Magnet, motor and generator on RTB basis
The R-T-B based magnet with controlled grain boundary phases and element ratios addresses high coercivity and magnetization fluctuations, enhancing motor efficiency by reducing the magnetizing field requirement and stabilizing magnetization.
Patent Information
- Application Number
- DE112019002738
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-05-29
- Filing Date
- 2019-05-17
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2039-05-17
AI Technical Summary
The existing R-T-B based magnets have high coercivity and require a large magnetizing field for saturation, exceeding the limits of stator coils in motors, and exhibit significant magnetization variation with magnetic field fluctuations, leading to inefficiencies in variable magnetic flux motors.
The R-T-B based magnet is composed of specific rare earth and transition metal elements with a tetragonal structure, including a grain boundary phase of R-T-M-C and R-O-C-N, with controlled crystal grain size and element ratios to reduce coercivity and enhance flatness of the hysteresis curve, allowing for high residual magnetic flux density and stable magnetization.
The solution results in a magnet with low coercivity and high residual magnetic flux density, enabling efficient operation of variable magnetic flux motors with reduced magnetization fluctuations and improved efficiency.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL AREA
[0001] The present invention relates to an RTB-based magnet, a motor, and a generator. More specifically, the invention relates to an RTB-based magnet suitable for a variable flux magnet that can be used in a variable magnetic force motor and a generator. BACKGROUND ART
[0002] A high-efficiency permanent magnet synchronous motor, which can save energy through inverter control, has been applied as power units for consumers, industry, and transportation equipment. However, in a permanent magnet synchronous motor, where the magnetic flux of a permanent magnet is constant, an induced voltage increases proportionally with the speed, making driving difficult over a wide speed range. Therefore, for the permanent magnet synchronous motor in a medium and high-speed range and under light load, a method called field weakening control is adopted. In field weakening control, a magnetic flux of a permanent magnet is canceled by a demagnetizing field due to an armature current, and a coupling magnetic flux is reduced so that the induced voltage does not exceed a supply voltage.However, in order to continue to apply the demagnetizing field continuously, the armature current, which does not contribute to the motor power, must flow continuously, which creates the problem of deteriorating motor efficiency.
[0003] To solve this problem, for example, Patent Document 1 discloses a variable magnetic force motor in which a low-coercive Sm-Co-based permanent magnet (variable flux magnet), whose magnetization changes reversibly by applying an external magnetic field, is combined with a fixed flux magnet that causes a magnetic field to act on the variable flux magnet. In the variable magnetic force motor, the induced voltage is reduced by reducing the magnetization of the variable flux magnet in the medium and high-speed ranges and under light load conditions, so that deterioration of motor efficiency due to conventional field weakening control can be suppressed.
[0004] However, the Sm-Co-based permanent magnet described in Patent Document 1 has the problem that Co, as the main raw material, is expensive. Furthermore, the saturation magnetization of the Sm-Co-based permanent magnet, which is the variable flux magnet, is approximately 1.25 T (equivalent to 12.5 kG) at its maximum, and does not reach the saturation magnetization of a neodymium magnet, which is the fixed flux magnet. As a result, a magnetic force difference occurs between the fixed flux magnet and the variable flux magnet, thus causing the performance and efficiency of the variable magnetic force motor to deteriorate.
[0005] Here, it is assumed that the RTB-based magnet is used as the magnet for the variable magnetic flux magnet.
[0006] Patent Document 2 discloses an RTB-based magnetic material in which the residual magnetic flux density Br is 1.1 T (equivalent to 11 kG) or more, the coercive force HcJ is 398 kA / m (equivalent to 5 kOe) or less, and an external magnetic field required to adjust the residual magnetic flux density Br to 0 is 1.10 HcJ or less. It is disclosed that the RTB-based magnetic material contains a crystal grain containing a rare earth element R, a transition metal element T, and boron B, and that the Cu content in the crystal grain is 0.5 to 0.6 atomic % with respect to the total elements in the crystal grain.
[0007] Patent Document 3 discloses a permanent magnet whose composition (Ce 1-x-y R1 x R2 y ) a Fe b Co c B d M e X f C g A hR1 is at least one type selected from Nd, Pr, Sm, and La, and R2 is at least one type selected from Tb, Dy, and elements not selected as R1. Furthermore, M is an element such as Ti, X is an element such as Ga, and A is at least one type selected from F and O. It is described that the permanent magnet can change a magnetization state and has a low coercive force.
