. 12B are cross-sectional views of additional layers formed on barrier-free or overcoat-free conductive structures formed on conductive cobalt structures in accordance with some embodiments. Fig. Figure 13 shows trends for the resistivity of ruthenium and the out-diffusion of cobalt as a function of annealing temperature and / or annealing time in accordance with some embodiments. Fig. 14 is a graphical illustration of an annealing process for coating-free conductive structures in accordance with some embodiments. DETAILED DESCRIPTION

[0004] The following disclosure provides many different embodiments, or examples, for implementing various features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the present disclosure. For example, in the description below, the formation of a first element on a second element may include embodiments in which the first and second elements are formed in direct contact with each other, but may also include embodiments in which additional elements are disposed between the first and second elements such that the first and second elements are not in direct contact with each other. Furthermore, the present disclosure may repeat reference numbers and / or characters in the various examples.This repetition does not, in itself, dictate any relationship between the various embodiments and / or configurations discussed.

[0005] Furthermore, terms of spatial relationships such as "beneath," "below," "low," "above," "upper," and the like may be used herein for the purpose of more conveniently describing the relationship of one element or feature depicted in the figures to another element or feature. The terms of spatial relationships are intended to encompass various orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be oriented differently (rotated 90 degrees or in other orientations), and the terms of spatial relationships used herein may thus be interpreted accordingly.

[0006] In some embodiments, the terms "about" and "substantially" may indicate a value of a particular amount that varies within 5% of the value (e.g., +1%, ±2%, ±3%, ±4%, ±5% of the value). These values ​​are, of course, only examples and should not be construed as limiting in any way. It should be noted that the terms "about" and "substantially" may refer to a percentage of the values ​​as interpreted by those skilled in the art in light of the teachings disclosed herein.

[0007] Active and passive devices in an integrated circuit (IC) are interconnected locally (e.g., within the same region of the IC) and globally (e.g., between different regions of the IC) by a number of conductive structures, such as metal contacts, metal vias, and metal lines. The conductive structures are arranged in vertically stacked metallization or interconnect layers. Design considerations are taken into account when stacking metallization layers with different conductive materials to prevent performance degradation due to undesirable interaction between the conductive materials—for example, diffusion. This is of great importance for conductive structures that do not utilize barrier, overlay, or liner layers.

[0008] Conductive structures without barrier or overcoating layers (also referred to herein as "overcoat or barrier-free conductive structures") are desirable because they exhibit lower electrical resistance compared to conductive structures with barrier or overcoating layers. This is because the overcoat or barrier layers—which exhibit greater resistance than the metal fill layer of the conductive structure—occupy space that might otherwise be occupied by the metal fill layer within the conductive structure. Therefore, by eliminating the overcoat or barrier layers in the conductive structures, the lower-resistance metal fill can occupy the entire volume of the conductive structure, further reducing the contact resistance of the conductive structure.

[0009] However, since the overcoat or barrier-free conductive structures do not have overcoat or barrier layers that can serve as diffusion barriers, overcoat or barrier-free conductive structures formed on conductive structures filled with another metal may not be able to prevent or suppress outdiffusion of the underlying metal under certain conditions. For example, overcoat or barrier-free conductive structures filled with ruthenium that are disposed over conductive cobalt structures (e.g., cobalt contacts) are unable to prevent or suppress outdiffusion of cobalt through the ruthenium metal grain boundaries when both structures are annealed or subjected to temperature cycling.The aforementioned behavior poses limitations for the implementation of coating-free or barrier-free conductive ruthenium structures and poses a challenge for the integration of coating-free or barrier-free conductive ruthenium structures with conductive cobalt structures.

[0010] To address the aforementioned deficiencies, this disclosure is directed to providing a method for forming overcoat-free or barrier-free conductive ruthenium structures that can reduce the out-diffusion of cobalt atoms from underlying conductive cobalt structures (e.g., cobalt contacts). In some embodiments, the overcoat-free or barrier-free conductive ruthenium structures are subjected to a low-temperature (e.g., less than about 360°C) annealing process that allows ruthenium grain growth and minimizes cobalt diffusion through the ruthenium metal grain boundaries. In some embodiments, the overcoat-free or barrier-free conductive ruthenium structures are formed with anchor points disposed within the conductive cobalt structures to prevent the "pull-out" of ruthenium metal during a planarization process.

[0011] In accordance with some embodiments, Fig. 1A is a partial isometric view of uncoated or barrier-free conductive structures 100 (uncoated conductive structures 100) filled with ruthenium metal 110 and formed on conductive cobalt structures 105. The conductive cobalt structures 105 are formed on epitaxial source / drain (S / D) structures 115, which in turn are grown on recessed portions of fin structures 120 on a substrate 125. Lower portions of the fin structure 120 and the epitaxial S / D structures 115 are surrounded by a first dielectric layer 130, which forms an isolation structure (e.g., a trench isolation structure) in accordance with some embodiments.

[0012] In addition, Fig. 1A, a transistor gate structure 140 arranged between conductive cobalt structures 105. The gate structure 140 is separated by spacers 145 and a Fig. 1A, a dielectric layer not shown is electrically insulated from the conductive cobalt structures 105. In some embodiments, the transistor gate structure 140, the fin structures 120, and the epitaxial S / D structures 115 form corresponding fin-based transistors. In some embodiments, the conductive cobalt structures 105 form S / D contacts for the Fig. 1A. In some embodiments, the conductive cobalt structures 105 have an elongated rectangular shape and may extend into two or more epitaxial S / D structures 105. Consequently, one or more bare conductive structures 100 may be formed on each of the conductive cobalt structures 105.

[0013] As in Fig. As shown in Figure 1A, lower portions of the unclad conductive structures 100 include an "anchor point" 160 formed within an upper portion of the conductive cobalt structures 105. In some embodiments, the anchor points 160 have an arcuate or hemispherical shape to prevent ruthenium metal 110 from being "pulled out" during a ruthenium planarization process. The anchor points 160 also increase the surface area between the ruthenium metal 110 and the conductive cobalt structures 105, reducing the contact resistance between the two structures. In some embodiments, a silicide layer 165 is disposed between the conductive cobalt structures 105 and the epitaxial S / D structure 115 to provide a further reduction in contact resistance.

