Magnetic composite component, method for manufacturing and using the magnetic composite component
The use of a laser-processed roughened contact surface with a coarse and fine structure enables a stable, direct connection of magnetic elements to carriers in magnetic composite components, reducing manufacturing effort and cycle time while maintaining robust adhesion, addressing the inefficiencies of previous methods.
Patent Information
- Application Number
- DE102020132148
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-03
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-12-03
AI Technical Summary
Existing methods for producing magnetic composite components require significant additional effort and resources, such as special surface treatments and adhesion promoters, leading to increased cycle times and material costs, which are contrary to process economy and efficiency.
A magnetic composite component is produced with a roughened contact surface created by laser beam processing, featuring a coarse structure with an average roughness depth greater than 10 μm and a fine structure within, allowing the magnetic element to be sprayed directly onto the carrier without additional adhesion means, utilizing magnetic powder with a filling level of 60% to 95% by mass and average particle diameters between 1 μm and 5 μm or 50 μm and 500 μm.
This method results in a stable, full-surface connection with reduced manufacturing effort and cycle time, ensuring the magnetic element remains attached even under adverse conditions, without the need for additional holding means, thus enhancing process economy and efficiency.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a magnetic composite component comprising at least one carrier with a contact surface and at least one injection-molded magnetic element sprayed onto said carrier according to the preamble of claim 1. The invention also relates to a method for producing such a magnetic composite component and its use.
[0002] A magnetic composite component of this type is described in DE 10 2016 218 930 A1. In this known magnetic composite component, which is part of an encoder, a compound consisting of a plastic and magnetic filler is injection-molded directly onto a carrier part, provided it has sufficient adhesion. Pretreatment such as roughening can promote adhesion. To ensure reliable adhesion, which results in high bond strengths even under adverse operating conditions, additional adhesion promoters are proposed.
[0003] A magnetic composite component is also shown in DE 10 2011 089 903 A1. In this known magnetic composite component, a magnetic element is arranged on the front end area of a gear wheel or on a driven wheel interacting with it. The gear wheel or driven wheel is made of plastic in the connection area with the magnetic element. The magnetic element, in turn, consists of magnetically active particles bound and distributed in a plastic mass and is connected to the front of the gear wheel or drive wheel using an injection molding process.
[0004] DE 10 2008 040 782 A1 describes the application of a plastic injection-molded element to a carrier with a roughened surface structure, which is produced, for example, by laser beam treatment and has a microstructure with a diameter in the range between 1 µm and approximately 999 µm and a superimposed nanostructure in the range between approximately 1 nm and approximately 999 nm. Preferably, the carrier is encapsulated with the plastic to create a positive connection.
[0005] US 2004 / 0 045 635 A1 discloses a magnet compound made of magnetic powder embedded in plastic material, wherein an average magnetic powder particle size of between 5 µm and 150 µm and a fill level of 50 wt.% to 97 wt.% are specified.
[0006] DE 10 2014 018 783 A1 discloses a sensor assembly for a torque and / or angle sensor, comprising a tubular segment-shaped magnet ring that is attached to a support sleeve via an intermediate element. The magnet ring is designed as a plastic-bonded magnet made of a plastic material filled with magnetic particles, and the intermediate element is made of a plastic, at least in the area of the joining surface. The plastic material of the magnet ring is integrally bonded to the plastic of the intermediate element in the area of the joining surface.
[0007] Further magnetic composite components and the joining techniques used are presented in "Permanent Magnets: Materials, Magnet Technology, Applications": Verlag Moderne Industrie, 2016, pp. 47-50, including in the context of injection molding technology. Accordingly, other joining techniques are possible for the connection between such an injection-molded, plastic-bonded magnet and an associated carrier of the magnetic composite component or assembly, such as full-surface adhesive bonding, overmolding, mechanical and thermal joining processes such as pressing or fitting, shrink-fitting, laser welding, ultrasonic welding, caulking, or joining by form-fitting at specially designed undercuts or apertures in the carrier.
[0008] Previously known joining techniques require considerable additional effort in the manufacturing process of the composite component or assembly to create the connection, such as special surface treatment to remove loose surface layers or particles, improving wettability, improving adhesion, geometric adjustments in the joining area, specially adapted injection molding tool design, and post-treatment in the joining area, e.g., to remove burrs. Such additional measures to create the connection lead to increased cycle times and potentially additional material costs, such as adhesives, and are detrimental to process economy and efficiency.