[0008] Patent Document 4 discloses an R-Fe-B-based magnet. In the R-Fe-B-based magnet, the average crystal grain size is 0.01 to 2 µm, and powder grains have a texture of Nd2T crystal phases. 14 B-types are coupled, a rare earth element-rich phase exists at a position between the powder grains, and the number density of the rare earth element-rich phase is 11.6×10 4 pieces / mm 2or more. However, the R-Fe-B-based magnet is designed to achieve high coercive force and does not have magnetic properties applicable to the variable flux magnet.
[0009] Patent Document 5 describes a permanent magnet based on RTB. Among other things, it addresses the composition of the permanent magnet and the size of the main phase grains. REFERENCE PATENT DOCUMENT Patent Document 1: JP 2010-34522 A Patent document 2: WO 2012 / 090765 A Patent Document 3: JP 2010-74084 A Patent Document 4: JP 2012-99852 A Patent document 5: DE 10 2017 203 059 A1 SUMMARY OF THE INVENTION PROBLEM TO BE SOLVED BY THE INVENTION
[0010] The RTB-based magnetic material described in Patent Document 2 has a higher residual magnetic flux density than the Sm-Co-based magnet for the conventional variable magnetic force motor, so high performance and high efficiency of the variable magnetic force motor are expected. However, the RTB-based magnetic material described in Patent Document 2 only describes magnetic properties in a saturated magnetization state.
[0011] Here, the saturation magnetization state indicates a state in which a sample is magnetized by applying a saturation magnetic field. In the RTB-based magnetic material described in Patent Document 2, a magnetization field Hmag that is at least three times or more of the coercive force is required to realize the residual magnetic flux density in the saturation magnetization state. Therefore, in the RTB-based magnetic material described in Patent Document 2, the magnetization field Hmag required for magnetization switching of the RTB-based magnetic material increases regardless of the low coercive force. As the magnetization field Hmag increases, there is a problem that it exceeds the upper limit of a magnetic field that can be applied with a stator coil of a motor.
[0012] Furthermore, the present inventors found that in order to expand the high-performance operating range of the variable magnetic force motor, it is preferable that the difference in induced voltage in the operating state between the magnetized state and the demagnetized state of a magnet be large. For this purpose, it is necessary that a magnetization variation relative to a magnetic field change in a sub-loop related to magnetization switching be small. Specifically, it is preferable that the magnetization change from the second and third quadrants to the first and fourth quadrants of a hysteresis curve be small. This preferable condition is expressed in this specification as "the flatness of the sub-curve is high."
[0013] However, in the RTB-based magnetic material described in Patent Document 2, even in the saturation magnetization state, the magnetization variation relative to the magnetic field variation is large. Accordingly, in the sub-loop, when magnetized in a magnetic field lower than the saturation magnetic field, there is a problem that the magnetization variation relative to the magnetic field variation further increases.
[0014] Furthermore, Patent Document 3 discloses that the flatness of the sub-curve in the second and third quadrants is relatively satisfactory when the magnetizing field is 796 kA / m (equivalent to 10 kOe), but there is no evaluation of the flatness of the sub-curve in the first and fourth quadrants. In a case where the flatness of the sub-curve in the first and fourth quadrants is low, it is difficult to specify a reverse magnetic field to change the magnetization, and magnetization control is difficult.
[0015] The invention has been made in consideration of such circumstances, and an object thereof is to provide an RTB-based magnet in which the coercive force and the magnetizing field are small, the residual magnetic flux density is high even in a low magnetizing field state, and the flatness of the sub-curve is high, and a motor and a generator incorporating the RTB-based magnet. PROBLEM-SOLVING MEANS
[0016] To achieve the object according to one aspect of the invention, the following RTB-based magnet is provided.
[0017] [1] An RTB-based magnet containing one or more rare earth elements, one or more transition metal elements, including iron, or two or more transition metal elements, including iron and cobalt, boron, an element M which is gallium or gallium and aluminum, and carbon, in which a content proportion of rare earth elements is “a”, a content proportion of transition metal elements is “b”, a content proportion of boron is “c”, a content proportion of element M is “d”, and a content proportion of carbon is “e”, when the sum of the elements contained in the RTB-based magnet is 100 atom%, and a, b, c, d and e satisfy the following relationships, 14 atom%≤a≤20 atom%, 70 atom%≤b≤82 atom%, 4 atom%≤c≤7 atom%, 0.010≤d / b≤0.035, and 0.033≤e / b≤0.055, the RTB-based magnet main phase crystal grains consisting of a compound with a tetragonal structure of R2T 14 B-type and contains a grain boundary phase present between the main phase crystal grains, the grain boundary phase comprises an RTMC phase containing one or more of the rare earth elements, one or more of the transition metal elements or two or more of the transition metal elements, the element M and carbon, the RTMC phase the relationships R RC > R MP , T RC < T MP , M RC > M MP and C RC > C MP fulfilled, and R RC and M RC the relationship 0.07 ≤ M RC / R RC ≤ 0.65 if the content proportions of the rare earth elements, the transition metal elements, the element M and the carbon contained in the crystal grains of the main phase are each expressed as R MP , T MP , M MP and C MP and the content proportions of the rare earth elements, the transition metal elements, the element M and the carbon contained in the RTMC phase are each defined as R RC , T RC , MRC and C RC be determined.
