WAFER MANUFACTURING APPARATUS FOR PRODUCING A WAFER FROM A SEMICONDUCTOR RINGOT

The described apparatus addresses the inefficiencies in SiC wafer production by using a laser-formed peeling layer and ultrasonic oscillation to efficiently peel wafers from ingots of varying sizes, enhancing productivity and reducing the need for chuck table replacements.

DE102021214125B4Active Publication Date: 2025-10-02DISCO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE102021214125
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-17
Filing Date
2021-12-10
Publication Date
2025-10-02
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

The inefficient production of SiC wafers due to the high hardness of SiC single crystal ingots, leading to low productivity and high piece costs, and the need for frequent replacement of chuck tables in existing wafer manufacturing apparatuses.

Method used

A wafer manufacturing apparatus that forms a peeling layer using a laser beam with a wavelength transmissible through the ingot, combined with an ultrasonic oscillation unit and a chuck table with a porous plate and adjustable pressure regions, allowing for efficient peeling of wafers from ingots of varying diameters without requiring table replacement.

Benefits of technology

Enhances productivity and reduces the need for chuck table changes by effectively peeling SiC wafers, improving efficiency and cost-effectiveness in wafer production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A wafer manufacturing apparatus (30) for manufacturing a wafer (11) from a semiconductor ingot (1, 1-1, 1-2) in which a stripping layer (13) is formed by positioning a focal point (22) of a laser beam (21) having a wavelength transmittable through the semiconductor ingot (1, 1-1, 1-2) at a depth (23) corresponding to a thickness (14) of the wafer (11) to be manufactured, and applying the laser beam (21), the wafer manufacturing apparatus comprising: a chuck table (31) configured to hold the semiconductor ingot (1, 1-1, 1-2) on a suction surface (32) with the wafer (11) to be produced on an upper side; an ultrasonic oscillating unit (34) having an end surface (341) facing the wafer (11) to be produced and configured to oscillate an ultrasonic wave; a water supply unit (33) configured to supply water (331) between the wafer (11) to be produced and the end face (341) of the ultrasonic oscillation unit (34); a pulling unit (35) configured to suck and hold the wafer (11) to be produced and to pull the wafer (11) to be produced from the semiconductor ingot (1, 1-1, 1-2); and a water receiving unit (36) arranged to surround the chuck table (31) and to receive the water (331) which is discharged after being supplied from the water supply unit (33) to the semiconductor ingot (1, 1-1, 1-2) and flows on the suction surface (32) of the chuck table (31) on a circumference of the semiconductor ingot (1, 1-1, 1-2), wherein the clamping table (31) comprises a porous plate (40) forming the suction surface (32), and a base (50) supporting the porous plate (40) and having a connecting passage (54) arranged to apply a negative pressure to the porous plate (40), and wherein the chuck table (31) sucks and holds the semiconductor ingot (1, 1-1, 1-2) even in a state in which an area of ​​a lower surface (3) of the semiconductor ingot (1, 1-1, 1-2) is smaller than an area of ​​the suction surface (32) and the water (331) flows on the suction surface (32) exposed on the periphery of the semiconductor ingot (1, 1-1, 1-2).
Need to check novelty before this filing date? Find Prior Art

Description

BACKGROUND OF THE INVENTION FIELD OF THE INVENTION

[0001] The present invention relates to a wafer manufacturing apparatus. DESCRIPTION OF THE RELATED PRIOR ART

[0002] Various types of electronic device chips, such as integrated circuits (ICs), large-area integration (LSIs), light-emitting diodes (LEDs), and power devices, are manufactured by forming devices by forming tiny circuits on a wafer thinly sliced ​​from a single-crystal semiconductor ingot made of silicon, sapphire, silicon carbide (SiC), or the like with a wire saw, and then dicing the wafer into individual chips. However, if the wafer is manufactured by cutting the single-crystal semiconductor ingot with a wire saw and polishing the top and bottom surfaces of the wafer, 70 to 80% of the volume of an ingot is wasted, which is uneconomical.

[0003] In particular, the single-crystal SiC ingot presents problems in the efficient production of wafers because the single-crystal SiC ingot has high hardness, so it is difficult to cut the single-crystal SiC ingot with the wire saw, and cutting the single-crystal SiC ingot takes a lot of time, resulting in low productivity, and the unit cost of the single-crystal SiC ingot is high.

[0004] To solve these problems, a technology has been proposed (see, for example, Japanese Unexamined Patent Application No. JP 2019 - 102 513 A) that forms a separation layer in a planned cutting surface by positioning a focal point of a laser beam transmitted through the single-crystal SiC ingot inside the ingot and applying the laser beam, and separating the wafer.

[0005] Furthermore, DE 10 2019 204 741 A discloses a method for producing a wafer from a hexagonal single crystal ingot, comprising the steps of planarizing an end side of the hexagonal single crystal ingot, forming a peel layer in the hexagonal single crystal ingot by applying a pulsed laser beam. SUMMARY OF THE INVENTION

[0006] There are various types of single-crystal SiC ingots, ranging in diameter from, for example, 7.62 cm (3 inches) to 15.24 cm (6 inches). A puller disclosed in Japanese Patent Application Laid-Open No. 2019-102513 uses a chuck table with suction grooves in a suction surface that correspond to the sizes of the respective ingots. Therefore, in the puller disclosed in Japanese Patent Application Laid-Open No. 2019-102513, the chuck table must be replaced each time the size of an ingot is changed.

[0007] It is therefore an object of the present invention to provide a wafer manufacturing apparatus that can reduce the change of a chuck table.

[0008] In accordance with one aspect of the present invention, a wafer manufacturing apparatus for manufacturing a wafer from a semiconductor ingot is provided, in which a peel-off layer is formed by positioning a focal point of a laser beam having a wavelength transmittable through the semiconductor ingot at a depth corresponding to a thickness of the wafer to be manufactured and applying the laser beam, wherein the wafer manufacturing apparatus comprises a chuck table configured to hold the semiconductor ingot with the wafer to be manufactured on an upper side on a suction surface, an ultrasonic oscillation unit having an end surface facing the wafer to be manufactured and configured to oscillate an ultrasonic wave, a water supply unit configured to supply water between the wafer to be manufactured and the end surface of the ultrasonic oscillation unit, a peel-off unit,which is configured to suck and hold the wafer to be produced and to pull the wafer to be produced from the semiconductor ingot, and has a water absorption unit configured to surround the chuck table and absorb the water discharged after being supplied to the semiconductor ingot by the water supply unit and flowing on the suction surface of the chuck table at a periphery of the semiconductor ingot. The chuck table includes a porous plate forming the suction surface, a base supporting the porous plate and having a connecting passage configured to exert negative pressure on the porous plate. The chuck table sucks and holds the semiconductor ingot even in a state where an area of ​​a lower surface of the semiconductor ingot is smaller than an area of ​​the suction surface, and the water flows on the suction surface exposed at the periphery of the semiconductor ingot.