[0009] The present invention is based on the object of providing a magnetic composite component of the type mentioned above and a method for its production, which results in the lowest possible production effort and good adaptation options to different requirements.
[0010] This object is achieved by a magnetic composite component having the features of claim 1 and by a method having the features of claim 10. Advantageous fields of application are specified in claim 11.
[0011] In the case of the magnetic composite component, the invention provides that the contact surface is provided with a roughened structure to which the sprayed-on magnetic element is held by positive locking. The invention further provides that the magnetic element is held by positive locking solely by means of the roughened structure, the roughened structure has a coarse structure with an average roughness depth greater than 10 µm, in particular greater than 20 µm, and less than 1 mm, in particular less than 500 µm and a fine structure at least locally within the coarse structure, in the range of 1 µm or less, in particular between 100 nm and 1 µm, that the magnetic element contains magnetic powder with a fill level between 60 mass% and 95 mass%, preferably between 75 mass% and 90 mass% of the total mass of the magnetic element and the powder particles of the magnetic powder have on average a maximum diameter between 1 µm and 5 µm or between 50 µm and 500 µm.
[0012] The method is designed according to the invention in that the contact surface is roughened by means of laser beam processing before the magnetic element is sprayed on, wherein the roughened structure has a coarse structure with an average roughness depth greater than 10 µm, in particular greater than 20 µm, and less than 1 mm, in particular less than 500 µm and a fine structure, at least locally within the coarse structure, in the range of 1 µm or less, in particular between 100 nm and 1 µm. The magnetic element is sprayed directly (i.e. without an intermediate layer that mediates the connection) onto the roughened contact surface. For the magnetic element, magnetic powder with a fill level of between 60 mass% and 95 mass% of the total mass of the magnetic element is used, wherein the powder particles of the magnetic powder have an average maximum diameter of between 1 µm and 5 µm or between 50 µm and 500 µm.
[0013] With these measures, as the inventors have determined in extensive investigations, a stable, virtually full-surface connection is achieved between the injection-molded element, in particular the magnetic element, and the carrier in the area of the roughened contact surface. As a result of the roughened contact surface, the injection-molded element is held to the carrier over the entire surface area, so that (similar to an adhesive surface), even in the event of cracks or breaks in the injection-molded element, virtually no fragments of the element can detach from the carrier, for example, in contrast to a connection with undercuts or individual fastening points in openings created for fastening."Quite full-surface" means that, compared to the entire contact surface, small unroughened areas may be present between the roughened structures across the contact surface, allowing various roughened structure patterns to be advantageously incorporated into the contact surface area, tailored to a specific application. The production of the roughened structure can be integrated into the manufacturing process of the magnetic composite component with relatively little effort.
[0014] According to the invention, the fact that the magnetic element is held on the contact surface by means of the roughened structure, solely through positive locking, without any additional holding means, contributes significantly to a short cycle time of the manufacturing process and to production efficiency. Apart from the roughening, no further measures are required to attach the injection-molded magnetic element to the carrier during injection molding.
[0015] As the inventors' investigations have shown, a roughened structure that is particularly advantageous for the form-fitting connection results from the roughening structure being produced by means of laser beam treatment. The roughened structure and its pattern across the contact surface can be particularly advantageously specified by laser beam treatment through controlled local guidance of the laser beam and the irradiation strength (intensity) as well as temporal control of the beam emission in coordination with the magnetic composite component to be produced and its intended use. This can also be influenced, for example, during the manufacturing process in order to optimize the quality of the connection in conjunction with other process parameters. The settings for producing the roughened structure and the roughening pattern (distribution across the contact surface) can also be advantageously tailored to the material of the carrier used (metal, e.g. steel, ceramic, plastic).
[0016] A stable connection between the magnetic element and the carrier is obtained according to the invention in that the roughened structure has a coarse structure with an average roughness depth greater than 10 µm, in particular greater than 20 µm, and less than 1 mm, in particular less than 500 µm, and a fine structure, in particular locally within the coarse structure in the range of 1 µm or less, in particular between 100 nm and 1 µm.