[0018] [2] The RTB-based magnet according to [1], wherein an average crystal grain size D50 of the main phase crystal grains is 2.50 µm or less.
[0019] [3] The RTB-based magnet according to [1] or [2], where the grain boundary phase contains an ROCN phase in which the contents of rare earth elements, oxygen, carbon and nitrogen are higher than the contents of rare earth elements, oxygen, carbon and nitrogen contained in the main phase crystal grains, an area fraction of the ROCN phase is 10% or more when an area of the grain boundary phase is set to 100%, and a maximum area of a phase in which the content of rare earth elements is higher than the content of rare earth elements contained in the main phase crystal grains, in the grain boundary phase 70 µm 2or less.
[0020] [4] The RTB-based magnet according to any one of [1] to [3], wherein a CV value of a concentration distribution of carbon is 0.85 or less.
[0021] [5] The RTB-based magnet according to any one of [1] to [4], wherein which comprise the rare earth elements Nd and one or more are selected from the group Y, Ce and Sm.
[0022] [6] The RTB-based magnet according to any one of [1] to [5], wherein the rare earth elements consist of R1, R2 and Sm, R1 is one or more of the rare earth elements and includes Nd and does not include Y, Ce and Sm, and R2 is one or more of the elements selected from Y and Ce, and in an (x, y) plane, x and y lie on straight lines forming a pentagon having a point A (0.000; 0.050), a point B (0.000; 0.150), a point C (0.700; 0.100), a point D (0.700; 0.000), and a point E (0.300; 0.000) as vertices, or lie in a region surrounded by the pentagon, wherein the total number of atoms of rare earth elements contained in the RTB-based magnet is set to 1, and a ratio of the number of atoms of R2 to the total number of atoms of rare earth elements is defined as "x", and a ratio of the number of atoms of Sm to the total number of atoms of rare earth elements is defined as "y".
[0023] [7] A motor including the RTB-based magnet according to any one of [1] to [6].
[0024] [8] A generator including the RTB-based magnet according to any one of [1] to [6]. EFFECT OF THE INVENTION
[0025] According to the invention, it is possible to provide an RTB-based magnet in which the coercive force and the magnetizing field are low, the residual magnetic flux density is high even in a low magnetizing field state, and the flatness of the sub-curve is high, as well as a motor and a generator incorporating the RTB-based magnet. BRIEF DESCRIPTION OF THE DRAWINGS Fig. Figure 1 is a schematic hysteresis loop describing properties required for a variable flux magnet; Fig. 2 is a schematic diagram showing a cross section of an RTB-based magnet according to this embodiment; Fig.3 is a diagram showing a relationship between a ratio of the number of R2 atoms and a ratio of the number of Sm atoms in a case where rare earth elements contained in the RTB-based magnet according to this embodiment are composed of R1, R2, and Sm, and a ratio of the total number of atoms is set to 1; Fig. 4 is a schematic cross-sectional view of a motor in which the RTB-based magnet according to this embodiment is incorporated into a rotor; Fig. 5 is a view showing a sub-loop in a case where a magnetic field is set to 240 kA / m, 280 kA / m and 320 kA / m in examples of the invention; Fig. 6 is a view showing a flatness of the sub-curve in the sub-loop in a case where a magnetic field is 320 kA / m in examples of the invention; Fig.Fig. 7 is a view showing a sub-loop in a case where the variation range of the magnetization of the variable magnetic flux magnet is set to a positive range of the magnetization in Fig. 5 is limited; Fig. Fig. 8 is a view showing the induced voltage characteristic of a motor evaluation device in examples of the invention; and Fig. 9 is a view showing the torque characteristic of the motor evaluation device in examples of the invention. EMBODIMENTS FOR CARRYING OUT THE INVENTION
[0026] In the following, the invention is described in detail using a concrete embodiment in the following order. 1. Required properties for variable flux magnet 2. RTB-based magnet 2.1 Main phase crystal grain 2.1.1 Composition of a main phase crystal grain 2.1.2 Crystal grain size of a main phase crystal grain 2.2 Grain boundary phase 2.2.1 RTMC Phase 2.2.2 ROCN Phase 2.2.3 R-rich phase 2.2.4 Identification of the phases forming the grain boundary phase 2.3 Composition of an RTB-based magnet 3. Method for producing an RTB-based magnet 3.1 Processes for producing alloys 3.1.1 HDDR treatment 3.2 Pulverization process 3.3 Shaping process 3.4 Sintering process 4. Engine 5. Effect in this embodiment (1. Required properties for variable flux magnet)
[0027] The RTB-based magnet of this embodiment is a variable flux magnet. The properties required for the variable flux magnet differ from those of a typical RTB-based magnet, which has a high coercive force. Here, the properties required for the variable flux magnet are first described.
