Cerium oxide-supported metal catalysts for the selective reduction of NOx
Patent Information
- Application Number
- DE112014005273
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2013-11-19
- Filing Date
- 2014-11-19
- Publication Date
- 2024-11-14
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates generally to a composition of matter comprising a cerium oxide support modified with catalytic cations and optionally with promoter cations, to a process for its preparation and, in particular, to the use of such a composition in the specific catalytic reduction of nitrogen oxides in a motor vehicle catalyst. BACKGROUND
[0002] Automotive catalyst technology has evolved, among other things, with the replacement of two-way catalyst technology with three-way catalyst technology. A three-way catalyst owes its name to the fact that it is capable of simultaneously catalyzing three chemical reactions involved in the oxidoreductive removal of pollutants from a combustion exhaust stream. These three reactions are, in general terms: i) oxidation of unburned hydrocarbons to carbon dioxide, ii) oxidation of incompletely combusted carbon monoxide to carbon dioxide, and iii) reduction of nitrogen oxides (primarily NO2 and NO) to nitrogen gas (N2).
[0003] Three-way catalysts currently employ a support structure such as ceria, which is capable of storing oxygen for use when the oxygen content in the exhaust stream is low. The ceria support can be doped with compounds such as aluminum or zirconium oxides to improve thermal stability, surface area, and oxygen storage capacity. Catalytic centers, which can be composed of noble metal cations (platinum, palladium, or rhodium), are integrated into the support structure and can act as direct mediators of exhaust gas oxidation / reduction.
[0004] While current catalysts exhibit promising properties in terms of capacity, efficiency and thermal stability, there is a constant need to find further improvements to meet increasingly demanding regulatory requirements.
[0005] Patent application 1 and patent application 2 disclose processes for producing catalysts. Patent application 1: US 2003 / 0 059 358 A1 Patent application 2: US 2013 / 0 029 839 A1 SUMMARY
[0006] The above-mentioned object is achieved by the subject matter of the independent claims. Advantageous embodiments of the present invention are the subject matter of the dependent claims.
[0007] Disclosed herein is a catalyst and a method for producing the catalyst. The catalyst discussed may be useful in treating automotive emissions or combustion emission components.
[0008] In one aspect, a method for preparing a catalyst is provided. The method comprises contacting a ceria-containing substrate with a solution containing catalytic cations; and contacting the substrate with a solution containing promoter cations; wherein the catalytic cations consist of iron, copper, cobalt, or a combination thereof, and the promoter cations consist of alkali metal cations or alkaline earth metal cations, or a combination thereof, and the catalytic cation-containing solution comprises at least one chelating agent.
[0009] In another aspect, a catalyst is provided. The catalyst comprises a substrate containing ceria, catalytic cations bound to substrate surfaces, and promoter cations bound to substrate surfaces. The catalytic cations may be iron, copper, cobalt, or a combination thereof, and the promoter cations may be alkali metal cations or alkaline earth metal cations, or a combination thereof, wherein the catalytic cations have a loading density of about 0.1-1.5 wt. % and the promoter cations are present in a stoichiometric ratio to the catalytic cations ranging from about 1:2 to 6:1, inclusive.
[0010] In some cases, the catalyst catalyzes reaction I, reaction II, or both: 2 NO + 2 H2 → N2 + H2O I, 2NO + 3H2 → 2NH3 + O2 II.
[0011] In some special cases, the catalyst has a %N2 selectivity of greater than about 67% or greater than about 90% according to equation A: %N2−Selectivity=(moles NO consumed by Reaction Imoles NO consumed by Reactions I and II)×100
[0012] In another aspect, a catalyst and its preparation process are provided. The process comprises contacting a cerium oxide-containing substrate with a solution containing catalytic cations and contacting the substrate with a solution containing promoter cations, wherein the catalytic cations consist of iron, copper, cobalt, or a combination thereof, and the promoter cations consist of alkali metal cations or alkaline earth metal cations, or a combination thereof. The catalytic cation-containing solution comprises at least one chelating agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Various aspects and advantages of the invention will become apparent and more readily understood from the following description of the various aspects taken in conjunction with the accompanying drawings. It shows: Fig. Figure 1 is a schematic representation of catalytic cations bound in various configurations to a surface of a substrate comprising cerium oxide; Fig. 2A is a flow diagram of a variant of a process for preparing a catalyst; Fig. Figure 2B is a flow diagram of another variation of a process for preparing a catalyst; Fig. Figure 3A is a kinetic curve of a nitric oxide reduction reaction in the presence of a catalyst; Fig. Figure 3B is a kinetic curve of a nitric oxide reduction reaction in the presence of a catalyst, including three periods of deliberate water addition; Fig. Figure 4A is a DR UV-vis spectrum of a catalyst prepared using Fe(NO3)3 on Na / CeO2; Fig. Figure 4B is a DR UV-vis spectrum of a catalyst prepared using NaFeEDTA on CeO2; Fig. Figure 5A is a temperature-programmed reduction curve of a catalyst prepared using Fe(NO3)3 on Na / CeO2; Fig. Figure 5B is a temperature-programmed reduction curve of a catalyst prepared using NaFeEDTA on CeO2; Fig. Figure 6A is a deconvoluted curve of a temperature-programmed reduction of a catalyst prepared using NaFeEDTA on CeO2 at a moderate loading density; Fig. Figure 6A is a deconvoluted curve of a temperature-programmed reduction of a catalyst prepared using NaFeEDTA on CeO2 at high loading density; Fig. Figure 7 is a graph of the reduction of catalytic cations for two catalyst types at different loading densities; Fig. Figure 8A is a graph of a redox-cycled temperature-programmed reduction of a catalyst prepared using Fe(NO3)3 on Na / CeO2; Fig. Figure 8B is a graph of a redox-cycled temperature-programmed reduction of a catalyst prepared using NaFeEDTA on CeO2; Fig. Figure 9A is a graph of the first and second cycle reductions of catalytic cations of a catalyst prepared using NaFeEDTA on CeO2; Fig. Figure 9B is a plot of the redox cycling fraction of catalytic cations as a function of loading density for a catalyst prepared using NaFeEDTA on CeO2; Fig. Figure 10A shows XANES spectra of two reference iron oxides and a catalyst prepared using NaFeEDTA on CeO2, which was coated with 1.5 Fe nm -2 was loaded at different temperatures; Fig. Figure 10B shows XANES spectra of two reference iron oxides and a catalyst prepared using NaFeEDTA on CeO2, which was coated with 0.9 Fe nm -2 was loaded at different temperatures; Fig. Figure 10C shows XANES spectra of two reference iron oxides and a catalyst prepared using NaFeEDTA on CeO2, which was coated with 0.6 Fe nm -2 was loaded at different temperatures; Fig. Figure 10D shows an XANES spectrum of two reference iron oxides and a catalyst prepared using Fe(NO3)3 on Na / CeO2, which was coated with 1.0 Fe nm -2 was loaded at different temperatures; Fig. Figure 11 is a plot of the oxidation state of catalytic cations as a function of temperature and measured by XANES for two catalyst types; Fig. Figure 12 is a bar graph of the nitric oxide reduction rate catalyzed by a catalyst or by a promoter cation-modified substrate at different temperatures; Fig. Figure 13A is a plot of the nitric oxide reduction rate as a function of loading density for two catalyst types and for a promoter cation-modified substrate with a Pd catalyst as a reference; Fig. Figure 13B is a plot of the conversion frequency of nitrogen monoxide reduction as a function of loading density for two catalyst types; Fig. Figure 14 is a plot of the nitric oxide reduction reaction rate for catalysts prepared using NH4FeEDTA on CeO2 with various alkali metal promoter cations; Fig. Figure 15 is a plot of the nitric oxide reduction rate for a catalyst prepared using NH4FeEDTA on CeO2 with various stoichiometric ratios of sodium promoter cations to catalytic cations; Fig. Figure 16 is a bar graph of nitric oxide reduction rates for various catalysts prepared using protected catalytic copper(II) cations; Fig. Figure 17 is a plot of nitrogen monoxide reduction rates for various catalysts prepared using protected catalytic copper(II) cations as a function of catalytic cation loading density; and Fig. Figure 18 is a bar graph of nitrogen monoxide reduction rates at different temperatures for three different catalysts prepared with catalytic iron, copper, or cobalt cations. DETAILED DESCRIPTION
[0014] Provided are a catalyst comprising a cerium oxide substrate having catalytic cations bound to its surface, and a process for preparing the catalyst. The process for preparing the catalyst may involve contacting a substrate with a solution containing catalytic cations and with a solution containing promoter cations. In certain variants, the catalytic cation-containing solution may contain chelated catalytic cations. The catalyst may comprise a cerium oxide-based substrate having catalytic cations of a transition metal, post-transition metal, or both bound thereto, and promoter cations of an alkali metal, alkaline earth metal, or both.
