Hot-dip galvanizing process and hot-dip galvanized component

By introducing a recess in components to collect excess zinc alloy, the method addresses the issue of zinc deposits in openings, reducing post-processing time and effort, and enhancing productivity and quality in hot-dip galvanizing processes.

DE102023113671B3Active Publication Date: 2024-10-17FONTAINE HLDG NV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
DE102023113671
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-05-03
Filing Date
2023-05-24
Publication Date
2024-10-17
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

Conventional hot-dip galvanizing processes result in zinc deposits and noses forming in openings of components, necessitating complex and time-consuming manual post-processing, especially for large-scale production with high tolerance requirements.

Method used

A method involving a recess made in components adjacent to openings to collect and drain excess zinc alloy, ensuring openings remain free of unwanted zinc deposits during hot-dip galvanizing, thereby reducing post-processing efforts.

Benefits of technology

The method significantly reduces post-processing time and effort by up to 20%, enhances productivity, and ensures higher quality components by minimizing zinc noses and clogging, particularly in large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a method for hot-dip galvanizing at least one component (1) having at least one opening (2) and / or edge (3), wherein the component (1) is immersed in a galvanizing bath (6) filled with a zinc alloy melt (5) to apply a zinc coating (4) to the component (1) and is immersed again after galvanizing. According to the invention, prior to galvanizing, at least one recess (7) adjacent to and opening into the opening (2) and / or edge (3) of the component (1) is formed in the component (1), which is designed to receive any zinc alloy that runs off.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to the technical field of galvanizing components, in particular iron-based or iron-containing components and / or steel-based or steel-containing components (steel components), by means of Hot-dip galvanizing (hot-dip galvanizing).

[0002] In particular, the present invention relates to a method for hot-dip galvanizing at least one at least one The present invention further relates to a hot-dip galvanized component which is produced according to the is or has been produced using the aforementioned processes.

[0003] In particular, hot-dip galvanizing is carried out in discontinuous operation (so-called batch galvanizing). As components Components containing iron and / or steel are preferably provided.

[0004] Metallic components of any kind made of ferrous material, especially components made of steel, require Often, due to their application, they provide effective protection against corrosion. Especially steel components for motor vehicles (Motor vehicles), such as cars, trucks, commercial vehicles, etc., require efficient corrosion protection, which also withstands long-term stress.

[0005] In this context, it is known to protect steel-based components against corrosion by galvanizing (galvanizing). During galvanizing, the steel is coated with a generally thin layer of zinc to protect it from To protect against corrosion, various galvanizing processes can be used to protect steel components galvanize, ie to cover with a metallic coating of zinc, whereby in particular hot-dip galvanizing (synonymously also called hot-dip galvanizing), spray galvanizing (flame spraying with zinc wire), Diffusion galvanizing (Sherard galvanizing), galvanic galvanizing (electrolytic galvanizing), non- electrolytic galvanizing using zinc flake coatings and mechanical galvanizing. There are major differences between the aforementioned galvanizing processes, particularly with regard to Process implementation, but also with regard to the nature and properties of the zinc layers produced. Zinc coatings.

[0006] The most important method for corrosion protection of steel by metallic zinc coatings is Hot-dip galvanizing (hot-dip galvanizing). In this process, steel is coated continuously (e.g. strip and wire) or piece by piece (e.g. Components) at temperatures of approximately 450 °C to 600 °C in a heated vessel with liquid zinc or a liquid zinc alloy (melting point of zinc: 419.5 °C), so that a resistant Forms an alloy layer of zinc.

[0007] In hot-dip galvanizing, a distinction is made between discontinuous batch galvanizing (cf. e.g. EN ISO 1461 and DIN 50997) and continuous strip galvanizing (DIN EN 10143 and DIN EN 10346). Both batch galvanizing and Strip galvanizing is a standardized process. Strip galvanized steel is a pre- or intermediate product. (semi-finished product) which is further processed after galvanizing, in particular by forming, punching, cutting, etc. whereas components to be protected by batch galvanizing are usually first completely or at least partially and only then hot-dip galvanized (which protects the components all around against corrosion). Piece galvanizing and strip galvanizing differ depending on the application conditions in terms of the phase structure as well as the thickness of the resulting zinc coatings, which can result in different protection periods. The zinc layer thickness of strip galvanized sheets is usually in the range of 10 to 35 micrometers, whereas the zinc layer thickness of batch galvanized steel parts is usually in the range of 50 to 200 micrometers and even more lay.

[0008] Hot-dip galvanizing provides both active and passive corrosion protection. Passive protection is achieved through the barrier effect of the zinc coating. The active corrosion protection is created by the cathodic effect of the Compared to more noble metals in the electrochemical series, such as iron, zinc serves as Sacrificial anode that protects the underlying iron from corrosion until it itself is completely corroded.

[0009] In the so-called piece galvanizing according to EN ISO 1461, the hot-dip galvanizing of mostly larger Steel components and structures. Steel-based blanks or (semi-)finished workpieces (components) are dipped into the molten zinc bath after a pre-treatment. The dipping process can also be used to treat interior surfaces, Weld seams and hard-to-reach areas of the workpieces or components to be galvanized can be easily reached.

[0010] Conventional hot-dip galvanizing is based in particular on dipping iron or steel components into a Zinc melts to form a zinc coating on the surface of the components. To ensure adhesion, The integrity and uniformity of the zinc coating generally requires careful Surface pretreatment and if necessary -preparation of the components to be galvanized is required, which usually involves degreasing followed by Rinsing process, a subsequent acid pickling with subsequent rinsing process and finally a Flux treatment (i.e. so-called fluxing) followed by a drying process.

[0011] The typical process sequence for conventional hot-dip galvanizing is usually as follows. For reasons of process economy and cost-effectiveness, batch galvanizing identical or similar components (e.g. series production of automotive components) these are typically used for the entire Process merged or grouped (especially by means of a common, for example as a traverse or Frame-shaped goods carrier or a common holding or fastening device for a large number of these identical or similar components). For this purpose, a plurality of components are fixed to the product carrier using holding devices, such as e.g., slings, tie wires, etc. are attached. The components are then grouped The components are then transported to the subsequent treatment steps or stages via the product carrier. Piece galvanizing using hot-dip galvanizing can also be treated individually.

[0012] First, the component surfaces of the components are degreased to remove residues of grease and To remove oils, the degreasing agents usually used are aqueous alkaline or acidic degreasing agents. After cleaning in the degreasing bath, a rinsing process usually follows, typically by immersion in a water bath to prevent degreasing agents from being carried over into the galvanized material subsequent process step of pickling, which is particularly important when changing from alkaline Defatting to an acid base is of great importance.

[0013] This is usually followed by a pickling treatment (pickling), which is used in particular to remove species-specific impurities such as rust and scale from the steel surface. Pickling is usually carried out in diluted Hydrochloric acid, whereby the duration of the pickling process depends, among other things, on the state of contamination (e.g. degree of rust) of the The galvanized material and the acid concentration and temperature of the pickling bath depend on this. To avoid or Minimization of carryover of acid and / or salt residues with the galvanizing material takes place after Pickling treatment usually involves a rinsing process (rinsing step).