[0014] In some embodiments, the Fig. 1B and Fig. 1C Partial cross-sectional views of Fig. 1A along the intersection lines AB and CD. For example, Fig. 1B sections of Fig. 1A along the zx-plane (e.g. along the fin structure 120), and Fig. 1C shows sections of Fig. 1A along the zy-plane (e.g. along the cobalt structure 105). Fig. 1B and Fig. 1C show additional layers, which in Fig. 1A are not shown. For example, these additional layers include an etch stop layer 150 and an interlayer dielectric (ILD) 155 surrounding the upper and middle portions of the uncoated conductive structures 100 (e.g., over the conductive cobalt structures 105), and a second dielectric 135 on the first dielectric 130 surrounding the upper portions of the epitaxial S / D structures 115 and conductive cobalt structures 105.

[0015] The Fig. 1B and Fig. 1C show details of the anchor point 160 at the aforementioned positions. As in Fig. 1B, the arcuate or hemispherical shape of the anchor point 160 is limited by the width of the conductive cobalt structures 105. This is because the width of the conductive cobalt structures 105 along the x-direction is narrower than the width of the anchor point 160. In contrast, in Fig. 1B, the arcuate or hemispherical shape of the anchor point 160 is not limited by the length of the conductive cobalt structures 105. Based on the above discussions and depending on the cutting direction, the anchor point 160 may appear to have a different shape. For conductive cobalt structures 105 with a greater width than the width of the anchor point 160, the shape of the anchor point 160 for any cutting direction would appear similar to that shown in Fig. 1C is shown.

[0016] The Fig. 1A, Fig. 1B and Fig. 1C are exemplary, and variations of these structures are included within the spirit and scope of this disclosure. For example, the shape of the conductive cobalt structures 105 and the shape of the epitaxial S / D structure 115 may be different than in the Fig. 1A, Fig. 1B and Fig. 1C. In some embodiments, the conductive structures 105 are shorter, longer, wider, or narrower than those that Fig. 1A, Fig. 1B and Fig. 1C. The conductive structures 105 may be circular contacts, oval contacts, rectangular contacts, or combinations thereof. In some embodiments, multiple uncoated conductive structures 100 may be formed on a conductive cobalt structure 105. In some embodiments, some or all of the uncoated conductive structures 100 do not have an anchor point 160. In some embodiments, uncoated conductive structures may extend beyond the Fig. 1A, Fig. 1B and Fig. 1C. The epitaxial S / D structure 115 may include additional facets. In some embodiments, the epitaxial S / D structure 115 is merged by adjacent fin structures 120 to form merged epitaxial S / D structures, on which a conductive cobalt structure 105 and one or more uncoated conductive structures 100 may be formed. Furthermore, some layers or structures are not shown in the Fig. 1A, Fig. 1B and Fig. 1C. Not shown are, for example, a dielectric gate stack, work function layers, barrier layers, and metal fillings for the gate structure 140. Furthermore, barrier layers for the conductive cobalt structures 105 and spacers on lower sidewall surfaces of the epitaxial S / D structures 115 above the first dielectric layer 130 are not shown. The aforementioned in the Fig. 1A, Fig. 1B and Fig. Layers and structures not shown in Figure 1C are included within the spirit and scope of this disclosure.

[0017] In some embodiments, the uncoated conductive structures 100 are formed directly on a conductive cobalt structure 105 without any intervening layers. For example, there are no barrier layers, overcoat layers, or adhesion layers between the ruthenium metal 110 in the uncoated conductive structures 100 and the conductive cobalt structures 105. By way of example, but not limitation, the uncoated conductive structures 100 form a network of vias connecting the cobalt structures 105 to upper metallization levels (e.g., copper metallization levels) formed in the Fig. 1A, Fig. 1B and Fig. 1C. In accordance with some embodiments, the uncoated conductive structures 100 are formed using a process that reduces the out-diffusion of cobalt toward the upper metallization levels through the uncoated conductive structures 100. The out-diffusion of cobalt may form voids in the conductive cobalt structures 105, which are detrimental to the contact resistance. For example, voids within the conductive structures 105 may increase the contact resistance by approximately 15%. Excessive out-diffusion of cobalt may lead to electrical discontinuities within the conductive cobalt structures 105.

[0018] In some embodiments, the Fig. 2A and Fig. 2B Flow diagrams of a manufacturing process 200 for the formation of the Fig. 1A, Fig. 1B and Fig. 1C. Other manufacturing operations may be performed between the various operations of method 200 and may be omitted only for clarity and ease of description. These various operations are included within the spirit and scope of this disclosure. Furthermore, not all of the operations may be required to practice the disclosure provided herein. Some of the operations may be performed simultaneously or in a different order than those described in Fig. 2A and Fig. 2B. In some embodiments, one or more operations may be performed in addition to or instead of the operations described herein. The method 200 is described with reference to Fig. 3A / B - 12A / B - where the Fig. 3A - 12A, like the Fig. 1B and Fig. 1C, cross-sectional views along the Fig. 1A are the section lines AB and CD.

[0019] In some embodiments, the Fig. 3A and Fig. 3B Intermediate structures for the procedure 200. In the Fig. 3A and Fig. 3B, the fin structure 120, the epitaxial source / drain structures 115, the first dielectric layer 130, the second dielectric layer 135, the gate structure 140, the spacers 145, the silicide layer 165, and the conductive cobalt structures 105 have been previously formed in operations not shown in method 200. In some embodiments, the Fig. 3A and Fig. 3B the structure of the Fig. 1A and Fig. 1B after the formation of the conductive cobalt structures 105 on the silicide layer 165 over the epitaxial source / drain structures 115. In the manufacturing stage, which is shown in the Fig. 3A and Fig. As shown in Figure 3B, the upper surface of the conductive cobalt structures 105 is substantially coplanar with the upper surface of the second dielectric layer 135. This can be achieved, for example, with a planarization process after the deposition of the cobalt metal.

