COMPOSITE MAGNET WITH L10-FeNi MAGNETIC POWDER
By employing L10-FeNi magnetic powder with specific size and sphericity, the bonded magnet achieves higher filling rates and orientation, enhancing its magnetic performance and flux density.
Patent Information
- Application Number
- DE112018002550
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-05-17
- Filing Date
- 2018-05-11
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2038-05-11
AI Technical Summary
Conventional bonded magnets face challenges in achieving high filling rates of magnetic powder without compromising flowability, leading to decreased magnetic performance due to lower orientation and residual magnetic flux density.
The use of L10-FeNi magnetic powder with an average particle size of 50 nm to 1 μm and sphericity of 0.9 or higher, combined with a large-sized magnetic powder, enhances the fluidity of the raw material and increases the filling rate, thereby improving the magnetic performance of the bonded magnet.
The increased filling rate of the magnetic powder results in enhanced residual magnetic flux density and orientation, resulting in improved magnetic performance without significantly reducing the flowability of the bonded magnet.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical area
[0001] The present invention relates to a bonded magnet. State of the art
[0002] A bonded magnet is known. The bonded magnet contains a base material and a magnetic powder dispersed in the base material. A bonded magnet is disclosed in JP H06-132107 A. The bonded magnet can be manufactured by injection molding or the like.
[0003] The publication by Gurmen, S., [et al.]: “Nanocrystalline Spherical Iron-Nickel (Fe-Ni) Alloy Particles Prepared by Ultrasonic Spray Pyrolysis and Hydrogen Reduction (USP-HR).” In: Journal of Alloys and Compounds, Vol. 480, No. 2, 2009, pp. 529-533, discloses a magnetic powder having: a mean particle size of 50 nm to 1 µm, and a mean sphericity P of nearly 1, where the sphericity P is defined as P = Ls / Lr, where Lr is the circumference of an L10-FeNi magnetic powder particle in a microscope image and Ls is the circumference of a perfect circle having the same area as the magnetic powder particle in the image for which Lr is calculated.
[0004] DE 11 2016 004 716 T5 discloses a method for producing an ordered FeNi alloy with an L1-type ordered structure. After performing a nitriding process for nitriding a powder sample of a disordered FeNi alloy placed in a tube furnace using an NH gas, a denitriding process for removing nitrogen from the disordered FeNi alloy processed by the nitriding process is performed using an H gas.
[0005] JP 2016 - 79 484 A discloses a bonded magnet comprising: a base material and a magnetic powder dispersed in the base material, wherein the magnetic powder contains an FeNi magnetic powder, and wherein a mass percentage of the FeNi magnetic powder in the magnetic powder is 5% or more. Summary of the invention
[0006] As a result of detailed studies conducted by the inventors, the following was discovered. When a composite magnet is manufactured by injection molding, it is necessary to ensure the flowability of the raw material. Furthermore, it is necessary to increase the degree of orientation of the magnetic powder. Increasing the fill rate of the magnetic powder in the composite magnet tends to decrease the flowability of the raw material. Therefore, increasing the fill rate of the magnetic powder in a conventional composite magnet is difficult. A low fill rate of the magnetic powder degrades the magnetic performance of the composite magnet. Additionally, increasing the fill rate of the magnetic powder in the composite magnet tends to decrease the degree of orientation of the magnetic powder.
[0007] The object of the present invention is to create a bonded magnet with improved magnetic performance. This object is achieved by a bonded magnet having the features of claim 1. The dependent claims are directed to advantageous developments of the invention.
[0008] According to one aspect of the present invention, an L10-FeNi magnetic powder in the bonded magnet has an average particle size of 50 nm to 1 µm and an average value of sphericity P of 0.9 or greater, wherein the sphericity P is defined by the following equation (1). P=Ls / Lr
[0009] In equation (1), Lr is the circumference of an L10-FeNi magnetic powder particle in a microscope image. In equation (1), Ls is the circumference of a perfect circle with the same area as the area of the L10-FeNi magnetic powder particle for which Lr is calculated.
[0010] The use of such L10-FeNi magnetic powder can improve the magnetic performance of the composite magnet.
