Bonding material, bonding process and semiconductor device for electrical energy

A silver-bismuth alloy with a specific bismuth content and heat treatment process addresses the challenge of high heat resistance and stress relief in semiconductor bonding, resulting in a strong, reliable bond for next-generation semiconductor components.

DE112014006349B4Inactive Publication Date: 2024-10-10MITSUBISHI ELECTRIC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
DE112014006349
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2014-12-26
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing bonding materials for semiconductor devices face challenges in achieving both high heat resistance and stress relief, particularly when bonding next-generation semiconductor components like silicon carbide and gallium nitride, which operate at high temperatures, as conventional methods lead to deterioration and reduced bond strength.

Method used

A bonding material composed of a silver-bismuth alloy with a bismuth content between 1 to 5% by weight is used, combined with a heat treatment process at 150°C to 300°C for 10 to 100 hours, promoting a solid phase diffusion reaction to form diffusion layers, enhancing both heat resistance and stress relief.

Benefits of technology

The silver-bismuth alloy achieves a strong, reliable bond that maintains heat resistance and stress relief capabilities, even under high temperature cycling, ensuring the longevity and efficiency of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0001_ABST
    Figure 00000000_0001_ABST
  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
  • Figure 00000000_0002_ABST
    Figure 00000000_0002_ABST
Patent Text Reader

Abstract

Bonding material (1) made from an alloy (1F) containing bismuth and consisting mainly of silver, which, when heated in a state where it is in contact with a metal material as the bonding object, forms a diffusion layer (Ld2, Ld3) of silver in the metal material as a result of a solid-phase diffusion reaction, so that it bonds to the metal material, wherein the bonding material (1) contains not less than 1 wt.% and not more than 5 wt.% bismuth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a sheet-like bonding material whose heat resistance temperature after bonding due to the use of a solid phase diffusion reaction of silver becomes higher than a bond Temperature, as well as a bonding process and a semiconductor device for electrical energy, each of which utilizes it. State of the art

[0002] Recently, there has been an increasing demand regarding the reliability of semiconductor devices for electrical energy. In particular, there is a need to improve the durability and reliability of a bonding area between a semiconductor component for electrical energy and a printed circuit board whose thermal Expansion coefficients between them have a large difference. Until now, semiconductor components for electrical Energy, whose materials are silicon (Si) and gallium arsenide (GaAs). Their operating temperatures range from 100 °C to 125 °C. When these elements are bonded to circuit boards, solder materials are often used.

[0003] From the point of view of saving energy, on the other hand, semiconductor components for electrical energy, whose Base materials silicon carbide (SiC) and gallium nitride (GaN) are, as next generation devices in a active development. They operate at high currents and have operating temperatures of 175 °C or more, and means that the temperature will reach 300 °C in the future.

[0004] In this context, in the event that the bonding is carried out by the bonding material itself is melted, such as solder, requires that the bonding be carried out at a temperature higher than the Heat resistance temperature of the bonding area, so that not only the number of choices for the bonding material itself, but there are also restrictions to prevent the deterioration of the bond object impede.

[0005] In this context, attention has been paid to a bonding material that is a so-called sinterable Metal or a metal paste in which metal particles of the nano- or micrometer size and a organic solvent are mixed together (see, for example, Patent Document 1).

[0006] The following applies to such a bonding material: If the organic components that form the surfaces of the Metal particles are decomposed by heat, then the metal particles are sintered together to form a Bonding area, and the heat resistance temperature after sintering (bonding) will be a temperature (e.g. 960 °C in the case of silver), which is almost equal to the melting point of the solid metal.

[0007] Although it depends on which organic component is used, the organic solvent is used at approximately 200 °C to 300 °C, so that it is possible to carry out the bonding at a temperature at which the bond object is not deteriorated and to achieve extended heat resistance after bonding.

[0008] As described in Patent Document 1, compared with the solid metal, the metal sintered material a lower modulus of elasticity because it has vacancies.

[0009] Nevertheless, its elastic modulus is still higher compared to conventional solders etc., so that whose stress relaxation capacity decreases during the heat cycle and consequently it is difficult to maintain the bond strength over a long period of time. In this context, a technology has been proposed that which contains metal particles with a lubricating property or fillers of a resin whose elastic modulus is lower than that of the metal particles, are mixed into the bonding material in order to reduce the tensions (see e.g. Patent Document 2 or 3).

[0010] Patent Document 4 discloses electrically and thermally conductive compositions for producing Compounds between electronic elements are described. The compositions have three or more Particle types made of metal or metal alloys and an organic carrier that has an application-specific The first type of particles contains a reactive metal with a high melting point that is mixed with at least one reactive metal with low melting point in the other particles reacts to form intermetallic species. The at least one reactive metal with a low melting point is two different particle shapes. The first reactive metal particle with a low melting point contains a support that facilitates the reaction with the reactive metal with a high melting point. The second reactive Low melting point metal particles serve as a source of the reactive low melting point metal.

