Semiconductor device and manufacturing process of a semiconductor device

DE102021106596B4Active Publication Date: 2024-11-14MITSUBISHI ELECTRIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
DE102021106596
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-17
Filing Date
2021-03-18
Publication Date
2024-11-14
Estimated Expiration
2041-03-18

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Semiconductor device (100), comprising: a resin-sealed copper base plate (1) comprising a copper base plate (1a), an insulating layer (1b) arranged on an upper surface of the copper base plate (1a) and a circuit structure (1c) arranged on an upper surface of the insulating layer (1b); a semiconductor element (2) mounted on an upper surface of the resin-insulated copper base plate (1); a housing (4) which is connected to an outer circumferential part of the insulating layer (1b) via an adhesive (9); a sealing material (8) which seals the upper surface of the resin-insulated copper base plate (1) and the semiconductor element (2) in the housing (4); and a metal spacer (12) which is provided on the upper surface of the insulating layer (1b) such that the circuit structure (1c) is completely enclosed in plan view.
Need to check novelty before this filing date? Find Prior Art

Description

Background of the inventionField of the invention

[0001] The present disclosure relates to a semiconductor device including a resin-insulated copper base plate and its manufacturing method. Description of the background technology

[0002] A semiconductor device has been proposed that includes a resin-insulated copper base plate, which includes a copper base plate, an insulating layer disposed on the upper surface of the copper base plate, and a circuit pattern disposed on the upper surface of the insulating layer, a semiconductor element, and a sealing material. The semiconductor element is mounted on the upper surface of the resin-insulated copper base plate. A case is bonded to the outer peripheral part of the resin-insulated copper base plate via an adhesive. The sealing material seals the upper surface of the resin-insulated copper base plate and the semiconductor element inside the case (see JP 2016-096188 A).

[0003] JP 2004 - 228 286 A discloses a semiconductor device comprising a heat sink, an insulating substrate connected to the heat sink via a lower solder, a semiconductor element connected to the insulating substrate via the lower solder, and a molding resin molded around the insulating substrate, wherein the height of the molding resin from the heat sink is set higher than the upper surface of the insulating substrate but lower than the upper surface of the semiconductor element. Summary

[0004] In recent years, cases where a semiconductor device operates at high temperatures have become increasingly common. For example, the operating temperature of a semiconductor device using silicon (Si) as its base material is 175°C. A desired operating temperature of a wide-band-gap semiconductor device using silicon carbide (SiC) and gallium nitride (GaN) as its base material is 200°C. Therefore, the glass transition temperature of a sealing material filled inside must exceed the operating temperature of the semiconductor device.

[0005] Furthermore, a resin having substantially similar properties to the sealing material is used as the adhesive for bonding the housing and the resin-insulated copper base plate. Sealing materials and adhesives suitable for such high-temperature operation have high viscosity and poor fluidity; therefore, filling a narrow gap between the housing and the resin-insulated copper base plate, or in a warped gap, with such sealing materials and adhesives is difficult without leaving an unfilled portion.

[0006] If there is an unfilled portion in the adhesive, it contains air, which often forms bubbles. This poses a problem in that when the bubbles in the adhesive reach the circuit structure, the insulation properties of the semiconductor device deteriorate due to the generation of a creeping discharge caused by the bubbles.

[0007] An object of the present disclosure is to provide a technique capable of suppressing insulation defects caused by the impact of bubbles contained in an adhesive on a circuit pattern in a semiconductor device.

[0008] This problem is solved by the features of the independent claim. The subclaims contain advantageous embodiments of the invention.

[0009] In the present semiconductor device, insulation defects caused by the impact of bubbles on the circuit structure are suppressed.

[0010] These and other objects, features, aspects and advantages of the present invention will become more apparent from the following detailed description of the present invention when taken in conjunction with the accompanying drawings. Short description of the drawings Fig. 1 is a cross-sectional view of a semiconductor device according to a comparative example; Fig. 2 is a cross-sectional view of a semiconductor device according to an embodiment of the invention; and Fig. 3 is a plan view of a resin-insulated copper base plate included in a semiconductor device according to another comparative example and its surroundings. Description of the preferred embodiment and examples <vergleichsbeispiel>

[0011] A comparative example is described below with reference to the drawings. Fig. 1 is a cross-sectional view of a semiconductor device 100 according to a comparative example.

[0012] As in Fig. 1, the semiconductor device 100 includes a resin-insulated copper base plate 1, a semiconductor element 2, a package 4, an electrode terminal 6, a sealing material 8, and roughening structures 11.

