Method for forming a semiconductor device
A combined liner layer of ruthenium and cobalt, enhanced by hydrogen plasma treatment, addresses adhesion and electromigration issues in semiconductor devices, enhancing yield and reliability through improved filling and reduced crushing.
Patent Information
- Application Number
- DE102020127319
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-09
- Filing Date
- 2020-10-16
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-10-16
AI Technical Summary
The challenge of downscaling semiconductor devices has introduced issues with the adhesion and flowability of conductive materials, leading to electromigration and crushing in upper portions of openings, which affects the yield and reliability of integrated circuits.
A combined liner layer composed of ruthenium and cobalt is used, with a hydrogen plasma treatment to enhance adhesion and dewettability, allowing the conductive material to fill lower portions of openings effectively, reducing electromigration and crushing.
The combined liner layer improves the yield and reliability of conductive features by ensuring complete filling of openings without crushing and minimizing electromigration, resulting in higher performance and reliability of semiconductor devices.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND
[0001] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological Advances in IC materials and design have produced generations of ICs, with each generation producing smaller and more complex circuits than the previous generation. In the course of IC evolution, the functional density (e.g. the number of interconnected devices per chip area) has generally increased, while the geometric size (e.g. the smallest component (or line) that can be produced in a manufacturing process) This process of scaling down generally brings benefits by increasing the Production efficiency and reduction of associated costs.
[0002] With the downscaling of devices, manufacturers have started to use new and different materials and / or combinations of materials to enable the downscaling of devices. Downscaling, alone or in combination with new and different materials, has also led to challenges, which may not have been an issue in previous generations with larger geometries.
[0003] From US 2018 / 0053725 A1 a method for producing a metal conductor is known, wherein a pattern in a dielectric layer is provided, whereby an adhesion-promoting layer is formed thereover. The The method comprises depositing a ruthenium layer arranged on the adhesion layer, depositing a Cobalt layer over the ruthenium layer and performing a high-temperature thermal annealing, which Ruthenium-cobalt alloy layer is created. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] Aspects of the present disclosure are best understood from the following detailed description understand when read with the accompanying figures. It is pointed out that, in accordance with In accordance with industry standard practices, various features are not drawn to scale. In fact, the Dimensions of the various features can be enlarged or reduced as required for a better overview. Fig. 1, Fig. 2, Fig. 3, Fig. 4, Fig. 5, Fig. 6, Fig. 7, Fig. 8, Fig. 9, Fig. 10, Fig. 11, Fig. 12, Fig. 13, Fig. 14, Fig. 15, Fig. 16, Fig. 17 and Fig. 18 illustrate cross-sectional views of intermediate steps in the Forming interconnect structures of integrated circuits according to some embodiments. DETAILED DESCRIPTION
[0005] The following disclosure provides many different embodiments or examples for implementing different features of the invention. Below are concrete examples of the components and Arrangements are described to simplify the present disclosure. These are, of course, merely examples and they are not intended to be limiting. The formation of a first feature over or on a second feature in the The following description may, for example, include embodiments in which the first and second features are direct contact, and may also include embodiments in which additional features between the first and the second feature, so that the first and the second feature may not be in direct contact. In addition, the present disclosure may contain reference numbers and / or -letters in the various examples. This repetition serves the purpose of simplification and Clarity and does not in itself dictate a relationship between the various embodiments discussed and / or configurations.
[0006] Furthermore, spatially relative terms such as ´´below´´, ´´under´´, ´´deeper´´, ´´over´´, ´´upper´´ and the like, to simplify the description, to show the relationship of an element or feature to one or more other elements or features as illustrated in the figures. It is It is intended that the spatially relative terms refer to different orientations of the device in use or in Operation in addition to the orientation shown in the figures. The device may also be used in other oriented (rotated by 90 degrees or other orientations) and the spatially relative Descriptors can also be interpreted accordingly.
[0007] Conductive features, such as conductor tracks and metallization layers, are used in an interconnect structure, and methods for forming them according to some embodiments. In particular, the conductive Features with a barrier layer, multiple lining layers (forming a combined lining layer) and a conductive material is formed to fill the conductive features. The combined lining layer has a strong Adhesion to the barrier layer and at the same time improves the ability of the conductive material (e.g. during and after deposition), to flow over the combined lining layer to fill lower sections of the openings, and to avoid crushing in the upper sections of the openings. In addition, at least one of the several lining layers contain a material similar to a material in a covering layer that will later be the conductive material and the combined lining layer. Presence of this material in the combined lining layer reduces electromigration of this similar material from the cover layer to the combined lining layer during use of the finished semiconductor device. To achieve this and other advantages, the multiple lining layers are also selected according to their ability to combine with other to form a continuous layer (e.g. the combined lining layer) while simultaneously benefits from certain properties of each of the multiple lining layers, such as interactions with nearby and adjacent layers. Due to the stronger adhesion between the combined lining layer and the barrier layer, improved flowability of the conductive material over the combined lining layer and Reducing the electromigration of the material from the cover layer into the combined lining layer can resulting conductive features are formed with a greater yield and they operate with higher Reliability.
[0008] Figures 1 to 18 illustrate cross-sectional views of intermediate stages in the formation of conductive Features and interconnect structures of integrated circuits according to some embodiments. Figures 1 to 13 may Formation of interconnection patterns using a single damascene process Figures 14 to 18 can illustrate the formation of a metallization layer (including metallization lines and conductive vias) of an interconnect structure using a double damascene process illustrate.
[0009] Fig. 1 illustrates a cross-sectional view of a semiconductor structure on a wafer 100 having a substrate 50 (e.g. B. a semiconductor substrate) in which various electronic devices are formed over the substrate 50, according to some embodiments. In the following figures, a multi-level connection system can be various electronic devices and the substrate 50. In general, Fig. 1 illustrates how to be explained in more detail below, a fin field effect transistor (FinFET) device 60 on a Substrate 50 with multiple interconnect layers formed thereon in later figures. To the extent contemplated However, this disclosure also includes planar transistors, gate-all-around transistors (GAA transistors) and other Types of devices.
[0010] In general, the substrate 50 illustrated in Fig. 1 may be a bulk semiconductor substrate or a silicon-based Insulator substrate (SOI substrate). An SOI substrate contains an insulating layer under a thin Semiconductor layer that is the active layer of the SOI substrate. The semiconductor of the active layer and the bulk semiconductor generally comprise the crystalline semiconductor material silicon, but it can also include one or more other Semiconductor materials include, such as germanium, silicon-germanium alloys, composite semiconductors (e.g. GaAs, AlAs, InAs, GaN, AlN and the like) or their alloys (e.g. GaAlAs, GaAlN, InGaAs and the like), x 1-xx 1-xx 1-x Oxide semiconductors (e.g. ZnO, SnO, TiO, GaO and the like) or combinations thereof. The semiconductor materials can 2 2 2 3 doped or undoped. Other substrates that can be used include multilayer substrates, Gradient substrates or hybrid orientation substrates.