[0015] A method for producing a catalyst includes a step of contacting a substrate with a solution containing catalytic cations, alternatively referred to as a catalytic cation solution. The substrate comprises cerium oxide, where "cerium oxide" refers to an oxide of cerium. In various variants, the substrate may optionally contain various ceramic or metal oxides, for example, oxide of zirconium, aluminum, or silicon, in admixture with the cerium oxide.
[0016] The substrate may include solid-phase material in any physical configuration. In some aspects, the substrate may include cerium oxide, which has a high surface-to-mass ratio. In some variations, a high surface-to-mass ratio greater than about 20 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 50 m 2 ·G -1In some variants, a high surface-to-mass ratio greater than about 75 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 100 m 2 ·G -1 be.
[0017] Suitable physical substrate configurations with a high surface-to-mass ratio may include a honeycomb structure, any porous structure, powder, or any other configuration that has a high surface-to-mass ratio. In some cases, the substrate will be in a powder form with a particle size of 25 nm to 200 µM. In some examples, the substrate will be in a powder form with a surface-to-mass ratio of about 100 m 2 ·G -1 present.
[0018] Suitable catalytic cations employed in the process can be taken from a group including transition metal cations and post-transition metal cations. In some aspects, the catalytic cations can include any transition metal cations or post-transition metal cations. As used herein, a transition metal can be any D-block metal from Groups 4-13. A post-transition metal can be any metal from the group including aluminum, gallium, indium, tin, thallium, lead, or bismuth. In some aspects, suitable catalytic cations can include cations of one or more Period 4 transition metals, a group including scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, and zinc. In some cases, suitable catalytic cations will include cations of iron, copper, or cobalt, or combinations thereof.
[0019] In some aspects, the catalytic cation-containing solution may include at least one chelating agent. As used herein, a chelating agent is a soluble, multidentate ligand capable of forming more than one coordinate bond with a central metal cation. Non-limiting examples of chelating agents that may be employed include ethylenediaminetetraacetic acid (EDTA), diethylenetriaminepentaacetic acid (DTPA), ethylene glycoltetraacetic acid (EGTA), nitrilotriacetic acid (NTA), citric acid, ethylenediamine, 2,3-dimercapto-1-propanesulfonic acid, dimercaptosuccinic acid, desferrioxamine mesylate, oxalic acid, tartaric acid, or ascorbic acid. It should be understood that a chelating agent may include one or both of a conjugate acid / base pair.
[0020] It is contemplated that in variants of the process employing a chelating agent, a chelate complex may be preformed between the chelating agent and the catalytic cations before the catalytic cations are introduced into the catalytic cation solution. As used herein, a chelating complex may be a coordination moiety comprising at least one chelating agent molecule and one catalytic cation. In other cases, the chelating agent and the catalytic cations may be introduced separately into the catalytic cation-containing solution.
[0021] Suitable chelating agents that can be used in the process can include any chelating agent that can form a thermodynamically stable chelate complex with the catalytic cations. For example, a chelating agent can be chosen that forms a chelate complex with catalytic cations that has a dissociation constant (K d ) of less than 1 µM. A chelating agent can be chosen which, under standard conditions, forms a chelate complex with K d of less than about 0.1 µM. A chelating agent can be chosen which, under standard conditions, forms a chelate complex with K d of less than about 0.01 µM. A chelating agent can be chosen which, under standard conditions, forms a chelate complex with K dof less than about 0.001 µM. As used herein, the dissociation constant is defined as the product of the concentration of free catalytic cations and the concentration of free chelating agent divided by the sum of all chelate complex species, including fully and partially coordinated complexes.
[0022] In variants of the catalyst preparation process that employ a chelating agent, the catalytic cations can be described as “protected catalytic cations.” Without being bound by any particular theory and as schematically shown in Fig. As illustrated in Figure 1, it is believed that carrying out the process can result in catalytic cations being bound to substrate surfaces in one or more different configurations. These configurations include isolated ions or small clusters, two-dimensional sheets, and three-dimensional crystallites. Again, without being bound by any particular theory, it is further believed that the use of a chelating agent can influence the distribution of catalytic cations on substrate surfaces, particularly by inhibiting the formation of isolated ions or small clusters.
[0023] It is contemplated that in cases where a chelating agent is employed, the chelating agent may be present in the catalytic cation solution in an approximately equimolar amount relative to catalytic cations. Alternatively, the chelating agent may be present in molar excess over catalytic cations. In some cases, a suitable chelating agent will be one capable of forming a chelate complex with the catalytic metal cation, the complex possessing a net negative charge. In some cases, a suitable chelating agent will be a tetradentate ligand. In some cases, a suitable chelating agent will be EDTA.
[0024] The catalytic cations of the catalytic cation solution may comprise metal atoms in any positive oxidation state. Suitable oxidation states may, in some cases, include those in which the catalytic cations employed can form a thermodynamically stable chelate complex with any chelating agent employed.
[0025] The catalyst preparation process may additionally include a step of contacting the substrate with a solution containing promoter cations, alternatively referred to as a promoter cation solution. Promoter cations may include cations of one or more elements from a group consisting of alkali metals and alkaline earth metals. In some cases, the promoter cations may be cations of at least one of the following elements: lithium, sodium, potassium, rubidium, and cesium.
[0026] In some aspects of the process, the substrate can be contacted with the catalytic cation-containing solution, the promoter cation-containing solution, or both via incipient wetness impregnation (IWI). In IWI, the substrate is wetted to the incipient wetness volume, the minimum volume of solution required to fill the volume inside and between the particles. The incipient wetness volume can be determined by any suitable means. One example of a suitable means for determining the incipient wetness volume of the substrate is based on the total volume uptake during N2 physisorption.