[0011] The reference numerals in parentheses in the claims indicate a correspondence to specific devices described in the following embodiments and do not limit the technical scope of the present invention. Short description of the drawings Fig. Figure 1 is an explanatory diagram showing Lr and Ls. Fig. Figure 2 is an explanatory diagram showing the structure of a composite magnet. Description of the embodiments
[0012] An exemplary embodiment of the present invention is described below with reference to the drawings. 1. Composition of the L10-FeNi magnetic powder
[0013] L10-FeNi refers to FeNi with an L10 structure. An L10-FeNi magnetic powder of the present invention is a magnetic powder consisting of L10-FeNi.
[0014] A mean value of the sphericity P in the L10-FeNi magnet powder (hereinafter referred to as mean value P) avg The sphericity P is defined by the following equation (1). P=Ls / Lr
[0015] As it is in Fig. As shown in Figure 1, Lr in equation (1) is the circumference of the L10-FeNi magnetic powder particle 1 in a microscope image. In the above equation (1), Ls is the circumference of a perfect circle 3 having the same area S as the area S of the L10-FeNi magnetic powder particle 1 in the microscope image for which Lr is calculated.
[0016] The mean P avgcan be calculated as follows. First, a SEM or TEM image (hereinafter referred to as a microscope image) is obtained in which the L10-FeNi magnetic powder appears. For each individual L10-FeNi magnetic powder particle in the microscope image, the sphericity P is calculated based on equation (1). Then, the mean value P avg The sphericity P of one hundred L10-FeNi magnetic powder particles in the microscope image was calculated.
[0017] The average particle size D avg The particle size of the L10-FeNi magnetic powder of the present invention is 50 nm to 1 µm. A measurement method for the mean particle size D av The following is done. First, a microscope image is obtained in which the L10-FeNi magnetic powder appears. For each individual L10-FeNi magnetic powder particle, the particle size D, represented by the following equation (2), is calculated. D=Ls / π
[0018] In equation (2), Ls is the circumference of a perfect circle with the same area as the area of the L10-FeNi magnetic powder particle in the microscope image for which the particle size D is to be calculated. The mean particle size D over 100 L10-FeNi magnetic particles in the microscope image is given as the mean particle size D. avg of the L10-FeNi magnetic powder.
[0019] The L10-FeNi magnetic powder of the present invention can be used as a magnetic powder, for example, in a composite magnet. The L10-FeNi magnetic powder of the present invention exhibits a high residual magnetic flux density. When the L10-FeNi magnetic powder of the present invention is used as a magnetic powder in a composite magnet together with a larger-sized magnetic powder described later, the flowability of the raw material of the composite magnet is unlikely to decrease. Therefore, the filling rate of the magnetic powder in the composite magnet can be increased. Consequently, when the L10-FeNi magnetic powder of the present invention is used as a magnetic powder in a composite magnet together with a larger-sized magnetic powder, the residual magnetic flux density of the composite magnet can be increased.Note that the filling rate of the magnetic powder is a ratio of the mass of the magnetic powder to the total mass of the composite magnet.
[0020] Furthermore, when the L10-FeNi magnetic powder of the present invention is used as a magnetic powder in combination with a larger-sized magnetic powder in a composite magnet, the degree of orientation of the magnetic powder within the composite magnet can be increased. The mean particle size D avg The particle size of the L10-FeNi magnetic powder of the present invention is preferably 400 nm to 1 µm. If the mean particle size D avg Since the L10-FeNi magnetic powder of the present invention is 400 nm to 1 µm, the residual magnetic flux density of the composite magnet is even greater, and the degree of orientation of the magnetic powder in the composite magnet is also greater.
[0021] The L10-FeNi magnetic powder is produced, for example, by a process of nitriding and denitriding after one or more laser irradiation, thermal plasma and gas sputtering treatment of FeNi particles serving as raw material, or similar processes. 2. Composite magnet
[0022] As it is in Fig. As shown in Figure 2, the composite magnet 5 of the present invention comprises a base material 7 and a magnetic powder 9 dispersed in the base material 7. The magnetic powder 9 contains the L10-FeNi magnetic powder 11 of the present invention and a large-size magnetic powder 13 having a mean particle size of 1 µm to 500 µm. The mass percentage of the L10-FeNi magnetic powder 11 in the magnetic powder 9 is 5% or more.
[0023] In the composite magnet 5, the filling rate of the magnetic powder 9 can be increased without significantly reducing the flowability of the raw material of the composite magnet 5. As a result, the residual magnetic flux density of the composite magnet 5 can be increased. Even with a high filling rate of the magnetic powder 9 in the composite magnet 5, the orientation of the magnetic powder 9 is high.