[0011] The FinFET device 60 illustrated in Fig. 1 is a three-dimensional metal-on-semiconductor Field-effect transistor (MOSFET) structure that consists of fin-like strips of semiconductor protrusions called fins 58. The cross section shown in Fig. 1 runs along a longitudinal axis of the fin in a Direction parallel to the direction of current flow between the source and drain regions 54. The fin 58 can be Structuring the substrate using photolithography and etching techniques. It can For example, a Spacer Image Transfer (SIT) structuring technique can be used. In this process, a sacrificial layer is formed over a substrate and used to form mandrels using suitable photolithography and etching processes. Along the mandrels, spacers are formed. Then the sacrificial layer is removed by a suitable selective etching process. Each The remaining spacer can then be used as a hard mask for structuring the respective fin 58 by etching a trench in the substrate 50, for example, using reactive ion etching (RIE). Fig. 1 illustrates a single fin 58, although the substrate 50 may include any number of fins.
[0012] In Fig. 1, shallow trench isolation (STI) regions 62 are shown along opposite side walls of the Fin 58 is illustrated. STI areas 62 can be formed by deposition formed by one or more dielectric materials (e.g. silicon oxide) to form the trenches around the fins completely, and then by removing the upper surface of the dielectric materials. The dielectric Materials of STI ranges 62 can be deposited using high-density chemical vapor deposition Plasma (HDP-CVD), low pressure CVD (LPCVD), subatmospheric CVD (SACVD), flowable CVD (FCVD), spin- on and / or the like or a combination thereof. After deposition, a Tempering or hardening process may be performed. In some cases, the STI areas 62 may Lining, such as a thermal oxide lining grown by oxidizing the silicon surface. The recessing process can, for example, be a planarization process (e.g. chemical-mechanical polishing (CMP)), followed by a selective etching process (e.g. wet etching or dry etching or a combination thereof) which can recess the upper surface of the dielectric materials in the STI region 62 such that a upper portion of the fins 58 protrudes from the surrounding insulating STI areas 62. In some cases, the hard mask used to form the fins 58 must also be removed by the planarization process.
[0013] In some embodiments, the gate structure 68 of the FinFET device 60 illustrated in Figure 1 is a High-k metal gate-gate structure (HKMG gate structure) fabricated using a gate load process flow can be formed. In a gate-last process flow, a sacrificial dummy gate structure (not shown) after forming the STI regions 62. The dummy gate structure may include a dummy gate dielectric, a dummy gate electrode and a hard mask. First, a dielectric dummy gate material (e.g. silicon oxide, silicon nitride, silicon oxynitride or the like). Next, a dummy gate Material (e.g. amorphous silicon, polycrystalline silicon or the like) over the dummy gate dielectric and then planarized (e.g. by CMP). A hard mask layer (e.g. silicon nitride, silicon carbide or the like) is formed. Then the dummy gate Structure by structuring the hard mask and transferring this structure to the dummy gate dielectric and the Dummy gate material is formed using suitable photolithography and etching techniques. The dummy gate Structure may extend along several sides of the projecting fins 58 and between the fins 58 over the surface of the STI regions 62. As described in more detail below, the dummy gate structure can be replaced by the gate structure 68, as illustrated in Fig. 1. The gate structure 68 illustrated in Fig. 1 on the right side (on the top side of the fin 58) is an example of an active gate structure that extends, for example, along side walls of and over the portion of the fin 58 that projects beyond the STI region 62. The gate Structure 68 on the left side of Fig. 1 is an example of a gate structure extending over the STI region 62, such as between adjacent fins 58. The materials used to form the dummy gate structure and the Hard masks can be deposited using any suitable process, such as CVD, plasma-enhanced CVD (PECVD), atomic layer deposition (ALD), plasma-enhanced ALD (PEALD) or the like, or by thermal oxidation of the semiconductor surface or combinations thereof.
[0014] Source and drain regions 54 and spacers 72 of FinFET 60, as illustrated in Fig. 1, are For example, self-aligned to the dummy gate structures. Spacers 72 can be formed by deposition and anisotropic etching of a dielectric spacer layer, which after completion of the dummy gate patterning The dielectric spacer layer may comprise one or more dielectrics, such as Silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, the like, or a combination thereof. The anisotropic etching process removes the dielectric spacer layer from above the top of the dummy gate Structures and leaves the spacers 72 along the side walls of the dummy gate structures, which are laterally a section of the surface of the fin 58 (as illustrated on the right side of Fig. 1) or the surface of the STI- area 62 (as illustrated on the left side of Figure 1).
[0015] Source and drain regions 54 are semiconductor regions in contact with the fin 58. In some embodiments The source and drain regions can have 54 heavily doped regions and relatively lightly doped drain extensions (LDD) In general, the heavily doped regions are isolated from the dummy gate structures using the Spacers 72 are spaced apart, while the LDD regions can be formed before the formation of the spacers 72 and thus extends under the spacers 72 and, in some embodiments, further into a portion of the semiconductor under the dummy gate structure. The LDD regions can be created, for example, by implanting dopants (e.g. As, P, B, In or the like) using an ion implantation process.
[0016] The source and drain regions 54 may comprise an epitaxially grown region. After forming the LDD regions For example, the spacers 72 can be formed and then the heavily doped source and Drain regions are formed self-aligned to the spacers 72. The heavily doped source and drain In particular, areas can be created by first etching the fins to form recesses and then depositing a crystalline semiconductor material in the recess by a selective epitaxial growth process (SEG), which can fill the recess and typically extends beyond the original surface of the fin and beyond to form a raised source / drain structure as illustrated in Fig. 1. The crystalline semiconductor material can be elemental (e.g. Si or Ge or the like) or an alloy (e.g. Si C , or 1-xx SiGe, SiGeC or the like). The SEG process can use any suitable epitaxial growth method 1-xx 1-xy xy such as vapor / solid / liquid phase epitaxy (VPE, SPE, LPE) or metal-organic CVD (MOCVD) or molecular beam epitaxy (MBE) or the like. The heavily doped source and drain regions 54 can be situ during the SEG or by an ion implantation process performed after the SEG or by a 14 -2 16 -2 Combination of these, a high dose (e.g. from about 10 cm to 10 cm ) of dopants can be introduced. Source and drain regions 54 may also be formed by other processes, such as ion implantation of dopants and the like.