[0011] Patent Document 5 describes a brazing material containing one or more main components from the group consisting of Sn, Sb, Zn and Bi and has a melting point of 600°C or less. Bibliography Patent documents Patent Document 1: Japanese Patent Application Laid-Open No. JP 2012-054358 A (para.

[0010] , Fig. 1) Patent Document 2: Japanese Patent Application Laid-Open No. JP 2010-267579 A (para.

[0013] ; Fig. 1) Patent Document 3: Japanese Patent Application Laid-Open No. JP 2011-198674 A (paragraphs

[0010] to

[0013] ); Fig. 1, Fig. 2) Patent document 4: US 2010 / 0 252 616 A1 Patent Document 5: JP S58-6 793 A Summary of the invention Problems to be solved with the invention

[0012] However, it is difficult to make the heat resistance temperature of the resin material higher than the operating temperature which is targeted for the next generation device, and if a high temperature is used, This leads to a decrease in bond strength due to the deterioration of the resin in the bonding material. difficult to achieve a bonding that meets both good heat resistance and the ability to Tension relief.

[0013] The present invention has been conceived to solve the problems described above. Its object is to provide a Bonding that meets both good heat resistance and stress relief capability. Ways to solve the problems

[0014] The problem is solved by a bonding material having the features of claim 1. Advantageous Further developments of the bond material result from subclaims 2 and 3. Furthermore, the solution to the problem by a method having the features of claim 4. Advantageous further developments of the method result from the subclaims 5 to 7. Furthermore, the problem is solved by a semiconductor device with the Features of claim 8. Advantageous developments of the semiconductor device result from the subclaims 9 to 11. Effect of the invention

[0015] Since according to the invention bismuth is added to the silver in a ratio within a specific range it is possible to achieve a bonding that has both heat resistance and the ability to Stress relief is fulfilled. When such bonding is used, it is also possible to achieve a high-temperature compatible and highly reliable semiconductor device for electrical energy. Brief description of the drawings Fig. 1A to Fig. 1C are cross-sectional views - in the respective steps - of a bonding material or a bonding Area to illustrate a bonding process using the bonding material according to Embodiment 1 of the invention. Fig. 2 is a cross-sectional view showing a configuration of a semiconductor device for electric power, which are produced using the bonding material and the bonding method according to Embodiment 1 of the invention is manufactured. Fig. 3A and Fig. 3B are schematic cross-sectional views of the bonding material according to Embodiment 1 of the Invention. EMBODIMENTS OF THE INVENTION Embodiment 1

[0016] Fig. 1 and Fig. 2 are drawings for illustrating a bonding material, a bonding method under Use of the bonding material and a semiconductor device for electrical energy which, using the same, according to embodiment 1 of the invention. Fig. 1 shows cross-sectional views - in the respective Steps - of the bonding material or the bonding area when bonding a semiconductor component for electrical energy to a Printed circuit board using the bonding material, where Fig. 1A is a cross-sectional view showing how a Alloy material is rolled into a thin film form to be used as the bonding material, where Fig. 1B is a cross-sectional view showing the state before bonding objects are bonded together, and where Fig. 1C is a cross-sectional view showing the state of a bonding area after bonding.

[0017] Furthermore, Fig. 2 is a cross-sectional view showing a configuration of a semiconductor device for electric power after bonding (manufactured) using the bonding material and the bonding process.

[0018] Before describing the bonding material and the bonding method using the bonding material, a Configuration of a semiconductor device for electrical energy is described, which is an object in which this are preferably applicable.

[0019] As shown in Fig. 2, a semiconductor device 100 for electric power is one in which vertical Semiconductor components 2A, 2B for electrical energy (collectively referred to as semiconductor components 2 for electrical energy) on the circuit side (the conductor layer 3a) of a DBC plate 3 (DBC: Direct Bonded Copper) as printed circuit board, wherein copper (Cu) conductor layers 3a, 3b are formed on both sides of a base material 3i which is made of silicon nitride (Si N ). 3 4

[0020] On each of the surface electrodes of the semiconductor components 2A, 2B for electrical energy, a connecting conductor 4 is provided as a Wiring material bonded using a sheet-like bonding material 1, which mainly consists of Silver, and their back surfaces are also bonded to the DBC plate 3 using a bonding material 1 bonded. Except for the back surface side (the conductor layer 3b) of the DBC plate 3 and the end side of the connecting conductor 4, which are to be connected to an external circuit, they are everywhere sealed by means of a sealing material 5 sealed so that they are molded into a housing.

[0021] Each semiconductor component 2 for electric power may be an ordinary element using a silicon wafer as its base material. However, in this invention, for the purpose of applying a so-called Semiconductor material with a large band gap, such as silicon carbide (SiC), gallium nitride (GaN) or diamond, whose band gaps are larger than those of silicon, silicon carbide is used as the base material. Examples of the device type include the The following: A switching element, such as an IGBT (insulated gate bipolar transistor) or a MOSFET (metal oxide semiconductor field-effect transistor) and a rectifier element, such as a diode.

[0022] In the case of the MOSFET, a drain electrode on a surface of the semiconductor device 2 is provided for electrical energy formed, which is arranged on the DBC plate 3.