[0014] Subsequently, the so-called fluxing (flux treatment) usually takes place, whereby the previously degreased and pickled steel surface with a so-called flux, which is typically an aqueous solution of inorganic chlorides, most commonly a mixture of zinc chloride (ZnCl ) and ammonium chloride (NH Cl), 2 4 On the one hand, the flux is designed to prevent the steel surface from reacting with the molten zinc to carry out a final intensive fine cleaning of the steel surface and to dissolve the oxide film of the zinc surface and to prevent re-oxidation of the steel surface until the galvanizing process. On the other hand, the Flux improves the wettability between the steel surface and the molten zinc. After Flux treatment is usually followed by drying to form a solid flux film on the steel surface. and to remove adhering water, so that subsequent undesirable reactions (in particular the formation of water vapor) in the liquid zinc dip bath should be avoided.

[0015] The components pretreated in the above-mentioned manner are then immersed in the liquid zinc melt Hot-dip galvanized. During hot-dip galvanizing, the zinc content of the melt is at least 98.0 wt. according to DIN EN ISO 1461. -%. After immersing the galvanized material in the molten zinc (or zinc alloy), it remains for a sufficient time in the molten zinc bath, especially until the galvanized material has reached its temperature and coated with a layer of zinc. Typically, the surface of the zinc melt is covered with oxides, Zinc ash, flux residues and the like, before the galvanized material is removed from the zinc melt The component hot-dip galvanized in this way is then subjected to a cooling process (e.g. in air or in a water bath). Finally, the holding devices for the component, such as lifting gear, Tie wires or similar are removed. Following the galvanizing process, a partial complex post-processing or post-treatment. This removes excess zinc residues, especially so-called drips of zinc solidifying at the edges, as well as oxide or ash residues that remain on the component adhere, as far away as possible.

[0016] One criterion for the quality of a hot-dip galvanizing is the thickness of the zinc coating in µm (micrometers). In the standard DIN EN ISO 1461 specifies the minimum values ​​of the required coating thicknesses, as they are required depending on the material thickness when In practice, the layer thicknesses are significantly higher than those specified in DIN EN ISO 1461. Minimum layer thicknesses. In general, by batch galvanizing Zinc coatings had a thickness in the range of 50 to 200 micrometers and even more.

[0017] During the galvanizing process, a mutual diffusion of the liquid zinc with the Steel surface on the steel part a coating of variously composed iron / zinc alloy layers. When the hot-dip galvanized objects are removed, a layer of galvanized metal remains on the top layer of the alloy - also known as A layer of zinc, known as a pure zinc layer, is adhered, the composition of which corresponds to that of molten zinc. Due to the high temperatures during hot dipping, a relatively high brittle layer based on an alloy (mixed crystals) between iron and zinc and only above that the pure Zinc layer. The relatively brittle iron / zinc alloy layer improves the adhesion to the base material, However, this makes the formability of galvanized steel more difficult. Higher silicon contents in steel, which are particularly important for so-called calming of the steel during its production, lead to increased reactivity between the zinc melt and the base material and consequently to a strong growth of the iron / zinc Alloy layer. In this way, relatively large total layer thicknesses are formed. enables a very long corrosion protection period, but it also increases with increasing zinc layer thickness the Danger that the layer will chip off under mechanical stress, especially local, sudden impacts, and the The corrosion protection effect is thereby impaired.

[0018] In order to address the previously described problem of the occurrence of rapidly growing, brittle and thick iron / zinc alloy layer and also to achieve lower layer thicknesses with simultaneously high corrosion protection in the To enable galvanizing, it is known from the state of the art to add the zinc melt or the liquid zinc bath For example, adding 5 wt.% aluminum to a liquid Zinc melt produces a zinc / aluminum alloy with a lower melting temperature than pure zinc. By using a zinc / aluminium melt (Zn / Al melt) or a liquid zinc / aluminium bath (Zn / Al- Bath), on the one hand, significantly lower layer thicknesses can be achieved for reliable corrosion protection (in generally below 50 micrometers); on the other hand, the formation of brittle iron / tin Alloy layer, since the aluminum - without committing to a specific theory - initially forms a barrier layer on the steel surface of the component in question, onto which the actual zinc layer Components hot-dip galvanized with a zinc / aluminium melt can therefore be easily formed, However, despite the significantly lower layer thickness compared to conventional hot-dip galvanizing, with a virtually aluminum-free zinc melt - has improved corrosion protection properties. The zinc / aluminium alloy used in the hot-dip galvanizing bath has improved fluidity properties compared to pure zinc In addition, zinc coatings produced using such zinc / aluminium alloys hot-dip galvanizing, greater corrosion resistance (which is two to six times better than those made from pure zinc), improved formability and better paintability than those made from pure zinc Zinc coatings. Furthermore, this technology can also be used to produce lead-free zinc coatings.

[0019] Such a hot-dip galvanizing process using a zinc / aluminium melt or using a zinc / aluminium hot-dip galvanizing bath is known, for example, from WO 02 / 042 512 A1 and the relevant Document equivalents to this patent family (e.g. EP 1 352 100 B1, DE 601 24 767 T2 and US 2003 / 0 219 543 A1). Suitable fluxes for hot-dip galvanizing using zinc / aluminium baths are also disclosed there, since Flux compositions for zinc / aluminium hot-dip galvanizing baths are different from those for conventional hot-dip galvanizing with pure zinc. The process disclosed therein allows corrosion protection coatings with very low layer thicknesses (generally well below 50 micrometers and typically in the range of 2 up to 20 micrometers) and with very low weight and high cost efficiency, which is why the process described there ® Process is used commercially under the name microZINQ process.

[0020] The disadvantage of the known batch galvanizing is that when the components are removed from the molten zinc inevitably leads to the zinc flowing off and dripping off at the edges and corners of the component, but also in the area of ​​openings within the component. This results in so-called zinc noses on the component at edges and in openings. In the worst case, smaller openings in the component become clogged with solidified zinc melt. ´´excess´´, later solidified zinc melt in the subsequent step, which is usually done manually, represents a represents a significant cost and effort factor, especially when it comes to galvanizing large quantities and / or compliance with high tolerance requirements is important. For example, in the case of a fully loaded product carrier, a plurality of to galvanizing components into the zinc melt, it is usually not possible to reach all components on the product carrier and to remove the zinc noses of the individual components directly at the galvanizing point.

[0021] Ultimately, zinc noses and / or partially or completely clogged Openings on the galvanized components that must be removed by manual reworking. Please note that rework does not only mean cleaning or repair, but also, in particular, visual inspection is included. Due to the process, all components have a tendency to have zinc noses and / or The openings have become clogged, which must be removed accordingly. Therefore, all components must be individually This inspection alone, without any necessary subsequent work steps, represents a very high effort, especially when it involves a large number of components in a Large-scale production with very high quality requirements.

[0022] US 2017 / 0 072 886 A1 relates to a rear impact protection device which is configured to be attached to the rear of a trailer, wherein the rear impact protection first, second, third and fourth support bases, which connected to the rear of the trailer, as well as first, second, third and fourth bumper support elements, which are connected, wherein the first, second, third and fourth support base and a bumper which is attached to the lower ends of the first, second, third and fourth bumper support elements.

[0023] DK 173011 B1 relates to a method for stamping the gutter holder in the rivet in order to achieve an optimal To achieve galvanization between the surfaces, a star-shaped punched hole is made in the gutter holder to which the front spring is riveted.

[0024] Finally, DE 10 2015 108 193 A1 relates to a receiving element, in particular for a door handle device, which a door handle for operating a door lock and a door handle carrier, in a vehicle with at least a first and second holding means for fastening the receiving element to the door handle carrier, and at least one Fastening means for fastening a mechanical connecting element for actuating the door lock, wherein at least the first holding means serves for the positive fastening of the receiving element to the door handle carrier.