[0020] Referring to Fig. 2A, the method 200 begins with the operation 210 and the process of depositing an etch stop layer (e.g., similar to the etch stop layer 150 shown in the Fig. 1C and Fig. 1D) on an underlying conductive structure (e.g., the conductive cobalt structures 105). By way of example but not limitation, the etch stop layer 150 may be deposited to cover the upper surface of the conductive cobalt structures 105 and the second dielectric layer 135, as shown in FIGS. Fig. 4A and Fig. 4B. In some embodiments, the etch stop layer 150 facilitates the formation of the overcoat-free conductive structures 100. By way of example and not limitation, the etch stop layer 150 may include silicon nitride (Si3N4), silicon oxynitride (SiON), silicon carbide (SiC), silicon carbonitride (SiCN), or any combination thereof. Furthermore, the etch stop layer 150 may be deposited by low-pressure chemical vapor deposition (LPCVD), plasma-enhanced chemical vapor deposition (PECVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), or any other suitable deposition process to a thickness of between about 1 nm and about 3 nm.

[0021] Referring to Fig. 2A, the method 200 continues at operation 220 and the process of depositing the ILD 155 on the etch stop layer 150, as shown in FIGS. Fig. 5A and Fig. 5B. By way of example, but not limitation, the ILD 155 may include a low-k dielectric material having a dielectric constant of less than about 3.9, such as a carbonaceous silicon oxide layer. In some embodiments, the ILD 155 includes hydrogen and / or nitrogen. By way of example, the ILD 155 may be deposited using a CVD process, a plasma-enhanced CVD (PECVD) process, or any other suitable deposition process. By way of example, but not limitation, the ILD 155 is deposited to a thickness of between about 50 nm and 70 nm, depending on the desired aspect ratio of the unclad conductive structures 100.

[0022] Referring to Fig. 2A, the method 200 continues with operation 230 and the process of forming openings in the ILD 155 and the etch stop layer 150 to expose the conductive cobalt structures 105. In some embodiments, openings may be formed simultaneously to expose upper portions of the conductive cobalt structures 105. By way of example but not limitation, the Fig. 6A and 6B the structures of the Fig. 5A and Fig. 5B after the formation of the openings 600 according to process 230. In some embodiments, the openings 600 are formed using photolithographic and etching processes. For example, a photoresist layer may be deposited on the ILD 155 and subsequently patterned to form an etch mask. A dry etch process etches portions of the ILD 155 and the etch stop layer 150 that are not covered by the photoresist etch mask to form the openings 600, which are in the Fig. 6A and Fig. 6B are shown.

[0023] Further, since the ILD 155 and the etch stop layer 150 contain different materials, a dry etch chemistry with different etch selectivity may be used for each of the etched layers. In some embodiments, the dry etch process may comprise two or more sub-operations, each of the sub-operations using a different etchant based on the material being etched (e.g., ILD 155 or etch stop layer 150). For example, a first sub-operation etches the ILD 155 and terminates at the etch stop layer 140. A second sub-operation etches the etch stop layer 150 and terminates at the conductive cobalt structure 105. Additional sub-operations may be used to over-etch the conductive cobalt structure 105 and / or remove a polymer material formed during the etching operations.

[0024] Referring to the Fig. 6A and Fig. 6B, the openings 600 have a sidewall angle θ1 along the x-axis and a sidewall angle θ2 along the y-axis. The sidewall angles θ1 and θ2 can be modulated by the conditions of the etching process. The sidewall angles θ1 and θ2, which can be independently tuned, are formed between the sidewall surfaces of the opening 600 and the horizontal xy-plane. Furthermore, each of the angles θ1 and θ2 can range between approximately 85° and approximately 90°. In some embodiments, the sidewall angles θ1 and θ2 are substantially equal. In some embodiments, a top width 600tw of the openings 600 (e.g., in the x- or y-direction) can be substantially equal to or greater than a bottom width 600bw (e.g., along the x- or y-direction, respectively). In some embodiments, the aspect ratio of the openings 600 (e.g.The aspect ratios (i.e., the ratio of the height 600h to a top width 600tw) may be in the range of between about 3 and about 4. However, this is not a limitation, and aspect ratios of less than about 3 or greater than about 4 are within the spirit and scope of this disclosure.

[0025] Referring to Fig. 2A, the method 200 continues with operation 240 and the process of etching the exposed conductive cobalt structures 105 with a wet etch process to form an anchor recess (e.g., in each of the conductive structures 105). By way of example, but not limitation, the Fig. 7A and 7B the structures of the Fig. 6A and Fig. 6B after the wet etching process according to operation 240. In some embodiments, the etching chemical includes an aqueous solution of butoxyethanol (C6H 14 O2), hydroxylamine (H3NO) and diethylenetriaminepentaacetic acid (C 14 H 23 N3O 10), in which the main etchant is water, and C6H 14 O2, H3NO and C 14 H 23 N3O 10 serve as a cobalt surface protectant. The wet etching chemical, which is selective for cobalt, etches the exposed cobalt metal isotropically in all directions. Consequently, an arcuate or hemispherical anchor depression is formed on an upper portion of the conductive cobalt structure 105, as shown in the Fig. 7A and Fig. 7B shown.

[0026] As mentioned above with reference to the Fig. 1A, Fig. 1B and Fig. 1C, the anchor recess is limited by the width of the conductive cobalt structures 105 in the x-direction, as shown in Fig. 7A. If the width of the conductive cobalt structures 105 is equal to or greater than the width of the anchor recess, the anchor recess in the conductive cobalt structures 105 would be Fig. 7A and Fig. 7B look the same.