[0017] Still referring to Fig. 1, a first dielectric interlayer (ILD- Layer) 76 is deposited. In some embodiments, prior to deposition of the ILD material, a Contact etch stop layer (CESL) (not shown) of a suitable dielectric (e.g. silicon nitride, silicon carbide or the like or a combination thereof). A planarization process (e.g. CMP) be performed to remove excess ILD material and remaining hard mask material from above the dummy gates to form a top surface, exposing the top surface of the dummy gate material and in the may be substantially coplanar with the upper surface of the first ILD layer 76.
[0018] The HKMG gate structures 68 illustrated in Fig. 1 can then first be produced by removing the dummy gate Structures are removed using one or more etching techniques, creating gaps between respective spacers 72. Next, a replacement gate dielectric layer 66, which may be one or several dielectrics, followed by a conductive replacement gate layer 64 comprising one or more conductive materials are deposited to completely fill the recesses. The dielectric gate layer 66 contains, for example, a dielectric material with a high k-value, such as oxides and / or silicates of metals (e.g. Oxides and / or silicates of Hf, Al, Zr, La, Mg, Ba, Ti and other metals), silicon nitride, silicon oxide and the like, Combinations thereof, and multilayers thereof. In some embodiments, the conductive gate layer 64 a multilayer metal gate stack comprising a barrier layer, a work function layer and a gate fill layer which is successively formed on top of the gate dielectric layer 66. Exemplary materials for a Barrier layer include TiN, TaN, Ti, Ta, TiSiN, TaSiN or the like or a multilayer combination thereof. Work function layer can be TiN, TaN, Ru, Mo, Al for a p-type FET and Ti, Ag, TaAl, Ta AlC, TiAlN, TaC, TaCN, TaSiN, Mn, Zr for an n-type FET. Other suitable work function materials or combinations or Multilayers of these can be used. The gate fill layer, which fills the rest of the recess, can be metals such as such as Cu, Al, W, Co, Ru or the like or combinations thereof or multilayers thereof. The materials used to form the gate structure can be deposited by any suitable method, for example CVD, PECVD, physical vapor deposition (PVD), ALD, PEALD, electrochemical plating (ECP), electroless plating and / or the like. Excess portions of the gate structure layers 64 and 66 may be deposited over the upper surface of the first ILD layer 76, for example, using a CMP process The resulting structure, as illustrated in Fig. 1, can be a substantially coplanar surface that an exposed upper surface of the first ILD layer 76, the spacers 72 and remaining portions of the HKMG gate Layers (ie, the gate structure layers 64 and 66) inserted between respective spacers 72, include.
[0019] A second ILD layer 78 may be deposited over the first ILD layer 76, as illustrated in Fig. 1. In some embodiments, the insulating materials for forming the first ILD layer 76 and the second ILD layer 78 silicon oxide, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), a dielectric with a low dielectric constant (low k-value), such as Fluorosilicate glass (FSG), silicon oxycarbide (SiOCH), carbon-doped oxide (CDO), flowable oxide or porous oxides (e.g., xerogels / aerogels) or the like, or a combination thereof. The materials used to form the first ILD layer 76 and the second ILD layer 78 dielectric materials may be selected using any suitable process such as CVD, PVD, ALD, PEALD, PECVD, SACVD, FCVD, spin-on and / or the like or a combination thereof. In some embodiments, one or more etch stop layers (not specifically illustrated) over the structure above and / or below the illustrated ILD layers.
[0020] As illustrated in Fig. 1, electrodes of electronic devices formed in the substrate 50 be electrically connected to conductive features of a first connection level (which will be formed in later figures using conductive connectors (e.g. contact plug 74) which are connected by the intermediate dielectric layers are connected. In the example illustrated in Fig. 1, the contact plugs represent 74 electrical connections to the source and drain regions 54 of the FinFET 60. Contact plug 74 to gate electrodes are typically formed over STI regions 62. A separate gate electrode 64 (shown left in Fig. 1) illustrates such contacts. The contact plugs 74 can be formed using photolithography techniques For example, a structured mask can be formed over the second ILD layer 78 and used to etch openings extending through the second ILD layer 78 to form a portion of the gate Electrodes 64 over STI areas 62, as well as etching openings over the fins 58, which extend further through the first ILD layer 76 and the CESL liner (not shown) extend under first ILD layer 76 to form portions of the source and drain regions 54. In some embodiments, an anisotropic dry etching process may be used etching is carried out in two consecutive steps. The particles formed in the first step of the etching process used etchants have a higher etching rate for the materials of the first and second ILD layers 76 and 78 in Compared to the etch rate for the materials used in the conductive gate layer 64 and the CESL, which upper surface of the heavily doped regions of the source and drain regions 54. After the first step of the etching process has exposed the CESL, the second step of the etching process can be carried out, whereby the Etchant can be changed to selectively remove the CESL. Although the two ILD layers (e.g. the first ILD Layer 76 and the second ILD layer 78), there is only a single ILD layer or three or more ILD Layers also within the intended scope of revelation.
[0021] In some embodiments, a conductive lining may be provided in the openings in the first ILD layer 76 and the second ILD layer 78. The openings are then filled with a conductive filler material. The lining includes barrier metals that are used to prevent the diffusion of conductive materials from the Contact plugs 74 into the surrounding dielectric materials. In some embodiments, the Lining comprise two barrier metal layers. The first barrier metal comes into contact with the semiconductor material in the source and drain regions 54 and can then be chemically reacted with the heavily doped semiconductor in the source and Drain regions 54 to form a low-ohm contact, after which the unreacted metal can be removed. If the heavily doped semiconductor in the source and drain regions 54 is, for example, a silicon or silicon-germanium alloy semiconductor, then the first barrier metal can be Ti, Ni, Pt, Co, other suitable metals or their alloys. The second barrier metal layer of the conductive lining may additionally comprise other Containing metals (e.g. TiN, TaN, Ta or other suitable metals or their alloys). Above the conductive Lining layer can be used to fill the contact openings using an acceptable deposition technique (e.g. CVD, ALD, PEALD, PECVD, PVC, ECP, electroless plating, the like or a combination thereof) a conductive Filler material (e.g. W, Al, Cu, Ru, Ni, Co, alloys thereof, the like or a combination thereof) deposited Next, a planarization process (e.g. CMP) can be used to remove excess sections of all conductive materials from above the surface of the second ILD layer 78. The resulting conductive plugs extend into the first and second ILD layers 76 and 78 and form contact plugs 74, the physical and make electrical connections to the electrodes of electronic devices, such as tri-gate FinFETs, as described in Fig. 1. In this example, contacts are made to electrodes via STI area 62 and to electrodes via Fins 58 are formed simultaneously using the same processing steps. In other embodiments However, these two types of contacts can also be formed separately.