[0027] The catalytic cation-containing solution and the promoter cation-containing solution may each comprise a solvent. It is contemplated that a suitable solvent will include any solvent capable of solvating substrate surfaces, solvating a promoter cation or a salt or chelate complex thereof, solvating a catalytic cation or a salt thereof, or any combination of the foregoing. In some cases, the solvent may be water. In some cases, the solvent may be a water / organic substance mixture, such as water / methanol. In some cases, the solvent may be a polar organic solvent. The catalytic cation-containing solution and the promoter cation-containing solution may comprise identical or different solvents.
[0028] In some cases of the catalyst preparation process that include a step of contacting the substrate with a promoter cation solution, the catalytic cation solution and the promoter cation solution may be different. In different variations of such cases, the substrate may be contacted with the promoter cation solution before or during its contact with the catalytic cation solution. In other cases, the catalytic cation solution and the promoter cation solution may be the same solution, meaning that a single solution containing both promoter cations and catalytic cations may be used.
[0029] In cases where the substrate is contacted with a promoter cation solution before contacting the substrate with a catalytic cation solution, the solvent of the promoter cation solution can be removed from the substrate before contacting the substrate with the catalytic cation solution. Such removal can be achieved, for example, by heating or applying a vacuum to the substrate.
[0030] In some additional aspects, contacting the substrate with a catalytic cation solution may be followed directly or indirectly by removing the solvent of the catalytic cation solution. In other additional aspects, contacting the substrate with a catalytic cation solution may be followed directly or indirectly by heating the catalyst under oxidative conditions. In still other additional aspects, contacting the substrate with a catalytic cation solution may be followed directly or indirectly by removing the solvent and heating the catalyst under oxidative conditions. As used herein, the phrase "under oxidative conditions" may mean under conditions sufficient to oxidize organic substances adsorbed onto the catalyst. Such organic substances could include, for example, chelating agents.Heating the substrate under oxidative conditions may serve to combust any organic residues remaining from the IWI step(s) and / or evaporate any volatile components retained in the composition. In some variations, heating under oxidative conditions may involve heating the catalyst to about 550°C in ambient air.
[0031] In aspects of the process where contacting the substrate with a catalytic cation solution is followed by solvent removal, a sequence comprising those steps may be repeated at least once. Such repetition may be useful, for example, in cases where the catalytic cation solution is present at a concentration not high enough to produce a desired loading density of catalytic cations bound to the substrate.
[0032] Fig. Figure 2A provides a schematic representation of one possible format of a method 100 for preparing a catalyst according to the present disclosure. In step 102, the substrate may be modified by IWI with a solution containing promoter cations, for example, a NaHCO3 solution. In step 104, the solvent is removed, for example, by temporarily placing the substrate under vacuum. Step 106 involves modifying the substrate by IWI with a solution containing catalytic cations, for example, an NH4FeEDTA solution. In step 108, the solvent is removed, for example, by temporarily placing the substrate under vacuum. In step 110, the substrate is heated under oxidative conditions.
[0033] Fig. Figure 2B illustrates another possible format of a method 112 for preparing a catalyst according to the present disclosure. In step 114, the substrate is modified by IWI with a solution containing promoter cations and catalytic cations, for example, a NaFeEDTA solution. In step 116, the solvent is removed, for example, by temporarily placing the substrate under vacuum. In step 118, the substrate is heated under oxidative conditions.
[0034] Also disclosed is a catalyst comprising a substrate and catalytic cations bound to substrate surfaces. The substrate comprises cerium oxide, where "cerium oxide" refers to an oxide of cerium. In various variants, the substrate may optionally comprise various ceramic or metal oxides, for example oxide of zirconium, aluminum, or silicon, in admixture with the cerium oxide. The catalytic cations may be bound to substrate surfaces in geometries including isolated ions or small clusters, two-dimensional sheets, or three-dimensional crystallites, as schematically shown in Fig. 1. In some variants, catalytic cations can be bound predominantly in two-dimensional sheet structures to the substrate surface.
[0035] A substrate may include solid-state ceria in any physical configuration. In some aspects, the substrate may include ceria having a high surface area to mass ratio. In some variations, a high surface area to mass ratio greater than about 20 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 50 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 75 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 100 m 2 ·G -1 be.
[0036] It should be understood that a substrate having a high surface area to mass ratio may include a substrate with a honeycomb structure, a substrate with a porous structure, a powder, or any other configuration having a high surface area to mass ratio. In some cases, the substrate will be in a powder form with a particle size of 25 nm to 200 µm. In some examples, the substrate will be in a powder form with a surface area to mass ratio of about 100 m 2 ·G -1 present.
[0037] In various aspects, the catalytic cations bound to substrate surfaces may comprise transition metal cations or post-transition metal cations. As used herein, a transition metal may be any D-block metal from Groups 4-13. A post-transition metal may be any metal from the group including aluminum, gallium, indium, tin, thallium, lead, or bismuth. Non-limiting examples of suitable catalytic cations may include cations of cadmium, cobalt, copper, chromium, iron, manganese, gold, silver, platinum, titanium, nickel, niobium, molybdenum, rhodium, palladium, scandium, vanadium, or zinc. In some aspects, suitable catalytic cations may be those capable of forming a stable chelate complex with a chelating agent.
[0038] In some aspects, the catalytic cations may be Period 4 transition metal cations, a group that includes cations of any of the following: scandium, titanium, vanadium, manganese, iron, cobalt, nickel, copper, or zinc. In some variations, the catalytic cations may consist of cations of one element. In other variations, the catalytic cations may include cations of more than one element. It is contemplated that catalytic cations may be bound to substrate surfaces via coordinate bonds. Such coordinate bonds may be oxide bonds.
[0039] Catalytic cations may be present in the catalyst at any loading density. As used herein, the phrase "loading density" refers to the portion of a catalyst consisting of catalytic cations. The loading density may sometimes be described in weight percent units, in other cases in mole units of catalytic cations per mass of catalyst, and in still other cases in units of the number of catalytic cations per surface area of catalyst. In some aspects, catalytic cations may be present at a loading density of at least 0.1 wt. %. In other aspects, catalytic cations may be present at a loading density of less than 2.0 wt. %.
[0040] In some aspects, the catalytic cations may be present in the catalyst in an amount sufficient to achieve, but not exceed, monolayer coverage of substrate surfaces. In other aspects, the catalytic cations may be present in the catalyst in an amount sufficient to achieve, but not exceeding, monolayer coverage of substrate surfaces. In some aspects, the catalytic cations may be present in the catalyst in an amount insufficient to achieve monolayer coverage of substrate surfaces.
[0041] The catalyst may additionally include promoter cations bound to the substrate surface. The promoter cations may include cations of an alkali metal or an alkaline earth metal. In some cases, suitable promoter cations may include cations of any element selected from the group consisting of lithium, sodium, potassium, rubidium, and cesium. It should be understood that promoter cations may be bound to substrate surfaces via coordination bonds, including oxide bonds. Oxides that can bind promoter cations to the substrate include cerium oxide and oxide of a catalytic cation.
[0042] Promoter cations may be present in the catalyst in any stoichiometric ratio relative to catalytic cations. In some cases, the stoichiometric ratio of coordinated promoter cations to catalytic cations may range from 1:2 to 6:1, or any ratio in between.
[0043] In some aspects, the catalyst may catalyze the reaction of gases that may be present in combustion exhaust, particularly gases that may be present in the combustion exhaust stream of an internal combustion engine. In some cases, the catalyst may catalyze the reduction of an oxide of nitrogen. In some cases, the catalyst may catalyze the specific reduction of nitrogen monoxide.