[0027] In some embodiments, the duration of exposure of the conductive cobalt structures 105 to the wet etch chemical is controlled to control the size of the hemispherical or arcuate anchor recess. For example, depending on the etch rate at which cobalt metal is consumed by the etch chemical, the exposure time may range from approximately 50 seconds to approximately 100 seconds or more. Fig. 8A is an enlarged view of the hemispherical or arcuate anchor recess shown in FIG. 7B. In some embodiments, the hemispherical or arcuate anchor recess has a width A along the y-direction in a range from about 21 nm to about 39 nm. In some embodiments, the hemispherical or arcuate anchor recess has a height H of between about 7 nm and about 13 nm. In some embodiments, a ratio A / H is about 3. The foregoing ranges are not to be construed as limiting, and larger or smaller recess sizes are within the spirit and scope of this invention. In some embodiments, a larger anchor recess may be more difficult to fill, while a smaller anchor recess may not prevent metal pullout during a planarization process.In accordance with some embodiments, the width A of the hemispherical or arcuate anchor recess is greater than the bottom width 600bw of the opening 600 (e.g., A > 600bw), which is in a range from about 13 nm to about 15 nm. In some embodiments, a ratio A / 600bw is in a range from about 1.7 to about 2.6, and a ratio 600bw / H is in a range from about 1 to about 2. Consequently, an undercut having a width along the y-direction of about (A - 600bw) / 2 is formed on each side of the anchor recess below the etch stop layer 150. In some embodiments, the undercut is in a range from about 4 nm to about 12 nm.

[0028] As previously discussed, the width of the hemispherical or arcuate anchor recess differs along the x-direction, which in Fig. 7A, from the width A along the y-direction due to the smaller width of the cobalt structures 105 along the x-direction. This is also shown in Fig. 8B, which is a plan view of the anchor recess through the opening 600. In Fig. 8B, a width C of the anchor recess along the x-direction is limited by the physical width of the conductive cobalt structure 105; thus, the width C along the x-direction is narrower than the width A of the anchor recess along the y-direction. In other words, the anchor recess appears to have a hemispherical or arcuate shape when viewed along the y-direction, as in Fig. 7B, and as if it had a “truncated” hemisphere or arc shape when viewed along the x-direction, as in Fig. 7A shown.

[0029] In accordance with some embodiments, the anchor recess serves two different purposes: (1) it provides an anchor point for the metal fill 110 to prevent pull-out of the metal fill 110 into the opening 600 during a subsequent planarization process, and (2) it increases the contact area between the underlying conductive cobalt structure and the metal fill to improve the overall contact resistance.

[0030] Referring to Fig. 2B, the method 200 continues with operation 250 and the process of depositing a metal to fill the openings 600. In some embodiments, the metal is deposited directly on the cobalt structure 105 in operation 250, without the formation of overlay or barrier layers therebetween. In some embodiments, and prior to metal deposition, a pre-clean is performed to remove native oxide layers (e.g., cobalt oxide) that have formed on exposed surfaces of the conductive cobalt structures 105 and to prepare the surfaces of the opening 600 for metal deposition. In some embodiments, the pre-clean comprises an argon plasma (Ar plasma) treatment, a hydrogen plasma (H2 plasma) treatment, or combinations thereof. In some embodiments, the hydrogen pre-clean treatment is performed at a temperature equal to or higher than that of the Ar pre-clean treatment.In some embodiments, a bias voltage is applied to the substrate during each of the treatments, wherein the bias voltage during the Ar pre-cleaning treatment is greater than that of the H2 plasma pre-cleaning treatment.

[0031] In some embodiments, the ruthenium metal is deposited at operation 250 using a thermal CVD process at a temperature of less than about 200°C (e.g., about 180°C) using a ruthenium carbonyl precursor chemical, such as triruthenium dodecacarbonyl (Ru3(CO) 12). By way of example and not limitation, the ruthenium metal is deposited to a thickness of approximately 20 nm or a thickness sufficient to fill the openings 600 including the anchor recess. In some embodiments, the growth of the ruthenium metal occurs from the bottom up. For example, ruthenium nucleation initially occurs at exposed surfaces of the conductive cobalt structure 105 and then continues vertically along the z-direction until the opening 600 is substantially filled. In some embodiments, a deposition temperature of less than 200°C promotes the growth of the ruthenium metal from the bottom up.

[0032] In accordance with some embodiments, Fig. 9 an enlarged view of Fig. 8A after process 250 and the deposition of ruthenium metal 110 in opening 600. In some embodiments, the deposited ruthenium metal 110 extends beyond the ILD 155 outside of the opening 600, forming an "overlay" that is removed using a planarization process, such as a chemical mechanical planarization (CMP) process. In some embodiments, the thickness of the overlay is less than approximately 20 nm due to the bottom-up growth process and the low deposition rate of ruthenium metal 110 on the ILD 155.

[0033] In some embodiments, the deposited ruthenium metal 110 is polycrystalline with small grains that together form a large number of grain boundaries that are Fig. 9 are represented by dashed lines. In some embodiments, the large number of grain boundaries is attributed to the low deposition temperature (e.g., less than about 200°C) of ruthenium metal 110. A large number of grain boundaries is undesirable because they increase the resistivity of ruthenium metal 110. For example, the grain boundaries act as scattering centers for electrons when current flows through the contact. Higher deposition temperatures (e.g., higher than about 200°C) may result in fewer grain boundaries, but do not promote the bottom-up growth of ruthenium metal 110 described above. Thus, higher deposition temperatures (e.g., above about 200°C) may lead to incomplete filling with seams or voids, which may also increase the contact resistance and become a cause of defects.

[0034] Referring to Fig. 2B, the method 200 continues with operation 260, where the ruthenium metal 110 is subjected to an annealing process. In some embodiments, the annealing process serves two distinct purposes: (1) it promotes the growth of ruthenium grains, and (2) it assists in the formation of a ruthenium oxide interfacial layer between the ruthenium metal 110 and the ILD 155. A side effect of an annealing process with long annealing times and / or high heat budgets is the outdiffusion of cobalt from the conductive cobalt structures 105, which is discussed below.

[0035] Grain formation is desirable because ruthenium metal with larger grains has lower electrical resistivity compared to ruthenium metal with smaller grains. This is because a metal with larger grains has fewer grain boundaries (e.g., sites for electron scattering) than a metal with smaller grains.