[0017] Different patterns of the roughening structure for a good connection across the contact surface consist of the roughening structure being formed in a line pattern, in particular a cross pattern, e.g. at a distance of between 0.5 mm and 10 mm (also depending on component size and material) and / or in a point pattern with roughening points distributed across the contact surface at close intervals of less than 3 mm. A particularly stable connection is achieved by the cross pattern, with the intersecting lines running at an angle (e.g. at an angle range between 10° and 80°) with respect to an (imaginary) radial straight line at the relevant point. Other patterns, such as ring-shaped patterns and / or curved lines, can also be considered. In addition to depressions, raised areas are also advantageously formed, which also contribute to adhesion or holding force.
[0018] A magnetic composite component designed for corresponding applications is obtained by having a flat or curved contact surface. The contact surface is formed, for example, by or within a surface of the support that extends in an axial plan view of the support, so that, for example, the magnetic element is held solely by the roughened structure without any internal or external enclosure (such as when applied to the inner or outer wall of a cylindrical support). A magnetic composite component with such a planar arrangement of a magnetic element can offer advantages for a wide variety of applications, such as on the end face of a shaft or the top or bottom of a disk.
[0019] Various advantageous further design options for the magnetic composite component include the contact surface being continuously extended or formed from spaced-apart surface sections, or having at least a partially circumferential annular shape. Thus, for example, at least partially annular areas or spaced-apart surface areas on a carrier can be provided with magnetic elements with efficient production, depending on the application or the task to be solved.
[0020] Magnetic composite components for various requirements can furthermore advantageously be provided by the carrier being made of metal, ceramic material or plastic, at least in the area of the contact surface.
[0021] Further advantageous design variants of the magnetic composite component include the injection-molded magnetic element being made of one of the plastics polyamide, polyphenylene sulfide, or thermoplastic elastomer, or having such a plastic material as a matrix. These variants also offer advantageous adaptation options for different operating conditions.
[0022] Further embodiments of the magnetic composite component according to the invention with a stable connection of the magnetic element result from the fact that the injection-molded magnetic element contains magnetic powder with a filling level between 60 mass% and 95 mass%, preferably between 75 mass% and 90 mass% of the total mass of the magnetic element.
[0023] Various further design variants of the magnetic composite component consist in the magnetic element containing hard ferrite magnetic powder or rare earth magnetic powder in isotropic or, preferably, anisotropic form as magnetic powder.
[0024] Various embodiments of the magnetic composite component according to the invention further include the powder particles of the magnetic powder having an average maximum diameter between 1 µm and 5 µm or between 50 µm and 500 µm. The smaller diameter range of the powder particles corresponds to hard ferrite magnetic powder, and the larger diameter range corresponds to rare earth magnetic powder, in particular of the neodymium-iron-boron type or the samarium-cobalt type.
[0025] Magnetic composite components that are advantageous for various applications require a thickness of the injection-molded magnetic element or magnetic element of no more than 2.0 mm or even up to 5 mm (or even more in special applications), preferably between 0.2 mm and 1.5 mm. For example, with today's sensitive signal acquisition technology for sensors, very thin magnetic elements can be sufficient, resulting in advantages in terms of size and material savings.
[0026] The invention will be explained in more detail using exemplary embodiments with reference to the drawings. They show: Fig. 1 a ring-shaped carrier in a perspective view obliquely from above with a contact surface on the top and a roughened structure in a cross pattern introduced therein, Fig. 2 the carrier after Fig. 1 with a ring-shaped magnetic element sprayed onto the contact surface in a perspective view obliquely from above, Fig. 3 enlarged views of a roughened structure in a dot-shaped pattern (left image) and a roughened structure in a cross pattern (right image) and Fig. 4 an enlarged view of a roughened structure in a partial cross-section of a carrier with a magnetic element sprayed onto it.
[0027] Fig. 1 shows a carrier 10 of an annular magnetic composite component 1 (cf. Fig. 2) in a perspective view obliquely from above with a contact surface 100 located at the top (with respect to the figure) and a roughened structure 11 incorporated into the contact surface 100. The, for example, circular-ring-shaped carrier 100 in this case has a flat surface in axial plan view (perpendicular to the central axis), and the roughened structure 11 is formed in a cross pattern into the surface in the region of the circular-ring-shaped contact surface 100. The linear sections of the cross pattern 110 run obliquely with respect to a radial straight line from the center of the carrier through the intersection points at an inclination angle of between approximately 30° and 60°, for example approximately 45°, with one section of the intersecting sections of the cross pattern 110 running clockwise in front of the radial straight line and one section running clockwise behind the radial straight line. This results in 110 X-shaped pattern elements in the cross pattern shown.