[0024] Examples of base material 7 include a resin. Examples of resin include polyamide, chlorinated polyethylene, ABS, and similar materials. The large-size magnetic powder 13 is not particularly restricted, and a suitably selected magnetic powder can be used as a large-size magnetic powder 13. Examples of large-size magnetic powder 13 include a rare-earth magnetic powder. Examples of large-size magnetic powder 13 materials include SmFeN, NdFeB, and SmCo. The mean value P avgthe sphericity P in the large size magnetic powder 13 is preferably in the range of 1.0 to 0.4.
[0025] The mass percentage of the L10-FeNi magnetic powder 11 in the magnetic powder 9 is preferably 10% or more. If the mass percentage of the L10-FeNi magnetic powder 11 in the magnetic powder 9 is 10% or greater, the residual magnetic flux density of the composite magnet 5 can be further increased. The degree of orientation of the magnetic powder 9 in the composite magnet 5 can also be further increased.
[0026] The filling rate of the magnetic powder 9 in the bonded magnet 5 is preferably 80 mass percent or more, and more preferably 90 mass percent or more. When the filling rate of the magnetic powder 9 is 80 mass percent or more, the residual magnetic flux density of the bonded magnet 5 can be further increased. 3. Method for manufacturing the bonded magnet
[0027] The composite magnet of the present invention can be produced, for example, as follows. First, the L10-FeNi magnet powder of the present invention and the base material are mixed in a predetermined mass ratio, and this mixture is kneaded under vacuum to create a pre-composite or pre-bond. The base material is, for example, a resin. The temperature during vacuum kneading is, for example, 140°C. The duration of the vacuum kneading is, for example, 10 hours.
[0028] The pre-compound is then reduced to a size of, for example, 1 mm or less using a grinding machine or similar equipment. The reduced compound and a larger magnetic powder are then mixed using, for example, a mixer, and this mixture is vacuum kneaded to create a composite compound. The temperature during vacuum kneading is, for example, 140°C. The duration of the vacuum kneading process is, for example, 10 hours.
[0029] The composite compound is then molded into a predetermined shape using a process such as injection molding. Examples of the predetermined shape include a cylinder. A heat treatment is then performed while applying a magnetic field in a specific direction to the molded product to perfect the bonded magnet. The heat treatment temperature is, for example, 180°C. The heat treatment time is, for example, 4 hours. 4. Working Example 4-1 Production of magnetic powder C1, C2
[0030] FeNi spherical particles A were prepared as a raw material. These FeNi spherical particles A were specially ordered and manufactured by Nisshin Engineering Inc. They were produced using a known thermal plasma process. The composition ratio of the FeNi spherical particles A was Fe:Ni = 50:50. The unit of composition ratio is atomic percent.
[0031] The following laser irradiation procedure was carried out with regard to the above FeNi spherical particles A.
[0032] Laser irradiation method: A suspension was prepared by adding 1% or less by mass of FeNi spherical particles A to a thicker sodium silicate-based aqueous solution and dispersing it using an ultrasonic homogenizer. In this suspension, nanoparticles of FeNi spherical particles A were dispersed in water. The output of the ultrasonic homogenizer was 150 W.
[0033] The suspension was irradiated with a YAG pulsed laser for 1 to 4 hours to sinter and grow the FeNi spherical particles A. FeNi spherical particles B with particle sizes ranging from 200 nm to 500 nm were obtained. The wavelength of the YAG pulsed laser was 1064 nm. The laser intensity of the YAG pulsed laser was 75 mJ / pulse. The pulse width of the YAG pulsed laser was 6 ns. The repetition rate of the YAG pulsed laser was 10 Hz. Several types of FeNi spherical particles B with different particle sizes were obtained by varying the irradiation time of the YAG pulsed laser.
[0034] Subsequently, the different types of FeNi spherical particles B were each subjected to a subsequent nitration-denitration treatment to obtain several types of FeNi spherical particles C. The nitration-denitration treatment is a process that causes the FeNi spherical particles to exhibit an L10 structure.
[0035] The nitration-denitration treatment was carried out as follows: FeNi spherical nanoparticles B were arranged on a sample boat. The sample boat was housed in a tubular furnace. The tubular furnace was capable of introducing ammonia and hydrogen gas. The atmosphere of the tubular furnace consisted of ammonia gas, and the nitration treatment was performed at 350°C for 50 hours.