[0036] The growth of ruthenium oxide is desirable because it promotes adhesion between ruthenium metal 110 and the ILD 155. Thus, ruthenium is less likely to be "pulled out" during a subsequent planarization process. For example, the presence of a ruthenium oxide layer can provide additional adhesion in situations where the anchor point is not formed to prevent ruthenium pullout.

[0037] In some embodiments, the annealing process is performed in a temperature range of between approximately 200°C and approximately 360°C to reduce the out-diffusion of cobalt from the underlying conductive cobalt structures 105. In some embodiments, low annealing temperatures (e.g., closer to approximately 200°C) are combined with long annealing times of between approximately 5 min. and approximately 10 min. In contrast, high annealing temperatures (e.g., closer to approximately 360°C) are combined with short annealing times of between approximately 1 min. and approximately 5 min. In some embodiments, the annealing environment includes nitrogen (N2), argon (Ar), helium (He), hydrogen (H2), a forming gas (e.g., a mixture of hydrogen and nitrogen), or any combination thereof.Oxygen or oxidizing gases are undesirable because the ruthenium metal would convert to ruthenium oxide, which has a higher electrical resistivity than ruthenium metal. In some embodiments, the annealing process is performed at a process pressure of between about 2 Torr and about 20 Torr. Higher or lower annealing pressures are possible and are within the spirit and scope of this disclosure. In accordance with some embodiments, the annealing temperature and time are critical process parameters for controlling ruthenium grain size and cobalt outdiffusion, as discussed below.

[0038] The out-diffusion of cobalt is undesirable because it creates voids in the conductive cobalt structure 105 and increases the resistance of the conductive cobalt structures. Furthermore, the out-diffusion of cobalt increases the resistivity of the uncoated conductive structures because cobalt metal is more resistive than ruthenium metal. The main mechanism behind the out-diffusion of cobalt is thermally driven diffusion, which is described by Fick's law. Therefore, the annealing temperature (e.g., the heat budget) may be the main contributor to the out-diffusion of cobalt. The diffusion of cobalt occurs through the grain boundaries of the ruthenium metal 110. Therefore, fewer grain boundaries can result in fewer diffusion paths for cobalt atoms. Once diffused, the cobalt atoms can move further toward the top surface of the ruthenium metal 110 and agglomerate there to form cobalt nodes.If suppressed, the cobalt nodes can electrically short-circuit neighboring conductive structures. As discussed above, outdiffusion of cobalt is also undesirable, as it leads to voids and a deterioration in contact resistance.

[0039] In some embodiments, annealing temperatures below 200°C may retard cobalt outdiffusion at the expense of ruthenium grain size. This means that there is a temperature threshold above which ruthenium grain growth occurs and a measurable resistance advantage is achieved. In contrast, annealing temperatures above approximately 360°C are sufficient to promote ruthenium grain growth, but may significantly increase cobalt outdiffusion through the ruthenium grain boundaries. For example, annealing temperatures exceeding approximately 360°C (e.g., 380°C, 400°C, or more) may cause large voids in the conductive cobalt structure 105 due to an accelerated cobalt outdiffusion process. For example, the voids in the conductive cobalt structure 105 caused by cobalt outdiffusion may have a length and width of approximately 55 nm and a height of approximately 26 nm.Therefore, tempering temperatures above approximately 360 °C should be avoided if possible.

[0040] In some embodiments, the electrical resistivity of ruthenium decreases for higher annealing temperatures and / or longer annealing times due to the grain formation process. At the same time, the outdiffusion of cobalt increases under the same annealing conditions. This behavior regarding the electrical resistivity of ruthenium and the outdiffusion of cobalt is shown in Fig. 13, where trends for the electrical resistivity of ruthenium and the out-diffusion of cobalt as a function of the annealing temperature for a specific annealing time or as a function of the annealing time for a specific annealing temperature are shown. It is therefore essential that the annealing temperature and the annealing time are controlled to achieve a balance between the desirable electrical properties for the ruthenium fill and the "undesired" out-diffusion of cobalt. In some embodiments, high annealing temperatures (e.g., higher than approximately 360°C) or long annealing times (e.g., longer than 10 min) reduce the resistivity benefits achieved by the grain formation process due to the out-diffusion process of cobalt.In some embodiments, annealing times greater than about 10 minutes may result in out-diffusion of cobalt, even at a low annealing temperature of about 200°C, without providing any additional benefits in terms of contact resistance. Furthermore, longer annealing times (e.g., longer than 10 min.) unnecessarily increase the duration of the annealing process, which in turn leads to higher manufacturing costs. In contrast, annealing times of less than about 1 min. may not allow for significant growth of the ruthenium grains and may reduce the electrical resistivity of the ruthenium metal 110. In some embodiments, annealing conditions having an annealing temperature of between about 200°C and about 360°C combined with the appropriate annealing time discussed above result in a cobalt concentration within the ruthenium metal 110 of less than about 6 atomic percent (at.%).

[0041] In some embodiments, the selection of the annealing temperature depends on the volume of ruthenium metal 110 to be annealed. For example, a high aspect ratio contact (e.g., with an aspect ratio of about 5 or 6) containing ruthenium metal may require a higher annealing temperature (e.g., closer to about 360°C) and a shorter annealing time (e.g., between about 1 min. and about 5 min.). In contrast, a low aspect ratio via (e.g., with an aspect ratio of about 3) containing less ruthenium metal may require a lower annealing temperature (e.g., closer to about 200°C) and a longer annealing time (e.g., between about 5 min. and about 10 min.).Since it is possible for uncoated conductive structures with high and low aspect ratios to be arranged on the same substrate, selecting an appropriate combination of annealing temperature and annealing time provides favorable contact resistance for uncoated conductive structures with higher and lower aspect ratios.