[0028] The variable magnetic flux magnet is a magnet capable of switching a magnetization state by repeated magnetization and demagnetization by an external magnetic field, reversibly realizing a high magnetization state and a low magnetization state.In a variable magnetic force motor in which the variable magnetic flux magnet is installed, a magnetization state of the variable magnetic flux magnet is controlled by driving a magnetic field of an armature in accordance with the number of revolutions and a load condition, so that a large magnetic flux is exhibited at an operation time of the magnetization state when high torque is required (at the time of low-speed or high-load rotation), and a small magnetic flux is exhibited at an operation time of the demagnetization state when high torque is not required (at the time of high-speed or low-load rotation).In a variable magnetic flux magnet, the difference between the magnetization at the time of operation in the magnetized state and the magnetization at the time of operation in the demagnetized state increases. Thus, the rate of change of the induced voltage of a motor increases at the time of the magnetized state and the time of the demagnetized state. As a result, the torque variation rate of the variable magnetic flux motor increases, and thus, the efficiency of the motor can be increased.
[0029] A magnetization state of the variable magnetic flux magnet can be switched in accordance with a predetermined sub-loop. The sub-loop is a magnetization change behavior that occurs in a case where, after applying a negative reversing magnetic field, a magnetic field on a Fig.1. The secondary loop in this embodiment is a magnetization change behavior, which is evident in a case where, after magnetization by applying a positive magnetic field Hmag, a negative reversing magnetic field Hrev is applied and then the magnetic field is returned to the magnetic field Hmag.
[0030] As parameters required for the variable flux magnet, the magnetization field Hmag required for magnetization switching must first be reduced, taking into account energy conservation and the upper limit of an externally applied magnetic field. In this embodiment, the magnetization field Hmag is defined as the minimum necessary magnetic field to achieve reproducibility for repeated measurements. To reduce the magnetization field Hmag, the coercive field strength of the variable flux magnet must be small.
[0031] In addition, it is necessary to increase the amount of magnetization fluctuation between the time of magnetization state and the time of demagnetization state of the variable magnetic flux magnet in order to expand a range in which the variable magnetic force motor can operate with high efficiency, and for this purpose, it is required that the residual magnetic flux density Br of the sub-loop in the magnetizing field Hmag is high.
[0032] Furthermore, when passing through a magnetic field from the negative reversal magnetic field Hrev to the magnetic field Hmag on the sub-loop, it is desirable that the magnetization does not vary up to a magnetic field as close as possible to Hmag, i.e., from the second and third quadrants to the first and fourth quadrants of a hysteresis curve. This is because varying magnetization causes problems such as narrowing the variable magnetization range and resulting in difficulties in magnetization control.
[0033] As described above, a variation state of magnetization can be expressed by an index as the flatness of the sub-curve. In this embodiment, the flatness of the sub-curve is defined as a ratio of a magnetic field H _50%Js , in which a magnetization of the secondary loop of 0 is reversed by 50% compared to a saturation magnetization Js, and the coercive field strength HcJ_Hmag . That is, the flatness of the secondary curve is 100 × (H_ 50%Js / HcJ _Hmag ). Since the flatness of the sub-curve is higher, a magnetization deviation from the negative reversal magnetic field Hrev to the magnetic field Hmag becomes smaller, which is preferable.
[0034] If, for example, Fig. 1 the negative reversal magnetic field Hrev = -HcJ _Hmag is applied to Hmag and then the magnetic field is returned to Hmag, the magnetization varies in accordance with ML1 or ML2. In a case where the magnetization varies in accordance with ML1, even when passing from Hrev to Hmag, the magnetization change is small, and H _50%Js is very close to HcJ _Hmag . Accordingly, in a case where the magnetization varies in accordance with ML1, the flatness of the sub-curve is high.
[0035] On the other hand, in a case where the magnetization varies in accordance with ML2, the magnetization varies immediately when passing from Hrev to Hmag, and H _50%Js is considerably smaller than HcJ _Hmag Accordingly, in a case where the magnetization varies along ML2, the flatness of the sub-curve is low.