[0013] The resin-insulated copper base plate 1 includes a copper base plate 1a, an insulating layer 1b, and a circuit pattern 1c. The copper base plate 1a, the insulating layer 1b, and the circuit pattern 1c are integrated. The copper base plate 1a is formed in a rectangular shape in plan view. The insulating layer 1b is arranged over the entire upper surface of the copper base plate 1a. The insulating layer 1b is made of a resin and has a thickness of 0.2 mm. The circuit pattern 1c is arranged on the upper surface of the insulating layer 1b except for the outer peripheral part. The circuit pattern 1c is made of copper and has a thickness of 0.5 mm.

[0014] The semiconductor element 2 is mounted on the upper surface of the circuit structure 1c via a solder 3. The housing 4 is formed in a rectangular frame shape in plan view and is bonded to the outer peripheral part of the resin-insulated copper base plate 1 via an adhesive 9. Furthermore, the housing 4 is made of resin and has an insulating property.

[0015] The electrode terminal 6 is arranged in the housing 4 and is connected to the circuit structure 1c and the semiconductor element 2 via aluminum wires 7. The sealing material 8 is made of, for example, an epoxy resin and is filled into the interior of the housing 4. As a result, the sealing material 8 in the housing 4 seals the upper surface of the resin-insulated copper base plate 1 and the semiconductor element 2.

[0016] Two roughened structures 11 are formed on the upper surface of the insulating layer 1b so that the circuit structure 1c is doubly enclosed therewith in plan view. Each roughened structure 11 is formed in a rectangular shape in plan view. It should be noted that the number of roughened structures 11 is not limited to two, and three or more roughened structures 11 may be formed. Furthermore, each roughened structure 11 may be formed continuously or intermittently.

[0017] Each roughened structure 11 is formed at a position on the upper surface of the insulating layer 1b at a distance of 500 µm or more from the end portion of the circuit pattern 1c. Furthermore, each roughened structure 11 has a width of 200 µm and a depth of 1 / 3 of the thickness of the insulating layer 1b.

[0018] A manufacturing method of the semiconductor device 100 will be described below. First, the resin-insulated copper base plate 1 is manufactured. Only the formation of the characteristic part of the resin-insulated copper base plate 1 will be described here. In the manufacturing process of the resin-insulated copper base plate 1, after the circuit pattern 1c is formed on the upper surface of the insulating layer 1b, the insulating layer 1b is laser-machined or machined to form the roughened structures 11. Machining includes, for example, polishing or cutting.

[0019] Next, the semiconductor element 2 is bonded to the upper surface of the resin-insulated copper base plate 1 with a solder 3. After that, the adhesive 9 is applied to the outer peripheral part of the resin-insulated copper base plate 1. In a state where the case 4, in which the electrode terminal 6 is inserted, is attached to the outer peripheral part of the resin-insulated copper base plate 1, the temperature is raised to cure the adhesive 9, thereby completing the bonding. When the internal wiring of the aluminum wires 7 is completed, filling of the epoxy resin serving as the sealing material 8 is performed next. The semiconductor device 100 is completed by raising the temperature of the semiconductor device 100 to cure the epoxy resin.

[0020] The size of the bubbles 10 contained in the adhesive 9 is, for example, 0.1 mm or more and 0.2 mm or less. Although the adhesive 9 containing the bubbles 10 tends to move from the lower side of the housing 4 toward the circuit pattern 1c, the adhesive 9 containing the bubbles 10 is less likely to reach the circuit pattern 1c. This is because the surface area of ​​the periphery of the circuit pattern 1c on the upper surface of the insulating film 1b is increased by the formation of the roughened structures 11, that is, the path from the lower side of the housing 4 to the circuit pattern 1c is lengthened.

[0021] As described above, the semiconductor device 100 according to this comparative example includes the resin-insulated copper base plate 1 having the copper base plate 1a, the insulating layer 1b disposed on the upper surface of the copper base plate 1a, and the circuit pattern 1c disposed on the upper surface of the insulating layer 1b, the semiconductor element 2 mounted on the upper surface of the resin-insulated copper base plate 1, the case 4 bonded to the outer peripheral part of the resin-insulated copper base plate 1 via the adhesive 9, the sealing material 8 sealing the upper surface of the resin-insulated copper base plate 1 and the semiconductor element 2 in the case 4, and the roughened patterns 11 formed on the upper surface of the insulating layer 1b so as to enclose the circuit pattern 1c in plan view.