[0042] In accordance with some embodiments, Fig. 14 is a graphical representation of the annealing process described above. In some embodiments, after the deposition of the ruthenium metal 110, the wafer (e.g., the substrate) is transferred to an annealing reactor. By way of example and not limitation, the annealing reactor may be arranged on the same leadframe as the deposition reactor, or on a different leadframe. In some embodiments, the annealing reactor is a single-wafer reactor or a batch reactor (e.g., a furnace). The wafer enters the annealing reactor at a temperature T1, which corresponds to a temperature lower than that of the ruthenium metal deposition (e.g., less than approximately 200°C) and higher than room temperature (e.g., higher than approximately 24°C). Subsequently, the wafer is heated to the annealing temperature T2. The heating process has a duration t1, which, depending on the reactor design and its capabilities, may range from approximately 30 seconds to approximately 60 seconds.The wafer is then annealed at the target annealing temperature T2 (e.g., between approximately 200°C and approximately 360°C) for an annealing time t2, which ranges from approximately 1 min to approximately 10 min, depending on the annealing temperature T2 discussed above. At the end of the annealing process, the wafer is cooled to temperature T3, which corresponds to room temperature (e.g., approximately 24°C). The duration t3 of the cooling process ranges from approximately 30 sec to approximately 60 sec, depending on the reactor design and its capabilities. At this point, the wafer is removed from the annealing reactor. In some embodiments, the annealing temperature T2 is controlled to within 5°C or even more precisely to ensure the accuracy and repeatability of the annealing process.As discussed above, the annealing process is carried out in a non-oxidizing environment containing N2, Ar, He, H2, a forming gas, or any combination thereof at a pressure of between about 2 Torr and about 20 Torr.

[0043] The Fig. The annealing process described in Figure 14 is not intended to be limiting. For example, the heating process (upward ramp) and / or the cooling process (downward ramp) may be non-linear. Thus, non-linear heating and / or cooling processes are included within the spirit and scope of this disclosure.

[0044] As discussed above, another reason for the annealing process is to form a ruthenium oxide interfacial layer between the ruthenium metal 110 and the ILD 155. In some embodiments, oxygen from the ILD 155 combines with the ruthenium metal atoms during the annealing process to form a ruthenium oxide interfacial layer. In some embodiments, the thickness of the ruthenium oxide interfacial layer is less than approximately 1 nm. In some embodiments, due to the poor interfacial separation between the ruthenium metal 110 and the ruthenium oxide layer, it may be challenging to determine the thickness of the ruthenium oxide layer by electron microscopy based on techniques such as scanning electron microscopy (SEM) and transmission electron microscopy (TEM).

[0045] Fig. 10 shows the structure of Fig. 9 during the tempering process described above with respect to operation 260. As in Fig. 10, the grain boundaries represented by dashed lines 900 merge as the grain size of the ruthenium metal 110 increases. Cobalt atoms diffuse from the conductive cobalt structure 105 into the ruthenium metal 110, as indicated by arrows at the interface between the ruthenium metal 110 and the conductive cobalt structure 105. Furthermore, a ruthenium oxide layer 1000 forms at the interface between the ruthenium metal 110 and the ILD 155. In some embodiments, no ruthenium oxide forms at the interface between the ruthenium metal 110 and the etch stop layer 150 because the etch stop layer 150 does not contain oxygen.

[0046] Unlike other metals—such as tungsten, aluminum, and copper—whose oxides are non-conductive, the oxide of ruthenium metal is conductive. Although the electrical resistivity of ruthenium oxide is higher than that of ruthenium, ruthenium oxide is more conductive than, for example, an overlay, lining, cladding, or barrier layer such as titanium nitride or tantalum nitride. Furthermore, because the ruthenium oxide layer 1000 occupies a small portion of the total volume of the ruthenium metal 110, the influence of the ruthenium oxide layer on the overall resistance is negligible. As discussed above, one advantage of the ruthenium oxide layer 1000 is that it improves the adhesion between the ruthenium metal 110 and the ILD 155, which can be beneficial during a ruthenium planarization process.For example, a planarization process, such as a CMP process used to remove the ruthenium metal overlay over the ILD 155, may generate mechanical forces or capillary forces sufficient to pull ruthenium metal 110 out of the contact opening. The hemispherical or arcuate anchor points and the ruthenium oxide layer 1000 may prevent the pullout of the ruthenium metal 110 during the planarization process.

[0047] Referring to Fig. 2B, the method 200 continues with operation 270 and the process of planarizing the ruthenium metal 110 such that the top surface of the ruthenium metal 110 and the top surface of the ILD 155 are substantially coplanar, as shown in Fig. 11. In accordance with some embodiments, Fig. 11 the coating-free conductive structure 100. In some embodiments, the planarization process is a CMP process that removes excess ruthenium metal deposited on the ILD 155 and planarizes the top surface of the resulting structure. In some embodiments, the planarization process of operation 270 reduces the height of the ILD 155 to approximately half, or less than half, of its original height. For example, if the original height of the ILD 155 was approximately 50 nm, the height of the ILD 155 may have been reduced to approximately 30 nm or less (e.g., to approximately 20 nm) after the planarization process of operation 270. This reduction in height may reduce the aspect ratio of the resulting coating-free conductive structure 100 shown in the Fig. 1A, Fig. 1B and Fig. 1C shown.

[0048] Referring to Fig. 11 the grain boundaries are shown by the dashed lines 900 compared to the ruthenium metal 110 before annealing, which is in Fig. 9. This reduction is a result of grain formation occurring during the annealing process described in operation 260. Furthermore, as discussed above, some cobalt diffusion occurs under the annealing conditions described in operation 260. As a result, pockets of cobalt atoms 1100, as shown in Fig. 11, along the interface between the ruthenium metal 110 and the conductive cobalt structure 105, along the sidewall and top surfaces of the uncoated conductive structure 100, and along the grain boundaries of the ruthenium metal 900. In some embodiments, traces of cobalt within the ruthenium metal 110 in the aforementioned positions can be detected by energy-dispersive X-ray spectroscopy (EDS, EDX, EDXS, or XEDS). In some embodiments, from 1 to about 3 monolayers of cobalt form along the ruthenium grain boundaries.