[0044] In different cases, the catalyst can catalyze reaction I, reaction II or both: 2NO + 2H2 → N2 + 2H2O I. 2NO + 3H2 → 2NH3 + O2 II.
[0045] In cases where the catalyst catalyzes both reactions I and II, the catalyst can be characterized by having a percent N2 selectivity as defined according to equation A: %N2−Selectivity=(moles NO consumed by Reaction Imoles NO consumed by Reactions I and II)×100
[0046] In some cases, the catalyst can catalyze reactions I and II with a %N2 selectivity greater than or equal to about 67%. In some cases, the N2 selectivity can be greater than or equal to about 90%. Fig. Figure 3A illustrates a case of a catalyst catalyzing reactions I and II with an N2 selectivity of approximately 67%. A catalyst was exposed to a 450°C gas stream containing NO and H2. The exhaust gas was monitored for N2 and NH3 content using mass spectrometry. The results were converted into the conversion frequency (TOF, moles of product per mole of catalyst per time) based on the amount of active catalytic cations. Since TOF is proportional to the NO consumption for each reaction, the results indicate a preference of approximately 2:1 for NO consumption by reaction I, or an N2 selectivity of approximately 67%.
[0047] In other cases, the catalyst can catalyze reaction III or reaction IV: 2NO + 2CO → N2 + 2CO2 III. 18NO + 2C3H6 → 9N2 + 6H2O + 6CO2 IV.
[0048] In such cases, the catalyst can additionally or alternatively catalyze incomplete redox reactions between nitrogen monoxide and carbon monoxide or propylene. Incomplete reactions can yield products such as various nitrates or nitriles.
[0049] In certain aspects, the catalyst may be water-stable by retaining its catalytic activity after exposure to water. Such exposure to water may occur, in addition to product formation, for example, through the presence of water vapor in a combustion exhaust stream to which the catalyst is exposed. One such aspect is Fig. 3B. The Fig. The experiment shown in Figure 3B is similar to that of Fig. Similar to Figure 3A, but with the added feature of three time-limited additions of water vapor lasting one hour, each indicated by vertical dashed lines, with the H2 input stream passed through a H2O bubbling device. As shown, the catalyst retains ~90% of its activity during one water pulse and regains full activity once the water pulse ends. The apparent sharp increase in NH3 production during each water pulse is due in part to the mass spectrometer's inability to distinguish water from ammonia.
[0050] In some aspects, at least 30% of the substrate-bound catalytic cations may be capable of undergoing at least two reduction / oxidation cycles under conditions where reduction reaction temperatures do not exceed 550°C. These aspects of the catalyst are discussed in more detail in Examples 41-44 below.
[0051] Also disclosed is a catalyst comprising a substrate and catalytic cations and prepared by a process comprising contacting a cerium oxide substrate with a solution containing promoter cations and contacting the substrate with a solution containing catalytic cations. The substrate comprises a cerium oxide preparation and, in some variations, may include a ceramic or metal oxide in admixture with the cerium oxide.
[0052] In various aspects, the substrate may include solid-phase ceria in any physical configuration. In some aspects, the substrate may include ceria having a high surface area to mass ratio. In some variations, a high surface area to mass ratio greater than about 20 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 50 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 75 m 2 ·G -1 In some variants, a high surface-to-mass ratio greater than about 100 m 2 ·G -1 be.
[0053] It should be understood that a cerium oxide support comprising cerium oxide having a high surface area to mass ratio may include a cerium oxide substrate with a honeycomb structure, a cerium oxide substrate with a porous structure, cerium oxide powder, or any other configuration having a high surface area to mass ratio. In some cases, the cerium oxide support will be in a powder form with a particle size of 25 nm to 200 µm. In some examples, the cerium oxide support will be in a powder form with a surface area of about 100 m 2 ·G -1 present.
[0054] Catalytic cations can include transition metal or post-transition metal cations bound to substrate surfaces. In some variants, catalytic cations can include Period 4 transition metals. Catalytic cations can be coordinated by the substrate surface when the substrate comes into contact with a solution containing catalytic cations. Catalytic cations can be coordinated by the substrate surface via oxide bonds. Catalytic cations can be arranged on the substrate surface in isolated ions or small clusters, two-dimensional sheets, three-dimensional sheets, or combinations thereof.
[0055] A solution containing catalytic cations may include a salt comprising catalytic cations. In some cases, a solution containing catalytic cations may include a chelating agent. As mentioned above, catalytic cations coordinated by a chelating agent may be referred to as chelated catalytic cations or protected catalytic cations.
[0056] Suitable promoter cations that can be used in the promoter cation-containing solution can include alkali metal cations, alkaline earth metal cations, or both. In some cases, promoter cations can be cations of at least one element from a group consisting of lithium, sodium, potassium, rubidium, and cesium.
[0057] In some aspects, the catalyst may catalyze the reaction of gases that may be present in combustion exhaust, particularly gases that may be present in the combustion exhaust stream of an internal combustion engine. In some cases, the catalyst may catalyze the reduction of an oxide of nitrogen. In some cases, the catalyst may catalyze the specific reduction of nitrogen monoxide.
[0058] As illustrated by the following examples, catalysts according to the disclosure prepared by a process in which the catalytic cation-containing solution includes chelated catalytic cations can possess catalytic properties that differ from those of catalysts prepared by a process in which no chelated catalytic cations are employed. Without being bound by any particular theory, it is believed that a process employing protected catalytic cations in the catalytic cation-containing solution can promote the formation of two-dimensional sheets, possibly by sterically and / or electronically preventing the catalytic cations from adsorbing to isolated sites on substrate surfaces.In this aspect, chelating agents that possess significant steric mass and / or chelating agents whose chelate complexes with catalytic cations have a negative net charge may be useful. EXAMPLES
[0059] The following examples are provided for illustrative purposes only and are not to be interpreted as limiting the scope of the present invention. Examples 4 to 6 are not according to the invention. The examples provide a clearer understanding of the features and advantages of the invention.
[0060] Examples 1-33 describe the preparation of various catalysts according to the methods of Fig. 3A, Fig. 3B, wherein working examples 4 to 6 are not according to the invention. In Examples 1-19, the substrate was cerium oxide, and the catalytic cations were iron(III) cations. Solutions containing catalytic cations included either protected (NaFeEDTA or NH4FeEDTA) or unprotected (Fe(NO3)3) cations. Examples whose preparation involved the use of NaFeEDTA were prepared according to the method of Fig. 3B. Examples involving the use of NH4FeEDTA or Fe(NO3)3 were prepared according to the method of Fig. 3A, with steps 106 and 108 included in some, but not all, of these examples.
[0061] Unless otherwise stated, the substrate was NanoTek CeO2 powder with a surface area to mass ratio of 101 m purchased from CI Kasei Co., Ltd. 2 ·G -1The substrate was dried at 120°C under ambient atmosphere for >12 h prior to use. All other reagents were purchased from Sigma-Aldrich and used as is. N2 physisorption isotherms were obtained using a Micromeritics ASAP 2010 analyzer. Promoter-modified and unmodified supports were degassed for 6 h at >5 mTorr and 120°C to release absorbed water prior to physisorption. Elemental analysis of catalyst compositions was performed using a Varian MPX ICP-OES instrument.