[0022] The surface area of ​​the periphery of the circuit pattern 1c on the upper surface of the insulating layer 1b is accordingly increased with the roughened structures 11; therefore, the path from the bottom side of the housing 4 to the circuit pattern 1c is extended, and this prevents the adhesive 9 containing the bubbles 10 from reaching the circuit pattern 1c. That is, the bases 10 are prevented from reaching the circuit pattern 1c. Consequently, insulation defects in the semiconductor device 100 caused by the impact of the bubbles 10 on the circuit pattern 1c are suppressed. This leads to long-term use of the semiconductor device 100.

[0023] Each roughened structure 11 is also formed at a position on the upper surface of the insulating layer 1b at a distance of 500 µm or more from the end portion of the circuit pattern 1c. Therefore, the inflow of bubbles 10 within 500 µm from the end portion of the circuit pattern 1c on the upper surface of the insulating layer 1b is suppressed. As a result, the required insulation withstand voltage of 2500 V or higher is ensured in the semiconductor device 100.

[0024] Each roughened structure 11 also has a width of 200 µm and a depth of 1 / 3 of the thickness of the insulating layer 1b. Therefore, the bubbles 10 contained in the adhesive 9 are trapped by the roughened structures 11. Furthermore, if the roughened structures 11 extend through the insulating layer 1b and reach the copper base plate 1a, there is a concern that the insulation properties of the semiconductor device 100 will deteriorate; however, no such problem occurs because the roughened structures 11 have a depth of 1 / 3 of the thickness of the insulating layer 1b.

[0025] Furthermore, in the manufacturing method of the semiconductor device according to this comparative example, after the circuit pattern 1c is formed, the roughening patterns 11 are formed by laser machining or machining the insulating layer 1b; therefore, the roughening patterns 11 are easily formed on the upper surface of the insulating layer 1b. <Ausführungsform>

[0026] A semiconductor device 100 according to an embodiment will be described below. Fig. Figure 2 is a cross-sectional view of a semiconductor device 100 according to the embodiment. In the embodiment, the same components as those described in the comparative example are denoted by the same reference numerals, and their descriptions are omitted.

[0027] As in Fig. 2, in the embodiment, the semiconductor device 100 has a metal spacer 12 instead of the roughening structures 11.

[0028] The metal spacer 12 is provided on the upper surface of the insulating layer 1b so as to continuously surround the circuit pattern 1c in plan view. The spacer 12 is made of metal that adheres to the insulating layer 1b and is formed in a rectangular shape in plan view. Although examples of the metals that adhere to the insulating layer 1b include copper, nickel, aluminum, and the like, copper is preferable considering that the spacer 12 is formed together with the circuit pattern 1c, as described later.

[0029] A method for manufacturing the semiconductor device according to the embodiment will be described below. Only steps different from those of the comparative example will be described here. In the manufacturing process of the resin-insulated copper base plate 1, etching is performed when the circuit pattern 1c is formed on the upper surface of the insulating layer 1b, thereby forming the metal spacer 12 together with the circuit pattern 1c. Therefore, the thickness of the metal spacer 12 is 0.5 mm, which is equal to the thickness of the circuit pattern 1c. A slight difference between the thickness of the circuit pattern 1c and the thickness of the metal spacer 12 due to manufacturing errors and the like is allowable.

[0030] The metal spacer 12 is arranged at a position on the upper surface of the insulating layer 1b at a distance of 500 μm or more from the end part of the circuit pattern 1c. The metal spacer 12 has a thickness of 500 μm or more and 1.0 mm or less to block the adhesive 9, preventing the adhesive 9 from reaching the circuit pattern 1c.

[0031] As described above, the semiconductor device 100 according to the embodiment includes the resin-insulated copper base plate 1 having the copper base plate 1a, the insulating layer 1b disposed on the upper surface of the copper base plate 1a, and the circuit pattern 1c disposed on the upper surface of the insulating layer 1b, the semiconductor substrate 2 mounted on the upper surface of the resin-insulated copper base plate 1, the case 4 bonded to the outer peripheral part of the resin-insulated copper base plate 1 via the adhesive 9, the sealing material 8 sealing the upper surface of the resin-insulated copper base plate 1 and the semiconductor element 2 in the case 4, and the metal spacer 12 disposed on the upper surface of the insulating layer 1b so as to enclose the circuit pattern 1c in plan view.