[0025] The object of the present invention is to avoid the aforementioned disadvantages or at least to Essentially to reduce.

[0026] To achieve the above-mentioned object, the present invention proposes - according to a first aspect of present invention - a method for hot-dip galvanizing according to claim 1. Further and / or advantageous Embodiments of the hot-dip galvanizing process according to the invention are the subject of the relevant Subclaims.

[0027] Furthermore, the present invention relates - according to a second aspect of the present invention - to a Hot-dip galvanized component produced by the process according to claim 1, according to the independent Product claim.

[0028] It is understood that in the following statements, configurations, embodiments, advantages and the like, which in the following, for the purpose of avoiding repetition, only relate to one aspect of the invention are of course also valid with regard to the other aspects of the invention, without this requires a separate mention.

[0029] Furthermore, the person skilled in the art - depending on the application or the individual case - can benefit from the following Range specifications may deviate if necessary without departing from the scope of the present invention.

[0030] In addition, all values ​​or parameter specifications or the like mentioned below are generally standardized or explicitly specified determination methods or otherwise with the expert can be determined using methods of determination or measurement that are common in this field.

[0031] Having said that, the present invention will now be explained in detail below.

[0032] The invention relates to a method for hot-dip galvanizing at least one piece of material having at least one opening Component, wherein the component is placed in a zinc alloy for applying a galvanizing layer to the component containing molten zinc and is immersed in a galvanizing bath and then removed again after galvanizing, wherein, prior to galvanizing, at least one adjacent to the opening of the component and opening into the opening A recess has been made in the component to accommodate the zinc alloy that runs off, wherein the recess has been formed in such a way is that when the component is removed from the galvanizing bath, zinc alloy running off the component surface from the area of ​​the opening in the recess, so that after solidification of this expired Zinc alloy quantity does not protrude into the opening and / or so that the opening is free from applied hot-dip galvanized layer of excess zinc alloy and / or such that the opening is at least substantially free of zinc alloy clogging the opening; where the ratio of the radius of the opening to the volume of the recess, with a maximum component thickness of up to 3 including 3 mm, with an opening diameter of less than or equal to 10 mm less than 30 cm / cm and / or 3 where the diameter of the opening is greater than 10 mm, the ratio is less than 90 cm / cm or where the ratio of the radius the opening to the volume of the recess, with a maximum component thickness greater than 3 mm, with a diameter of the 3 Opening less than or equal to 10 mm less than 50 cm / cm and / or with an opening diameter greater than 10 mm 3 is less than 100 cm / cm.

[0033] In particular, the present invention relates to batch galvanizing, preferably in discontinuous operation.

[0034] The component can be introduced into the galvanizing bath by means of a conveyor device or a product carrier or the like It can also be provided that the component is immersed together with other components in the The galvanizing bath is immersed in a basket, which is then conveyed into the galvanizing bath can be implemented according to the invention.

[0035] Surprisingly, it is possible within the scope of the present invention to provide a component which, according to the Hot-dip galvanizing at least essentially with non-zinc-adherent or zinc-deposited According to the invention, this is achieved by additionally introducing a recess into the component before hot-dip galvanizing. This means that a separate, additional step for processing the component before Hot-dip galvanizing, which is also carried out at the same time when the openings are made in the component can be.

[0036] In connection with the experiments carried out during the development of the invention, it has been found that that despite the additional process step of creating the recess in the component, a more efficient The process flow can be guaranteed, especially since a complex, manual post-processing of the hot-dip galvanized component can be avoided or at least reduced.

[0037] Thus, the recess can ensure that a ´´predefined´´ area on the component for flowing Zinc deposits are present, which can become clogged - in a desired and defined manner. By clogging the recess with zinc running off or zinc deposits after hot-dip galvanizing, the opening as such can at least in Essentially free from unwanted zinc adhesions or zinc deposits. This ensures a predefined Recess used to absorb zinc deposits after hot-dip galvanizing.

[0038] If, in connection with the present invention, zinc deposits, zinc noses or the like When we speak of zinc melt, we mean the zinc melt that runs off and contains a zinc alloy and which, after Accordingly, zinc adhesions and / or zinc deposits can occur in addition to zinc / Zinc alloy may also contain other components if required.

[0039] Furthermore, it is understood that the recess is not considered as part of the opening, but represents a separate area, but is open towards the opening.

[0040] As a result, the invention differs from the prior art in that it is specifically - depending also on the Size of the opening of the component - a supplementary recess in the component before immersion in the zinc bath and preferably in connection with the manufacture of the component. Particularly preferred is the Recess is dimensioned or designed depending on the dimensions of the respective opening assigned to it. In this In this context, it is understood that not every opening in the component necessarily has to be provided with a recess However, according to the invention, at least one opening of the component is provided with the recess associated with this opening equipped.

[0041] Preferably, such openings are assigned to recesses or adjacent to the opening in the component where zinc deposits clogging the opening are to be avoided and / or Such adhesions require a significantly increased processing effort with corresponding manual post-processing This applies in particular to openings where, during later use, a special dimensional accuracy is required.

[0042] A particular advantage of the invention is that by introducing the recess into the component, an exact and / or targeted manipulation of the component can be carried out to ensure its dimensional accuracy without reworking.

[0043] If necessary, it can also be provided that the opening is already provided with the production of the component as such a corresponding recess. The recess is nevertheless to be understood as an independent area, since the recess is specifically used to at least partially, preferably completely, with the zinc melt running off to be filled so that the opening is at least essentially free of unwanted zinc deposits or Zinc deposits can remain. This can significantly reduce the amount of post-processing required, sometimes even eliminating it entirely. be avoided.

[0044] Consequently, the invention offers the possibility that undesirable zinc adhesions and / or zinc deposits can be significantly reduced because the galvanizing process can be optimized through the recesses.

[0045] In connection with the present invention, it has been found that, taking into account the Invention partly no longer necessary post-processing the total production time in the manufacture of galvanized components can even be reduced compared to the state of the art, so the invention ultimately represents a higher productivity, especially because the manual post-processing required at the stand This is especially true if the recess is already made after the The component must be inserted into the component before hot-dip galvanizing. This can be done by punching, Milling, laser cutting or similar. Ultimately, the cost of additionally installing the The cost of the recess is disproportionate to the very complex post-processing required with the current state of the art.

[0046] As a result, the invention produces components of higher quality. Also from an economic perspective The invention offers economic advantages over the prior art, since the production time is Taking into account the no longer necessary or sometimes very low post-processing, up to 20% can be reduced can.

[0047] In terms of the process, it is generally the case that the galvanizing layer is at least largely within 0.02 to 10 minutes, preferably between 0.5 and 3 minutes, after emerging from the zinc melt. The hot-dip galvanizing layer on the component has solidified, which is ensured by the recess designed for the opening, that excess zinc deposits are absorbed and solidified in the recess and the opening is free of unwanted zinc deposits or zinc noses or the like, which in particular exceed the specified Galvanizing layer protrudes.

[0048] For the purposes of the present invention, ´´zinc noses / unwanted zinc deposits´´ also includes in particular to understand that refers to excess or unwanted zinc / zinc alloy, which after solidification protrudes and / or exceeds the specified (regular) layer thickness of the hot-dip galvanized layer.