[0036] The atmosphere of the tubular furnace was then replaced with hydrogen gas, and a denitration treatment was performed at 300°C for 2 hours. After cooling the tubular furnace, the sample boat was removed. The result was magnetic powder C, provided as FeNi spherical particles with the L10 structure.
[0037] P avg , D avgThe magnetic properties of magnetic powders C1 and C2, Ms and Hc, were measured for the different types of magnetic powder C. The results are shown in Table 1 below. Magnetic powders C1 and C2 differ with respect to P due to the different irradiation times of the YAG laser in the laser irradiation process. avg and D avg .
[0038] In Table 1, Ms is the magnetization measured by a VSM (vibrating sample magnetometer) method. In Table 1, Ms is a value obtained at an external magnetic field of 3 T. Hc is a coercive force measured using a VSM method after magnetic alignment of the compound, which has a magnetic powder ratio of 10% by mass. Table 1 Magnetic powder material Manufacturing process P avg D avg Ms (emu / g) Hc (kOe) C1 L10-FeNi Laser irradiation 0,96 550 nm 140 3,5 C2 L10-FeNi laser irradiation 0,95 400 nm 142 3,1 D1 L10-FeNi Thermal plasma treatment 0,95 120 nm 139 1,6 D2 L10-FeNi Thermal plasma treatment 0,90 60 nm 139 2,2 D3 L10-FeNi Thermal plasma treatment 0,91 30 nm 137 2,0 F1 L10-FeNi Gas atomization 0,84 5,8 µm 151 0,4 F2 L10-FeNi Gas atomization 0,81 3,0 µm 150 0,4 G NdFeB Jet mill comminution 0,43 0,8 µm 98 4,5 L SmFeN - 0,62 3,5 µm 133 14,0 4-2 Production of magnetic powder D1-3
[0039] Three types of FeNi spherical particles A with different particle sizes were prepared or produced. Each of the three types of FeNi spherical particles A was subjected to a nitriding-denitriding treatment. This nitriding-denitriding treatment was the same as the treatment used to produce the magnetic powder C. As a result, magnetic powders D1 to D3 were obtained, consisting of FeNi spherical particles with an L10 structure. avg , D avg , Ms, and Hc in magnetic powders D1 to D3 were measured. The results are shown in Table 1 above. 4-3 Production of magnetic powders F1 and F2
[0040] Two types of FeNi spherical particles E with different particle sizes were prepared or manufactured as raw materials. The FeNi spherical particles E were specially ordered and manufactured by Nisshin Engineering Co. Ltd. They were produced using a known gas sputtering process. The composition ratio of Fe:Ni in the FeNi spherical particles E was 50:50. The unit of composition ratio is atomic percent.
[0041] The two types of FeNi spherical particles E were each subjected to the nitriding-denitriding treatment. The nitriding-denitriding treatment was the same as the treatment used to produce the magnetic powder C. As a result, magnetic powders F1 and F2 were obtained, consisting of FeNi spherical particles with an L10 structure. avg , D avgMs and Hc in the magnetic powders F1 and F2 were measured. The results are shown in Table 1 above. 4-4 Production of magnetic powder G
[0042] An NdFeB-sintered magnet was pulverized using a jet mill to produce a magnetic powder G composed of NdFeB. avg , D avg Ms and Hc in the magnetic powder G were measured. The results are shown in Table 1 above. 4-5 Production of large-sized magnetic powder L
[0043] A large-size magnetic powder L was produced. The large-size magnetic powder L was a magnetic powder consisting of SmFeN and was a commercial product. P avg , D avg Ms and Hc were measured in the large-size magnetic powder L. The results are shown in Table 1 above. 4-6 Production of the composite magnets M1 to M8
[0044] Composite magnets M1 to M8 were manufactured as follows. A small-scale magnetic powder and a resin were mixed in a predetermined mass ratio, and this mixture was vacuum kneaded at 140°C for 10 hours to create a pre-compound. The small-scale magnetic powder was one of the following: C1, C2, D1 to D3, F1, F2, and G. The correspondence between the composite magnet and the small-scale magnetic powder it contained was as shown in Table 2 below. Table 2 shows the composition of the small-scale magnetic powder contained in the composite magnets M1 to M8. In each of the composite magnets M1 to M8, the resin was polyamide. Table 2 magnet Contents of the included magnetic powder, small size Composite magnet evaluation result Ratio of small-sized magnetic powder: 10 mass percent Ratio of small-sized magnetic powder: 20% by mass Type P avg D avg Ms(T) Mr(T) Mr / Ms Ms(T) Mr(T) Mr / Ms M1 C1 0,96 550 nm 0,92 0,85 0,92 0,98 0,90 0,92 M2 C2 0,95 400 nm 0,95 0,86 0,9 1,00 0,91 0,91 M3 D1 0,95 120 nm 0,84 0,76 0,9 0,88 0,78 0,88 M4 D2 0,90 60 nm 0,86 0,75 0,87 0,88 0,75 0,86 M5 D3 0,91 30 nm 0,82 0,70 0,85 0,78 0,66 0,84 M6 F1 0,84 5.8 µm 0,90 0,70 0,78 0,94 0,71 0,75 M7 F2 0,81 3.0 µm 0,86 0,73 0,85 0,90 0,71 0,79 M8 G 0.43 0.8 µm 0,80 0,68 0,85 0,74 0,60 0,81 M9 - - - 0,86 0,74 0,86
[0045] The pre-compound was then ground to particles of 1 mm or less using a comminution machine. The ground pre-compound was then mixed with a large-size magnetic powder (L) using a mixer, and this mixture was vacuum kneaded at 140°C for 10 hours to form a composite compound.