[0036] Incidentally, RTB-based magnets have a nucleation-type magnetization reversal mechanism. Accordingly, the main-phase crystal grains typically have a multi-domain structure, and within each grain, a magnetic domain boundary exists that remains continuous up to a high magnetic field Hmag. Accordingly, the magnetic domain boundary easily moves in accordance with an externally applied magnetic field, and the magnetization varies greatly. Furthermore, since the nucleation magnetic field is different for each grain, the magnetization also varies greatly in accordance with the externally applied magnetic field due to this factor.
[0037] This means that the RTB-based magnet exhibits poor magnetization performance at a low magnetization field Hmag due to a magnetization reversal mechanism specific to the RTB-based magnet. Furthermore, when passing through a magnetic field from the negative reversal magnetic field Hrev to the magnetic field Hmag on the sub-loop, the magnetization of the RTB-based magnet is more likely to vary compared to a pinning-type magnet due to the magnetization reversal mechanism specific to the RTB-based magnet.
[0038] Therefore, in the RTB-based magnet, in a demagnetization process after magnetization by the positive magnetic field Hmag and in a magnetization process by the negative reverse magnetic field Hrev, in order to suppress the magnetization fluctuation of the magnet, it is preferable that a main phase crystal grain R2T 14B, which is responsible for the magnetic properties of the RTB-based magnet, has a single-domain structure, and the single-domain structure is stable after magnetization even in a case where the magnetizing field Hmag is low. (2nd RTB-based magnet)
[0039] The RTB-based magnet according to this embodiment contains one or more kinds of rare earth elements (R), one or more kinds of transition metal elements (T) including iron, or two or more kinds of transition metal elements (T) including iron and cobalt, boron (B), an element M and carbon (C).
[0040] The rare earth element (R) includes scandium (Sc), yttrium (Y), and lanthanide elements, which belong to Group 3 of the detailed periodic table. The lanthanide elements are lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu). Furthermore, the rare earth element in this embodiment preferably includes Nd and one or more species selected from Y, Ce, and Sm.
[0041] The element M is gallium (Ga), or gallium (Ga) and aluminum (Al). This means that the element M contains gallium.
[0042] Additionally, as in Fig. 2, an RTB-based magnet 1 according to this embodiment includes a main phase crystal grain 2 consisting of a compound having a tetragonal structure of R2T 14B-type, and a grain boundary phase 4, which exists between the main phase crystal grains. The following describes the connection with the tetragonal structure of R2T 14 B-Type also as R2T 14 B compound. As the RTB-based magnet with the Fig. The structure shown in Fig. 2 exemplifies a sintered magnet obtained by sintering a green compact obtained by molding a raw material alloy powder.
[0043] In this embodiment, the RTB-based magnet may include a protective film of a resin, a metal, or the like on a surface to prevent oxidation. (2.1 Main phase crystal grain)
[0044] In this version, the main phase crystal grain resulting from the R2T 14 B compound, exhibits ferromagnetism and is responsible for the magnetic properties of the RTB-based magnet. (2.1.1 Composition of the main phase crystal grain)
[0045] Most of the rare earth elements contained in the RTB-based magnet are contained in the main phase crystal grain. Accordingly, the type of rare earth elements that make up the R2T 14 B compound typically matches the type of rare earth elements contained in the RTB-based magnet, but a match may not be established. This means that some of the rare earth elements contained in the RTB-based magnet may not be included as the rare earth elements that constitute the main phase crystal grain.
[0046] In this embodiment, T is in the R2T 14B compound for one or more types of transition metal elements, including iron (Fe), or for two or more types of transition metal elements, including iron (Fe) and cobalt (Co). Co is an element found in the R2T 14 B compound is included in accordance with the properties required for the RTB-based magnet, and its amount can be determined according to the properties. In this embodiment, when the amount of T is set to 100 atomic%, the amount of Co is preferably 0 to 10 atomic%.
[0047] By adjusting the Co amount within the above-described range, the Curie temperature in the RTB-based magnet can be raised, thus suppressing a decrease in coercive force associated with temperature rise. Furthermore, the corrosion resistance of the RTB-based magnet can be improved.
[0048] In the R2T 14 In the B compound of this design, B stands for boron. Part of the boron (B) can be replaced with carbon (C) in accordance with the properties required for the RTB-based magnet, but it is preferable that the amount of C present within the main phase crystal grain is small. Specifically, a content fraction (concentration) of T contained in the main phase crystal grain is referred to as T. MP (Atom%) and a content fraction (concentration) of C as C MP (atom%), although it is preferable to use a ratio of C MP / T MP ≤ 0.01.