[0028] In a preferred embodiment, the roughened structure 11 is produced by laser processing in accordance with the applied pattern, in which Fig. 1, i.e., in the form of the cross pattern 110, is incorporated by means of a control device for automatically guided laser beams. Other patterns of the roughened structure 11 can also be easily specified by appropriate programming of the control device using the laser device and incorporated via the laser beam. The incorporation of such a roughened structure 11 can be completed within a few seconds, so that it represents a relatively short sub-step in relation to the overall cycle time during the production of the composite component, in this case, the magnetic composite component 1.
[0029] The carrier 10 consists of a material suitable for the intended application, for example a metal such as steel, a ceramic material, a glass or glass-like material or a plastic.
[0030] After producing the roughened structure 11, the magnetic composite component 1 is, as in Fig. 2, provided with an injection-molded plastic element, in this case a plastic-bonded magnetic element 20, which is injection-molded directly onto the contact surface 100 with the roughened structure 11 without any additional binding agents. The injection-molded magnetic element 20 contains magnetic powder particles distributed in the plastic mass, in particular hard ferrite magnetic powder particles or rare earth magnetic powder particles, such as magnetic powder particles of the neodymium-iron-boron type or cobalt-samarium type. The injection-molded magnetic element 20 sprayed on in this way bonds stably to the carrier 10 with a form-fit connection in the roughened structure 11, as extensive investigations by the inventors have shown. The thickness of the injection-molded magnetic element 20 can be, for example, 0.3 mm or up to 10 mm; thus, even very thin magnetic elements 20 and even thicker ones can be applied to the carrier 10 with a stable connection.Different types of plastics can be used, which, in a plastic-bonded magnetic element 20, form the relevant matrix for embedding the magnetic powder particles. Thermoplastics, thermosets, injection-molded elastomers, or injection-molded thermoplastic elastomers, such as PA compounds, PPS compounds, or TPE compounds, e.g., a TPC elastomer material, are particularly used as plastics. Immediate or direct injection molding means, in this case, that the plastic material, optionally with the magnetic particles, is brought into direct contact with the contact surface 100 and the surface of the roughened structure 11 formed therein, without an additional intermediate layer or bonding materials. The injection molding of the injection-molded element orThe magnetic element 20 can be formed without any intermediate processing step before the roughened structure 11 is formed, in order to keep the overall cycle time during the production of the magnetic composite component 1 as short as possible. Of course, it is also possible to produce the injection-molded element or magnetic element 20 at a later time or in a separate production line.
[0031] In the inventors’ investigations, as mentioned, a roughened structure 11, which is introduced by means of laser processing, has proven to be particularly advantageous for the stable connection of the sprayed-on injection-molded magnetic elements 20, whereby a cross pattern 110, as in Fig. 1, a particularly stable connection over the entire contact surface 100, virtually over the entire surface. However, other patterns of the roughened structure 11 are also possible, such as a (in Fig. 3) dot pattern 111 with closely spaced roughening points, which can also be advantageously produced by processing with a laser beam.
[0032] Fig. 3 shows, on the left side, a highly enlarged area with a “roughened point” of a dot pattern 111 and, on the right side, an enlarged view of a section of the cross pattern 110 in the area of the intersection point of the line-like pattern sections (the terms “point” and “line” are not to be understood in the mathematically strict sense, but in the practically relevant sense as an extended point or a widened line, as can also be seen from the illustration according to Fig. 3).
[0033] In the figure after Fig. 3, 1 cm corresponds to approximately 100 µm of the actual roughened structure. Accordingly, a roughened point of the dot pattern 111 extends approximately 500 µm in diameter, and the line width of the roughened structure 11 in the cross pattern 110 extends approximately 150 to 200 µm. The roughening depth for the line is, for example, 20 µm to 200 µm, and for the dot pattern, for example, between 200 µm and 600 µm. Within this coarse (macroscopic) roughened structure, which is achieved in particular by the laser treatment, there are finer (microscopic) roughened areas with lower roughness depths, approximately in the range of a few µm or even less than 1 µm. The size and shape of these macroscopic and microscopic roughening structures can be suitably varied by influencing the laser beam (irradiance, shape, exposure time), also depending on the carrier material, in order to obtain an optimal connection between the carrier 10 and the injection-molded element or magnetic element 20.