[0022] In Fig. 2, an etch stop layer 108 is formed over the FinFETs 60 and other electronic devices, the second ILD layer 78 and the contact plugs 74 are formed. The etch stop layer 108 can be made of silicon carbide, silicon nitride, Silicon oxynitride, silicon carbonitride or the like. The etch stop layer 108 can be formed by chemical Chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), a spin- on-dielectric-Pro process, the like, or a combination thereof. The etch stop layer 108 may be formed to a thickness of about 2 nm to about 20 nm, such as about 10 nm.
[0023] Still referring to Fig. 2, an intermetallic dielectric Layer (IMD layer) 110 is formed. The IMD layer 110 may be a layer made of a dielectric material having a low k value with a k value less than about 3.0. The IMD layer 110 may be a layer that made of an extra-low-k dielectric material (ELK) with a k-value of less than 2.5. In some embodiments, the IMD layer 110 may be formed of an oxygen-containing and / or a carbonaceous dielectric material with low k-value, hydrogen silses quioxane (HSQ), methyl silses quioxane (MSQ) or the like. The material of the etch stop layer 108 has a high etch selectivity towards the IMD layer 110 and thus the etch stop layer 108 can be used to prevent the etching of the IMD layer 110 in to stop subsequent processing steps.
[0024] In some embodiments, the IMD layer 110 is formed from a porous material, such as SiOCN, SiCN, SiOC, SiOCH or the like, and it can be prepared by initially forming a precursor layer over the Etch stop layer 108 can be formed. The precursor layer can be either a matrix material or a matrix material interspersed with porogen or alternatively the matrix material without the porogen. In some In some embodiments, the precursor layer can be formed, for example, by co-deposition of the matrix and the porogen formed using a process such as plasma-enhanced chemical vapor deposition (PECVD), where the matrix material is deposited simultaneously with the porogen, forming the precursor layer with the mixing of matrix material and porogen. However, experts will recognize that joint Deposition using a simultaneous PECVD process is not the only process used to form the Any suitable process, such as premixing the matrix material and the porogen material as a liquid and then spin-coating the mixture onto the etch stop layer 108, be used.
[0025] The matrix material or dielectric base material can be produced using a process such as PECVD, formed, although any suitable process such as CVD, PVD or even spin-on coating can be used alternatively The PECVD process can use precursors such as methyldiethoxysilane (DEMS), although other precursors, such as other silanes, alkylsilanes (e.g. trimethylsilane and tetramethylsilane), alkoxysilanes (e.g., methyltriethoxysilane (MTEOS), methyltrimethoxysilane (MTMOS), methyldimethoxysilane (MDMOS), trimethylmethoxysilane (TMMOS) and dimethyldimethoxysilane (DMDMOS)), linear siloxanes and cyclic siloxanes (e.g. Octamethylcyclotetrasiloxane (OMCTS) and tetramethylcyclotetrasiloxane (TMCTS)), combinations thereof or the like may be used alternatively. However, as those skilled in the art will recognize, the materials listed herein and processes are merely illustrative and not intended to limit the embodiments, since any other suitable matrix precursor can be used alternatively.
[0026] The porogen may be a molecule that can be removed from the matrix material after the matrix material has settled to form pores within the matrix and thereby reduce the overall value of the dielectric constant of the IMD layer 110. The porogen may be a material large enough to form the pores while at the same time is small enough so that the size of the individual pores does not displace the matrix material excessively. the porogen may contain an organic molecule such as alpha-terpinene (ATRP) (1-isopropyl-4-methyl-1,3- cyclohexadiene) or cyclooctane (boat form) or 1,2-bis(triethoxysilyl)ethane silicon.
[0027] After the precursor layer has been formed with the porogen dispersed in the matrix material, the Porogen is removed from the matrix material to form the pores in the matrix material. In one embodiment, the Removal of the porogen is carried out by an annealing process that decomposes and evaporates the porogen material which allows the porogen material to diffuse and leave the matrix material, creating a structurally intact porous dielectric material remains as the IMD layer 110. For example, annealing in a range of about 200 °C and about 500 °C, such as about 400 °C, for a period in the range of about 10 seconds to about 600 seconds, such as about 200 seconds. Alternatively, other methods can be used to remove the porogen. suitable processes are used, such as irradiating the porogen with ultraviolet (UV) radiation, to to decompose, or using microwaves to decompose the porogen.
[0028] In Fig. 3, a film stack is formed over the IMD layer 110. According to some embodiments, the Film stacks are used to form conductive lines that are electrically connected to the contact points ckern 74 and substrate 50. The film stack includes a buffer layer 124 and a mask layer 126. In In some embodiments, the film stack includes more than one buffer layer and mask layer arranged on alternating way can be formed.
[0029] The buffer layer 124 is formed over the IMD layer 110 and the mask layer 126 is formed over the buffer layer 124. The buffer layer 124 may be formed from a dielectric, such as silicon oxide, and may by CVD, PVD, ALD, a spin-on dielectric process, or the like. The mask layer 126 may formed from a material containing a metal, such as titanium nitride, titanium, tantalum nitride, tantalum or the like, and it can be formed by PVD, radio frequency PVD (RFPVD), ALD or the like. In the following Processing steps, a structure is formed on the mask layer 126. The mask layer 126 is then used as a Etching mask is used, wherein the structure of the mask layer 126 is used to etch the IMD layer 110. The Buffer layer 124 provides stress reduction between IMD layer 110 and mask layer 126.
[0030] In Fig. 4, openings 130 are formed in the mask layer 126. Formation of the openings 130 can be performed by Photolithography process for etching the mask layer 126 to form initial openings. The Photolithography process may include forming a photoresist (not specifically shown) over the mask layer 126, Structuring the photoresist with openings corresponding to the openings 130, extending the openings 130 by the mask layer 126 and then removing the photoresist.
[0031] In Fig. 5, the openings 130 are extended by the buffer layer 124 and the IMD layer 110. The openings 130 may be extended using acceptable etching techniques. In one embodiment, the openings 130 is formed by an anisotropic dry etching process. The etching process can, for example, be a dry etching process using a reaction gas that selectively etches the IMD layer 110 without damaging the mask layer 126 to etch significantly. The etching process is carried out until the openings 130 expose the etch stop layer 108. The Etching process can, for example, involve the formation of a reactive species from an etching gas using a plasma In some embodiments, the plasma may be a remote plasma. The etching gas may be a Fluorocarbon chemistry, such as CF / CF / CF and NF / O / N / Ar / H / H , the like, or a combination thereof. In 4 6 4 5 3 2 2 3 2 In some embodiments, the etchant uses fluorocarbon chemistry with O or Ar as the carrier gas. 2
[0032] In Fig. 6, portions of the etch stop layer 108 in the openings 130 are removed to expose the underlying Target contact plug 74. The etch stop layer 108 can be formed using an anisotropic wet or dry etching, which is selective to the material of the etch stop layer 108. The etch stop layer 108 can be removed, for example, using an anisotropic wet etching that uses etchant reactants, such as HO . The etching process used to remove the etch stop layer 108 may differ from the etching processes 2 2 used to form the openings 130 (e.g., other etchants and / or other etching process parameters are used).