[0062] Examples 34-58 describe various analytical techniques applied to the catalysts of Examples 1-33 to investigate their chemical, structural, and catalytic properties. Examples 1-3
[0063] NaFeEDTA and NH4FeEDTA were prepared by stirring 10 mmol of H4EDTA and 10 mmol of Fe(NO3)3 9H2O in 25 mL of H2O at 60°C until all solids dissolved. After dissolution, 40 mmol of NaHCO3 or NH4HCO3 was slowly added, and the resulting solution was reduced to 5 mL by rotary evaporation and stored overnight at -20°C. The resulting crystals were collected by filtration, washed in acetone, and dried at 20 mTorr for 12 hours. Thermogravimetric analysis revealed >99% purity of the iron(III) chelates.
[0064] (NH4)2CoEDTA was prepared by stirring 10 mmol H4EDTA and 10 mmol Co(NO3)3·6H2O in 25 mL H2O at 60°C until all solids dissolved.
[0065] After dissolution, 40 mmol of NH4HCO3 was slowly added, and the resulting solution was completely reduced by rotary evaporation. The complex was purified by heating under vacuum to remove residual NH4NO3. Non-inventive examples 4-6
[0066] Catalysts were prepared using a cerium oxide substrate to which unprotected, catalytic iron(III) cations and sodium promoter cations were bound in a 1:1 stoichiometric ratio of catalytic to promoter cations. Cerium oxide powder was contacted with an IWI volume of 200, 400, or 600 mM NaHCO3. The modified substrates were dried for 24 hours in a partially covered container under ambient conditions, then heated to 120°C for 12 hours. Each of the modified substrates was then placed in an IWI volume of the same Fe(NO3)3 concentration (200, 400, or 600 mM, respectively). The catalysts were dried for 24 hours in partially covered containers under ambient atmosphere and then for 12 hours under dynamic vacuum (~20 mTorr). The dried catalysts were heated from room temperature to 550°C at a temperature rise rate of 10°C / min in still ambient air. Examples 7-13
[0067] Catalysts were prepared with protected catalytic iron(III) cations and sodium promoter cations in a single solution. CeO2 powder with a surface area of 101 m 2 ·G -1 was added to a humidified volume, determined by N2 physisorption, with a concentration of 100, 200, or 300 mM NaFeEDTA as prepared in Example 1. The impregnated materials were dried for 24 hours in partially covered containers under ambient atmosphere and then for 12 hours under dynamic vacuum (~20 mTorr). Since the solubility of NaFeEDTA limits the loading density from a single impregnation to approximately 0.6 Fe·nm -2 limited, multiple impregnation and drying steps were used to achieve higher densities. The dried catalysts were heated from room temperature to 550°C in still ambient air at a temperature ramp rate of 10°C / min. Examples 14-15
[0068] Catalysts were prepared with protected catalytic iron(III) cations without promoter cations. Cerium oxide powder was added to a humidified volume determined by N2 physisorption containing 100 or 200 mM NH4FeEDTA as prepared in Example 2. The impregnated materials were dried for 24 hours in partially covered containers under ambient atmosphere and then for 12 hours under dynamic vacuum (~20 mTorr). The dried catalysts were heated from room temperature to 550°C in still ambient air at a temperature ramp rate of 10°C / min. Examples 16-19
[0069] Catalysts were prepared with protected catalytic iron(III) cations and with a range of alkali metal promoter cations in 1:1 stoichiometric ratios. Cerium oxide powder was added to a humidified volume containing 100 mM LiOH, NaHCO3, KHCO3, or CsHCO3. The modified material was dried in a partially covered container under ambient conditions for 24 hours, then heated at 120°C for 12 hours to produce a range of alkali-modified supports. The modified, dried material was then added to an IWI volume containing 100 mM NH4FeEDTA as prepared in Example 2. The impregnated catalysts were dried in partially covered containers under ambient conditions for 24 hours and then under dynamic vacuum (~20 mTorr) for 12 hours.The dried catalysts were heated from room temperature to 550°C at a temperature rise rate of 10°C / min in still ambient air. Examples 20-22
[0070] Catalysts were protected with catalytic iron(III) cations at ~0.5 Fe·nm -2and prepared with sodium promoter cations at different loading densities. Cerium oxide powder was added to an IWI volume of 100, 200, or 300 mM NaHCO3, and the modified substrates were dried in a partially covered container for 24 hours under ambient conditions, then heated to 120°C for 12 hours. The modified substrates were then added to an IWI volume of 200 mM NH4FeEDTA as prepared in Example 2. The impregnated materials were dried in partially covered containers under ambient conditions for 24 hours and then under dynamic vacuum (~20 mTorr) for 12 hours. The dried catalysts were heated from room temperature to 550°C in still ambient air at a temperature ramp rate of 10°C / min. Examples 23-30
[0071] Catalysts were prepared with protected catalytic copper(II) cations and sodium promoter cations in a single solution. Cerium oxide powder with a surface area of 101 m 2 ·G -1 was added to a humidified volume determined by N2 physisorption containing 100, 200, or 300 mM Na2CuEDTA purchased from Sigma. The impregnated materials were dried for 24 hours in partially covered containers under ambient atmosphere and then for 12 hours under dynamic vacuum (~20 mTorr). Since the solubility of Na2CuEDTA limited the loading density from a single impregnation to approximately 0.6 Cu·nm -2 limited, multiple impregnation and drying steps were used to achieve higher densities. The dried catalysts were heated from room temperature to 550°C in still ambient air at a temperature ramp rate of 10°C / min. Examples 31-33
[0072] CeO2 / ZrO2 powder with a surface area of 108 m 2 ·G -1was added to a KHCO3 IWI volume. The impregnated material was dried in a partially covered container under ambient conditions for 24 hours, then heated at 120°C for 12 hours to generate the alkali-modified substrate. The promoter cation-modified substrate was added to a humidified volume containing 200 mM (NH4)2CoEDTA. The impregnated material was dried in partially covered containers for 24 hours under ambient conditions and then for 12 hours under dynamic vacuum (~20 mTorr). Otherwise equivalent catalysts were prepared using protected catalytic iron(III) or copper(II) cations instead of cobalt cations. Stoichiometric ratios of promoter cations to catalytic cations were 1:1 for the iron(III) and cobalt-containing catalysts and 2:1 for the copper(II)-containing catalyst. The loading density of catalytic cations was ~0.4 cations per nm2 , equivalent to about 0.4 wt%. Table 1: Properties of the materials discussed in Examples 4-31 Example Catalytic cation Promoter cation Catalytic cation loading density Cat. / Prom. Vorläufer Vorläufer Gew.-% µmol·g -1 Atom·nm -2 Verhältnis 4 Fe(NO3)3 NaHCO3 0,43 82 0,49 1:1 5 Fe(NO3)3 NaHCO3 0,87 164 0,98 1:1 6 Fe(NO3)3 NaHCO3 1,35 255 1,52 1:1 7 NaFeEDTA N.A. 0,18 32 0,19 1:1 8 NaFeEDTA N.A. 0,34 60 0,36 1:1 9 NaFeEDTA N.A. 0,52 92 0,55 1:1 10 NaFeEDTA N.A. 0,53 94 0,56 1:1 11 NaFeEDTA N.A. 0,81 145 0,87 1:1 12 NaFeEDTA N.A. 1,16 207 1,23 1:1 13 NaFeEDTA N.A. 1,38 246 1,47 1:1 14 NH4FeEDTA Kein Vorläufer 0,23 41 0,24 1:0 15 NH4FeEDTA Kein Vorläufer 0,48 86 0,51 1:0 16 NH4FeEDTA LiOH 0,22 40 0,27 1:1 17 NH4FeEDTA NaHCO3 0,23 41 0,27 1:1 18 NH4FeEDTA KHCO3 0,23 42 0,28 1:1 19 NH4FeEDTA CsHCO3 0,22 39 0,26 1:1 20 NH4FeEDTA NaHCO3 0,47 83 0,50 2:1 21 NH4FeEDTA NaHCO3 0,49 87 0,52 1:1 22 NH4FeEDTA NaHCO3 0,49 87 0,52 2:3 23 Na2CuEDTA N.A. 0,23 36 0,22 1:2 24 Na2CuEDTA N.A. 0,31 49 0,29 1:2 25 Na2CuEDTA N.A. 0,36 57 0,34 1:2 26 Na2CuEDTA N.A. 0,61 96 0,57 1:2 27 Na2CuEDTA N.A. 0,54 86 0,51 1:2 28 Na2CuEDTA N.A. 0,89 139 0,83 1:2 29 Na2CuEDTA N.A. 1,21 191 1,14 1:2 30 Na2CuEDTA N.A. 1,51 236 1,41 1:2 31 NH4CoEDTA KHCO3 0,42 71 0,4 1:1 Examples 34-35 UV-vis in diffuse reflection
[0073] Catalysts prepared according to Examples 4-13 were analyzed by diffuse reflectance UV-visible (DRUV-vis) spectroscopy to assess the coordination chemistry of catalytic cations on substrate surfaces as a function of the loading density of catalytic cations and the protected or unprotected nature of the catalytic cations. It is expected that isolated Fe 3+ -ions absorb below 300 nm, two-dimensional surfaces absorb between 300 nm and 500 nm, and three-dimensional crystallites absorb above 500 nm. Bands associated with isolated Fe 3+are masked by the dominating absorption of CeO2 below 350 nm, while bands corresponding to two-dimensional sheets and three-dimensional crystallites may appear as a shoulder on the CeO2 band or as a peak centered at λ > 500 nm, respectively.