[0034] For full-surface bonding, the density of the roughening points or lines of the roughening structure 11 can also be varied. The density, depth, and shape of the roughening structure can be adjusted to suit the specific application and the material partner (carrier / injection-molded magnetic element). For example, the line density of the roughening structure 11 is at least 2 or 4 lines per cm, and the point density is at least 10 points per cm. 2 . As in particular Fig. As shown in Figure 3, laser processing during roughening results in additional roughening effects due to lateral protrusions next to the recesses of the roughening structure 11 in the contact surface 100, which also contribute to the stability of the connection. In addition to the width and depth of the roughening structure 11, the shape and edge angle of the roughening pits also contribute to the holding force.
[0035] Fig.Figure 4 shows a greatly enlarged cross-sectional area of a support 10 (here, for example, a steel support) with an injection-molded magnetic element 20 sprayed onto its roughened structure 11. The roughness depth in the area of the macroscopic depressions or indentations produced by laser processing (between the two faintly visible vertically spaced lines from the base of the depression to the top of the support) is 72.88 µm according to the entered dimensions. The indentations have a macroscopically rounded shape in cross-section and are narrowed in their clear width towards the top opening, creating undercuts where the injection-molded magnetic element 20 is stably held by the penetrated plastic material. Furthermore, microscopic indentations also form additional holding structures, some of which include microscopic undercuts, within the macroscopic indentations.
[0036] Using the connection technology between the carrier 10 and the injection-molded magnetic element 20 by creating a roughened structure 11 on a contact surface 100 of the carrier 10 and injecting the injection-molded magnetic element 20, a wide variety of other magnetic composite components 20 of different geometries, sizes, and arrangements of injection-molded magnetic elements 20 on a carrier 10 can also be produced, such as, for example, cylindrical magnetic composite components with magnetic elements 20 mounted on an inner and / or outer surface of the cylinder, which can also be distributed differently. Various fields of application are also possible, such as in sensor technology or electrical machines.
[0037] For magnetic sensors, even small magnetic fields are sufficient for detection, which can be generated by thin layers of magnetic elements 20. This can further shorten process times and save material during manufacturing. In electrical machines, such as small drives or generators with rotors based on plastic-bonded magnetic materials, axles or shafts are often overmolded with plastic-bonded magnetic material. Using the joining technology presented here, such composite components can be manufactured cost-effectively and with high process reliability.
[0038] In the case of magnetic composite components 1 with plastic-bonded magnetic elements 20, different filling levels can be selected, wherein the proportion of magnetic powder particles is, for example, in the range between 60 and 95, in particular 75 and 90, preferably between 80 and 90 wt.% (or mass %) of magnetic powder in the total weight or the total mass of the magnetic element.
[0039] Investigations by the inventors have shown that a stable connection between magnetic elements and carrier is achieved with magnetic composite components of the aforementioned design. For this purpose, various magnetic composite components were manufactured. An annular steel carrier with an outer diameter of 81.3 mm, an inner diameter of 69.5 mm, and a height (thickness in the axial direction) of 4.8 mm was selected as the carrier 10. The upper side of the steel carrier was provided with a roughened structure 11 by laser processing. A plastic-bonded annular magnetic element 20 with an outer diameter of 80.3 mm, an inner diameter of 72.3 mm, and a height of 1 mm was sprayed directly onto the roughened structure. The magnetic composite component 1 (assembly) was then examined with regard to the stability of the connection between the carrier and the magnetic element 20 and, as a further property, also for crack formation.
[0040] Different roughening structures 11 and patterns of the roughening structure 11 as well as different plastic materials were used for the magnetic composite components: 1. For a PA plastic material and a filler content of 89.3 mass% (Ma-%), a cross pattern with a roughness depth of the roughened structure resulted in good demoldability from the injection mold and a stable connection of the magnetic element to the steel carrier. 2. Even for a magnetic element made of PPS plastic material with a filling ratio of 84 wt%, good demoldability from the injection mold and a stable connection were achieved using the cross pattern, with the roughening depth being about 30 µm. 3. Similarly, a magnetic element made of a PPS plastic material with a filling level of 82.8 wt% showed good demoldability and a stable connection with the cross pattern and the roughness depth of 30 µm. 4. For a magnetic element made of TPE plastic material with a filling ratio of 82.5 wt%, the cross pattern also showed good demoldability and a stable connection, with a roughening depth of 30 µm.