[0033] In Fig. 7, a barrier layer 140 is formed on the exposed surface of the wafer 100 and in the openings 130. According to some embodiments, the formation of the barrier layer 140 may be PVD, ALD or a combination thereof In some exemplary deposition processes, Ar is introduced into the respective deposition chamber (not shown), + + placed in the wafer 100, to form metal ions (such as (Ti ) or tantalum (Ta )) or atoms without charges (such as titanium (Ti) or tantalum (Ta)) from the respective target (not shown) used in the PVD. Nitrogen can be added to the process gases. The sputtered metal ions are deposited on wafer 100, which forms the barrier layer 140, which is conductive. During the deposition of the barrier layer 140, a DC and / or a radio frequency (RF) power is applied. After deposition, the barrier layer comprises 140 sections directly above the IMD layer 110, portions on the side walls of the openings 130 (e.g., side walls of the mask layer 126, the buffer layer 124, the IMD layer 110 and the etch stop layer 108) and portions at the bottom of the openings 130.
[0034] In Fig. 8, a first lining layer 142 is deposited on the exposed surface of the wafer 100 and in the openings 130. The first lining layer 142 may be formed of ruthenium, molybdenum, rhodium or the like and it can be deposited by a deposition process such as CVD, PVD, ALD, the like or a combination According to some embodiments, the first liner layer 142 may be formed using a CVD Process by flowing a precursor molecule containing ruthenium bonded to one or more alkyl groups (e.g. hexadiene, pyridine, butadiene and cycloheptadiene), one or more carbonyl groups, one or more other functional groups, or combinations thereof. The first lining layer 142 can be formed, for example, by CVD using tricarbonyl hexadiene ruthenium as the precursor molecule The first liner layer 142 may be formed to a thickness of about 0.5 or 0.6 nm to about 2 nm, such as about 1.2 nm. Depending on the method of formation, a minimum thickness of about 0.5 or 0.6 nm allow at least a full monolayer of coverage of the first lining layer 142.
[0035] In Fig. 9, a second liner layer 142 is deposited over the first liner layer 142 on the exposed surface of the wafer 100. Lining layer 144 is formed. The second lining layer 144 may be made of cobalt, tantalum, magnesium or the like and it can be formed by a deposition process such as CVD, PVD, ALD or the like. According to some embodiments, the second liner layer 144 may be formed using a CVD process by flowing a molecule containing cobalt bound to one or more alkyl groups, one or more Carbonyl groups, one or more other functional groups or combinations thereof are bonded An advantage of forming the cobalt of the second lining layer 144 over the ruthenium of the first lining layer is that the cobalt can adhere better to the ruthenium than it can to the barrier layer 140 (e.g. TaN) The second lining layer 144 may be formed to a thickness of about 1 nm to about 3 nm or about 1 nm to about 2.5 nm, such as about 1.8 nm. As discussed in more detail below, although typically a Minimum deposition of 0.5 to 0.6 nm can enable a complete monolayer of the cover, a thickness of the second lining layer 144 greater than or equal to about 1 nm, help mixing of the first lining layer 142 and the second lining layer 144 such that a resulting upper surface of the combined Lining layer a sufficient proportion of the material of the second lining layer 144 (e.g. cobalt) to Reducing electromigration from overlying layers (e.g. a cobalt top layer, which is explained below) during use of the finished device, as discussed in more detail below. In addition, a thickness of the second lining layer 144 of less than or about 3.0 nm, the degree of mixing between the first lining layer 142 and the second lining layer 144, which in a sufficient amount of the material of the first lining layer 142 (e.g. ruthenium) along the upper surface of the combined lining layer to provide advantages in terms of dewettability of an overlying layer (e.g. a conductive material), as discussed in more detail below. In some embodiments, the thickness of the first Lining layer 142 and the second lining layer 144 are selected such that a sum of the thicknesses about 2 nm to about 4 nm, while in the preferred ranges described above for the first Lining layer 142 and the second lining layer 144 remain.
[0036] An advantage of forming the first liner layer 142 (e.g., ruthenium) directly on the barrier layer 140 (e.g., TaN) before forming the second lining layer 144 (e.g. cobalt) is that the first lining layer 142 has a stronger Adhesion to the barrier layer 140 may be greater than the second lining layer 144 to the barrier layer 140 Thus, the first lining layer 142 and the second lining layer 144 together have a more robust cover. While a second lining layer 144, for example made of cobalt, is applied directly above the barrier layer 140 is deposited, may have a coverage of 70% or more, a first lining layer 142, for example, ruthenium deposited directly over the barrier layer 140 (as described above), a can have coverage of about 90% or more.
[0037] In Fig. 10, a combined lining layer 148 can be formed by performing a hydrogen soaking treatment and / or a hydrogen plasma treatment on the wafer 100. During the Hydrogen soaking treatment diffuses hydrogen gas into the combined lining layer 148 to prevent deformations to repair and realign molecules, causing mixing of the first lining layer 142 and the second lining layer 144. The hydrogen soaking treatment can be carried out at an elevated temperature between about 100 °C and about 400 °C, such as about 200 °C, and at an elevated pressure between about 1333 Pascal and about 6666 Pascal, such as 4666.6 Pascal. Hydrogen plasma treatment can also involve mixing the first lining layer 142 and the second lining layer 144. In addition, Hydrogen ions the first lining layer 142 and the second lining layer 144 to form carbon and To remove oxygen impurities from these layers, while at the same time the metal diffusion constant is increased. According to some embodiments, the hydrogen plasma treatment comprises bombarding the wafer 100 with hydrogen plasma for a period of about 10 seconds to about 60 seconds or about 30 seconds. The Hydrogen plasma treatment can be carried out at a temperature between about 100 °C and about 400 °C and at a pressure between about 1 and about 2000 Pascal, such as about 400-667 Pascal. The flow rate of hydrogen plasma can be between about 1,000 sccm (standard cubic centimeters per minute) and 12,000 sccm and last about 5 seconds to about 5 minutes or about 24 seconds.