[0009] Preferably, the suction surface of the porous plate has a first region corresponding to a first semiconductor ingot having a first diameter and a second region surrounding the first region, wherein communication passages configured to selectively apply a negative pressure or a positive pressure are connected to a surface of the porous plate with regions corresponding to the first region and the second region, respectively, the surface being on the opposite side to the suction surface, and when the first semiconductor ingot is sucked and held, the negative pressure is applied through the communication passage connected to the first region and the positive pressure is applied through the communication passage connected to the second region.

[0010] Preferably, a decompression pump as a suction source is coupled to the connecting passage of the chuck table, a pressure gauge is installed on the connecting passage, and a difference between the measured values ​​of the pressure gauge when the decompression pump is actuated in a state where nothing is attached to the suction surface of the porous plate and in a state where the ingot is placed on the suction surface of the porous plate is equal to or greater than 5 kPa.

[0011] The above and other objects, features and advantages of the present invention and the mode for carrying them out will become more apparent and the invention itself will be best understood by studying the following description and the appended claims with reference to the accompanying drawings which show a preferred embodiment of the invention. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a plan view of a SiC ingot as a processing target of a wafer manufacturing apparatus in accordance with an embodiment; Fig. 2 is a side view of the Fig. 1 SiC ingots shown; Fig. 3 is a perspective view of a wafer manufactured by the wafer manufacturing apparatus according to the embodiment; Fig. 4 is a perspective view showing a state during formation of a peeling layer in the Fig. 1 represents the SiC ingot; Fig. 5 is a side view showing a state during formation of the peeling layer in the Fig. 4 represents the SiC ingot; Fig. 6 is a perspective view schematically illustrating an example of a configuration of the wafer manufacturing apparatus according to the embodiment; Fig. 7 is a sectional view showing the Fig. 6 schematically illustrates the wafer manufacturing apparatus shown; Fig. 8 is a perspective view of a clamping table of the Fig. 6 illustrated wafer manufacturing apparatus; Fig. 9 is an exploded perspective view of the Fig. 8 shown clamping table; Fig. 10 is a sectional view schematically illustrating the wafer manufacturing apparatus according to the embodiment at a time of processing a second SiC ingot; Fig. 11 is a sectional view schematically illustrating the wafer manufacturing apparatus according to the embodiment at the time of processing a first SiC ingot; Fig. 12 is a sectional view showing the Fig. 10 schematically shows the second SiC ingot removed from the wafer; and Fig. 13 is a sectional view schematically illustrating a chuck table of a wafer manufacturing apparatus according to a modification of the embodiment. DETAILED EXPLANATION OF THE PREFERRED EMBODIMENT

[0012] An embodiment of the present invention will be described in detail below with reference to the drawings.

[0013] A wafer manufacturing apparatus according to the embodiment of the present invention will be described with reference to the drawings. First, a SiC ingot as a processing target ingot of the wafer manufacturing apparatus according to the embodiment will be described. Fig. 1 is a plan view of the SiC ingot as a processing target of the wafer manufacturing apparatus according to the embodiment. Fig. 2 is a side view of the Fig. 1 shown SiC ingots. Fig. 3 is a perspective view of a wafer manufactured by the wafer manufacturing apparatus according to the embodiment. Fig. Fig. 4 is a perspective view showing a state of forming a peeling layer in the Fig. 1 represents the SiC ingot. Fig. 5 is a side view showing a state of forming the peeling layer in the Fig. 4 represents the SiC ingot.

[0014] The Fig. 1 and Fig. The SiC ingot 1 shown in Figure 2 is formed as a whole with a cylindrical shape in the embodiment. In the embodiment, the SiC ingot 1 is a hexagonal single-crystal SiC ingot.

[0015] As in Fig. 1 and Fig. As shown in Figure 2, the SiC ingot 1 has a first surface 2 as a circular end surface, a circular second surface 3 (corresponding to a bottom surface) at the bottom of the first surface 2, and a peripheral surface 4 connected to the outer edge of the first surface 2 and the outer edge of the second surface 3. Furthermore, the SiC ingot 1 has, on the peripheral surface 4, a first alignment plane 5 indicating a crystal orientation and a second alignment plane 6 perpendicular to the first alignment plane 5. The length of the first alignment plane 5 is longer than the length of the second alignment plane 6.

[0016] Furthermore, the SiC ingot 1 has a c-axis 9 that is inclined by a deviation angle α with respect to a normal 7 to the first surface 2 in an inclination direction 8 toward the second alignment plane 6, and a c-plane 10 that is perpendicular to the c-axis 9. The c-plane 10 is inclined by the deviation angle α with respect to the first surface 2 of the SiC ingot 1. The inclination direction 8 of the c-axis 9 from the normal 7 is perpendicular to the extension direction of the second alignment plane 6 and parallel to the first alignment plane 5. At the molecular level of the SiC ingot 1, an infinite number of c-planes 10 are arranged in the SiC ingot 1. In the embodiment, the deviation angle α is set to 1°, 4°, or 6°. However, within the scope of the present invention, the SiC ingot 1 can be produced with a deviation angle α which can be freely adjusted, for example, in a range of 1° to 6°.

[0017] In addition, the first surface 2 of the SiC ingot 1 is formed into a mirror surface by subjecting it to polishing processing by a polishing device after a grinding device has subjected the first surface 2 to grinding processing.

[0018] One in Fig. The wafer 11 shown in FIG. 3 is manufactured by peeling off a part of the SiC ingot 1 and subjecting a peeled surface 12 of the SiC ingot 1 to grinding, polishing, and the like. After the wafer 11 is peeled off the SiC ingot 1, devices are formed on the upper surface of the wafer 11. In the embodiment, the devices are metal-oxide-semiconductor field-effect transistors (MOSFETs), micro-electromechanical systems (MEMS), or Schottky barrier diodes (SBDs). However, in the present invention, the devices are not limited to MOSFETs, MEMS, and SBDs. Otherwise, the same parts of the wafer 11 as those of the SiC ingot 1 are denoted by the same reference numerals, and their description will be omitted.