[0074] DRUV-vis experiments were performed on a Shimadzu 3600 UV-vis-NIR spectrometer equipped with a Harrick-Praying-Mantis diffuse reflectance attachment and PTFE as the baseline standard. All materials were diluted 1:5 in PTFE and ground with a mortar and pestle before spectra were recorded. Diffuse reflectance spectra were converted to pseudoabsorption spectra using the Kubelka-Munk transformation (Kubelka et al., Z. Tech. Phys. 12, 593-6011 (1931)).
[0075] Representative DRUV-vis spectra are shown in the Fig. 4A and Fig. 4B for catalysts with integrated sodium promoter cations and with different loading densities of catalytic iron(III) cations, where the thin lines are the catalysts and the thick lines are cerium oxide substrate as reference. Fig. The catalysts shown in Figure 4A were prepared according to non-inventive examples 4-6, while those shown in Fig. 4B were prepared according to Examples 7-13. The spectra of Fig. 4A exhibit a minimal shoulder on the ceria peak below 500 nm and virtually none above 500 nm, even at the highest iron(III) loading densities. This indicates that unprotected catalytic cations are predominantly integrated into the catalyst as isolated ions or small clusters.
[0076] The spectra of Fig. 4B have a shoulder below 500 nm even at the lowest loading densities of catalytic cations. At the highest loading densities, especially above 0.6 catalytic cations per nm 2 , the spectra in Fig. 4B shows large shoulders below 500 nm and a significant absorption above 500 nm. This indicates that the use of protected catalytic cations in the catalyst preparation process improves the incorporation of catalytic cations into two-dimensional sheets and, at high loading densities, into three-dimensional crystallites. Examples 36-40 Temperature-programmed reduction
[0077] Temperature-programmed reduction (TPR) experiments were performed on catalysts prepared according to Examples 4-13 to evaluate the reduction of catalytic cations (H2O release) for catalysts prepared with protected versus unprotected catalytic cations. Monomeric catalytic cation structures that strongly interact with the substrate oxide support are expected to be reduced at a higher temperature than agglomerates, which bear a stronger resemblance to bulk oxides of catalytic cations. For example, isolated iron(III) cations are expected to be reduced between 600°C and 700°C, while two-dimensional sheets and three-dimensional crystallites are expected to be reduced at approximately 400–500°C and 300–400°C, respectively.
[0078] TPR experiments were performed on a TA Instruments Q500 TGA equipped with a Pfeiffer Thermostar Q200 process mass spectrometer. The compositions were analyzed at a temperature gradient of 10°C min -1 under a flow of 90% O2 / 10% He at 100 standard cubic centimeters per minute (sccm) and held for 15 minutes. The heat-treated samples were cooled in 100 sccm He to a temperature close to ambient temperature before being heated to 10°C min -1 in 100 sccm of 4.5% H2, 4.5% Ar, 91% He were heated to 550°C. The resulting water signal was normalized against the constant argon signal and calibrated against a copper(II) oxide reference standard.
[0079] Representative TPR samples are shown in the Fig. 5A, Fig. 5B. Those in Fig. 5A originate from catalysts prepared according to non-inventive examples 4-6, while those in Fig. 5B originate from catalysts prepared according to Examples 7-13. In the Fig. 5A, Fig. In Figure 5B, the thick line represents a scan of the substrate only, while the thin lines represent scans of catalysts at different loading densities of catalytic cations. Scans of catalysts are separated from the substrate scans for clarity. Catalysts prepared using protected catalytic cations, as in Fig. 5B, show strong increases in the water produced with increased loading density of catalytic cations, especially at about 300-400°C. Catalysts prepared using unprotected catalytic cations, as in Fig. 5A, show much smaller increases in oxygen produced even at high loading densities.
[0080] The Fig. 6A, Fig. Figure 6B shows TPR peak deconvolution and assignment for catalysts prepared according to Examples 9 and 12, respectively. The thin solid line indicates the data acquired for the catalyst, while the dashed line shows the background TPR scan of the ceria substrate. The dashed line(s) indicate new, deconvoluted peaks representing the difference between the TPR of the catalyst and the substrate. The thick solid line shows the calculated background spectrum plus the peak at 400°C, as well as its close agreement with the acquired spectrum. Fig. Figure 6A shows only a single unfolded peak centered at about 400°C, while Fig. 6B has a much broader unfolded peak centered at approximately 400°C and a second unfolded peak centered at approximately 325°C. Due to its lower temperature and its presence only in catalysts prepared with high loading densities, the reduction process centered at approximately 325°C is assigned to the reduction of catalytic iron(III) cations in three-dimensional aggregates. The reduction process centered at approximately 400°C is assigned to the reduction of catalytic iron(III) cations in two-dimensional sheets.
[0081] Fig. Figure 7 is a graph of the total oxygen produced as a function of the loading density of catalytic Fe 3+-cations for catalysts prepared using protected cations (solid line) and unprotected catalytic cations (dashed line). The slope of the solid line, 0.23 mol H2O per mol catalytic Fe 3+ -cation, corresponds to a reduction of 45% of the catalytic cations in the catalyst prepared using protected catalytic cations over the temperature range of the TPR (since for each H2O molecule produced, two Fe 3+ -cations must be reduced). In contrast, the slope of the dashed line corresponds to 0.11 mol H2O per mol catalytic Fe 3+ -cation, a reduction of only 22% of the catalytic cations in the catalyst prepared using unprotected catalytic cations over the TPR temperature range.