[0038] Hydrogen soaking and hydrogen plasma treatment serve several purposes. As a result of one or both treatments, according to the invention, a mixing of the first lining layer 142 and the second lining layer 144, thereby causing an exposed upper surface of the combined Lining layer 148 contains about 5% to about 20% ruthenium. These proportions can also be found in the final structure. In addition, the degree of mixing in an upper section of the combined Lining layer near upper portions of the openings 130 compared to a lower portion of the combined lining layer near lower sections of the openings 130. The combined Lining layer 148 may provide a gradient of ruthenium and cobalt concentrations through the thickness such include that from the lower surface (ie adjacent to the barrier layer 140) to the upper surface, the cobalt concentration in the generally decreases, while the ruthenium concentration generally increases. Mixing is more effective when the first lining layer 142 and the second lining layer 144 together are about or less than 9 total monolayers.
[0039] In Fig. 11, a conductive material 150 is filled into the openings 130. Excess conductive material 150 may also be formed along upper surfaces of the combined lining layer 148. The conductive material 150 may be a metallic material, including a metal or metal alloy such as copper, silver, gold, Tungsten, cobalt, aluminum or alloys thereof. In some embodiments, the formation of the conductive Materials 150 Depositing a thin growth layer (not shown) which may contain copper or a copper alloy, and filling the rest of the openings 130 using CVD, PVD, ALD, ECP, such as high voltage ECP, or electroless plating.
[0040] According to some embodiments, a deposition process, such as PVD, may be used to form the conductive material 150 in the openings 130. A first deposition of copper can, for example, room temperature, followed by a melting process at about 150 °C to about 300 °C for about 1 minute to about 5 minutes. The first cycle may be followed by one or more depositions of copper and Melting processes follow. In total, there can be one to five or more alternating cycles of deposition and melting processes.
[0041] An advantage of the hydrogen plasma treatment in the previous step is that the resulting upper surface the combined lining layer 148 with about 5% to about 20% ruthenium, the efficiency and yield of filling the Openings 130 with conductive material 150. In particular, the presence of ruthenium on the surface of the combined lining layer 148 represents due to the increased Cu dewettability from the combined Lining layer 148 provides improved deposition and melting of the conductive material 150. With other In other words, it is less likely that the conductive material 150 (e.g. copper) will react immediately and strongly upon contact at the combined lining layer 148. Thus, the conductive material 150 is less likely to adhere to upper sections of the openings 130, which would otherwise result in crushing in these upper sections Instead, more of the conductive material 150 reaches and fills the lower portions of the openings 130 before filling the upper portions of the openings 130. In addition, as far as accumulation and / or crushing of the conductive material 150 at upper portions of the openings 130, this occurrence by the Melting process(es) due to the improved mobility of the conductive material 150 over the ruthenium in the combined lining layer 148 reduced or weakened - ie due to the improved dewettability between the layers. In any case, the openings 130 can be more effectively filled by the conductive material 150, resulting in fewer or no voids. A concentration of less than about 5% ruthenium in the upper Area of the combined lining layer 148 may result in a greater decrease in the dewettability of copper from the combined lining layer 148, which has the advantages described above in terms of dewettability reduce or substantially eliminate ruthenium. Furthermore, a concentration greater than about 20% of ruthenium in the upper surface of the combined lining layer 148 with a low total concentration of cobalt in the combined lining layer 148, which could lead to electromigration problems, as detailed below discussed.
[0042] In Fig. 12, a planarization process may be performed to remove excess conductive material 150, the combined lining layer 148 and barrier layer 140, thereby Conductive tracks 160 are formed in the openings 130. In addition, the planarization process can remove remaining Remove portions of the mask layer 126 and the buffer layer 124, thereby exposing the IMD layer 110. The Planarization process can be a grinding or a CMP and it can be carried out in such a way that the upper Surfaces of the conductive material 150, the combined liner layer 148, the barrier layer 140 and the IMD layer 110 are flat or substantially flat. The conductive paths 160 contain remaining portions of the conductive Material 150 and the remaining portions of the combined lining layer 148 and the barrier layer 140, the extending along the side walls and bottoms of the conductive material 150. The conductive tracks 160 are therefore physically and electrically connected to the contact plugs 74.
[0043] In Fig. 13, a cover layer 170 may be formed over the IMD layer 110, the barrier layer 140, the combined Lining layer 148 and the conductive material 150 using CVD, PECVD, PVD, ALD, PEALD, ECP, electroless plating and / or the like. The cap layer 170 may comprise cobalt, ruthenium, the like or a combination thereof. The cover layer 170 can be considered as part of the conductive traces 160 According to some embodiments, the cap layer 170 is deposited using CVD. Deposition may use a cobalt precursor containing a molecule comprising cobalt bonded to carbon, Oxygen, hydrogen, or combinations thereof. After deposition of the material for the top layer 170 Excess sections can be removed by a suitable method, such as using lithography Thus, a photoresist (not specifically illustrated) may be formed over the material of the cap layer 170 and structured to expose portions of the material of the cover layer 170 that are not directly above the conductor tracks 160 (e.g., the combined lining layer 148 and the conductive material 150). The exposed sections can then be removed by etching or any suitable method. In some embodiments, the Cover layer 170 is selectively deposited over the conductive material 150. In addition, portions of the Cover layer 170 also deposited over the combined lining layer 148 and perhaps the barrier layer 140 The cover layer 170 may be deposited using any of the techniques known in the art with respect to the Barrier layer 140, the first lining layer 142, the second lining layer 144 or the conductive material 150 The cover layer 170 may, according to some embodiments, have a thickness of between about 1.5 nm and about 5 nm.
[0044] According to some embodiments and not specifically illustrated, upper portions of the conductive traces 160 (e.g. the conductive material 150 and the combined lining layer 148) before deposition of the cover layer 170 etched and recessed by between about 0 nm and about 5 nm. Next, the material of the cover layer can selectively deposited over the structure and into the recesses by one of the methods listed above become.
[0045] An advantage of the second lining layer 144 can be achieved by the presence of the cover layer 170 by a Reducing the electromigration of the material of the cover layer 170 and the material of the conductive material 150 into the combined lining layer 148 during use of the finished semiconductor device. For example, the use of cobalt in the cover layer 170 can help prevent diffusion of copper from the conductive material 150 into the combined lining layer 148, since cobalt forms a strong bond with copper. In addition, the use of cobalt in the combined lining layer 148 can contribute Diffusion of cobalt from the cover layer 170 into the combined lining layer 148 due to a lower diffusion gradient of cobalt and the strong bonding of cobalt and copper. Although it is not necessary Each chip or wafer is tested as part of the manufacturing process for reliable semiconductor devices However, a subset of the chips or wafers must be tested. Thus, electromigration tests can be included to demonstrate that the devices meet certain electromigration specifications, such as sufficient low electromigration of the material of the cover layer 170 into the combined lining layer 148. This means that mere presence of the material in both layers (and effectively a lower concentration gradient of the material between both layers) reduces the diffusion of this material from the cover layer 170 into the combined Lining layer 148 during prolonged use of the semiconductor device.