[0019] After the Fig. 1 and Fig. 2 has formed a peel layer 13 as shown in Fig. 4 and Fig. 5, the wafer 11 to be produced is peeled off the SiC ingot 1 with the peel layer 13 as a starting point. The peel layer 13 is formed inside the SiC ingot 1 by forming a focal point 22 (shown in Fig. 5) a pulsed laser beam 21 (shown in Fig. 5) with a wavelength that is transparent to the SiC ingot 1 from the first alignment plane 2 of the SiC ingot 1 at a depth of 23 (shown in Fig. 5) is positioned, which has a thickness 14 (shown in Fig. 3) of the wafer 11 to be produced, and the pulsed laser beam 21 is applied along the second alignment plane 6.

[0020] When the SiC ingot 1 is irradiated with the pulsed laser beam 21 having the wavelength transmissible through the SiC ingot 1, a modified portion 24 is formed inside the SiC ingot 1 along the second alignment plane 6, in which SiC is separated into silicon (Si) and carbon (C) by the application of the pulsed laser beam 21, the next applied pulsed laser beam 21 is absorbed by the previously formed C and SiC is separated into Si and C in a chain-like manner, and a crack extending from the modified portion 24 along the c-plane 10 is generated. Therefore, when the SiC ingot 1 is irradiated with the pulsed laser beam 21 having the wavelength transmissible through the SiC ingot 1, the peel layer 13 including the modified portion 24 and the crack formed by the modified portion 24 along the c-plane 10 is formed.

[0021] After the SiC ingot 1 is irradiated with the laser beam 21 over its entire length in a direction parallel to the second alignment plane 6, the SiC ingot 1 and a laser beam irradiation unit (not shown) that applies the laser beam 21 are adjusted relative to each other along the first alignment plane 5. An adjustment movement distance 25 at this time is equal to or smaller than the width of the crack. A peel layer 13 is again formed inside the SiC ingot 1 by positioning the focal point 22 at the depth 23 corresponding to the thickness 14 of the first surface 2 and applying the pulsed laser beam 21 along the second alignment plane 6. The process of irradiating the SiC ingot 1 with the laser beam 21 along the second alignment plane 6 and the process of adjusting the laser beam irradiation unit relatively along the first alignment plane 5 are repeated.

[0022] Consequently, in the SiC ingot 1, the peel layer 13, which has the modified portion 24 where SiC is separated into Si and C and the crack, and which has lower strength than the other parts, is formed at the depth 23 corresponding to the thickness 14 of the wafer 11 at each moving distance of the attitude from the first surface 2. In the SiC ingot 1, the peel layer 13 is formed at the depth 23 corresponding to the thickness 14 at each moving distance 25 of the attitude over the entire length in the direction parallel to the first alignment plane 5 from the first surface 2.

[0023] In addition, there are several types of SiC ingots 1 that differ in diameter 26. In the embodiment, a wafer manufacturing apparatus 30 manufactures the wafer 11 from a first SiC ingot 1-1 (corresponding to a first ingot) having a first diameter 26-1 and a second SiC ingot 1-2 (corresponding to a second ingot) having a second diameter 26-2 larger than the first diameter 26-1, as SiC ingot 1. (Wafer manufacturing device)

[0024] Next, the wafer manufacturing apparatus is described below. Fig. 6 is a perspective view schematically illustrating an example of a configuration of the wafer manufacturing apparatus according to the embodiment. Fig. 7 is a sectional view showing the Fig. 6 schematically illustrates the wafer manufacturing apparatus shown. Fig. 8 is a perspective view of a clamping table of the Fig. 6 shown wafer manufacturing apparatus. Fig. 9 is an exploded perspective view of the Fig. 8. The wafer manufacturing apparatus 30 in accordance with the embodiment is an apparatus that Fig. 3 by peeling the wafer 11 from the SiC ingot 1-1 or 1-2 in which the peel layer 13 is formed.

[0025] As in Fig. 6 and Fig. 7, the wafer manufacturing apparatus 30 includes a chuck table 31, a water supply unit 33 (only in Fig. 6), an ultrasonic oscillating unit 34 (only in Fig. 6), a pull-off unit 35 (only in Fig. 6), a water intake unit 36 ​​and a control unit 100 (only in Fig. 6).

[0026] The chuck table 31 holds the SiC ingot 1-1 or 1-2 with the wafer 11 to be manufactured on an upper side. The upper surface of the chuck table 31 is a suction surface 32 parallel to a horizontal direction. The second surface 3 of the SiC ingot 1-1 or 1-2 is attached to the suction surface 32, and the chuck table 31 holds the SiC ingot 1-1 or 1-2 by the suction surface 32 with the first surface 2 facing upward. Incidentally, a detailed configuration of the chuck table 31 will be described later.

[0027] The water supply unit 33 supplies water 331 (shown in Fig. 10) between the wafer 11 to be produced and an end surface 341 of the ultrasonic oscillation unit 34. The water supply unit 33 is a pipe that supplies water 331 supplied from a water supply source (not shown) at its lower end. In the embodiment, the water supply unit 33 supplies the water 331 to the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31. Incidentally, in the embodiment, the water supply unit 33 is provided in a casing 342 of the ultrasonic oscillation unit 34 and supplies the water 331 from the outside of the end surface 341 of the ultrasonic oscillation unit 34.

[0028] The ultrasonic oscillation unit 34 is housed in the housing 342. The ultrasonic oscillation unit 34 faces the wafer 11 to be produced, of the SiC ingot 1-1 or 1-2 held on the chuck table 31, with its end face 341. The ultrasonic oscillation unit 34 oscillates an ultrasonic wave and applies the oscillated ultrasonic wave to the SiC ingot 1-1 or 1-2. The end face 341 of the ultrasonic oscillation unit 34 faces the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31 in a direction perpendicular to the suction surface 32 and the first surface 2.

[0029] The ultrasonic oscillation unit 34 includes an ultrasonic vibrator and a sonotrode, the end surface 341 of which faces the wafer 11 to be produced. The ultrasonic vibrator is formed, for example, by a known piezoelectric element. Power is supplied to the ultrasonic vibrator from a power source (not shown), so that the ultrasonic vibrator vibrates along the above-described perpendicular direction at a frequency equal to or higher than 20 kHz and equal to or lower than several gigahertz with an amplitude of several micrometers to several tens of micrometers (this vibration is hereinafter referred to as ultrasonic vibration). The sonotrode is formed in a columnar shape and attached to an end surface of the ultrasonic vibrator that is closer to the suction surface 32.