[0049] In some embodiments, operations 260 and 270 may be performed in reverse order. For example, the annealing process of operation 260 may be performed after the planarization process of operation 270. In some embodiments, the ruthenium metal 110 would lack the ruthenium oxide layer 1000, which serves as an adhesion layer preventing the pullout of ruthenium metal if the planarization process is performed before the annealing process.

[0050] In some embodiments, after the planarization process of operation 270, a metal oxide etch stop layer 1200 is deposited or applied over the entire surface of the ILD 155 to prevent the Fig. 12A and Fig. 12B. By way of example and not limitation, the metal oxide etch stop layer 1200 may comprise an aluminum oxide (Al2O3) layer with a thickness of approximately 3 nm. In some embodiments, the metal oxide etch stop layer 1200 serves as a capping layer that suppresses cobalt agglomeration on upper surfaces of the uncoated conductive structures 100 and the formation of cobalt nodes at the free surface of the ruthenium metal 110. This is because the metal oxide etch stop layer 1200 is configured to prevent cobalt atoms from diffusing through the upper surfaces of the uncoated conductive structures 100, even when the uncoated conductive structures 100 are subjected to additional annealing cycles, for example, during subsequent processing.In some embodiments, cobalt agglomeration is prevented even when subsequent annealing cycles occur at temperatures greater than about 400°C. Because the diffused cobalt atoms are trapped within the coating-free conductive structure 110 in some embodiments, the cobalt diffusion process reaches a saturation limit and then ceases.

[0051] In some embodiments, additional layers may be formed on the metal oxide etch stop layer 1200, such as an intermetal dielectric (IMD) 1210, which may be formed in the Fig. 12A and Fig. 12B. The IMD 1210 may include a low-k dielectric (e.g., a dielectric with a dielectric constant of less than about 3.9), such as carbonaceous silicon oxide. Additional conductive structures may be formed within the IMD 1210 to connect the uncoated conductive structures 100 to upper metallization levels formed in the Fig. 12A and Fig. 12B are not shown.

[0052] As mentioned above with reference to the Fig. 1B and Fig. 1C, the Fig. 12A and Fig. 12B Details of anchor point 160 along various cutting positions. As in Fig. 12A, the arcuate or hemispherical shape of the anchor point 160 is limited by the width of the conductive cobalt structures 105 along the x-direction. This is because the width of the conductive cobalt structures 105 along the x-direction may be narrower than the width of the anchor point 160. In contrast, in Fig. 12B, the arcuate or hemispherical shape of the anchor point 160 is not limited by the length of the conductive cobalt structures 105. Based on the above discussion and depending on the cutting direction, the anchor point 160 may appear to have a different shape. For conductive cobalt structures 105 with a greater width than the width of the anchor point 160, the shape of the anchor point 160 for any cutting direction (e.g., x or y) would appear similar to that shown in Fig. 12B is shown.

[0053] In accordance with some embodiments, the dimensions of the anchor point 160 are shown in the Fig. 12A and Fig. 12B similar to those shown in relation to the anchor recess in the Fig. 8A and Fig. 8B. For example, the width W y along the y-direction of the width A of the anchor recess shown in Fig. 8A (e.g. between about 21 nm and about 39 nm), and the width W x along the x-direction corresponds to the width C of the anchor recess shown in Fig. 8B. In some embodiments, W x and C is substantially equal to an upper width of the conductive cobalt structure 105, as shown in Fig. 12A. Furthermore, the height H' of the anchor point 160 corresponds to the height H of the anchor recess shown in Fig. 8A (e.g. between 7 nm and approximately 13 nm), and the width 600bw of the anchor recess in Fig. 8A corresponds to the width L of the anchor point 160 at the same position (e.g., between 13 nm and approximately 15 nm). In some embodiments, the ratio Wy / H' approximately 3. In some embodiments, a ratio W y / H' of more than approximately 3 in a wider and flatter anchor point 160, the formation of which can be challenging due to the isotropic nature of the etching process. On the other hand, a ratio W y / H' of less than about 3 in a narrower and deeper anchor point 160, which may make the coating-free conductive structure 110 more susceptible to ruthenium pullout during CMP. In some embodiments, the ratio W y / L in a range of about 1.7 to about 2.6. In some embodiments, ratios W y / L of less than approximately 1.7 in a narrower anchor point 160, which may make the coating-free conductive structure 110 more susceptible to ruthenium pullout during CMP. On the other hand, ratios W y / L of greater than about 2.6 in an enlarged anchor point, which may be more challenging to fill. In some embodiments, the L / H' ratio is in a range of about 1 to about 2.

[0054] In some embodiments, an undercut having a width along the y-direction of approximately (W y - L) / 2 is formed on each side of the anchor point 160 below the etch stop layer 150. In some embodiments, the undercut in the x- and y-directions ranges from approximately 4 nm to approximately 12 nm. In some embodiments, an undercut of less than approximately 4 nm may not prevent the uncoated conductive structure 110 from being pulled out during a CMP process, while an undercut of greater than approximately 12 nm may be more difficult to form by isotropic etching and subsequently fill with ruthenium metal.

[0055] In some embodiments, cladding-free conductive structures 100 provide lower resistance than conductive structures filled with other metals (e.g., tungsten), which require one or more cladding or barrier layers. By way of example but not limitation, the resistance of a single cladding-free conductive structure 100 may be less than about 80 Ω (e.g., about 60 Ω), depending on the aspect ratio of the cladding-free conductive structure.

[0056] Coatless conductive structures 100 fabricated using method 200 are not limited to cobalt source / drain contacts. For example, coating-free conductive structures 100 can be formed using method 100 on cobalt gate contacts or any other type of cobalt conductive structure used in integrated circuits.