[0049] Particularly preferably, the component is galvanized over its entire surface and has a The (desired) galvanizing layer forms as a zinc deposit. However, zinc snags are unwanted, additional deposits.

[0050] According to the invention, it is provided that the recess is designed in such a way that when Pulling the component out of the galvanizing bath zinc alloy running off the component surface - that is especially before the zinc alloy solidifies - from the area of ​​the opening in the recess or in This runs in. The zinc alloy running off the component surface collects in the holder in such a way that after solidification of this expired amount of zinc alloy, it no longer protrudes into the opening and / or such that the opening is free of any protruding material and / or excess zinc alloy and / or such that the opening is at least substantially free of the opening According to the invention, it is thus possible to store the draining zinc alloy in the recess completely, keeping the opening free of unwanted zinc alloy. This reduces the The previously mentioned post-processing effort of the galvanized component is drastically reduced. In particular, that an opening after hot-dip galvanizing no longer has the original or nominal, for the later function necessary dimensions, but has become completely or partially clogged with the zinc alloy.

[0051] Furthermore, in a further particularly preferred embodiment of the inventive concept, be that the component is removed from the galvanizing bath in such a way that the recess in the lower, the area facing away from the pull-out direction and / or in the lower half of the opening facing away from the pull-out direction is arranged, especially in the lower Apex and / or at the lowest point and / or lowest area of ​​the opening when positioned on the product carrier during the galvanizing process. Such an arrangement is particularly advantageous because the zinc alloy that flows out during When removed from the galvanizing bath, the metal is subject to gravity and thus runs downwards or is pulled. The arrangement of the recess, particularly preferably in the lower area of ​​the opening, can then Zinc alloy so that it does not protrude into the opening. This lower area of ​​the component is defined procedurally by the way in which and at which point the component is held or fastened, when the component is immersed in the galvanizing bath and then removed again. Finally, the lower After holding or securing the component, the area should point downwards for immersion into the melt. Accordingly, the recess is also immediately after the component has been removed from the melt into the Opening opened upwards.

[0052] Preferably, the recess is at least substantially circular segment-shaped in plan view of the opening, arched, triangular and / or rectangular. Basically, a wide variety of shapes are possible for the recess is possible. However, in the development of the invention it has been shown that the aforementioned shapes on the one hand, they can be incorporated into the component relatively easily without high processing costs and on the other hand, efficient collection of the draining zinc alloy can be ensured.

[0053] The recess can be made before hot-dip galvanizing by drilling and / or milling and / or by a thermal and / or non-thermal cutting process, such as laser, oxyfuel, plasma and / or water jet cutting Thus, according to the invention, the recess can be designed depending on the component-specific parameters and / or in Depending on the material of the component, they can be introduced into the component using different methods. Different processes are suitable for different recesses and / or openings. the opening may be circular and / or elliptical in cross-section and / or formed as an elongated hole.

[0054] Particularly preferably, in further embodiments it can be provided that the opening has a material removal in the component, wherein the opening may be designed as a breakthrough and / or as a drainage opening can, but does not have to be designed. For openings of different shapes and types, in practice the The problem is that these become clogged when they are removed from the zinc alloy. According to the invention, this can now be avoided by targeted introduction of the recess(es) can be avoided.

[0055] In addition, the opening may have a clear diameter of at least 5 mm before the recess is made, preferably at least 8 mm, more preferably at least 10 mm. The inventive principle of The use of the recess can ultimately also be used for larger openings of up to 50 cm, preferably 25 cm, preferably 10 cm, are used.

[0056] In principle, different galvanizing processes are suitable for the present invention. Galvanizing can be a classic, quasi-pure zinc melt or a zinc alloy with a higher concentration, e.g. with aluminum The different galvanizing processes are regulated by corresponding standards, which are referred to below. is referred to.

[0057] A particularly preferred choice is between a standard galvanization according to EN ISO 1461 (as of March 2023) and a Thin-layer galvanizing according to DIN 50997 (as of March 2023).

[0058] In the development of the invention, it has been shown that certain relationships between the radius of the Opening, which is in particular circular or has another shape, to the volume of the recess in particular Dimensions are advantageous. The radius of the opening in the case of a non-circular opening is particularly the maximum The maximum radius is half the maximum clear diameter of the Opening.

[0059] According to the present invention, it is provided that, in particular for galvanizing according to EN ISO 1461 (status March 2023), the ratio of the radius of the opening to the volume of the recess, with a maximum component thickness of up to 3 including 3 mm, with an opening diameter of less than or equal to 10 mm less than 30 cm / cm, preferably 3 3 3 less than 20 cm / cm, in particular between 1 and 20 cm / cm, and / or greater than 1 cm / cm, preferably greater than 5 cm 3 3 3 / cm , and / or with an opening diameter of greater than 10 mm less than 90 cm / cm , preferably less than 50 cm / cm , 3 in particular between 1 and 40 cm / cm .

[0060] In the development of the invention, it was found that preferably for different opening widths different ratios are provided. The radius ratio can also depend on the component thickness. It should be provided that for components with a higher component thickness, the ratio of r / V (i.e. the ratio of Radius of the opening to the volume of the recess) The recess can also be adjusted to suit different maximum opening widths. The above-mentioned ratios ultimately indicate that, depending on the different sizes of the Recess of the opening the recess according to the expiring (expected) amount of zinc deposit Thus, during the development of the invention, it was found that, depending on Different dimensions of the openings also require different recesses. understandable that a larger opening also requires a larger recess compared to a smaller opening with a smaller recess and the like. The above r / V ratios indicate the This creates a possibility for the specialist to create the recess depending on the to fit the respective opening into the component.

[0061] In addition, for a component thickness of more than 3 mm, in particular for galvanizing according to EN ISO 1461 (as of March 2023), the ratio of the radius of the opening to the volume of the recess with a diameter of 3 3 Opening less than or equal to 10 mm less than 50 cm / cm , preferably less than 40 cm / cm , in particular between 1 and 30 cm / cm 3 3 3 , and / or with an opening diameter of more than 10 mm less than 100 cm / cm , preferably less than 80 cm / cm , 3 in particular between 1 and 70 cm / cm. The aforementioned component thickness greater than 3 mm is the maximum component thickness. Thus, the r / V ratio is adjusted depending on the component thickness (up to and including 3 mm and from 3 mm). is determined depending on different components and depending on the functions provided in the respective components Openings ensure appropriate dimensioning of the respective recess.

[0062] In the case of thin-layer galvanizing according to DIN 50997 (as of March 2023), the ratio of the Radius of the opening to the volume of the recess (r / V ratio) for a diameter of the opening less than or equal to 3 10 mm for a, preferably maximum, component thickness less than or equal to 3 mm less than 20 cm / cm, preferably less than 15 cm / cm 3 3 , in particular between 1 and 20 cm / cm , and / or with a diameter of the opening greater than 10 mm less than 100 cm 3 3 3 / cm , preferably less than 70 cm / cm , in particular between 1 and 60 cm / cm .

[0063] For thin-layer galvanizing, an adjustment of the r / V ratio can be particularly advantageous. This is especially true for thin-layer galvanizing according to DIN 50997 (as of March 2023) the ratio of the radius of the opening to the volume of the recess (r / V ratio) for a Diameter of the opening of less than or equal to 10 mm for a, preferably maximum, component thickness greater than 3 mm 3 3 3 less than 30 cm / cm , preferably less than 20 cm / cm , in particular between 1 and 30 cm / cm , and / or with a diameter 3 3 3 the opening larger than 10 mm less than 100 cm / cm , preferably less than 80 cm / cm , in particular between 1 and 70 cm / cm , be.