[0082] Taken together, these results indicate that the use of protected catalytic cations in the process results in a catalyst with catalytic cations bound in lower proportions as isolated ions and in higher proportions in two-dimensional sheets. The results further indicate that increasing the inventory of two-dimensional sheets results in a larger proportion of catalytic cations available for reduction within the tested temperature range. Examples 41-44 Fe 3+ ⇌ Fe 2+ Redox cycling
[0083] Several TPR cycles (i.e., redox cycles) were performed on catalysts prepared according to Examples 4-13. This allowed an assessment of the redox cyclability of catalytic cations, and in particular of catalytic cations bound to substrate surfaces in different geometries.
[0084] Samples were analyzed as in the TPR experiments (Examples 31-35) with the following additional steps. After the initial TPR scan, the samples were cooled in 100 sccm of helium to near ambient temperature and then oxidized, cooled, and gradually reduced a second time, as in the initial TPR experiment.
[0085] The Fig. 8A, Fig. Figure 8B shows TPR scans of first and second reductions at two loading densities of catalytic cations for catalysts prepared using unprotected catalytic cations and protected catalytic cations, respectively. Fig. As can be seen in Figure 8A, the second reduction was similar to the first reduction for catalysts prepared using unprotected catalytic cations, except that the reduction feature centered at about 400°C was shifted to about 380°C. As shown in Fig. As can be seen in Figure 8B, the second reduction was essentially equal to the first reduction for catalysts prepared using protected catalytic cations when the catalytic cations were incorporated at low loading densities. At high loading densities, however, the reduction process centered at approximately 325°C, which is attributed to the reduction of catalytic cations incorporated into three-dimensional crystallites, fails completely. This indicates that it is relatively impossible for catalytic cations incorporated into three-dimensional crystallites to undergo redox cycling, which may be the case for bulk oxides.
[0086] Also in Fig. 8B, it can be observed that the 400 / 380°C reduction process in the second TPR cycle for the catalyst prepared according to Example 12 decreased by about 42%. Fig. 9A, Fig. 9B illustrate the loss of catalytic cations that can undergo a second reduction in catalysts prepared using protected catalytic cations with high loading densities. It should be noted that in the catalysts of Fig. 9B, prepared using protected catalytic cations at a low to moderate loading density according to Examples 7, 10 and 11, the proportion of catalytic cations capable of undergoing multiple oxidation / reduction cycles under conditions where the reduction temperatures do not exceed 550°C is about 45%. Examples 45-49 X-ray spectroscopy
[0087] X-ray absorption spectroscopic experiments were performed on catalysts prepared according to Examples 4, 9, 10 and 12 to evaluate the oxidation state as a function of temperature and surface geometry of catalytic cations at different loading densities and for unprotected or protected catalytic cations.
[0088] X-ray near-edge absorption (XANES) spectroscopy experiments were conducted at the D-beamline of the DuPont-Northwestern Collaborative Access Team (DND-CAT) deflection magnet at Sector 5 of the Advanced Photon Source, Argonne National Laboratory. Incident and transmitted intensities were measured using Canberra ionization chambers. Beam energies were calibrated against Fe metal foil measured in transmission, and its K-edge was set to 7112 eV. FeO and Fe2O3 standards were coated on Kapton tape, and their spectra were also measured in transmission.
[0089] Supported Fe materials were pressed into 50 mg pellets with a diameter of 2.5 cm. Individual pellets were mounted on a heated stainless steel cell designed for transverse gas flow and sealed with a rear Be window and a front Kapton window. The empty space between the two windows was filled with quartz wool before placing the pellet to ensure its adherence to the front Kapton film during the experiments. Due to the low Fe content of the pellets, spectra were measured as fluorescence intensity using a four-channel SII Vortex ME4 detector. Samples were mounted at an incidence angle of θ=45x to the beam and detector, which were perpendicular to each other. Before starting the temperature program, the pellets loaded into the sample holder were compared with those of the corresponding powder materials coated on Kapton tape and also measured as fluorescence intensity.
[0090] Subsequently, the transverse flow of 50 sccm of 3.5% H2 and the balance He began. The heated flow cell was held at ambient temperature, 150°C, 250°C, 340°C, and 430°C for two hours each while spectra were recorded. Temperatures are measured inside the cell. Between residence times, the temperature was maintained at ~10 °C min -1 booted up.
[0091] Fig. Figure 10 shows representative XANES spectra of four different catalysts, each analyzed over a temperature range of 20–430°C. Dashed black lines indicate reference spectra of iron and iron(III) oxide. All tested materials exhibited stronger pre-edge features of the bulk oxides, which is characteristic of undercoordinated iron species. The pre-edge features decreased in intensity for catalysts prepared using protected catalytic cations, indicating a reduced dispersion of catalytic cations on substrate surfaces. The pre-edge feature is also stronger for the catalyst prepared using unprotected catalytic cations ( Fig. 10D), compared to the catalyst prepared using a protected catalytic cation at a similar loading density ( Fig. 10B).
[0092] Fig. Figure 11 shows the fraction of Fe species present as iron(III) or iron cation at different temperatures for a catalyst prepared using unprotected catalytic cations and for a catalyst prepared using protected catalytic cations. The fraction of Fe species present as iron(III) or iron cation under each condition was determined by linear interpolation of the spectra in Fig. 10 between the iron and iron(III) oxide reference spectra. The results agree almost exactly with the fractional reduction determined by TPR. In particular, the results show a larger fraction of reducible iron(III) species for the catalyst prepared using protected catalytic cations. Examples 50-55 Catalytic reduction of NO by H2
[0093] Kinetic measurements of nitric oxide reduction reactions were performed using hydrogen gas as the reducing agent and in the presence of catalysts prepared according to Examples 4-30 to evaluate the catalytic efficiency of catalysts as a function of the identity of catalytic cations, the protected or unprotected nature of catalytic cations, the identity of promoter cations, and the loading density.
[0094] NO reduction by H2 was carried out at atmospheric pressure in a quartz U-tube reactor (OD 1 / 4", ID 1 / 8") loaded with 25 mg of catalyst diluted in 0.50 g of non-porous quartz sand previously calcined at 600°C, packed in descending flow between beds of quartz wool. The U-tube reactor was lowered into a vertical tube furnace (ID 2.5"), and a thermocouple placed at the top of the catalyst bed was used to control and record the bed temperature. The thermocouple and quartz diluent showed no catalytic activity in control experiments. The reactor inlet was connected to a gas manifold, and the outlet to a Pfeiffer Thermostar mass spectrometer. The reactor was then fed with 50 sccm of 3.3% NO, 3.3% H2, 3.3% Ar, 90% He and heated to 10°C min -1heated to 150°C, 250°C, 350°C, 450°C, and 550°C and held at each temperature for 1 h. Within 20 minutes at 150°C, a complete disappearance of signals corresponding to atmospheric N2, O2, H2O, and CO2, as well as surface H2O, was observed.
[0095] Fig. Figure 12 shows the amounts of NH3 and N2 product produced by a catalyst prepared using protected catalytic cations and a catalyst prepared using unprotected catalytic cations. A reaction temperature of 450°C demonstrated high specificity for N2 production and showed large differences between catalysts prepared using protected catalytic cations compared to catalysts prepared using unprotected cations, and was thus used for future catalytic reduction experiments.