[0057] Various embodiments consistent with this disclosure describe a method for fabricating uncoated or barrier-free conductive structures. In some embodiments, the uncoated or barrier-free conductive structures are filled with ruthenium metal, which is deposited directly onto conductive cobalt structures without the use of intervening layers, such as adhesion layers, overcoat layers, or barrier layers. In some embodiments, the ruthenium metal fill is annealed at an annealing temperature of between about 200°C and about 360°C for about 5 min to reduce the electrical resistivity of the ruthenium metal and form a ruthenium oxide layer between the ruthenium metal and the surrounding ILD. In some embodiments, the ruthenium oxide layer enhances the adhesion of the ruthenium metal to the surrounding ILD.In accordance with some embodiments, annealing temperatures of between about 200°C and about 360°C may promote grain formation while also reducing the out-diffusion of cobalt from the underlying conductive cobalt structures 105. The uncoated or barrier-free conductive structures include anchor points that help reduce the pullout of ruthenium metal during a subsequent ruthenium metal planarization process.

Claims

[1] Method comprising: Applying an etch stop layer (150) on a cobalt contact (105) arranged on a substrate (125); Applying a dielectric (155) on the etch stop layer (150); Etching the dielectric (155) and the etch stop layer (150) to form an opening (600) to expose a top surface of the cobalt contact (105); Etching the exposed upper surface of the cobalt contact (105) to form a recess in the cobalt contact (105), the recess extending laterally below the etch stop layer (150); depositing a ruthenium metal (110) to substantially fill the recess and the opening (600); Annealing the ruthenium metal (110) to form an oxide layer between the ruthenium metal (110) and the dielectric (155); Planarizing the ruthenium metal (110) to substantially planarize the surfaces of the ruthenium metal (110) and the dielectric (155) together; and Applying a metal oxide etch stop layer (1200) over the entire surface of the planarized ruthenium metal (110) and the dielectric (155). [2] The method of claim 1, wherein the metal oxide etch stop layer (1200) is an aluminum oxide layer having a thickness of 3 nm. [3] The method of claim 1 or 2, wherein annealing the ruthenium metal (110) comprises annealing the ruthenium metal (110) in a non-oxidizing environment. [4] The method of any preceding claim, wherein annealing the ruthenium metal (110) comprises annealing the ruthenium metal (110) in nitrogen (N2), argon (Ar), helium (He), hydrogen (H2), a forming gas, or a combination thereof. [5] The method of any preceding claim, wherein annealing the ruthenium metal (110) comprises performing an annealing process in a non-oxidizing environment at an annealing temperature of between about 200°C and about 360°C. [6] The method of any preceding claim, wherein annealing the ruthenium metal (110) comprises performing an annealing process having a duration of between about 1 min and 10 min. [7] The method of any preceding claim, wherein depositing the ruthenium metal (110) comprises depositing the ruthenium metal (110) in physical contact with the cobalt contact (105). [8] The method of any preceding claim, wherein depositing the ruthenium metal (110) comprises depositing the ruthenium metal (110) in physical contact with the etch stop layer (150) and the dielectric layer. [9] The method of any preceding claim, wherein etching the exposed upper surface of the cobalt contact (105) comprises etching the cobalt contact (105) with a wet etching chemical containing an aqueous solution. [10] Method comprising: Forming a conductive structure (105) on a substrate (125), the conductive structure (105) comprising a first metal; Forming a coating-free conductive structure (100) on the conductive structure (105), the coating-free conductive structure (100) comprising a second metal different from the first metal; wherein forming the coating-free conductive structure (100) comprises: Applying an etch stop layer (150) on the conductive structure (105); Applying a dielectric layer (155) on the etch stop layer (150); Performing a first etch to form a via opening (600) in the dielectric (155) and the etch stop layer (150) exposing the first metal; performing a second etch through the via opening (600) to form a recess in the conductive structure (105); depositing a second metal to substantially fill both the recess and the via opening (600), wherein the second metal is deposited in physical contact with the first metal, the etch stop layer (150), and the dielectric layer; annealing the second metal to reduce a resistance of the second metal; Planarizing the second metal to substantially planarize the surfaces of the second metal and the dielectric layer (155) together; and Applying a metal oxide etch stop layer (1200) over the entire surface of the planarized second metal and the dielectric layer (155). [11] The method of claim 10, wherein forming the conductive structure (105) comprises forming the conductive structure (105) with cobalt. [12] The method of claim 10 or 11, wherein depositing the second metal comprises depositing ruthenium metal (110). [13] The method of any one of claims 10 to 12, wherein performing the first etching comprises etching with a dry etching process, and performing the second etching comprises etching with a wet etching process. [14] The method of any one of claims 10 to 13, wherein annealing the second metal comprises annealing the second metal between about 200°C and 360°C for a duration of about 5 minutes. [15] The method of any one of claims 10 to 14, wherein annealing the second metal comprises growing a metal oxide on sidewall surfaces of the uncoated conductive structure (100) between the second metal and the dielectric layer (155). [16] The method of claim 15, wherein the second metal is a ruthenium metal (1000). [17] The method of any one of claims 10 to 16, wherein annealing the second metal comprises reducing a number of grain boundaries in the second metal. [18] Structure: A contact (105) with a first metal on a substrate (125); a plating-free via (100) within the contact (105), the plating-free via (100) comprising: a second metal in physical contact with the first metal; and a first metal oxide layer surrounding portions of the second metal not in contact with the first metal; and a metal oxide etch stop layer (1200) over the entire surface of a top surface of the second metal and on a top surface of a dielectric (155) planarized with the top surface of the second metal and having an opening (600) through which the second metal extends. [19] The structure of claim 18, wherein the first metal comprises cobalt and the second metal comprises ruthenium. [20] The structure of claim 18, wherein the first metal oxide layer comprises ruthenium oxide and the metal oxide etch stop layer comprises aluminum oxide.

Citation Information

Patent Citations

  • METHOD FOR PRODUCING A CONTACT STRUCTURE FOR A SEMICONDUCTOR COMPONENT

    DE102017127206A1

  • Self assembled monolayer for improving adhesion between copper and barrier layer

    US20090304914A1

  • Cobalt based interconnects and methods of fabrication thereof

    US20140183738A1

  • Conductive Feature Formation and Structure Using Bottom-Up Filling Deposition

    US20190287851A1

  • Utilization of annealing enhanced or repaired seed layer to improve copper interconnect reliability

    US6506668B1