[0030] The ultrasonic oscillating unit 34 applies an ultrasonic wave to the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31 by immersing the end surface 341 in the water 331 supplied from the water supply unit 33 (shown in Fig. 10), the end surface 341 is ultrasonically vibrated by the ultrasonic vibration of the ultrasonic vibrator, thereby ultrasonically vibrating the first surface 2 of the SiC ingot 1-1 or 1-2 via the water 331. Furthermore, in the embodiment, the water supply unit 33 and the ultrasonic oscillation unit 34 are provided so that they can be raised and lowered by a lifting and lowering mechanism (not shown).

[0031] The peeling unit 35 sucks and holds the wafer 11 to be produced from the SiC ingot 1-1 or 1-2, to which the ultrasonic wave is applied, and peels the wafer 11 from the SiC ingot 1-1 or 1-2. The peeling unit 35 includes a transfer pad 351 that sucks and holds the wafer 11 to be produced on a lower surface thereof, and an unillustrated moving unit that freely moves the transfer pad 351 in the horizontal direction and raises or lowers the transfer pad 351 above the chuck table 31. The movable unit moves the transfer pad 351 along the horizontal direction between a position above the chuck table 31 and a position retracted from above the chuck table 31.

[0032] The water receiving unit 36 ​​surrounds the chuck table 31. The water receiving unit 36 ​​receives the water 331 supplied from the water supply unit 33 to the SiC ingot 1-1 or 1-2 and flows onto the suction surface 32 of the chuck table 31 on the periphery of the SiC ingot 1-1 or 1-2. In the embodiment, the water receiving unit 36 ​​is formed into a box shape with a closed bottom and has an opening in an upper portion thereof, has the chuck table 31 installed on the bottom, and surrounds the chuck table 31. As shown in Fig. As shown in Figure 7, a drain opening 361 opens in the bottom of the water intake unit 36, which releases the water 331 to the outside.

[0033] As in Fig. 7, Fig. 8 and Fig. As shown in Figure 9, the chuck table 31 includes a porous plate 40 and a base 50. The upper surface of the porous plate 40 forms the suction surface 32, and the porous plate 40 is formed into a disc shape whose outer diameter is larger than the second diameter 36-2 of the second SiC ingot 1-2 and whose thickness is uniform. Therefore, the area of ​​the second surface 36 of the SiC ingot 1-1 or 1-2 is smaller than the area of ​​the suction surface 32 of the chuck table 31.

[0034] The porous plate 40 is formed by a porous ceramic as the porous material. In the embodiment, the porous ceramic of the porous plate 40 is prepared, for example, by mixing alumina abrasive grains of a predetermined size, a frit, and a liquid adhesive, and firing the mixture at 600°C to 1300°C after pressing the mixture into a disc shape.

[0035] As a result of manufacturing by the above-described manufacturing method, the porosity of the porous ceramic constituting the porous plate 40 is equal to or more than 40% and equal to or less than 70% in volume ratio, and the diameter of the vent holes formed by pores is equal to or more than 10 μm and equal to or less than 25 μm. In the embodiment, the porous plate 40 is set so that in a case where a decompression pump 56 (shown in Fig. 7) connected to the chuck table 31 as a suction source is operated in a state where nothing is mounted on the suction surface 32, a pressure value measured by a pressure gauge 57 provided to a converging communication passage 54-2 described later is within a predetermined range smaller than that of a conventional embodiment. In the embodiment, the predetermined range is, for example, between -65 kPa (gauge pressure) and -20 kPa (gauge pressure).

[0036] In addition, the suction surface 32 of the porous plate 40 in the embodiment has a first region 321 (region of the suction surface 32 which is located on the inside of a dashed line in Fig. 6, Fig. 8, Fig. 9 or the like) corresponding to the first SiC ingot 1-1, and a second region 322 (region of the suction surface 32 located on the outside of the dashed line in Fig. 6, Fig. 8, Fig. 9 or the like) surrounding the first region 321. In the embodiment, the planar shape of the first region 321 and the second region 322 is a circular shape coaxial with the planar shape of the suction surface 32. Furthermore, in the embodiment, the diameter of the first region 321 is equal to the first diameter 26-1 of the first SiC ingot 1-1.

[0037] Therefore, the first region 321 is attached to the first SiC ingot 1-1 when the suction surface 32 holds the first SiC ingot 1-1. The first region 321 and the second region 322 are attached to the second SiC ingot 1-2 when the suction surface 32 holds the second SiC ingot 1-2. While the boundary between the first region 321 and the second region 322 is indicated by the dashed line in Fig. 6, Fig. 8, Fig. 9 or the like, the boundary between the first region 321 and the second region 322 is not displayed on the suction surface 32 of an actual porous plate 40.

[0038] The base 50 supports the porous plate 40. The base 50 includes communication passages 54 that apply negative pressure to the porous plate 40. In the embodiment, the base 50 is formed of a metal such as stainless steel, has a disc-like shape whose outer diameter corresponds to the outer diameter of the porous plate 40 and whose thickness is uniform, and is installed at the center of the bottom of the water receiving unit 36.

[0039] The base 50 supports the porous plate 40, and the porous plate 40 is attached to an upper surface 51 parallel to the horizontal direction. Therefore, the upper surface 51 of the base 50 is attached to a surface 41 of the porous plate 40 located on a side opposite the suction surface 32. A central recessed portion 52 having a circular planar shape and a plurality of annular recessed portions 53 having a ring shape are formed in the upper surface 51 of the base 50.

[0040] In the embodiment, the central recessed portion 52 and the plurality of annular recessed portions 53 are formed at positions coaxial with the upper surface 51 of the base 50. In the embodiment, the diameter of the central recessed portion 52 is smaller than the diameter of the first region 321. In the embodiment, three annular recessed portions 53 are formed in the upper surface 51. However, in the present invention, the number of the annular recessed portions 53 formed in the upper surface 51 is not limited to three. Incidentally, the three annular recessed portions 53 will be described hereinafter as a first annular recessed portion 53-1, a second annular recessed portion 53-2, and a third annular recessed portion 53-3 in order from the inside.

[0041] The inner diameter and outer diameter of the first annular recessed portion 53-1 are larger than the diameter of the middle recessed portion 52 and smaller than the diameter of the first region 321. The inner diameter and outer diameter of the second annular recessed portion 53-2 are larger than the inner diameter and outer diameter of the first annular recessed portion 53-1 and the diameter of the first region 321. The inner diameter and outer diameter of the third annular recessed portion 53-3 are larger than the inner diameter and outer diameter of the second annular recessed portion 53-2 and the diameter of the first region 321.