[0023] Furthermore, on a surface on the opposite side of the drain electrode (the top side in the drawing) a gate electrode and a source electrode are formed, which are spatially spaced from each other. For simplification However, the description is made by showing only one source electrode for main electrical energy on the surface on the top.

[0024] The DBC plate 3 has dimensions of 40 mm x 40 mm, its thickness configuration is as follows: Conductor layer 3a with 0.4 mm; base material 3i with 0.3 mm; conductor layer 3b with 0.4 mm. Regarding the drain electrode in the electrodes of the Semiconductor component 2 for electrical energy, the following applies: its surface, which serves as a bonding side to the DBC plate 3 (through the bonding material 1) is covered with gold (Au: surface layer 2f). Furthermore, one surface in these is covered by the Conductor layers 3a, 3b of the DBC plate 3, which serves as a bonding side to the semiconductor component 2 for electrical energy (by the bond material 1) covered with silver (Ag: surface layer 3f).

[0025] Here, the semiconductor device 100 for electric power according to Embodiment 1 of the invention is characterized by the Use of a silver-bismuth alloy (alloy foil 1F) containing between 1 and 5 wt.% bismuth (Bi) as the bonding material 1 for bonding at least the semiconductor component 2 for electrical energy and the printed circuit board (e.g., the DBC board 3) or a wiring material (e.g., the connecting conductor 4). Furthermore, the bonding Method characterized by providing a heat treatment step in which the alloy foil 1F before Bonding is maintained at a temperature of 150 °C to 300 °C for 10 to 100 hours.

[0026] It should be noted that the bonding material 1 is an alloy composed mainly of silver, and which serves to carry out the bonding in such a way that silver components that are closer to their surface that is in contact with the bonding object, cause solid phase diffusion into a metal that is the bonding side of the bond object to form a diffusion layer of silver.

[0027] Consequently, this bonding material 1 does not change its shape before and after bonding. Consequently, In this description, especially when processes are described, there is a case in which ´´alloy Slide 1F'' is indicated when a pre-bonding condition is shown. However, this does not mean that this is different from the bond material 1.

[0028] In order to determine the composition and heat treatment conditions (temperature, holding time) of the bonding material 1 To optimize the performance of the alloys, using the bismuth content as a parameter, they were first tested in a thin-film Form (alloy foils 1F) were prepared, which should be used as bonding materials 1, and the presence / Absence of rolling crack at the time it is formed in the thin film form was evaluated.

[0029] Then, using alloy foils having compositions that do not cause rolling cracks caused the semiconductor component 2 for electrical energy and the DBC plate 3 are actually bonded together, and using these alloy foils 1F to prepare each bonded object 10 (as evaluation sample 10S), as shown in Fig. 1, which was then tested in terms of thermal cycle resistance using a thermal shock tests (heat cycle tests). A detailed description follows. Preparation of alloys (foils)

[0030] Granular silver with a purity of 99.9 wt.% and ground bismuth (needle crystal form) were each weighed using an electronic balance so that the bismuth content (wt%) in the alloy is desired content, and they were placed in a crucible made of quartz glass, where they are heated in the atmosphere using a gas burner or a high frequency induction heating device were melted.

[0031] While the kiln was kept at the melting point of silver or more, they were kept under Using a quartz glass protective tube, so that bismuth was evenly dispersed, and then they were cooled and hardened to prepare each sample alloy 1R. As shown in Fig. 1A, the Sample alloy 1R was subjected to rolling processing to form a thin alloy layer (alloy foil 1F) with a thickness of 50 to 100 µm and a width of 40 mm. Bismuth content

[0032] The evaluation result is set to ´´◯´´ if a rolling crack of 3 mm or more is not present on both End areas of the alloy foil 1F occurred due to the roll processing during the preparation of the alloy foil 1F is, whereas x is set if such a rolling crack has occurred. Six evaluation Samples 10S (Examples 1 to 3, Comparative Examples 1 to 3) were prepared while the bismuth content of 0.5 wt.% to 7 wt.%, and then they were evaluated. The evaluation results are shown in Table 1. It should be noted that with regard to the preparation process of the alloy foils 1F, a layer forming process, a Printing forms, a powder firing process or the like can be applied to it, so that it does not affect the Roll processing is limited. Table 1: Parameter Test result 1 Test object Test condition Evaluation result Bi content [wt.%] Tempering condition Temperature [°C] Time [hours] Rolling Crack H / C Resistance Comparison Example 1 0.5 200 48 ◯ x Example 1 1 200 48 ◯ ◯ Example 2 3 200 48 ◯ ◯ Example 3 5 200 48 ◯ ◯ Comparison example 2 6 200 48 Δ x Comparison example 3 7 200 48 x -

[0033] The result shows that, compared to the same roll processing basis, the following applies: If the Bismuth content ranges from 1 to 5 wt%, as shown by 0.5 wt% (Comparative Example 1), 1 wt% (Example 1), 3 wt% (Example 2) and 5 wt.% (Example 3) as an example, no rolling crack occurred, so that an excellent result (◯) was obtained.