[0049] At C MP / T MP To measure C, it is necessary to accurately measure the concentration of C in the main phase crystal grain. Examples of such a method include a method using a 3-dimensional atom probe (3DAP). (2.1.2 Crystal grain size of a main phase crystal grain)
[0050] In this embodiment, the crystal grain size of the main phase crystal grain is set small enough so that the main phase crystal grain stably exhibits the single-domain structure. This is because the crystal grain size of the main phase crystal grain has a great influence on the properties required for the variable magnetic flux magnet, particularly on the flatness of the sub-curve. In this embodiment, D50 in a crystal grain size distribution of the main phase crystal grain is preferably 2.50 μm or less. Hereinafter, D50 is referred to as the average crystal grain size of the main phase crystal grain. D50 is preferably 2.00 μm or less, and more preferably 1.00 μm or less. Furthermore, D50 is preferably 0.25 μm or more, and even more preferably 0.30 μm or more.D50 is an index of the crystal grain size of the main phase crystal grain, and in a case where D50 is within the range described above, it can be found that the crystal grain size of the main phase crystal grain is small.
[0051] Note that when HDDR treatment is performed, D50 is controlled by the HDDR treatment, an RTMC phase, sintering conditions, and the like, which will be described later. On the other hand, when HDDR treatment is not performed, D50 is controlled by the fine grinding conditions, the RTMC phase, sintering conditions, and the like, which will be described later.
[0052] In a case where D50 is too large, the crystal grain size of the main phase crystal grain increases, and therefore, the single-domain structure of the main phase crystal grain tends to become unstable and the flatness of the sub-curve decreases.
[0053] In a case where D50 is small and grain growth is insufficient, this case represents insufficient sintering, and there is a tendency for voids to form in a sintered body. When voids form, Br tends to decrease, which is undesirable. When D50 decreases, HcJ also tends to decrease. _Hmag tends to increase, which is undesirable. Accordingly, in this design, the lower limit of D50 is preferably 0.25 µm.
[0054] It should be noted that in this embodiment, D50 can be measured, for example, as follows.
[0055] On a polished cross-section of a magnet (sintered body) after sintering, a region with a predetermined area is observed using a scanning electron microscope (SEM) to obtain a backscattered electron image of the region. The polished cross-section can be parallel to an orientation axis, orthogonal to the orientation axis, or at any angle to the orientation axis. The obtained backscattered electron image is analyzed using known software to identify the main phase crystal grain. Contours of a predetermined number of main phase crystal grains are extracted to calculate an area of the main phase crystal grains, and a diameter of a circle (equivalent circle diameter) with an area in which an accumulated distribution of the area of the main phase crystal grains becomes 50% can be determined as D50.
[0056] For example, the area to be observed is preferably 10 to 40 µm square. Furthermore, the number of main phase crystal grains for which an area is calculated is preferably 150 to 300. (2.2 Grain boundary phase)
[0057] As in Fig. As shown in Figure 2, the grain boundary phase 4 exists between the main-phase crystal grains 2. The grain boundary phase 4 mainly includes a two-junction grain boundary 4a formed between two main-phase crystal grains and a three-junction grain boundary 4b formed between three or more main-phase crystal grains. The grain boundary phase consists of various phases with a composition different from that of the main-phase crystal grain. For example, the phases constituting the grain boundary phase can be identified by a method to be described later. (2.2.1 RTMC Phase)
[0058] In this embodiment, the grain boundary phase contains an RTMC phase. The RTMC phase contains at least one rare earth element, one transition metal element, one element M, and carbon. If the content ratios (atomic %) of the rare earth element, the transition metal element, the element M, and carbon contained in the main phase crystal grain are each expressed as R MP , T MP , M MP and C MP and the content proportions (atomic %) of the rare earth element, the transition metal element, the element M and the carbon contained in the RTMC phase are each expressed as R RC , T RC , M RC and C RC be set, then the RTMC phase is a range in which the relationships R RC > R MP , T RC < T MP , M RC > M MP , and C RC > C MP are fulfilled.
[0059] In other words, the grain boundary phase is a region where more elements M and carbon are present than the elements M and carbon contained in the main phase crystal grain. It is likely that the RTMC phase is formed due to the presence of a large amount of elements M and carbon in the grain boundary phase.
[0060] In this embodiment, the element M is gallium (Ga) or gallium (Ga) and aluminum (Al). This means that element M is present in the RTMC phase at least as gallium.
[0061] It should be noted that the rare earth element species contained in the RTMC phase may be equal to or less than the rare earth element species contained in the RTB-based magnet.