[0042] The communication passages 54 each have one end opening into the respective bottoms of the middle recessed portion 52, the first annular recessed portion 53-1, the second annular recessed portion 53-2, and the third annular recessed portion 53-3, and the other end communicating with the collecting communication passage 54-2 as a communication passage. The collecting communication passage 54-2 is connected to the decompression pump 56. The communication passages 54 and the collecting communication passage 54-2 are formed by flow passages formed in the base 50 or a pipe connected to the base 50, or the like.

[0043] The connecting passages 54 cause a negative pressure to act on the porous plate 40 attached to the base 50 by being sucked by the decompression pump 56, and suck and hold the porous plate 40 to the base 50, and suck and hold the SiC ingot 1-1 or 1-2 to the suction surface 32 by causing the negative pressure to act on the porous plate 40. Incidentally, the connecting passages 54, one end of which is connected to the central recessed portion 52, and the first annular recessed portion 53-1 are connecting passages connected to the first region 321.

[0044] Incidentally, in this embodiment, the decompression pump 56 is implemented as a waterproof vacuum pump. Furthermore, in this embodiment, the pressure gauge 57, which measures the atmospheric pressure in the collecting connection passage 54-2, is installed at the collecting connection passage 54-2. The pressure gauge 57 outputs a measurement result to the control unit 100.

[0045] Furthermore, one ends of the relief pressure communication passages 55 open as communication passages in the respective bottoms of the middle recessed portion 52, the first annular recessed portion 53-1, the second annular recessed portion 53-2, and the third annular recessed portion 53-3. The other ends of the relief pressure communication passages 55 communicate with a collective relief pressure communication passage 55-2. The collective relief pressure communication passage 55-2 is connected to a relief pressure source 58. The relief pressure communication passages 55 and the collective relief pressure communication passage 55-2 are formed by flow passages formed in the base 50 or a pipe or the like connected to the base 50.The positive pressure communication passages 55 act on the porous plate 40 attached to the base 50 by being supplied with a gas pressurized by the positive pressure source 58, and discharge gas from the vent holes in the suction surface 32 of the porous plate 40 by applying the positive pressure to the porous plate 40. Incidentally, the positive pressure communication passages 55, one end of which is connected to the second annular recessed portion 53-2 and the third annular recessed portion 53-3, are communication passages connected to the second region 322.

[0046] In addition, the communication passages 54, one ends of which open in the respective bottoms of the first annular recessed portion 53-1, the second annular recessed portion 53-2 and the third annular recessed portion 53-3, are each provided with an opening and closing valve 59.Hereinafter, the opening and closing valve 59 provided for the communication passage 54 with one end opening in the bottom of the first annular recessed portion 53-1 will be described as the first opening and closing valve 59-1, the opening and closing valve 59 provided for the communication passage 54 with one end opening in the bottom of the second annular recessed portion 53-2 will be described as the second opening and closing valve 59-2, and the opening and closing valve 59 provided for the communication passage 54 with one end opening in the bottom of the third annular recessed portion 53-3 will be described as the third opening and closing valve 59-3.

[0047] In addition, the relief pressure communication passages 55, one ends of which open in the respective bottoms of the first annular recessed portion 53-1, the second annular recessed portion 53-2 and the third annular recessed portion 53-3, are each provided with an opening and closing valve 60.Hereinafter, the relief pressure opening / closing valve 60 provided for the relief pressure communication passage 55, one end of which opens in the bottom of the first annular recessed portion 53-1, will be described as a first relief pressure opening / closing valve 60-1, the opening and closing valve 60 provided for the relief pressure communication passage 55, one end of which opens in the bottom of the second annular recessed portion 53-2 will be described as a second relief pressure opening / closing valve 60-2, and the opening and closing valve 60 provided for the relief pressure communication passage 55, one end of which opens in the bottom of the third annular recessed portion 53-3 will be described as a third relief pressure opening / closing valve 60-3.

[0048] In addition, the collective connection passage 54-2 is provided with a collective opening / closing valve 61 as an opening and closing valve, and the collective relief pressure connection passage 55-2 is provided with a collective relief pressure opening / closing valve 62 as an opening and closing valve.

[0049] Accordingly, the connecting passages 54, 55, 54-2, and 55-2 of the chuck table 31 are provided with the opening and closing valves 59-1, 59-2, 59-3, 60-1, 60-2, 60-3, 61, and 62, one ends of the connecting passages 54, 55, 54-2, and 55-2 open in the bottoms of the middle recessed portion 52, the first annular recessed portion 53-1, the second annular recessed portion 53-2, and the third annular recessed portion 53-3 in the upper surface 51 of the base 50, and the connecting passages 54, 55, 54-2, and 55-2 are connected to the decompression pump 56 and the relief pressure source 58. The connecting passages 54, 55, 54-2 and 55-2 thereby establish a negative pressure or an overpressure which selectively acts on regions of the surface 41 of the porous plate 40 which correspond to the first region 321 or the second region 322.Therefore, the communication passages 54, 55, 54-2, and 55-2, which selectively establish the negative pressure or the positive pressure, are connected to the regions of the surface 41 of the porous plate 40 that correspond to the first region 321 and the second region 322, respectively. Incidentally, the regions corresponding to the first region 321 and the second region 322 refer to regions of the surface 41 of the porous plate 40 that coincide with the first region 321 and the second region 322, respectively, in the thickness direction of the porous plate 40.

[0050] The control unit 100 causes the wafer manufacturing apparatus 30 to perform a processing process of the SiC ingot 1-1 or 1-2, that is, a manufacturing process of the wafer 11, by controlling the above-described components of the wafer manufacturing apparatus 30. Incidentally, the control unit 100 is a computer including an arithmetic processing device comprising a microprocessor such as a central processing unit (CPU), a storage device comprising a memory such as a read-only memory (ROM) or a random access memory (RAM), and an input / output interface device.The arithmetic processing means of the control unit 100 performs arithmetic processing in accordance with a computer program stored in the storage means and outputs a control signal for controlling the wafer manufacturing apparatus 30 to the above-described components of the wafer manufacturing apparatus 30 via the input-output interface means.

[0051] The control unit 100 is connected to a display unit (not shown), which is implemented as a liquid crystal display or the like, for displaying the processing status, an image, or the like, and to an input unit (not shown) used when an operator registers information about the processing content or the like. The input unit is implemented by at least one touch panel provided on the display unit and an external input device such as a keyboard.