[0034] When the bismuth content was 6 wt% (Comparative Example 2), which is higher than 5 wt%, a rolling crack of approximately 3 mm, which is approximately the same as that of the reference, so that Δ is indicated. If the Bismuth content is 7 wt.% (Comparative Example 3), then a rolling crack of more than 3 mm occurred, so ´´x´´ is indicated, and consequently no excellent result could be obtained.

[0035] Next, with the exception of the alloy foil 1F with the bismuth content of 7 wt.% (Comparative Example 3), which caused the rolling crack, the alloy foils 1F with the bismuth content of 0.5 to 5 wt.% each of a Tempering (heat) treatment under a nitrogen atmosphere at 200 °C for 48 hours.

[0036] As shown in Fig. 1B, the alloy foils 1F were then placed between the Semiconductor component 2 for electrical energy, which is made of SiC (0.3 mm thick x 5 mm x 5 mm) and whose surface was covered with gold (surface layer 2f) and the DBC plate 3 (in the drawing only a part of the conductor layer is 3a) whose surface to be bonded was provided with a silver coating (the surface layer 3f was formed).

[0037] In this state they were placed in a reducing atmosphere in formic acid and from ambient temperature, and when they reached the bonding temperature of 300 °C, the temperature immutable and maintained for 10 minutes as a bonding period while pressed at 10 MPa.

[0038] Due to such heating and pressing, it is possible to promote: A solid phase Diffusion reaction between the gold of the surface layer 2f as an electrode of an element and the alloy foil 1F (Formation of a diffusion layer Ld2 due to solid phase diffusion of silver contained in the alloy into the gold of the electrode of the element); and a solid-phase diffusion reaction between the silver of the surface layer 3f the DBC plate 3 and the alloy foil 1F (formation of a diffusion layer Ld3 due to diffusion of silver, which contained in the alloy, into the silver on the sides of the DBC plate 3). After this holding, the pressing interrupted, followed by cooling to thereby obtain each of the evaluation samples 10S (Examples 1 to 3, Comparative examples 1 to 2).

[0039] Then the evaluation samples 10S were placed in a heat cycle device and subjected to a thermal shock test under the condition of -55 °C x 30 min / 200 °C x 30 min.

[0040] At the time when the thermal shock cycles reached 1000 cycles, the evaluation samples 10s from the device and an observation of the diagonal cross-section of the component (observation length: 10 mm x √2 ≈ 14 mm) to measure the crack length at the edge of the bond area.

[0041] If a crack occurs at the bonding area, the heat dissipation capability at that point is impaired, and Therefore, a crack length that affects the heat dissipation ability in practical use is considered to be 1.4 mm which corresponds to 10% of the total length of 14 mm. Furthermore, the thermal cycle resistance (in the table: ´´H / C resistance´´) was evaluated as ´´x´´ if the crack length was 1.4 mm or more, and as ◯ if it was less than 1.4 mm.

[0042] If the bismuth content is 1 wt.% (Example 1), 3 wt.% (Example 2) or 5 wt.% (Example 3), i.e. in the range from 1 to 5 wt%, then the crack extension was less than 1.4 mm and therefore excellent (◯). When the bismuth content is 0.5 wt% (Comparative Example 1), which is less than 1 wt%, the crack expanded 1.4 mm or more, resulting in an ´´x´´, and also when it is 6 wt.% (Comparative Example 2), which is more than 5 wt%, then the crack extended 1.4 mm or more, resulting in an ´´x´´. It is thought that the The reason for this is the following: If the bismuth content is in the range of 1 to 5 wt.%, then bismuth, which is silver is added to finely divide the silver crystal grains, thus improving ductility.

[0043] Furthermore, it is considered that if the annealing treatment is applied to the Ag-Bi alloy foil 1F before bonding applied, this eliminates the work hardening that occurred at the time of rolling and that this further reduces the Silver crystal grains and a partially precipitated bismuth-rich precipitation phase accelerated so that they are finely dispersed are to increase the crystal grain boundaries, which promotes grain boundary slippage, so that promoting the Softening and improving ductility can be achieved.

[0044] Typical cross-sectional views of the bonding material are shown in Fig. 3. In Fig. 3, Fig. 3A shows the Cross-sectional view before annealing and in Fig. 3B after annealing. Furthermore, the area with white paint the bismuth-rich precipitate phase X, and the black color indicates a base material (Ag) phase Y. To measure the The imaging software ´´ImageJ´´ was used to determine the grain size of the bismuth-rich precipitate phase X.

[0045] In particular, the cross-sectional view was binarized to thereby reveal the bismuth-rich precipitate phase X in white color, and then the area was enclosed with white color, and its area S was calculated according to a scale that was previously estimated. From the area S thus obtained, a grain size L was calculated based on the calculated using the following formula: S = πx(L / 2)2 S: Area; L: Grain size of the bismuth-rich precipitate phase L = √(4× S / π)

[0046] When the bismuth content is between 1 and 5 wt.%, the grain size of the bismuth-rich precipitate was Phase X between 3 and 8 µm before annealing (Fig. 3A), but between 0.2 and 1.0 µm after annealing (Fig. 3B), and It is assumed that the above mechanism is also supported by this fact.