[0046] The composite material was then injection-molded into a cylindrical shape with a diameter of 3 mm and a height of 3 mm. Subsequently, it underwent heat treatment at 180°C for 4 hours while a magnetic field of 1.0 T was applied in the axial direction of the cylinder to perfect the composite magnets M1 to M8.
[0047] In bonded magnets M1 to M8, the mixing ratio of the small-size magnetic powder, the large-size L magnetic powder, and the resin was such that the filling ratio of the total magnetic powder was 93 mass percent. In each of the bonded magnets M1 to M8, there were two types of total magnetic powder; the mass ratio of the small-size magnetic powder to the total magnetic powder (hereinafter referred to as the small-size magnetic powder ratio) was 10 mass percent and 20 mass percent.
[0048] The manufacturing process was basically the same as that of bonded magnets M1 to M8, but the bonded magnet M9 was manufactured using only the large size L magnetic powder as the magnetic powder. Furthermore, the filling rate of the magnetic powder in the bonded magnet M9 was 93 mass percent. 4-7 Evaluation of the compound magnets M1 to M9
[0049] Ms and Mr were measured for each of the composite magnets M1 to M9. Additionally, Mr / Ms was calculated. The results are shown in Table 2 above. Mr is the residual magnetization measured using a VSM method. Mr is the magnetization value when, after applying an external magnetic field of 3 T, the external magnetic field is zero. Particularly in composite magnets M1 to M4, the values of Ms, Mr, and Mr / Ms were large.
[0050] A method for synthesizing small-sized magnetic powder may be different from the method described above.
Claims
[1] Bonded magnet (5) comprising: a base material (7); and a magnetic powder (9) dispersed in the base material (7), wherein the magnetic powder (9) contains: an L10-FeNi magnetic powder (11) which has: an average particle size of 50 nm to 1 µm; and a mean sphericity P of 0.9 or greater, where the sphericity P is defined as P = Ls / Lr, where Lr is a circumference of an L10-FeNi magnetic powder particle in a microscope image, and Ls is a circumference of a perfect circle having the same area as the L10-FeNi magnetic powder particle in the image for which Lr is calculated; and a large-size magnetic powder (13) having an average particle size of 1 µm to 500 µm, wherein a mass percentage of the L10-FeNi magnetic powder (11) in the magnetic powder (9) is 5% or more. [2] Bonded magnet (5) according to claim 1, wherein the average particle size is in a range of 400 nm to 1 µm. [3] The bonded magnet (5) according to claim 1 or 2, wherein a filling ratio of the magnetic powder (9) is 80 mass percent or greater. [4] The bonded magnet (5) according to any one of claims 1 to 3, wherein the mass percentage of the L10-FeNi magnetic powder (11) in the magnetic powder (9) is 10% or greater.
Citation Information
Patent Citations
Composite rare earth bond magnet
JP1994132107A
Ordered FeNi ALLOY AND PROCESS FOR PRODUCTION OF ORDERED FeNi ALLOY
DE112016004716T5
Magnetic nanoparticle, method for producing the same, and magnetic material
JP2016079484A