[0096] Fig. Figure 13A shows the reaction rates of NO reduction for catalysts prepared according to Examples 4-13. Substrates coated with 0, 0.25, 0.5, or 0.75 sodium promoter cations per nm 2loaded, but not with catalytic cations. The results are consistent with the TPR experiments, showing that catalysts prepared with protected catalytic cations generally catalyze NO reduction at a higher rate than comparable catalysts prepared with unprotected catalytic cations. Furthermore, for the catalyst prepared with protected catalytic cations, a plateau in activity at the highest loading densities is consistent with the TPR results. Substrates loaded with promoter cations, but not with catalytic cations, all exhibited the same activity as pure ceria, indicating that no promoter effect is present in the absence of catalytic cations. A star symbol on the y-axis of the Fig. Figure 13A shows the corresponding reaction rate catalyzed by a reference catalyst consisting of 1 wt% platinum (Pt) on alumina.
[0097] In Fig. In Figure 13B, the conversion frequency is calculated based on the fraction of reducible iron(III) species determined by TPR. The conversion frequency of catalytic sites in a platinum-based catalyst is represented by an asterisk. The results show that the conversion frequency is stable across loading densities and comparable to that of a platinum-based catalyst.
[0098] Fig. Figure 14 shows the reaction rate for various catalysts prepared using protected catalytic cations, with several alkali metals employed as promoter cations. The results indicate that the alkali metals employed as promoter cations are comparatively effective. All alkali promoter cations increase the reaction rate by approximately 30% when used in a 1:1 ratio to the protected catalytic cation, relative to the catalyst prepared using protected catalytic cations without the optional promoter cations. This similarity indicates that the effect of promoter cations is most likely not electronic but may be steric.Without being bound by any particular theory, one possible explanation for the uniform effect of different promoter cations is that the promoter cations occupy isolated sites on substrate surfaces, effectively blocking such isolated sites and hindering unproductive occupation by catalytic cations. In such a model, catalytic cations would then tend to aggregate on the substrate surface into two-dimensional sheet structures or, at high loading densities, into three-dimensional crystallites.
[0099] Fig. Figure 15 shows reaction rates catalyzed by catalysts prepared according to Examples 14, 19-21. These catalysts were prepared using protected catalytic iron(III) cations coated with ~0.5 Fe nm -2 were applied, with loading densities of sodium promoter cations ranging from 0 to ~0.75 Na·nm -2The results indicate a linear dependence of the reaction rate on the promoter cation loading density over the density range investigated.
[0100] In Fig. 16 shows reaction rates for a series of similar catalysts. The catalysts of the Fig. 16 were prepared using protected catalytic copper(II) cations. As can be seen from a comparison of the Fig. 16 to Fig. 12, the catalysts prepared using protected catalytic copper(II) cations are somewhat superior to those prepared using protected catalytic iron(III) cations. Without wishing to be bound by any theory, this may be due to an inherently better performance of copper(II) cations or the use of higher amounts of promoter cations due to the precursor used. As shown in Fig. As can be seen in Figure 17, the catalyst prepared using protected catalytic copper(II) cations also shows a rate plateau at high loading densities, although the plateau occurs at lower densities compared to similar catalysts prepared using protected catalytic iron(III) cations (cf. Fig. 17 to Fig. 13A). Examples 56-58 Comparison with cobalt
[0101] The results of NO reduction reaction rate measurements for the three catalysts at three temperatures are shown in Fig. 18. As shown in Fig. As shown in Figure 18, the catalyst prepared using protected catalytic cobalt(III) cations catalyzed the reaction at a similar rate to that of the catalysts prepared using protected catalytic iron(III) or copper(II) cations. Examples 59-63 Carbon monoxide and propylene as reducing agents
[0102] NO reduction activity using carbon monoxide as the reducing agent was measured for catalysts prepared essentially according to Examples 10, 11, and 13, but with slightly different loading densities (0.54, 0.89, and 1.32 wt.%), and for unmodified CeO2 substrate. Reaction and monitoring conditions were similar to those of Examples 50-55, except that the gas flow was 1000 ppm NO, 1000 ppm CO, and the balance HE at a flow rate of 100 sccm. The GHSV (gas hourly space velocity) was kept constant at ~30,000 h -1 The reactions were heated to 250°C, 350°C, 450°C, and 550°C and held at each temperature for ~1 h. A similar reaction was carried out using a catalyst prepared according to Example 13 with 1200 ppm NO, 133 ppm C3H6, and the balance He. The results of the carbon monoxide and propylene experiments are listed in Table 2. Beispiel NO reduction activity in CO (µmol·g Kat -1 s -1 ) 250 °C 350 °C 450 °C 550 °C 10 0,45 1,77 3,13 5,32 11 0,52 1,99 3,41 5,38 13 0,58 2,40 4,14 6,86 Substrat 0,03 0,43 0,99 2,79 NO reduction activity in C3H6 (µmol·g Kat -1 s -1 ) 13 0,00 0,00 0,81 3,09
[0103] The above description refers to the embodiments which, according to current assessment, are most practical.
Claims
[1] Catalyst comprising: a substrate containing cerium oxide; catalytic cations bound to substrate surfaces; and promoter cations bound to substrate surfaces; wherein the catalytic cations consist of iron, copper, cobalt or a combination thereof and the promoter cations consist of alkali metal cations or alkaline earth metal cations or a combination thereof, and the catalytic cations have a loading density of 0.1-1.5 wt.% and the promoter cations are present in a stoichiometric ratio to the catalytic cations ranging from 1:2 to 6:1 inclusive. [2] A catalyst according to claim 1, wherein at least 30% of catalytic cations are capable of undergoing two or more reduction / oxidation cycles at reduction temperatures not exceeding 550°C. [3] A catalyst according to claim 1 which catalyzes the reduction of nitrogen monoxide. [4] A catalyst according to claim 1 which catalyzes the reduction of nitrogen monoxide by carbon monoxide or propylene. [5] A catalyst according to claim 1, which catalyzes the reduction of nitrogen monoxide by hydrogen gas. [6] The catalyst of claim 1 having an N2 selectivity of greater than about 67%. [7] The catalyst of claim 1 having an N2 selectivity of greater than about 90%. [8] A process for producing a catalyst comprising: contacting a cerium oxide-containing substrate with a solution containing catalytic cations; and contacting the substrate with a solution containing promoter cations; wherein the catalytic cations consist of iron, copper, cobalt or a combination thereof and the promoter cations consist of alkali metal cations or alkaline earth metal cations or a combination thereof, and the solution containing catalytic cations comprises at least one chelating agent. [9] The method of claim 8, wherein contacting a substrate with a solution containing catalytic cations is repeated at least once. [10] The process of claim 8, wherein the promoter cations consist of alkali metal cations. [11] The method of claim 8, wherein the at least one chelating agent forms a chelate complex with catalytic cation having a negative net charge. [12] The method of claim 8, wherein the at least one chelating agent comprises EDTA.
Citation Information
Patent Citations
Catalyst, especially for purifying car exhaust gas, comprises a catalytically-active metal such as platinum immobilised on a more base metal such as tin or iron, all on a ceramic support
DE102006047932A1
SUPPORTED CATALYST FOR THE NONSELECTIVE OXIDATION OF ORGANIC COMPOUNDS, PROCESS FOR THE NONSELECTIVE OXIDATION, ESPECIALLY OF ORGANIC COMPOUNDS.
DE68903397T2
Lean NOx trap / conversion catalyst
US20030059358A1
Catalysts for the oxidative reforming of alcohols