[0064] The above-mentioned and preferred r / V ratios are dependent on the The tests carried out on the invention have shown that for a thin-layer galvanization, in particular a hot-dip galvanizing layer with a lower layer thickness compared to standard galvanizing particularly preferably appropriately adjusted r / V ratios as mentioned above are used can be.

[0065] Depending on the respective galvanizing process, the diameter of the opening and the component thickness, then an efficient specification of the volume of the recess can be made. In this context, it is understood that the The above-mentioned conditions can be understood in such a way that the range information also allows for a certain variation in Depending on the geometric shape of the recess, this can be guaranteed.

[0066] In addition, the hot-dip galvanizing layer can particularly preferably have a layer thickness in the range of 3 µm to 400 µm, preferably between 1 and 100 µm, can be applied to the component. The layer thickness can also be Depending on the respective galvanizing process, the hot-dip galvanized layer represents - unlike expiring Zinc noses - such zinc adhesion, which is desired and ultimately the component, which preferably contains iron and / or contains steel and protects against corrosion.

[0067] Furthermore, the component is particularly preferably moved at a speed of 0.05 to 1.5 m / min, preferably from 0.1 to 0.8 m / min, from the galvanizing bath. Speeds of the aforementioned type have proven to be particularly useful in transporting the zinc deposits into the recess.

[0068] The temperature of the zinc melt during hot-dip galvanizing can be between 400 °C and 500 °C. For hot-dip galvanizing according to EN ISO 1461 (as of March 2023), the galvanizing temperature range is in particular between 430 °C and 470 °C, more preferably between 435 °C and 465 °C. In thin-layer galvanizing According to DIN 50997 (as of March 2023), a slightly lower galvanizing temperature can be used if required, in particular the galvanizing temperature in the aforementioned thin-layer galvanizing is between 400 °C and 450 °C, preferably between 415 °C to 425 °C.

[0069] The viscosity of the zinc melt during hot-dip galvanizing can depend on the temperature and Alloy composition can be influenced. In particular, the viscosity during hot-dip galvanizing according to EN ISO 1461 (as of March 2023) between 0.025 to 0.04 poise, in particular between 0.035 to 0.039 poise, more preferably in the range of 0.037 poise + / - 5%, preferably at a galvanizing temperature of 435 °C and more preferably at a Galvanizing temperature above 435 °C, especially at 465 °C + / - 20%, between 0.025 to 0.039 poise, further preferably between 0.33 to 0.035 poise and especially 0.034 poise + / - 5%.

[0070] For thin-layer galvanizing according to DIN 50997 (as of March 2023), a slightly lower viscosity In particular, the viscosity at a zinc melt temperature of 400 °C + / - 20 % can be 0.023 to 0.038 poise, in particular between 0.030 and 0.034 poise and preferably 0.032 + / - 20% poise and at a Galvanizing temperature above 400 °C, especially at a zinc melt temperature of 450 °C + / - 20%, 0.020 to 0.030 poise, preferably between 0.023 to 0.029 poise and especially 0.027 + / - 20% poise.

[0071] In principle, the process according to the invention is also suitable for high-temperature galvanizing, in which a almost pure zinc melt is preferably used in a temperature range between 520 and 620 °C. In this case, The flow behavior of the zinc melt is very good due to the lower viscosity, so that when using the The recess according to the invention generally achieves a very high degree of hole freedom for different openings which is close to 100% hole-free. Another advantage at the aforementioned galvanizing temperatures is that the temperature difference between the temperature in the hot-dip galvanizing bath and the solidification temperature of the Zinc melt is very large, preferably around 100 K + / - 30 %, which is particularly important when the Zinc melting creates the possibility of a relatively long post-processing period. The recess according to the invention is also advantageous for high-temperature galvanizing, since the zinc also has sufficient time has to get into the corresponding recess.

[0072] In principle, the temperature difference between the temperature in the zinc melt and the Solidification temperature of the galvanizing layer must be significantly lower than 100 K and in particular between 10 K and 100 K, preferably between 20 K to 70 K and more preferably between 25 K to 50 K, in particular both for the standard galvanizing as well as for thin-layer galvanizing according to the above standards. The cooling rate depends on the surface-to-mass ratio of the component, but is usually different applications between 0.02 to 10 minutes preferably between 1 to 3 minutes, after leaving the Zinc melt or when emerging from the zinc melt.

[0073] The above-mentioned method is particularly preferred for comparatively large openings, in particular with a maximum diameter of more than 20 mm. However, according to the invention, it has also been found that the process is also suitable for smaller holes or openings and in particular leads to the This can result in a significantly lower post-processing effort. smaller than 10 mm, it may not be possible to guarantee 100% hole-free opening. Nevertheless, the The recess in the opening can reduce the amount of post-processing required. This results in in particular because the recess creates an area that ultimately serves to absorb excess Even if the hole is not 100% free, the previously discussed Advantages of reduced post-processing. The above diameters can refer to round holes, but also refer to non-circular holes, such as elongated holes and / or slots. Then the aforementioned diameter in particular the maximum clear diameter of the opening.

[0074] Advantageously, the component is pretreated, in particular cleaned, before hot-dip galvanizing. Different process steps can be provided for cleaning. Particularly preferred are those, especially in The following process steps are provided before hot-dip galvanizing: (a) degreasing treatment of the component, in particular in at least one degreasing bath; then (b) if necessary, rinsing the component degreased in process step (a); then (c) Pickling treatment of the material degreased in process step (a) and optionally in process step (b) rinsed component, in particular in at least one pickling bath; then (d) if necessary, rinsing the component pickled in process step (c); then (e) Flux treatment of the metal pickled in process step (c) and optionally in process step (d) rinsed component using a flux composition in a flux bath, (f) if necessary, drying treatment of the flux treatment carried out in step (e) subjected component, wherein optionally the process steps (a) to (f) are each repeated several times, preferably bundled and / or individually, as required, be performed.

[0075] The above-mentioned treatment can ensure that the component is optimally protected from treatment of the Hot-dip galvanizing can be carried out. Efficient cleaning is also beneficial for adhering zinc deposits, as This allows a galvanizing layer to be provided that extends evenly over the component surface.

[0076] Furthermore, it is understood that, if necessary, individual process steps may be carried out depending on different Components can be carried out multiple times. Some process steps are also optional, as is particularly the case with ´´where appropriate´´ is specified. Individual process steps can also be ´´grouped´´ / ´´bundled´´ multiple times For example, process steps (a) to (c) can be run twice for one component, which can then be fed to process steps (d) to (f). The sequence of the previously The specified process steps may be modified as required depending on the different components according to the respective needs of the component.

[0077] Furthermore, the present invention relates to a hot-dip galvanized component, wherein the component is subjected to a process of has been subjected to the aforementioned type.

[0078] The hot-dip galvanized component therefore has a recess in which solidified zinc alloy or zinc melt and further comprises at least one opening to which the recess is assigned. In the In particular, partially, preferably completely, solidified zinc melt is provided in the recess, the layer thickness or maximum height exceeds the layer thickness of the actual galvanizing layer, i.e. in particular is greater than 200 µm.

[0079] In connection with the hot-dip galvanized components, reference may be made to the above-mentioned statements on the process which, as explained above, also apply to the hot-dip galvanized component can.