[0052] A processing operation of the wafer manufacturing apparatus 30 according to the embodiment will be described below with reference to the drawings. Fig. 10 is a sectional view schematically illustrating the wafer manufacturing apparatus according to the embodiment at a time when the second SiC ingot is processed. Fig. 11 is a sectional view schematically illustrating the wafer manufacturing apparatus according to the embodiment at the time of processing the first SiC ingot. Fig. 12 is a sectional view schematically showing the wafer produced by the Fig. 10 shown second SiC ingot was withdrawn.

[0053] The wafer manufacturing apparatus 30 according to the embodiment starts the processing operation when the second surface 3 of the SiC ingot 1-1 or 1-2 in which the peel layer 13 is formed is mounted on the suction surface 32 of the chuck table 31, the control unit 100 receives information about the processing content through the input device and stores the information about the processing content in the storage device, and the control unit 100 receives an instruction to start the processing from the operator. Incidentally, the information about the processing content includes information about whether the processing target is the first SiC ingot 1-1 or the second SiC ingot 1-2.

[0054] In the processing operation, the wafer manufacturing apparatus 30 opens or closes the opening and closing valves 59-1, 59-2, 59-3, 60-1, 60-2, 60-3, 61, and 62 in accordance with whether the processing target is the first SiC ingot 1-1 or the second SiC ingot 1-2, and thereby sucks and holds the SiC ingot 1-1 or 1-2 as the processing target on the suction surface 32. As shown in Fig. 10, in a case where the processing target is the second SiC ingot 1-2, the wafer manufacturing apparatus 30 opens the opening and closing valves 59-1, 59-2, 59-3, and 61, and closes the opening and closing valves 60-1, 60-2, 60-3, and 62.

[0055] As in Fig. 11, in a case where the processing target is the first SiC ingot 1-1, the wafer manufacturing apparatus 30 opens the opening and closing valves 59-1, 60-2, 60-3, 61, and 62, and closes the opening and closing valves 59-2, 59-3, and 60-1. Thus, when the wafer manufacturing apparatus 30 sucks and holds the first SiC ingot 1-1 on the suction surface 32 of the chuck table 31, the wafer manufacturing apparatus 30 applies negative pressure through the connecting passages 54, one of which terminates in the middle recessed portion 52 and the first annular recessed portion 53-1 connected to the first region 321, and positive pressure through the connecting passages 55, one of which terminates in the second annular recessed portion 53-2 and the third annular recessed portion 53-3 connected to the second region 322.

[0056] In addition, the embodiment as in Fig. 10 and Fig. As shown in Figure 11, when the SiC ingot 1-1 or 1-2 is sucked and held by suction on the suction surface 32 of the chuck table 31, the pressure value measured by the pressure gauge 57 is in a second predetermined range in which both a lower limit and an upper limit are lower than those of the above-described predetermined range. In the embodiment, the second predetermined range is, for example, between -90 kPa (gauge pressure) and -70 kPa (gauge pressure).

[0057] During the processing, the wafer manufacturing apparatus 30 lowers the water supply unit 33 and the ultrasonic oscillation unit 34, and brings the water supply unit 33 and the ultrasonic oscillation unit 34 close to the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31, supplies the water 331 from the water supply unit 33 to the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31, and immerses the end surface 341 of the ultrasonic oscillation unit 34 into the water 331 on the first surface 2 of the held SiC ingot 1-1 or 1-2. The pressure value measured by the pressure gauge 57 at this time is within the second predetermined range.Since the porous plate 40 of the chuck table 31 is formed of a porous ceramic whose porosity is equal to or more than 40% and equal to or less than 70% as a volume ratio and the diameter of the vent holes formed by pores is equal to or more than 10 μm and equal to or less than 25 μm, a difference between the measured values ​​of the pressure gauge 57 when the decompression pump 56 is operated in a state where nothing is mounted on the suction surface 32 and in a state where the SiC ingot 1-1 or 1-2 is placed on the suction surface 32 is equal to or larger than a difference between the predetermined range and the second predetermined range, that is, 5 kPa.

[0058] Furthermore, during the machining process, the water 331 supplied to the first surface 2 of the SiC ingot 1-1 or 1-2 by the water supply unit 33 flows over the first surface 2 and runs downward along the peripheral surface 4 of the SiC ingot 1-1 or 1-2. The water 331 flows over the suction surface 32 exposed on the circumference of the SiC ingot 1-1 or 1-2, runs along the peripheral surface of the chuck table 31, and is absorbed by the water absorption unit 36. The water 331 is then discharged via the drain port 361.Since the porous plate 40 is formed of a porous ceramic whose porosity is equal to or more than 40% and equal to or less than 70% as a volume ratio and the diameter of the vent holes formed by pores is equal to or more than 10 μm and equal to or less than 25 μm, the chuck table 31 can suck and hold the SiC ingot 1-1 or 1-2 even in a state where the area of ​​the second surface 3 of the SiC ingot 1-1 or 1-2 is smaller than the area of ​​the suction surface 32 and the water 331 flows over the suction surface 32 exposed on the periphery of the SiC ingot 1-1 or 1-2.

[0059] When the porosity of the porous ceramic constituting the porous plate 40 is less than 40% of the volume as a volume ratio and the diameter of the vent holes formed by the pores is less than 10 μm, the SiC ingot 1-1 or 1-2 having the second surface 3 smaller than the area of ​​the suction surface 32 cannot be sucked with a sufficient suction force and held on the suction surface 32 even if leakage of the negative pressure can be suppressed. In addition, when the porosity of the porous ceramic constituting the porous plate 40 exceeds 70% in volume ratio and the diameter of the vent holes formed by the pores exceeds 25 μm, excessive negative pressure leakage occurs, and the SiC ingot 1-1 or 1-2 having the second area 3 smaller than the area of ​​the suction surface 32 cannot be sucked with a sufficient suction force and held on the suction surface 32.

[0060] The wafer manufacturing apparatus 30 oscillates the ultrasonic vibrator of the ultrasonic oscillation unit 34 for a predetermined period of time, thereby applying an ultrasonic wave to the first surface 2 of the SiC ingot 1-1 or 1-2 through the ultrasonic oscillation unit 34. Then, the ultrasonic wave of the ultrasonic oscillation unit 34 is applied to the first surface 2, stimulates the peel layer 13, and ruptures the SiC ingot 1-1 or 1-2 over the entire surface of the wafer 11 to be manufactured, with the peel layer 13 serving as the starting point.