[0062] When the RTMC phase is formed in the grain boundary phase during sintering, fine main phase crystal grains can grow evenly. As a result, the average grain size D50 of the main phase crystal grain after sintering does not increase too much compared to that before sintering and can be controlled within the range described above. As a result, it is possible to obtain a dense sintered body with few voids. In other words, since the RTMC phase is formed in the grain boundary phase, it is possible to control the grain growth of the main phase crystal grain, and it is easy to control the D50 of the main phase crystal grain within the range described above.
[0063] In this version, M RC / R RC in the RTMC phase 0.07 to 0.65. If M RC / R RCBy adjusting the ratio of the RTMC phase to the RTB-based magnet, the ratio of the RTMC phase to the RTB-based magnet becomes appropriate, and at a sintering temperature at which a dense sintered body is obtained, the main phase crystal grain is properly grown, and thus D50 can be adjusted within the range described above. Accordingly, the flatness of the sub-curve tends to be improved.
[0064] M RC / R RC is preferably 0.10 or more. In addition, M RC / R RC preferably 0.56 or less.
[0065] In a case where M RC / R RC is too large, the ratio occupied by the RTMC phase in the RTB-based magnet increases excessively, and thus the ratio occupied by the main phase tends to decrease. As a result, the residual magnetic flux density Br tends to decrease.
[0066] In a case where M RC / R RC If the sintering angle is too small, the RTMC phase tends to be less likely to form, the crystal grain size of the main phase grains is difficult to control, and abnormal grain growth and the formation of coarse main phase grains occur, even at a low firing temperature, which does not produce a dense sintered body. As a result, the flatness of the sub-curve tends to decrease.
[0067] In addition, the C RC / P RC -value in the RTMC phase preferably between 0.10 and 0.87. If C RC / R RCBy adjusting the RTMC phase within this range, the ratio occupied by the RTMC phase in the RTB-based magnet tends to become appropriate, and the main phase crystal grain is caused to grow appropriately at a sintering temperature at which a dense sintered body is obtained, so that D50 can be adjusted within the range described above. Furthermore, the magnetism of the RTMC phase tends to be non-ferromagnetic. As a result, the flatness of the sub-curve tends to be improved.
[0068] C RC / R RC is preferably 0.31 or more. On the other hand, C RC / P RC preferably 0.82 or less.
[0069] In a case where the C RC / R RCis excessively large, the sintering temperature at which the dense sintered body is obtained tends to become high. If the sintering temperature is too high, although the RTMC phase is formed, it is difficult to suppress abnormal grain growth. On the other hand, if sintering is carried out at a low firing temperature at which abnormal grain growth does not occur, voids tend to form in the sintered body. As a result, the residual magnetic flux density Br tends to decrease.
[0070] In a case where the C RC / R RCIf the RTMC phase is too small, it tends to be less likely to form, making it difficult to control the crystal grain size of the main phase crystal grain. Abnormal grain growth and the formation of coarse main phase crystal grains occur, even at a temperature where the dense sintered body cannot be obtained. As a result, the flatness of the sub-curve tends to decrease.
[0071] It should be noted that boron (B) may be present in the RTMC phase, but it is preferable that its concentration be low. Especially when a content fraction (atomic %) of the boron contained in the RTMC phase is considered as B. RC is defined, B RC / P RC preferably less than 0.30 and more preferably 0.24 or less.
[0072] In addition, oxygen (O) may be present in the RTMC phase, but it is preferable that its concentration is low. In particular, if a content fraction (atomic %) of the oxygen contained in the RTMC phase is expressed as O RC is defined as O RC / R RC preferably less than 0.20. (2.2.2 ROCN Phase)
[0073] In this embodiment, it is preferable that the grain boundary phase contains an ROCN phase. The ROCN phase is a region containing at least one rare earth element, oxygen, carbon, and nitrogen, and in which the content ratios (atomic %) of the rare earth element, oxygen, carbon, and nitrogen are higher than the content ratios (atomic %) of the rare earth element, oxygen, carbon, and nitrogen contained in the main phase crystal grain.
[0074] The ROCN phase is probably formed due to the presence of a large amount of carbon in the grain boundary phase.
[0075] It should be noted that the rare earth element species contained in the ROCN phase may be equal to or smaller than the rare earth element species contained in the RTB-based magnet.
[0076] In a case where the grain boundary phase includes the ROCN phase, when an area of the entire grain boundary phase is set to 100%, an area ratio of the ROCN phase is preferably 10% or more. In the grain boundary phase, the ROCN phase is likely to exist in a state of dispersion rather than in a state of aggregation. Accordingly, when the area ratio of the ROCN phase satisfies the above-described range, the ROCN phase is formed in a state where it is reasonably dispersed, and thus, among the phases constituting the grain boundary phase, an R-rich phase likely to aggregate into the triple junction is divided by the ROCN phase. As a result, it is possible to suppress a maximum area of the R-rich phase formed at the triple junction.