[0080] Further features, advantages and possible applications of the present invention will become apparent from the following description of embodiments based on the drawing and the drawing itself. All The features described and / or illustrated, individually or in any combination, constitute the subject matter of the present invention, regardless of its summary in the claims or their reference back.

[0081] It shows: Fig. 1 is a schematic perspective view of a galvanizing process according to the invention in a galvanizing bath, Fig. 2 shows a further schematic perspective view of a galvanizing of components according to the invention in a galvanizing bath, Fig. 3 is a schematic perspective view of a component according to the invention before hot-dip galvanizing, Fig. 4 is a schematic perspective view of a hot-dip galvanized component according to the invention, Fig. 5 is a further schematic perspective view of a non-inventive hot-dip galvanized component, Fig. 6 is a schematic cross-sectional view of another embodiment of a hot-dip galvanized component and Fig. 7 is a schematic representation of part of a hot-dip galvanizing process according to the invention.

[0082] In Fig. 1, a galvanizing bath 6 is shown, which is at least partially filled with a zinc melt 5. The Zinc melt 5 contains and / or consists of a zinc alloy. Figure 1 schematically illustrates that a component 1 for applying a galvanizing layer 4 to the component in the galvanizing bath 6 or in the zinc melt 5 of the galvanizing bath 6 and is then immersed again after galvanizing. The component 1 has an opening 2. In Fig. 1 shows that the component 1 has at least one opening 2. In Fig. 1, the component 1 is Conveyor device 15, in particular via a hook-like construction of the conveyor device 15, into the galvanizing bath 6 immersed.

[0083] Fig. 2 illustrates that a plurality of components 1 are also introduced together into the galvanizing bath 6 can be - for example via a goods carrier 16, as shown in Fig. 2. The goods carrier 16 can in particular be attached to a conveyor device 15 or be formed as part of the conveyor device 15. Thus, a plurality of components 1 are galvanized together, whereby at least one component 1 has at least one opening 2. In particular Preferably, however, all components 1 can also have at least one opening 2.

[0084] Fig. 1 further shows that the component 1 has a recess 7 which was introduced before galvanizing. The recess 7 is adjacent to the opening 2, preferably directly, or merges into it. The recess 7 is for Provided for the collection of draining zinc alloy and opened accordingly to opening 2. Expiring Zinc alloy accumulates in the area of ​​the recess 7 when the component 1 is pulled out in the direction of the pull-out direction F, which is shown schematically in Fig. 1, is pulled out of the galvanizing bath 6.

[0085] Accordingly, Fig. 1 shows a method for hot-dip galvanizing at least one Component 1, wherein the component 1 is placed in a galvanizing bath 6 for applying a galvanizing layer 4 to the component 1, the a zinc melt 5 containing a zinc alloy, immersed and removed again after galvanizing is, wherein before galvanizing at least one recess 7 adjacent to the opening 2 of the component 1 is formed in the component 1 has been installed, which is designed to collect draining zinc alloy and / or draining zinc melt 5 is intended.

[0086] In Fig. 2, the openings 2 are shown schematically, so that the method according to the invention can also be implemented here is.

[0087] The introduction of the recess 7 is not shown in detail in Fig. 1 and Fig. 2, but this is done Inserted during a process step that is carried out before hot-dip galvanizing. Ultimately, the recess is 7 are preferably individually adapted to the respective opening 2 in terms of their dimensions and are accordingly integrated into the component 1 The recess 7 allows for at least a substantial absence of holes after hot-dip galvanizing. be ensured, since the recess 7 creates a predetermined area in which excess or running zinc melt 5 can collect or accumulate, causing unwanted zinc noses, protruding Zinc deposits or the like can be avoided. This leads to a drastically reduced Post-processing effort for the galvanized components 1.

[0088] Fig. 6 shows a schematic cross-section of a component 1 which is provided on both outer sides with a corresponding galvanized layer 4. The galvanized layer 4 protrudes from / over the ungalvanized component surface 8 and is in particular at least substantially uniform in relation to the layer thickness 14. However, it is understood that also uneven galvanizing layers 4 can be realized in the method according to the invention, in particular wherein the openings 2 can be kept at least substantially free from the zinc melt 5.

[0089] The recess 7 is in particular not regarded as part of the opening 2, but represents a separate recording area.

[0090] In Fig. 3, different openings 2 are shown on a component 1, each of which has a differently designed Recess 7 is assigned. Different geometric shapes for the recess 7 allow for of component 1 the corresponding absorption of draining zinc alloy. In this context, it is understood that also different shapes of the opening 2 - for example non-round openings 2 - or the like can be realized can.

[0091] The recess 7 can, depending on the design of the opening 2 and / or other process parameters It is also understood that the component 1 has at least one opening 2 which is provided with a corresponding recess 7. Fig. 3 is intended to illustrate schematically that in principle different shapes of the recess 7 can be considered. Fig. 4 shows the component 1 shown in Fig. 3 after hot-dip galvanizing with a galvanizing layer 4 applied accordingly to the component surface 8.

[0092] Fig. 4 further shows that the recess 7 is filled with zinc alloy after hot-dip galvanizing, whereby the opening 7 - to which the recess 7 is not included in terms of area or volume - at least substantially Even if the opening 2 is at least partially blocked, the recess 7 still allows the The advantage is that post-processing can be simplified drastically, since in particular not the entire hole or the entire opening 2 has been filled with zinc alloy.

[0093] In Fig. 5, a component 1 is shown which has edges 3 (not according to the invention). For at least one edge 3 (also in the embodiment shown in Fig. 5 for several edges 3) a recess 7 is introduced which are used after hot-dip galvanizing to collect the zinc alloy or zinc melt 5 from The appropriately dimensioned recess 7 ensures that when pulling out of the component 1 from the galvanizing bath 6, the zinc alloy runs off the component surface 8 and in the area of ​​the edges 3 in the recesses 7, so that after the zinc alloy has solidified, no protruding zinc noses or the like are present.

[0094] The recesses 7 shown in Fig. 3 are designed in such a way that when the component 1 is pulled out from the galvanizing bath 6 from the component surface 8 accumulating zinc alloy from the area of ​​the opening 2 in the Recess 7 collects, preferably so that after solidification of this expired zinc alloy, it is no longer in the opening 2 protrudes or so that the opening 2 is free from the applied hot-dip galvanizing layer 4 excess zinc alloy and / or so that the opening 2 is at least substantially free of the opening 2 Small parts of the opening 2 can be used in other embodiments, which are not described in detail here. shown, may also be partially filled with zinc alloy. However, there is still an area free of zinc alloy the opening 2, which drastically simplifies the post-processing effort, since the opening 2 in particular is not completely blocked by the zinc alloy.

[0095] Fig. 1 shows that the recess 7 in the lower area facing away from the pull-out direction F or in the lower half of the opening 2 facing away from the pull-out direction F - the relevant arrangement results for the component 1 when emerging from the galvanizing bath 6. In particular, the recess 7 in the lower apex and / or at the lowest point and / or area of ​​the opening 2. The lower Vertex 10 of the opening 2 only arises when the corresponding extension direction F is known and / or in Knowledge of the design of the conveyor device 15 or the support point of the component 1 and the Conveyor device 15 caused pulling movement from the zinc melt 5.