[0061] After applying the power to the ultrasonic vibrator of the ultrasonic oscillation unit 34 for a predetermined period of time, the wafer manufacturing apparatus 30 stops the supply of water 331 through the water supply unit 33, opens the opening and closing valves 59-1, 59-2, 59-3, and 61, closes the opening and closing valves 60-1, 60-2, 60-3, and 62, and lifts the water supply unit 33 and the ultrasonic oscillation unit 34. The wafer manufacturing apparatus 30 moves the peeling unit 35 to a position above the chuck table 31, lowers the peeling unit 35 above the chuck table 31, and brings the lower surface of the transport pad 351 of the peeling unit 35 into contact with the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31.

[0062] The wafer manufacturing apparatus 30 sucks the first surface 2 of the SiC ingot 1-1 or 1-2 held on the chuck table 31 by the lower surface of the transport pad 351 of the peeling unit 35, holds it, and lifts the peeling unit 35, as shown in Fig. 12. The wafer manufacturing apparatus 30 pulls the wafer 11 to be manufactured from the SiC ingot 1-1 or 1-2 on the first surface 2 side and removes the SiC ingot 1-1 or 1-2 from the suction surface 32 of the chuck table 31. After the SiC ingot 1-1 or 1-2 has been removed from the suction surface 32 of the chuck table 31, the wafer manufacturing apparatus 30 supplies the pressurized gas from the positive pressure source 58 to the porous plate 40, that is, it applies positive pressure to the porous plate 40 by closing the opening and closing valves 59-1, 59-2, 59-3, and 61 and opening the opening and closing valves 60-1, 60-2, 60-3, and 62. The wafer manufacturing apparatus 30 thus expels the gas from the pores opening in the suction surface 32.

[0063] Moreover, the control unit 100 of the wafer manufacturing apparatus 30 stores the predetermined area and the second predetermined area in advance, and after sucking and holding the SiC ingot 1-1 or 1-2 on the suction surface 32 of the chuck table 31, the control unit 100 determines whether or not the SiC ingot 1-1 or 1-2 specified by the processing content information is sucked and held on the suction surface 32 of the chuck table 31 based on a measurement result of the pressure gauge 57.Specifically, in a case where the machining target specified by the machining content information is the first SiC ingot 1-1, the control unit 100 determines that the first SiC ingot 1-1 is sucked and held on the suction surface 32 when the measurement result of the pressure gauge 57 is within the second predetermined range after the SiC ingot 1-1 or 1-2 is sucked and held on the suction surface 32 of the chuck table 31, and the control unit 100 determines that the first SiC ingot 1-1 is not sucked and held on the suction surface 32 when the measurement result of the pressure gauge 57 is outside the second predetermined range. Also, in a case where the processing target specified by the processing content information is the second SiC ingot 1-2, the control unit 100 similarly makes the determination after sucking and holding the SiC ingot 1-1 or 1-2 on the suction surface 32 of the chuck table 31.

[0064] As described above, in the wafer manufacturing apparatus 30 according to the embodiment, the porosity of the porous ceramic constituting the porous plate 40 is equal to or more than 40% and equal to or less than 70% in volume ratio, and the diameter of the vent holes formed by the pores is equal to or more than 10 μm and equal to or less than 25 μm. Therefore, the wafer manufacturing apparatus 30 according to the embodiment can suck and hold the SiC ingot 1-1 or 1-2, which has a second surface 3 smaller than the area of ​​the suction surface 32, on the suction surface 32 of the chuck table 31 even under conditions where the water 331 flows on the suction surface 32.

[0065] Therefore, the wafer manufacturing apparatus 30 according to the embodiment includes the chuck table 31 that can suck and hold the SiC ingot 1-1 or 1-2 regardless of the area of ​​the second surface 3 of the SiC ingot 1-1 or 1-2, even under conditions where the water 331 flows on the suction surface 32, and achieves the effect that the chuck table 31 does not need to be replaced according to the size of the SiC ingot 1-1 or 1-2. Consequently, the wafer manufacturing apparatus 30 according to the embodiment achieves the effect that the replacement of the chuck table 31 can be reduced even when the diameter 26-1 or 26-2 as the size of the SiC ingot 1-1 or 1-2 to be processed is changed.

[0066] Furthermore, in the wafer manufacturing apparatus 30 according to the embodiment, a difference between the pressure values ​​measured when the decompression pump 56 applies negative pressure to the suction surface 32 in a state where there is nothing on the chuck table 31 and a state where the SiC ingot 1-1 or 1-2 is mounted on the chuck table 31 is equal to or greater than 5 kPa, and the pressure values ​​are thus different from each other. Consequently, the control unit 100 of the wafer manufacturing apparatus 30 can check whether the SiC ingot 1-1 or 1-2 is mounted on the suction surface 32 based on the measurement result of the pressure gauge 57.

[0067] Furthermore, according to the embodiment, the wafer manufacturing apparatus 30 can generate positive pressure from the suction surface 32 exposed on the periphery of the first SiC ingot 1-1, thus preventing waste generated during peeling from being sucked onto the exposed suction surface 32. As a result, the wafer manufacturing apparatus 30 can prevent dirt from accumulating on the suction surface 32. [Variations]

[0068] A wafer manufacturing apparatus according to a modification of the present embodiment will be described with reference to the drawings. Fig. Fig. 13 is a sectional view schematically illustrating a chuck table of the wafer manufacturing apparatus in accordance with the modification of the present embodiment. Incidentally, in Fig. 13, the same parts as in the embodiment are designated by the same reference numerals, and their description is omitted.

[0069] As in Fig. 13, the chuck table 31-1 of the wafer manufacturing apparatus 30 is arranged in accordance with the Fig. 13, except that the porous plate 40 and the base 50 are secured together by bolts 70. While in Fig. 13, the recessed portions 52, 53-1, 53-2, and 53-3 of the base 50, the communication passages 54, 54-2, 55, and 55-2, and the opening and closing valves are omitted, the chuck table 31 in the present invention has the recessed portions 52, 53-1, 53-2, and 53-3, and the communication passages 54 as in the embodiment.

[0070] The wafer manufacturing apparatus 30 according to the modification includes the chuck table 31-1 that can suck and hold the SiC ingot 1-1 or 1-2 regardless of the area of ​​the second surface 3 of the SiC ingot 1-1 or 1-2, even under conditions where the water 331 flows on the suction surface 32. As a result, as in the embodiment, the wafer manufacturing apparatus 30 produces the effect that the change of the chuck table 31-1 can be reduced even when the diameter 26-1 or 26-2 as the size of the SiC ingot 1-1 or 1-2 to be processed is changed.