Claims
[1] Magnetic composite component (1) comprising at least one carrier (10) with a contact surface (100) and at least one injection-molded magnetic element (20) sprayed onto the latter, wherein the contact surface (100) is provided with a roughened structure (11) on which the sprayed-on magnetic element (20) is held by positive locking, characterized by , that the magnetic element (20) is held by positive locking solely by means of the roughened structure (11), the roughened structure (11) has a coarse structure with an average roughness depth greater than 10 µm, in particular greater than 20 µm, and less than 1 mm, in particular less than 500 µm, and a fine structure at least locally within the coarse structure, in the range of 1 µm or less, in particular between 100 nm and 1 µm, that the magnetic element (20) contains magnetic powder with a filling level between 60 mass% and 95 mass%, preferably between 75 mass% and 90 mass% of the total mass of the magnetic element (20) and the powder particles of the magnetic powder have on average a maximum diameter between 1 µm and 5 µm or between 50 µm and 500 µm. [2] Magnetic composite component (1) according to claim 1, characterized by that the roughened structure (11) is produced by laser beam treatment. [3] Magnetic composite component (1) according to one of the preceding claims, characterized by that the roughening structure (11) is formed in a line pattern, in particular a cross pattern (110), and / or in a dot pattern (111) with roughening points distributed over the contact surface (100) at a close distance of less than 3 mm. [4] Magnetic composite component (1) according to one of the preceding claims, characterized by that the contact surface (100) is flat or curved. [5] Magnetic composite component (1) according to one of the preceding claims, characterized by that the contact surface (100) is extended in a continuous manner or is formed from spaced-apart surface parts, for example has an at least partially circumferential ring shape. [6] Magnetic composite component (1) according to one of the preceding claims, characterized by that the carrier (10) consists of metal, ceramic material or plastic at least in the region of the contact surface (100). [7] Magnetic composite component (1) according to one of the preceding claims, characterized by that the magnetic element has a plastic material made of one of the plastics polyamide, polyphenylene sulfide or thermoplastic elastomer as a matrix. [8] Magnetic composite component (1) according to one of the preceding claims, characterized by that the magnetic element (20) contains hard ferrite magnetic powder or rare earth magnetic powder in isotropic or, preferably, in anisotropic form as magnetic powder. [9] Magnetic composite component (1) according to one of the preceding claims, characterized by that the thickness of the magnetic element (20) is at most 5.0 mm, for example up to 2.5 mm, preferably between 0.2 mm and 1.5 mm. [10] Method for producing a magnetic composite component (1) according to one of the preceding claims, in which a magnetic element (20) with magnetic powder embedded in a plastic matrix is applied to a contact surface (100) of a carrier (10) by spraying, characterized by , that the contact surface (100) is roughened by means of a laser beam before the magnetic element (20) is sprayed on, wherein the roughened structure (11) has a coarse structure with an average roughness depth greater than 10 µm, in particular greater than 20 µm, and less than 1 mm, in particular less than 500 µm, and a fine structure at least locally within the coarse structure, in the range of 1 µm or less, in particular between 100 nm and 1 µm, that the magnetic element (20) is sprayed directly onto the roughened contact surface (100) and is held solely by means of the roughened structure (11), that magnetic powder with a filling degree between 60 mass% and 95 mass% of the total mass of the magnetic element (20) is used for the magnetic element (20), and wherein the powder particles of the magnetic powder have an average maximum diameter between 1 µm and 5 µm or between 50 µm and 500 µm. [11] Use of a magnetic composite component (1) according to one of claims 1 to 9 in a sensor unit or in an electrical machine.
Citation Information
Patent Citations
Component composite and methods for producing a component composite
DE102008040782A1
Device for detecting angular position of pinion of gear box drive device, has magnetic element whose magnetically active particles are bonded with each other through injection molding process and located on end face of wheel and gear
DE102011089903A1
Torque and / or angle sensor arrangement
DE102014018783A1
Abrasion-resistant and hydrolysis-resistant encoder, storage unit with encoder, and method for producing the encoder
DE102016218930A1
Polymeric resin bonded magnets
US20040045635A1