[0096] Different shapes of the recess 7 are shown in Fig. 3. The recess 7 can be seen in plan view of the Opening 2 is at least substantially circular segment-shaped, arc-shaped, triangular and / or rectangular shape. Different circular segment and / or rectangular shapes are also possible, such as This is also shown in Fig. 3. Finally, the shape of the recess 7 can be adapted to the shape of the corresponding opening 2, expected amount of zinc to be removed and / or other component-specific parameters.

[0097] It is not shown in detail how the recess 7 can be introduced before the hot-dip galvanizing of the component 1. The recess 7 can be introduced into the component 1 in particular by drilling and / or milling. Alternatively or In addition, it is also possible to cut the recess 7 by a thermal or non-thermal separation process, such as laser, Autogenous, plasma and / or water jet cutting, into the component 1. The recess 7 can together with the opening 2 but also in a subsequent process step.

[0098] In Fig. 3 it is shown that the opening 2 and the recess 7 are designed as a breakthrough and / or as a drainage opening is trained.

[0099] Furthermore, Fig. 3 shows that the opening 2 is circular or elliptical in cross-section. Not It is shown in more detail that the opening 2 can also be designed as an elongated hole.

[0100] The opening 2 can have a clear diameter 11 before the recess 7 is made, as shown in Fig. 3 shown schematically, of at least 5 mm, in particular of at least 10 mm. Smaller Diameter 11 can be equipped with a corresponding recess 7. It may then not be possible to have 100 % hole-freeness after galvanizing is guaranteed, but the advantageous effect is still maintained of the avoided clogging of the opening 2. Particularly preferably, the opening 2 can have a maximum clear Diameter of 50 cm, preferably 20 cm.

[0101] In the formation of the recess 7, certain relationships between the radius 12, the opening 2 and the Volume of recess 7 must be observed. Especially for galvanizing according to EN ISO 1461 (as of March 2023) the ratio of the radius 12 of the opening 2 to the volume of the recess 7 for a component thickness of 13 up to and including 3 mm, preferably with a maximum component thickness of 13 to 3 mm, with a diameter 11 of the opening 2 less than or equal to 3 3 3 10 mm less than 30 cm / cm , in particular between 1 and 20 cm / cm , and / or greater than 5 cm / cm .

[0102] For galvanizing according to EN ISO 1461 (as of March 2023) and with a maximum component thickness of 13 to including 3 mm, for a diameter 11 of the opening 2 greater than 10 mm, the above ratio 3 between the radius 12 of the opening 2 to the volume of the recess 7 less than 90 cm / cm , in particular between 1 to 3 40 cm / cm .

[0103] The above-mentioned r / V ratios change for component thicknesses 13 of greater than 3 mm. For a component thickness 13 of greater than 3 mm, especially for galvanizing according to EN ISO 1461 (as of March 2023), the ratio of the radius 12 of the Opening 2 to the volume of the recess 7 with a diameter 11 of the opening 2 less than or equal to 10 mm less than 50 3 3 cm / cm , in particular between 1 and 30 cm / cm , and / or with a diameter 11 of the opening 2 of greater than 10 mm 3 3 less than 100 cm / cm , especially between 1 and 70 cm / cm . The above conditions apply to a maximum Component thickness 13 of greater than 3 mm. An exact adjustment of the dimensions of the recess 7 can also be Shape of the opening 2 and the expected viscosity of the zinc melt 5, but especially in the above-mentioned magnitudes.

[0104] For thin-layer galvanizing according to DIN 50997 (as of March 2023), the above conditions adapted or optimized. For example, with thin-layer galvanizing according to DIN 50997 (as of March 2023), the Ratio of the radius 12 of the opening 2 to the volume of the recess 7 with a diameter 11 of the opening 2 smaller 3 or equal to 10 mm for a preferably maximum component thickness 13 of less than or equal to 3 mm less than 20 cm / cm , 3 in particular between 1 and 20 cm / cm . If the diameter of the opening 2 is greater than 10 mm, Thin-layer galvanizing according to DIN 50997 (as of March 2023) the ratio of the radius 12 of the opening 2 to the volume of the Recess 7 with a preferably maximum component thickness 13 of less than or equal to 3 mm with a diameter 11 3 3 the opening 2 of greater than 10 mm less than 100 cm / cm , in particular between 1 and 60 cm / cm .

[0105] If the components 1 are somewhat thicker, the ratios of r / V can also be adjusted. Thin-layer galvanizing according to DIN 50997 (as of March 2023) can thus reduce the ratio of the radius 12 of the opening 2 to the Volume of the recess 7 with a diameter 11 of the opening 2 less than or equal to 10 mm for a, preferably 3 3 maximum component thickness 13 of greater than 3 mm less than 30 cm / cm , in particular between 1 and 30 cm / cm , and / or 3 3 a diameter 11 of the opening 2 greater than 10 mm less than 100 cm / cm , in particular between 1 and 70 cm / cm , lay.

[0106] The applied hot-dip galvanizing layer 4 can in particular have a layer thickness 14 in the range between 3 µm to 400 µm, wherein the hot-dip galvanized layer 4 has been applied to the component 1, as shown in Fig. 6 shows schematically.

[0107] The speed at which the component 1 is removed from the zinc melt 5, as shown in Fig. 1, for example, can be adjusted according to the component 1 and the zinc melt 5 used. The However, speed can be between 0.1 and 0.8 m / min.

[0108] Before hot-dip galvanizing, component 1 can be pretreated accordingly. For pretreatment the steps (a) to (f) can be provided as shown in Fig. 7. The process steps can be in the order shown in Fig. 7 (i.e. one after the other). However, it can also be provided that at least one of the process steps (a) to (f) is exchanged accordingly and / or carried out several times and / or Optionally, process steps (a) to (f) can be carried out several times as required. and / or swapped with each other in the order. In particular, the following Steps planned: (a) degreasing treatment of the component 1, in particular in at least one degreasing bath; then (b) if necessary, rinsing the component 1 degreased in process step (a); then (c) Pickling treatment of the material degreased in process step (a) and optionally in process step (b) rinsed component 1, in particular in at least one pickling bath; then (d) if necessary, rinsing the component 1 pickled in process step (c); then (e) Flux treatment of the metal pickled in process step (c) and optionally in process step (d) rinsed component 1 by means of a flux composition in a flux bath, (f) if necessary, drying treatment of the flux treatment carried out in step (e) subjected component 1.

[0109] The process steps (a) to (f) are, as previously explained, also shown in Fig. 7.

[0110] Following process step (f), hot-dip galvanizing can be carried out. The introduction of the Recess 7 in the component 1 can be made between one of the steps (a) to (f), before step (a) and / or after step (f) - in any case before hot-dip galvanizing is carried out. After hot-dip galvanizing The galvanized component 1 can be quenched if necessary. A subsequent treatment may be necessary downstream for cooling the component 1, in the for example, passivation, sealing and / or organic or inorganic coating of the galvanized component 1 Any subsequent processing of component 1 that may still be required can also This post-processing is, however, made possible by the inventive introduction of the recess 7 significantly simplified.

[0111] The components 1 can, as previously explained, be placed together or separately in the galvanizing bath 6 be immersed - depending on the respective components 1.