[0047] Since silver has a thermal conductivity higher than that of bismuth, it is preferable from the standpoint bismuth to increase thermal conductivity. However, for example, the thermal conductivity of a tin-based (Sn) or lead-based (Pb) solder material is approximately 50 W / m·K, and the thermal conductivity of pure Silver is approximately 420 W / m·K.

[0048] When measured using an optical AC method at BETHEL Co., Ltd. JAPAN, the alloy 1F, whose bismuth content is between 1 and 5 wt.%, a thermal conductivity in Range of approximately 150 to 300 W / m·K, ensuring that the alloy has an approximately three times higher thermal conductivity than the solder and is therefore a superior material in heat dissipation capacity. Heat treatment conditions (temperature)

[0049] Next, an optimal temperature value for tempering treatment was investigated. The sample alloys 1R, whose bismuth content was adjusted between 1 and 5 wt.%, were rolled into the alloy foils 1F and then subjected to heat treatment using an annealing temperature as a parameter, while the annealing time was set to 48 hours, which is the same as the one above. Then, according to a similar processing as the above eight evaluation samples 10S (Examples 4 to 7, Comparative Examples 4 to 7) and their crack Expansion levels were evaluated by cross-sectional analysis after the heating cycles. Evaluation results are shown in Table 2. Table 2: Parameter Test result 2 Test object Test condition Evaluation result Bi content [wt.%] Tempering condition Temperature [°C] Time [hours] Rolling Crack H / C Resistance Comparison example 4 1 140 48 ◯ x Example 4 1 150 48 ◯ ◯ Example 5 1 300 48 ◯ ◯ Comparison example 5 1 320 48 ◯ x Comparison example 6 5 140 48 ◯ x Example 6 5 150 48 ◯ ◯ Example 7 5 300 48 ◯ ◯ Comparison example 7 5 320 48 ◯ x

[0050] From the evaluation results of Example 4 and Example 6, in which the tempering temperature was set to 150 °C and Example 5 and Example 7, where it is set to 300 °C, the crack extension was less than 1.4 mm in the area, where the tempering temperature was between 150 °C and 300 °C, resulting in a ´´◯´´. Meanwhile, when the tempering temperature is 140 °C (Comparative Example 4, Comparative Example 6), which is lower than 150 °C, then the crack expanded by 1.4 mm or more, as the softening due to structural refinement the Ag-Bi alloy was not accelerated and consequently the stress relief capacity was low, resulting in a ´´x´´ led.

[0051] When the tempering temperature is 320 °C (Comparative Example 5, Comparative Example 7), which is higher than 300 °C, then the crack expanded by 1.4 mm or more, resulting in an ´´x´´, presumably because instead of a fine- dispersing effect, a coarsening of the crystal grains of bismuth occurred due to the heat, and so It had the effect of preventing grain boundary slippage, so that the stress relief capacity was lower. According to this result, it is ensured that there are suitable values ​​(range) for the tempering temperature, and for the In the case of Ag-Bi alloys, whose bismuth content is between 1 and 5 wt.%, the suitable values ​​are between 150 °C and 300 °C. Heat treatment conditions (time)

[0052] Next, an optimal value for the treatment time for tempering was investigated. The sample alloys 1R, whose bismuth content was adjusted between 1 and 5 wt.%, were rolled into the alloy foils 1F and then subjected to a heat treatment using time as a parameter, at each of the tempera- Upper limit and lower limit temperatures described above.

[0053] Then, according to a similar processing as the above nineteen evaluation samples 10S (Examples 8 to 19, Comparative Examples 8 to 14) were prepared, and their crack expansion degrees were determined by cross-sectional analysis according to the heating cycles. The evaluation results are shown in Table 3. Table 3: Parameters Test result 3 Test object Test condition Evaluation result Bi content [wt.%] Tempering condition Temperature [°C] Time [hours] Rolling Crack H / C Resistance Comparison example 8 1 150 8 ◯ x Example 8 1 150 10 ◯ ◯ Example 9 1 150 30 ◯ ◯ Example 10 1 150 100 ◯ ◯ Comparison example 9 5 150 8 ◯ x Example 11 5 150 10 ◯ ◯ Example 12 5 150 30 ◯ ◯ Example 13 5 150 100 ◯ ◯ Comparison example 10 1 300 8 ◯ x Example 14 1 300 10 ◯ ◯ Example 15 1 300 30 ◯ ◯ Example 16 1 300 100 ◯ ◯ Comparison example 11 5 300 8 ◯ x Example 17 5 300 10 ◯ ◯ Example 18 5 300 30 ◯ ◯ Example 19 5 300 100 ◯ ◯ Comparison example 12 5 300 8 ◯ x Comparison example 13 1 300 120 ◯ x Comparison example 14 5 300 120 ◯ x

[0054] At a tempering temperature of 150 °C or 300 °C, the following applies: If the tempering time is set to 10 hours (Example 8, Example 11, Example 14, Example 17), if it is set to 30 hours (Example 9, Example 12, Example 15, Example 18) and when it is set to 100 hours (Example 10, Example 13, Example 16, Example 19), ie if the tempering time is in the range between 10 and 100 hours, then the crack Expansion less than 1.4 mm, resulting in a ´´◯´´.