[0046] In Fig. 14, an etch stop layer 208 is formed over the IMD layer 110 and the conductive lines 160. The Etch stop layer 208 may be formed from similar materials and via a similar process as described above in connection with the etch stop layer 108. The etch stop layer 208 may have a thickness of about 2 nm to about 20 nm, such as 10 nm.
[0047] Still referring to Fig. 14, an IMD layer 210 is formed over the etch stop layer 208. The IMD layer 210 can be made of similar materials and using a similar process formed as described above in connection with the IMD layer 110. The material of the etch stop layer 208 has a high etch selectivity compared to the IMD layer 210 and thus the etch stop layer 208 can be used to stop the etching of the IMD layer 210 in subsequent processing steps.
[0048] In Fig. 15, a film stack is formed over the IMD layer 210. According to some embodiments, the Film stacks for forming metallization lines and vias that are electrically connected to the conductor tracks 160 The film stack includes a buffer layer 224 and a mask layer 226. In some Embodiments, the film stack includes more than one buffer layer and mask layer arranged in an alternating manner The buffer layer 224 and the mask layer 226 may be made of similar materials and similar processes as described above in connection with the buffer layer 124 and the mask layer 126, be formed.
[0049] Still referring to Fig. 15, openings 230 are then formed in the mask layer 226 and the Openings 230 are extended by the buffer layer 224, the IMD layer 210 and the etch stop layer 208. The Openings 230 may be formed by acceptable etching techniques and etchants as described above in connection with openings 130 described, formed, and expanded. The openings 230 expose underlying conductive lines 160 (especially the cover layer 170, if used). The etch stop layer 108 can be removed using a anisotropic wet or dry etching that is selective to the material of the etch stop layer 108. The etch stop layer 108 may be removed, for example, using an anisotropic wet etching that Etching reactants are used, such as HO . The etching process used to remove the etch stop layer 108 may 2 2 differ from the etching processes used to form the openings 130 (e.g., other etchant and / or other etching process parameters are used).
[0050] As illustrated, the openings 230 may be patterned using a double damascene process Thus, the upper portions of the openings 230 can accommodate the metallization lines (see Fig. 18 below) and the lower sections of the openings 230 accommodate conductive vias (see Fig. 18 below) to electrically connect the metallization lines to the conductive lines 160 below.
[0051] In Fig. 16, a barrier layer 240, a third lining layer 242 and a fourth lining layer 244 in the openings 230. The barrier layer 240 can be formed from similar materials and by a similar process formed as described above in connection with the barrier layer 140. The third lining layer 242 can be formed from similar materials and through a similar process as described above in connection with the first lining layer 142. The fourth lining layer may be made of similar materials and have a similar process as described above in connection with the second lining layer 144.
[0052] In Fig. 17, a combined lining layer 248 can be formed by performing a hydrogen plasma treatment formed on the wafer 100. The hydrogen plasma treatment may cause mixing of the third Lining layer 242 and the fourth lining layer 244. According to some embodiments The hydrogen plasma treatment comprises bombarding the wafer 100 with hydrogen plasma for a period of approximately 10 seconds to about 60 seconds or about 30 seconds. As a result of the hydrogen plasma treatment, According to the invention, the exposed area of the combined lining layer 248 contains about 5% to about 20% ruthenium. combined lining layer 148 may have a thickness of about 1.5 nm to about 5 nm or about 2 nm to about 4 nm, such as about 3 nm.
[0053] In Fig. 18, a conductive material 250 is inserted into the openings 230 and along upper surfaces of the combined Lining layer 248 is filled and a planarization process is performed to remove excess conductive material 250, the combined lining layer 248 and the barrier layer 240 to form the metallization lines 260 The conductive material 250 can be formed from similar materials and via a similar process, as described above in connection with the conductive material 150.
[0054] According to some embodiments, a deposition process, such as PVD, may be used to form the conductive material 250 in the openings 230. A first deposition of copper can, for example, room temperature, followed by a melting process at about 150 °C to about 300 °C for about 1 minute to about 10 minutes. The first cycle can be followed by one or more depositions of copper and Melting processes follow. In total, there can be one to five alternating cycles of deposition and As discussed above, one advantage of hydrogen plasma treatment is that previous step that the upper surface of the combined lining layer 148, which comprises about 5% to about 20% ruthenium, improved Deposition and improved melting of the conductive material 150 due to the improved dewettability from the combined lining layer 148. Thus, it is less likely that the conductive material 250 at upper portions of the openings 230 or at upper portions of the conductive via portions of the openings 230, which may otherwise result in crushing at these upper sections. In addition, these phenomena, as far as accumulation and / or crushing occurs, are caused by the Melting process(es) reduced or weakened due to the improved dewettability between the layers.
[0055] Still referring to Fig. 18, a planarization process for removing excess of the conductive material 250, the combined lining layer 248 and the barrier layer 240, whereby metallization lines 260 and conductive vias 262 are formed in the openings 230. In addition, the planarization process may remove remaining portions of the mask layer 226 and the buffer layer 224 removing the IMD layer 210. The planarization process can be grinding or CMP and it can be carried out in such a way that the upper surfaces of the conductive material 250, the combined Lining layer 248, barrier layer 240 and IMD layer 210 are flat or substantially flat. Metallization lines 260 and the conductive vias 262 contain remaining portions of the conductive material 250 and the remaining portions of the combined lining layer 248 and the barrier layer 240, which extends along the side walls and bottoms of the conductive material 250. The metallization lines 260 are electrically connected to the conductive lines 160 by the conductive vias 262.
[0056] In addition, a cover layer 270 may be provided over the conductive material 250 and the combined Lining layer 248 of the metallization lines 260. The cover layer 270 can be made of similar materials (e.g. cobalt) and formed by a similar process as described above in connection with the Cover layer 170 is described. The cover layer 270 can be considered as part of the metallization lines 260. The Cover layer 270 may have a thickness between about 1.5 nm and about 5 nm. In addition, as part of the tests the subset of chips or wafers, as described above, electromigration tests may be included to determine show that the devices meet the electromigration specifications, such as sufficiently low electromigration of the material of the covering layer 270 into the combined lining layer 248.
[0057] After completion of the metallization lines 260 and the conductive vias 262, additional metallization lines over the metallization lines 260 using similar materials and similar processes as described above in connection with the conductive lines 160 or the metallization lines 260 described.