[0112] Furthermore, the invention also relates to a hot-dip galvanized component 1, as shown for example in Fig. 4 The hot-dip galvanized component 1 is manufactured according to a method of the aforementioned embodiments. Accordingly, the hot-dip galvanized component 1 has at least one opening 2, to which a corresponding recess 7 is assigned, which the hot-dip galvanizing at least partially, preferably completely, filled with draining zinc alloy or zinc melt 5 After hot-dip galvanizing, at least part of the opening 2 is free of the zinc alloy, preferably completely free. List of reference symbols: 1 component 2 Opening 3 edge 4 galvanizing layer 5 Zinc melt 6 Galvanizing bath 7 Recess 8 Component surface 9 lower half of 2, 3 10 lower vertex 11 clear diameter of 2 12 radius of 2 13 Component thickness 14 Layer thickness 15 Conveyor system 16 product carriers F Pull-out direction

Claims

1. A method for hot-dip galvanizing at least one component (1) having at least one opening (2), wherein the Component (1) for applying a galvanizing layer (4) to the component (1) in a with a zinc alloy having The galvanizing bath (6) filled with molten zinc (5) is immersed and removed again after galvanizing, wherein, prior to galvanizing, at least one adjacent to the opening (2) of the component (1) and extending into the opening (2) opening recess (7) has been introduced into the component (1) to accommodate the running zinc alloy is intended, wherein the recess (7) is designed in such a way that when the component (1) is pulled out of the The zinc alloy flowing from the component surface (8) in the galvanizing bath (6) is removed from the area of the opening (2) in the Recess (7) collects, so that after solidification of this expired amount of zinc alloy, it does not enter the opening (2) and / or so that the opening (2) is free from the applied hot-dip galvanizing layer (4) excess zinc alloy and / or so that the opening (2) is at least substantially free of the opening (2) zinc alloy to be added; wherein the ratio of the radius (12) of the opening (2) to the volume of the recess (7), at a maximum component thickness (13) up to and including 3 mm, with a diameter (11) of the opening (2) of less than or equal to 10 mm less than 30 cm 3 3 / cm and / or with a diameter (11) of the opening (2) greater than 10 mm, less than 90 cm / cm or where the ratio of the radius (12) of the opening (2) to the volume of the recess (7), with a maximum component thickness (13) 3 greater than 3 mm, with a diameter (11) of the opening (2) less than or equal to 10 mm less than 50 cm / cm and / or 3 if the diameter (11) of the opening (2) is greater than 10 mm, it is less than 100 cm / cm.

2. Method according to claim 1, wherein the component (1) is removed from the galvanizing bath (6) in such a way that the Recess (7) in the lower area facing away from the pull-out direction (F) and / or in the lower area facing away from the pull-out direction (F) opposite half (9) of the opening (2), in particular in the lower apex (10) and / or in the lowest point and / or area of the opening (2).

3. Method according to one of the preceding claims, wherein the recess (7) in plan view of the opening (2) is at least substantially circular segment-shaped, arc-shaped, triangular and / or rectangular.

4. Method according to one of the preceding claims, wherein the recess (7) is formed by drilling prior to hot-dip galvanizing and / or milling and / or a thermal or non-thermal cutting process, such as laser, oxyfuel, plasma or water jet cutting.

5. Method according to one of the preceding claims, wherein the opening (2) and / or the recess (7) is formed as an opening and / or as a drainage opening in the component (1) is and / or wherein the opening (2) is circular and / or elliptical in cross-section and / or is formed as an elongated hole.

6. Method according to one of the preceding claims, wherein the opening (2) before the introduction of the recess (7) a clear diameter (11) of at least 5 mm, preferably at least 8 mm, more preferably at least 10 mm, and / or that the opening (2) has a maximum clear diameter (11) of 50 cm, preferably 25 cm, more preferably 10 cm.

7. Method according to one of the preceding claims, wherein, in particular for galvanizing according to EN ISO 1461 (status March 2023), the ratio of the radius (12) of the opening (2) to the volume of the recess (7) at a maximum Component thickness (13) up to and including 3 mm, with a diameter (11) of the opening (2) less than or equal to 10 mm less than 20 3 3 3 3 cm / cm , in particular between 1 and 20 cm / cm , and / or greater than 1 cm / cm , preferably greater than 5 cm / cm , and / or at 3 3 a diameter (11) of the opening (2) greater than 10 mm less than 50 cm / cm , in particular between 1 and 40 cm / cm , amounts.

8. Method according to one of the preceding claims, wherein, in particular for galvanizing according to EN ISO 1461 (status March 2023), the ratio of the radius (12) of the opening (2) to the volume of the recess (7) at a maximum 3 Component thickness (13) greater than 3 mm with a diameter (11) of the opening (2) less than or equal to 10 mm less than 40 cm / cm 3 , in particular between 1 and 30 cm / cm , and / or with a diameter (11) of the opening (2) greater than 10 mm smaller 3 3 80 cm / cm , in particular between 1 and 70 cm / cm .

9. Method according to one of the preceding claims, wherein in the case of thin-layer galvanizing according to DIN 50997 (status March 2023) the ratio of the radius (12) of the opening (2) to the volume of the recess (7) with a diameter (11) the opening (2) less than or equal to 10 mm for a, preferably maximum, component thickness (13) less than or equal to 3 mm less 3 3 3 20 cm / cm , preferably less than 15 cm / cm , in particular between 1 and 20 cm / cm , and / or with a diameter (11) 3 3 the opening (2) larger than 10 mm less than 100 cm / cm , preferably less than 70 cm / cm , in particular between 1 and 60 cm / cm 3 , amounts.

10. Method according to one of the preceding claims, wherein in the case of thin-layer galvanizing according to DIN 50997 (as of March 2023) the ratio of the radius (12) of the opening (2) to the volume of the recess (7) at a Diameter (11) of the opening (2) less than or equal to 10 mm for a, preferably maximum, component thickness (13) greater than 3 3 3 3 mm less than 30 cm / cm , preferably less than 20 cm / cm , in particular between 1 and 30 cm / cm , and / or at a 3 3 Diameter (11) of the opening (2) greater than 10 mm less than 100 cm / cm , preferably less than 80 cm / cm , in particular 3 between 1 to 70 cm / cm .

11. Method according to one of the preceding claims, wherein the hot-dip galvanizing layer has a layer thickness (14) in the range of 3 µm to 400 µm, preferably 4 to 100 µm, is applied to the component (1).

12. Method according to one of the preceding claims, wherein the component (1) is moved at a speed of 0.05 to 1.5 m / min, preferably from 0.1 to 0.8 m / min, from the galvanizing bath (6).

13. A method according to any one of the preceding claims, wherein before carrying out the hot-dip galvanizing, the following Process steps are provided, preferably in the following order: (a) degreasing treatment of the component (1), in particular in at least one degreasing bath; then (b) if necessary, rinsing the component (1) degreased in process step (a); then (c) Pickling treatment of the component degreased in process step (a) and, if necessary, rinsed in process step (b) (1), in particular in at least one pickling bath; then (d) if necessary, rinsing the component (1) pickled in process step (c); then (e) flux treatment of the steel pickled in step (c) and optionally rinsed in step (d) component (1) by means of a flux composition in a flux bath, (f) if necessary, drying treatment of the component (1) subjected to flux treatment in process step (e), wherein process steps (a) to (f) are optionally carried out several times as required.

14. Hot-dip galvanized component (1), wherein the component (1) is subjected to a method according to one of claims 1 to 13 has been.

Citation Information

Patent Citations

  • fluxes AND GALVANIZING PROCESSES

    DE60124767T2

  • Flux and process for hot dip galvanization

    EP1352100B1

  • Flux and process for hot dip galvanization

    US20030219543A1

  • FLUX and process for hot dip galvanization

    WO2002042512A1

  • receiving element for a door handle device

    DE102015108193A1