[0055] When the annealing time is set to 8 hours (Comparative Example 8, Comparative Example 9, Comparative Example 10, Comparative Example 11), which is shorter than 10 hours, then the crack extended over 1.4 mm or more, because the Softening was not accelerated due to the structural refinement of the Ag-Bi alloy and consequently the Voltage relief capacity was low, resulting in an ´´x´´.

[0056] In the case where the temperature for the annealing treatment was 300 °C, which is the upper limit of the temperature range, when the sample was kept for 120 hours, which is beyond the above time range, the stress relief capacity was lower, and consequently the crack extended for 1.4 mm or more, resulting in an ´´x´´. It is suspected that the reason for this is not a fine-dispersing effect a coarsening of the crystal grains of bismuth occurs as a result of heat, and that this acts in such a way that it Prevents grain boundary slippage.

[0057] It should be noted that in this temperature range, the following applies: If the temperature is lower than 300 °C, It was confirmed that the thermal cycle resistance and crack resistance are given as ´´◯´´, respectively, and up to a holding time of 100 hours. However, it is unknown what extent of fine-dispersing effect for the case of a time that is longer.

[0058] However, in mass production processes it is desirable that the treatment is as short as possible so that If the tempering treatment takes 100 hours (approximately 4 days) or more, they are considered mass manufacturing process is unsuitable from the perspective of cycle time.

[0059] If it is ensured that the crack resistance is in the treatment range up to 100 hours, There is no problem with mass production. According to this result, the period for tempering Treatment ensures that in the case of tempering treatment at 150 °C to 300 °C for the Ag-Bi alloy, whose Bismuth content is between 1 and 5 wt.%, excellent results can be obtained if it is used for 10 to 100 hours suffices.

[0060] Regarding the bonding conditions, the bonding atmosphere, the bonding temperature, the applied pressure and the Holding time is mainly given as a parameter. In the aforementioned parameter test, a reducing Atmosphere with formic acid is used as the bonding atmosphere. However, a reducing atmosphere with be hydrogen.

[0061] Regarding the bonding temperature, it only has to be a temperature that allows a solid-phase diffusion reaction between the metal covering the bonding surface of the bonding object and the Ag-Bi alloy, and, although it is based on 300 °C in the parameter test, a similar effect can be obtained if it is in the range of 250 ° C to 300 °C. If the bonding temperature is set to a temperature lower than 250 °C, the solid phase Diffusion reaction with the bonding area is not accelerated, so that an excellent bonding area cannot be obtained Even if it is set to a temperature lower than 250 °C, the diffusion continues if the Holding time is set longer. However, it is assumed that this is due to mass production processes is practically unsuitable.

[0062] However, if the bonding temperature is set to a temperature higher than 300 °C, this leads to the occurrence of Softening of the copper forming the conductor layers 3a, 3b of the DBC plate 3. When the evaluation sample is heated for 10s at a bonding temperature higher than 300 °C, the following applies: Although the bonding area is initially excellent, then when the sample is subjected to a heat cycle test, a deformation occurs in the DBC plate 3, and its surface undulates into an uneven shape.

[0063] On this occasion, a crack occurs at one edge of the bonding area due to the deformation of the DBC plate 3, and on the inside of the bonding area, a crack occurs perpendicular to the bonding surface because it is not able to resist the Unevenness of the DBC plate 3. Consequently, the bonding temperature is preferably between 250 °C and 300 °C.

[0064] Regarding the bonding time, it only needs to be a period in which a solid phase diffusion reaction between the metal covering the bonding surface of the bonding object and the Ag-Bi alloy, and although it is above 10 minutes, an excellent bonding area was obtained even when it was 5 minutes. If the Bonding time is too long, this is disadvantageous because the cycle time in mass production is long, so 5 to 10 minutes on are most suitable.

[0065] The applied pressure depends on the flatness of the bonding surface, and the surface flatness Ra of each semiconductor device 2 for electrical energy used in the evaluation here was 50 nm or less, and the The surface flatness Ra of each DBC plate 3 used in the evaluation here was 1 µm or less. With such flatness, excellent bonding was achieved when the alloy foil 1F of the Ag-Bi series was heated at 10 MPa to 30 MPa. It should be noted that the alloy foils 1F were those with a surface flatness Ra of 1 µm each were used.

[0066] Regarding the metal covering the bonding surface, if it is gold, silver, copper or any Combination of these can provide excellent bonding for both the semiconductor component 2 for electrical energy, as also be obtained for DBC plate 3. It should be noted that although a good bond area can be obtained even can be used if it is tin, the melting point of tin is about 230 °C, and consequently it is used in bonding Temperature of 250 to 300 °C melted.