[0032] Accordingly, the adhesive 9 is blocked by the metal spacer 12; therefore, the adhesive 9 containing the bubbles 10 can be prevented from reaching the circuit structure 1c. That is, the bubbles 10 are prevented from reaching the circuit structure 1c. Consequently, insulation defects in the semiconductor device 100 caused by the impact of the bubbles 10 on the circuit structure 1c are suppressed. This leads to long-term use of the semiconductor device 100.

[0033] The metal spacer 12 is arranged at a position on the upper surface of the insulating layer 1b at a distance of 500 µm or more from the end portion of the circuit pattern 1c. Therefore, the inflow of the bubbles 10 within 500 µm from the end portion of the circuit pattern 1c on the upper surface of the insulating layer 1b is suppressed. As a result, the required insulation withstand voltage of 2500 V or higher is ensured in the semiconductor device 100.

[0034] Furthermore, the metal spacer 12 has a width of 500 μm or more and 1.0 mm or less and the same thickness as that of the circuit pattern 1c. Therefore, the bubbles 10 contained in the adhesive 9 are effectively blocked by the metal spacer 12.

[0035] Furthermore, in the method for manufacturing the semiconductor device according to the embodiment, the metal spacer 12 is formed by etching at the same time as the circuit pattern 1c is formed; therefore, the metal spacer 12 is formed together with the circuit pattern 1c. As a result, the metal spacer 12 is disposed on the upper surface of the insulating layer 1b without additional new steps. <Weiteres Vergleichsbeispiel >

[0036] A semiconductor device 100 according to another comparative example will be described below. Fig. 3 is a plan view of a resin-insulated copper base plate 1 included in a semiconductor device according to the comparative example and its surroundings. In the present example, the same components as those described above are denoted by the same reference numerals, and their descriptions are omitted.

[0037] In the embodiment, a metal spacer 12 is provided on the upper surface of the insulating layer 1b so as to continuously surround the circuit structure 1c in plan view. However, in the present example, the metal spacer 12 is arranged on the upper surface of the insulating layer 1b so as to intermittently surround the circuit structure 1c, as shown in Fig. 3. Therefore, the metal spacer 12 is provided with gaps 12a at predetermined intervals.

[0038] If the epoxy resin present between the circuit pattern 1c and the metal spacer 12 contains the bubbles 10 before the epoxy resin, which is to be the sealing material 8, is cured, the bubbles 10 are released through the gaps 12a of the metal spacer 12 to the outer peripheral side of the metal spacer 12. As a result, the bubbles 10 contained in the epoxy resin are kept away from the circuit pattern 1c. Here, a gap 12a larger than the size of a bubble 10 is formed, allowing the bubble 10 contained in the epoxy resin to pass through.

[0039] As described above, in the semiconductor device 100 according to the present comparative example, the metal spacer 12 is intermittently disposed. Therefore, the bubbles 10 contained in the epoxy resin serving as the sealing material 8 are prevented from reaching the circuit pattern 1c. As a result, in addition to the effect of the embodiment, insulation defects caused by the impact of the bubbles 10 on the circuit pattern 1c are suppressed in the semiconductor device 100.

[0040] Embodiments can be combined.< / vergleichsbeispiel>

Claims

[1] A semiconductor device (100) comprising: a resin-sealed copper base plate (1) comprising a copper base plate (1a), an insulating layer (1b) disposed on an upper surface of the copper base plate (1a), and a circuit pattern (1c) disposed on an upper surface of the insulating layer (1b); a semiconductor element (2) mounted on an upper surface of the resin-insulated copper base plate (1); a housing (4) connected to an outer peripheral part of the insulating layer (1b) via an adhesive (9); a sealing material (8) sealing the upper surface of the resin-insulated copper base plate (1) and the semiconductor element (2) in the housing (4); and a metal spacer (12) provided on the upper surface of the insulating layer (1b) so as to continuously surround the circuit structure (1c) in plan view. [2] The semiconductor device (100) according to claim 1, wherein the metal spacer (12) is formed at a position on the upper surface of the insulating layer (1b) at a distance of 500 µm or more from an end part of the circuit pattern (1c). [3] The semiconductor device (100) according to claim 1 or 2, wherein the metal spacer (12) has a width of 500 µm or more and 1.0 mm or less and a thickness the same as that of the circuit pattern (1c). [4] A manufacturing method of the semiconductor device (100) according to any one of claims 1 to 3, wherein the metal spacer (12) is formed by means of etching performed when the circuit pattern (1c) is formed.

Citation Information

Patent Citations

  • Power semiconductor device

    JP2004228286A

  • Semiconductor device

    JP2016096188A

  • JP002004228286A