[0071] Furthermore, the wafer manufacturing apparatus 30 according to the present invention can open the opening and closing valves 59-1, 59-2, 59-3, and 61 and close the opening and closing valves 60-1, 60-2, 60-3, and 62 after the processing target is mounted on the suction surface 32, and the control unit 100 can control the opening and closing of the opening and closing valves 59-1, 59-2, 59-3, 60-1, 60-2, 60-3, 61, and 62 based on the measurement result of the pressure gauge 57.Specifically, the wafer manufacturing apparatus 30 according to the present invention opens the opening and closing valves 59-1, 59-2, 59-3, and 61 and closes the opening and closing valves 60-1, 60-2, 60-3, and 62 after the processing target is attached to the suction surface 32, and when the measurement result of the pressure gauge 57 is within the second predetermined range, the control unit 100 continues the processing operation while maintaining a state in which the opening and closing valves 59-1, 59-2, 59-3, and 61 are opened and the opening and closing valves 60-1, 60-2, 60-3, and 62 are closed.

[0072] After the processing target is mounted on the suction surface 32, the wafer manufacturing apparatus 30 according to the present invention opens the opening and closing valves 59-1, 59-2, 59-3, and 61 and closes the opening and closing valves 60-1, 60-2, 60-3, and 62, and when the measurement result of the pressure gauge 57 is outside the second predetermined range, the control unit 100 closes the third opening and closing valve 59-3 and opens the third relief pressure opening and closing valve 60-3 and the relief pressure opening and closing accumulating valve 62, and the control unit 100 determines whether or not the measurement result of the pressure gauge 57 is again within the second predetermined range.

[0073] Thus, after the processing target is attached to the suction surface 32, the wafer manufacturing apparatus 30 according to the present invention opens the opening and closing valves 59-1, 59-2, 59-3, and 61 and closes the opening and closing valves 60-1, 60-2, 60-3, and 62, and until the measurement result of the pressure gauge 57 falls within the second predetermined range, the control unit 100 closes the opening and closing valves 59-1, 59-2, and 59-3 provided at the communication passages 54, one ends of which open in the annular recessed portions 53-1, 53-2, and 53-3, in an order starting from an outer peripheral side, and opens the relief pressure opening and closing collecting valve 62 and opens the relief pressure opening and closing valves 60-1, 60-2 and 60-3 provided on the overpressure communication passages 55, one ends of which open in the annular recesses 53-1, 53-2 and 53-3,in a sequence starting from an outer peripheral side.,

[0074] In this case, in addition to the effects of the embodiment, the wafer manufacturing apparatus 30 opens the opening and closing valves 59-1, 59-2, 59-3, and 61 and closes the opening and closing valves 60-1, 60-2, 60-3, and 62 after the processing target is mounted on the suction surface 32. The control unit 100 controls the opening and closing of the opening and closing valves 59-1, 59-2, 59-3, 60-1, 60-2, 60-3, 61, and 62 so that the measurement result of the pressure gauge 57 falls within the second predetermined range. Consequently, the wafer manufacturing apparatus 30 can properly suck and hold the SiC ingot 1-1 or 1-2 of any size on the suction surface 32 of the porous plate 40 of the chuck table 31. As a result, the wafer manufacturing apparatus 30 produces the effect that changes of the chuck table 31 can be further reduced even if the diameter 26-1 or 26-2 is changed as the size of the SiC ingot 1-1 or 1-2 to be processed.

Claims

[1] Wafer manufacturing apparatus (30) for producing a wafer (11) from a semiconductor ingot (1, 1-1, 1-2) in which a stripping layer (13) is formed by positioning a focal point (22) of a laser beam (21) having a wavelength transmittable through the semiconductor ingot (1, 1-1, 1-2) at a depth (23) corresponding to a thickness (14) of the wafer (11) to be produced, and applying the laser beam (21), the wafer manufacturing apparatus comprising: a chuck table (31) configured to hold the semiconductor ingot (1, 1-1, 1-2) on a suction surface (32) with the wafer (11) to be produced on an upper side; an ultrasonic oscillating unit (34) having an end surface (341) facing the wafer (11) to be produced and configured to oscillate an ultrasonic wave; a water supply unit (33) configured to supply water (331) between the wafer (11) to be produced and the end face (341) of the ultrasonic oscillation unit (34); a pulling unit (35) configured to suck and hold the wafer (11) to be produced and to pull the wafer (11) to be produced from the semiconductor ingot (1, 1-1, 1-2); and a water receiving unit (36) arranged to surround the chuck table (31) and to receive the water (331) which is discharged after being supplied from the water supply unit (33) to the semiconductor ingot (1, 1-1, 1-2) and flows on the suction surface (32) of the chuck table (31) on a circumference of the semiconductor ingot (1, 1-1, 1-2), wherein the clamping table (31) comprises a porous plate (40) forming the suction surface (32), and a base (50) supporting the porous plate (40) and having a connecting passage (54) arranged to apply a negative pressure to the porous plate (40), and wherein the chuck table (31) sucks and holds the semiconductor ingot (1, 1-1, 1-2) even in a state in which an area of ​​a lower surface (3) of the semiconductor ingot (1, 1-1, 1-2) is smaller than an area of ​​the suction surface (32) and the water (331) flows on the suction surface (32) exposed on the periphery of the semiconductor ingot (1, 1-1, 1-2). [2] Wafer manufacturing apparatus (30) according to claim 1, wherein the suction surface (32) of the porous plate (40) has a first region (321) corresponding to a first semiconductor ingot (1-1) having a first diameter, and a second region (322) surrounding the first region (321), connecting passages (54) which are designed to selectively allow a negative pressure or an overpressure to act, are connected to regions which correspond to the first region (321) or the second region (322) in a surface (41) of the porous plate (40), the surface (41) being on a side opposite the suction surface (32), and when the first semiconductor ingot (1-1) is sucked and held, the negative pressure is caused to act through the connection passage connected to the first region (321) and the positive pressure is caused to act through the connection passage connected to the second region (322). [3] The wafer manufacturing apparatus (30) according to claim 1 or 2, wherein a decompression pump (56) as a suction source is coupled to the connection passage (54) of the chuck table (31), a pressure gauge (57) is installed at the connection passage (54-2), and a difference between measured values ​​of the pressure gauge (57) is equal to or greater than 5 kPa when the decompression pump (56) is operated in a state where nothing is attached to the suction surface (32) of the porous plate (40) and in a state where the semiconductor ingot (1, 1-1, 1-2) is placed on the suction surface (32) of the porous plate (40).

Citation Information

Patent Citations

  • Method for producing a wafer

    DE102019204741A1

  • JP002019102513A