[0067] On this occasion, silver will diffuse into tin to form a eutectic phase of tin and silver (Sn- 3Ag (wt%)) with a melting point of 220 °C and a fine intermetallic compound (Ag3Sn). This impairs heat resistance and is therefore not preferred. Furthermore, this is not preferred because bismuth in tin to form a eutectic phase of tin and silver (Sn-58Bi (wt%)) with a melting point of 138 °C, which consequently impairs the heat resistance.

[0068] It should be noted that if there is a need to achieve bonding with the surface of tin, it is necessary to heat sufficiently so that a tin-only phase or a eutectic phase of tin and silver or a eutectic phase of tin and bismuth, each of which has a low melting point, not at the interface between Sn and of the Ag-Bi alloy. Furthermore, it is necessary to ensure that the interface area is completely at least one intermetallic compound of Ag3Sn or Ag5Sn.

[0069] In the semiconductor device 100 for electric power according to Embodiment 1, with respect to the bonding Object: A case was shown in which the Ag-Bi alloy bonding material 1 was used for bonding between the semiconductor component 2 for electrical energy and the DBC plate 3 or for bonding between the semiconductor component 2 for electrical energy and the connecting conductor 4.

[0070] However, in a semiconductor device 100 for electric power, a heat dissipating plate is provided under the PCB without being essentially limited to the DBC board 3, so that it is also possible to apply the bonding material 1 of the invention to the bonding between the circuit board and the heat dissipating plate.

[0071] Furthermore, in the semiconductor device 100 for electric power according to Embodiment 1, the case was shown, in which silicon carbide is used for the semiconductor component 2 for electrical energy, which serves as a switching element or as a rectifier element. However, this is not limiting, so that a conventional silicon based element can be used.

[0072] Nevertheless, in the case where an element is used which is a so-called semiconductor component with further band gap, such as silicon carbide, a gallium nitride series material or diamond, is as follows: Since its Power losses are lower than those of the conventionally used element made of silicon, the efficiency of the semiconductor device 100 for electrical energy can be improved.

[0073] Furthermore, its withstand voltage and also its allowable current density are high. Consequently, the Semiconductor device 100 for electrical energy can be reduced in size. Furthermore, the heat resistance of the semiconductor device with a wide band gap, and this consequently allows operation at high temperatures. This allows also a reduction in the size of a heat-dissipating fin of the heatsink and the replacement of a water-cooled unit by an air-cooled unit, so that the semiconductor device 100 for electrical energy can be further reduced in size can.

[0074] Meanwhile, in order to develop the possibility of a semiconductor device with a wide band gap, it is necessary to electrical resistance at the time when a current in the semiconductor device 2 for electrical energy flows, and to effectively dissipate the heat generated in the semiconductor component 2 for electrical energy.

[0075] When the semiconductor component 2 for electrical energy is produced using the bonding material 1 based on Ag-Bi- alloy described in the embodiment of the invention, a highly reliable Semiconductor device 100 for electrical energy can be obtained because not only a superior heat dissipating property and electrical conductivity can be obtained, but also a strong bond connection during heating cycles during their manufacture and / or operation.

[0076] According to the bonding material 1 according to this embodiment, as described above, this is a sheet-like bonding Material 1, which is made of a silver-bismuth alloy, which, when heated to a state in which it is in contact with a metal material as a bonding object (e.g. the surface layer 2f as the electrode of a Element of the semiconductor component 2 for electrical energy and the surface layer 3f of the conductor layer 3a of the DBC plate 3) in the metal material (as its material e.g. gold, silver or copper) a diffusion layer Ld2, Ld3 of silver as a result of the Solid phase diffusion reaction so that it is bonded to the metal material, whereby the bonding material is configured to contain not less than 1 mass% and not more than 5 mass% bismuth. Consequently, it is possible to reduce the elastic modulus appropriately to achieve a bonding that both the Heat resistance as well as stress relief capacity.

[0077] Furthermore, the bonding material 1 is a rolled material having a thickness of 50 µm to 100 µm, so that the bonded Object 10 can be formed without increasing its thickness too much, and consequently a compact and highly efficient semiconductor device 100 for electrical energy can be manufactured in a simple manner. In addition, it is possible to easily achieve the flatness accuracy appropriate for such bonding.

[0078] According to the bonding method according to this embodiment, it is intended to include: a Heat treatment step in which the bonding material 1 is heated at a temperature of not less than 150 °C and not more than 300 °C; and a diffusion layer forming step in which the bonding material 1, after it has been subjected to the heat treatment step, between two bonding objects (e.g. the semiconductor component 2 for electrical energy and the DBC plate 3) is sandwiched, and in which the latter is heated to a temperature which is lower than the melting point of the bonding material 1, thereby forming a diffusion layer Ld2, Ld3 of silver in each of the two bond objects. Consequently, it is possible to achieve a strong bond, whose voltage reduction capacity is superior.

[0079] When the period of heat treatment in the heat treatment step is not less than 10 hours and If the setting is not more than 100 hours, it is possible to safely achieve the stress-relieving effect.

[0080] Since the heating temperature in the diffusion layer forming step is not less than 250 °C and not more than 300 °C, it is possible to obtain a strong bond connection without deteriorating the bond object.