[0058] In the above embodiments, the same or similar materials and processes were used to form the conductive lines 160 (including the combined lining layer 148) and the metallization lines 260 with the conductive vias 262 (including the combined liner layer 248). In addition, one or more steps of forming the metallization lines 260 with the conductive Vias 262 using different materials and / or processes compared to the corresponding step of forming the conductive lines 160.
[0059] As discussed above, particular selection of lining layers and other related processing steps can help to produce conductive features with a higher yield and with higher Performance reliability. The conductive features may include, in order of formation, a barrier layer, a first lining layer, a second lining layer, a combined lining layer (which contains the first lining layer and the second lining layer), a conductive material and a cover layer. A first advantage is that a first material is selected in the first lining layer to ensure stronger adhesion and provide more thorough coverage of the first lining layer to the underlying barrier layer. The second advantage is that the first material of the first lining layer and a second material of the overlying second lining layer are mixed to form an upper surface of the resulting combined lining layer to enable certain advantageous properties from the first material of the first lining layer. The first material along the surface of the combined lining layer allows For example, the conductive material allows lower sections of the openings to be filled before the upper sections of these same openings. This prevents crushing of the conductive material in the upper sections of the openings reduced or avoided. Furthermore, the dewettability of the conductive material via the first material, insofar as pinching occurs, that these pinchings are caused by melting of the conductive A third advantage is that the second material of the second lining layer has a third material of the cover layer to electromigration of this third material from the cover layer into the combined lining layer during use of the finished semiconductor device. While The combination of ruthenium and cobalt lining layers was explained above, other Combinations of materials, such as combinations of other materials described above with respect to the corresponding lining layers have been discussed, provide similar benefits and they are within the considered Scope of this disclosure.
[0060] In one embodiment, a method of forming a semiconductor device comprises forming an opening in a dielectric layer and forming a barrier layer in the opening. Above the barrier layer, a first liner layer comprising ruthenium over the barrier layer, and next forming a second Lining layer comprising cobalt over the first lining layer, a combined lining layer formed. A conductive material layer comprising copper is formed over the combined lining layer and A thermal process is carried out to melt the conductive material layer.
[0061] In another embodiment, a method of forming a semiconductor device comprises depositing a dielectric layer over a substrate and patterning the dielectric layer to form an opening with Side walls and a bottom surface. A barrier layer is placed above the dielectric layer and in the opening A ruthenium layer is deposited over the barrier layer and a Cobalt layer is deposited. Then, to form a mixed binary layer comprising ruthenium and cobalt, a Hydrogen plasma treatment is carried out. A first copper layer is deposited over the mixed binary layer secluded.
[0062] In yet another embodiment, a dielectric layer comprises a trench; a barrier layer formed in the trench and over a sidewall of the dielectric layer; a liner layer disposed in the trench, wherein a side wall of the lining layer is arranged over a side wall of the barrier layer a bottom portion of the lining layer is arranged above a bottom portion of the barrier layer, the Lining layer comprises an upper surface and a bottom surface, a first composition of the Lining layer at a first location on the upper surface differs from a second composition of the lining layer at a second location on the floor surface; and a conductive filler material disposed in the trench and is arranged above the side wall and the bottom section of the lining layer.
Claims
1. Method for forming a semiconductor device (60), comprising: Forming an opening in a dielectric layer (110); Forming a barrier layer (140) in the opening; Forming a combined lining layer (148) over the barrier layer (140), the formation of the combined lining layer (148) includes: Forming a first lining layer (142) over the barrier layer (140), wherein the first lining layer is ruthenium includes; and Forming a second lining layer (144) over the first lining layer (142), wherein the second Lining layer (144) includes cobalt; Forming a conductive material layer (150) over the combined lining layer (148), wherein the conductive Material layer (150) comprises copper; and Performing a thermal process to melt the conductive material layer (150), whereby the formation of the combined lining layer (148) over the barrier layer (140) furthermore the execution of a Hydrogen plasma treatment includes, and during the hydrogen plasma treatment ruthenium is present in the first lining layer (142) mixed with cobalt in the second lining layer (144), which in the combined Lining layer (148) with an exposed area containing 5-20% ruthenium results.
2. The method according to claim 1, further comprising forming a cover layer (170, 270) over the conductive material layer, the top layer (170, 270) contains cobalt.
3. Method according to claim 2, wherein forming the top layer comprises (170, 270): Etching sections of the conductive material layer and the combined lining layer (148) to form a Trench; Deposition of cobalt in the trench and above the conductive material layer, the combined lining layer (148) and the barrier layer (140); and Planarizing the cobalt such that an upper surface of the cover layer (170, 270) is at the same level as an upper surface the barrier layer (140).
4. Method according to claim 1, wherein the barrier layer (140) is physically and electrically coupled to a contact plug (74). is.
5. Method according to claim 4, furthermore forming a metallization feature over and electrically with the conductive Material layer coupled comprehensively.
6. The method according to claim 5, furthermore, after forming the conductive material layer, planarizing the conductive material layer, an upper surface of the conductive material layer, which is connected to an upper surface of the combined The lining layer (148) and an upper surface of the dielectric layer (110) are at a height.
7. Method for forming a semiconductor device (60), comprising: Deposition of a dielectric layer (110) over a substrate (50); Structuring the dielectric layer (110) to form an opening (130), wherein the opening (130) has side walls and encompasses a floor area; Deposition of a barrier layer (140) over the dielectric layer (110) and in the opening (130); Deposition of a ruthenium layer over the barrier layer (140); Deposition of a cobalt layer over the ruthenium layer; Performing a hydrogen plasma treatment that results in a mixed binary layer containing ruthenium and Cobalt includes, and Deposition of a first copper layer over the mixed binary layer, following hydrogen plasma treatment an area of the mixed binary layer facing the substrate (50) between about 5% and about 20% Ruthenium is included.
8. The method of claim 7, wherein the ruthenium layer has a first thickness greater than or equal to about 0.5 nm.
9. The method of claim 8, wherein the cobalt layer has a second thickness greater than or equal to about 1 nm, where the sum of the first thickness and the second thickness lies between approximately 2 nm and approximately 4 nm.
10. Method according to claim 7, further comprising carrying out a first thermal process for melting the first copper layer.
11. The method of claim 7, further comprising: Deposition of a second copper layer over the first copper layer; and Performing a second thermal process to melt the first copper layer and the second copper layer.
12. Method according to claim 7, further comprising forming a cover layer (170, 270) over the first copper layer, wherein the top layer (170, 270) contains cobalt.
13. The method of claim 12, furthermore performing an electromigration test to measure electromigration of comprising cobalt atoms from the cover layer to the mixed binary layer.