[0081] Since the diffusion layer formation step is carried out in a reducing atmosphere (e.g., a formic acid atmosphere or a hydrogen atmosphere), no oxidized top layer appears on the bonded surface of the bonding material 1 or the bonding object. Consequently, it is possible to form the diffusion layers Ld2, Ld3 of silver to train safely.

[0082] The semiconductor device 100 for electric power according to this embodiment comprises: a Printed circuit board (DBC board 3) on which a circuit pattern (conductor layer 3a) is formed, and a semiconductor component 2 for electrical energy, which is bonded to the circuit pattern (conductor layer 3a), wherein the semiconductor component 2 for electrical energy and the circuit pattern (conductor layer 3a) by means of the bonding method according to this embodiment are bonded.

[0083] Consequently, the heat resistance of the bonding connection between the semiconductor component 2 for electrical energy and the DBC plate 3, and it is provided with a stress relief capability. Consequently, it is possible to highly reliable semiconductor device 100 for electrical energy, which has a strong bond connection itself when subjected to high temperature operation or power cycling.

[0084] Since at each of the mutually opposite surfaces of the semiconductor component 2 for electrical energy and the circuit pattern (conductor layer 3a) a metal layer 2f, 3f of any of gold, silver and copper as metal material, the diffusion layers Ld2, Ld3 of silver can be safely provided. Description of reference symbols 1 Bond material Alloy foil (bonding material) 1F 2 Semiconductor component for electrical energy 2f surface layer 3 DBC board (printed circuit board) 3a Conductor layer (circuit pattern) 3f surface layer 4 connecting conductors 5 Sealing material 10 bonded object 10S evaluation sample 100 semiconductor device for electrical energy

Claims

1. Bond material (1) made of an alloy (1F) containing bismuth and mainly silver and which, when heated in a state in which it is in contact with a metal material as Bond object is in which metal material forms a diffusion layer (Ld2, Ld3) of silver, as a result of a Solid phase diffusion reaction so that it is bonded to the metal material, wherein the bonding material (1) is not less than 1 wt% and not more than 5 wt% of bismuth.

2. Bonding material (1) according to claim 1, wherein in the silver-bismuth alloy (1F) the grain size of the bismuth-rich phase between 0.2 µm and 1.0 µm.

3. Bonding material (1) according to claim 1 or 2, which is a sheet material having a thickness of 50 µm to 100 µm has.

4. A method for bonding using the bonding material (1) according to any one of claims 1 to 3, comprising the following has: - a heat treatment step in which the bonding material (1) is heated at a temperature of not less than 150 °C and is not heat-treated more than 300 °C; and - a diffusion layer forming step (Ld2, Ld3), in which the bonding material (1), after being has undergone a heat treatment step, is sandwiched between two bonding objects, and which they are heated to a temperature lower than the melting point of the bonding material (1) in order to thereby forming the diffusion layer (Ld2, Ld3) of silver in each of the two bond objects.

5. Bonding method according to claim 4, wherein the period of time for heat treatment is not less than 10 hours and not more than 100 hours.

6. Bonding method according to claim 4 or 5, wherein the temperature in the diffusion layer forming step (Ld2, Ld3) is not less than 250 °C and not more than 300 °C.

7. Bonding method according to one of claims 4 to 6, wherein the diffusion layer forming step (Ld2, Ld3) is carried out in a reducing atmosphere.

8. A semiconductor device (100) for electrical energy, comprising: - a printed circuit board (3) on which a circuit pattern (3a) is formed; and - a semiconductor component (2) for electrical energy bonded to the circuit pattern (3a); wherein a bonding region between the circuit board (3) and the semiconductor component (2) for electrical energy is formed from the following: a first diffusion layer (Ld2) formed on the side of the semiconductor component (2) for electrical energy; a bonding Material (1) made of an alloy containing bismuth and consisting mainly of silver; and a second diffusion layer (Ld3) formed on the side of the circuit board (3); and wherein the first diffusion layer (Ld2) and the second diffus sion layer (Ld3) by diffusion of silver from the bonding material (1) to thereby bond to the bonding material (1) to be bonded.

9. A semiconductor device (100) for electric power according to claim 8, wherein the first diffusion layer (Ld2) and the second diffusion layer (Ld3) is formed in such a way that silver is incorporated into a metal layer of any Material made of gold, silver and copper diffuses.

10. Semiconductor device (100) for electric power according to claim 8 or 9, wherein the semiconductor component (2) for electrical energy is formed from a semiconductor material with a large band gap.

11. A semiconductor device (100) for electrical energy according to claim 10, wherein the semiconductor material with large Band gap of one of silicon carbide, a gallium nitride series material and diamond.

Citation Information

Patent Citations

  • Brazing filter metal

    JP1983006793A

  • Conductive adhesive, method of manufacturing semiconductor device using the same, and semiconductor device

    JP2010267579A

  • Conductive bonding material, semiconductor device using this, and manufacturing method of semiconductor device

    JP2011198674A

  • Method of manufacturing electronic device

    JP2012054358A

  • Conductive compositions containing blended alloy fillers

    US20100252616A1