[0077] The area ratio of the ROCN phase is preferably 30% or more, and more preferably 52% or more. On the other hand, the area ratio of the ROCN phase is preferably 60% or less, and more preferably 57% or less. (2.2.3 R-rich phase)
[0078] The R-rich phase is a phase in which the content ratio of the rare earth element contained in the R-rich phase is higher than the content ratio of the rare earth element contained in the main phase crystal grain. Examples of the R-rich phase include the RTMC phase described above and an RTBC phase in which the content ratios of the rare earth element, boron, and carbon are higher than the content ratios of the rare earth element, boron, and carbon contained in the main phase crystal grain, and the content ratio of the transition metal element is lower than the content ratio of the transition metal element contained in the main phase crystal grain.
[0079] In this embodiment, a maximum area of the R-rich phase in the grain boundary phase is preferably 70 µm 2 or less, preferably 60 µm 2 or less and more preferably 13.2 µm 2 or less.
[0080] The R-rich phase is likely to aggregate and form at the triple junction and is diamagnetic or paramagnetic. Accordingly, when the R-rich phase is formed at the triple junction, a stray magnetic field converges from a magnetization of a neighboring main-phase crystal grain and then penetrates and envelops the grain boundary phase, and a local demagnetization field is likely to be generated in the R-rich phase. When the area of the R-rich phase formed at the triple junction is large, the generated demagnetization field becomes large, and especially at high temperature, a nucleation field of the reverse magnetic domain of the main-phase crystal grain decreases significantly. As a result, an absolute value of the temperature coefficient β of the coercive force becomes large.
[0081] In other words, when the area ratio of the ROCN phase falls within the range described above, it is possible to reduce the area of the R-rich phase formed at the triple junction and thus suppress an absolute value of the temperature coefficient β of the coercive field strength.
[0082] It should be noted that since the proportion of the rare earth element contained in the ROCN phase is higher than that in the main phase crystal grain, the ROCN phase is also contained in the R-rich phase. However, as described above, the ROCN phase is likely to be formed in a dispersed state, and therefore, the possibility that the R-rich phase exhibiting the maximum area is the ROCN phase is very low.
[0083] Furthermore, the RTMC and RTBC phases are carbonaceous phases. Accordingly, the suppression of the maximum area of these phases at the grain boundary phase indicates that carbon is locally absent and distributed in a relatively dispersed state within the RTB-based magnet.
[0084] In this embodiment, the carbon concentration distribution is expressed by the value of the coefficient of variation (CV). The CV value of the carbon concentration distribution is preferably 0.85 or less, more preferably 0.67 or less, and even more preferably 0.50 or less. When the CV value falls within this range, it is possible to suppress the absolute value of the temperature coefficient β of the coercive force. (2.2.4 Identification of the phases that form the grain boundary phase)
[0085] In this embodiment, the identification of the phases constituting the grain boundary phase can be performed as follows. First, as in the D50 measurement of the main phase crystal grain, the main phase crystal grain and the grain boundary phase are identified from a backscattered electron image of a cross-section of the RTB-based magnet using an SEM.
[0086] In the backscattered electron image, the grain boundary phase is formed by a region where the contrast differs from that of the main phase crystal grain. Furthermore, the contrast difference reflects a compositional difference between the main phase crystal grain and the grain boundary phase. Accordingly, it can be understood that the grain boundary phase is formed by a phase with a different composition than the main phase crystal grain.
[0087] Next, with respect to the cross-section, a distribution of the elements present on the cross-section is measured with an electron probe microanalyzer (EPMA) using a wavelength dispersive X-ray spectrometer to obtain element mapping data.
[0088] Next, the composition of each grain boundary phase included in the elemental mapping data of the cross-section is quantitatively measured based on the characteristic X-ray intensity of each element, and a phase corresponding to the above-described composition conditions of the phase on the backscattered electron image is specified. That is, from the composition measurement results of the grain boundary phase, a region belonging to the RTMC phase, the ROCN phase, the RTBC phase, or the like is specified.
[0089] In addition, M RC / R RC and C RC / R RCcalculated from values of the characteristic X-ray intensity of the respective element in the identified RTMC phase.
[0090] After specifying the respective phases on the backscattered electron image with respect to a single enclosed region belonging to the R-rich phase, the number of pixels is calculated. A phase in which the number of pixels is the largest is the R-rich phase with the largest area. Furthermore, an area of one pixel is calculated from a scale bar of the backscattered electron image or the like. The product of the number of pixels of the R-rich phase with the largest area and the area of the one pixel can be set as the maximum area of the R-rich phase. Furthermore, an area ratio of the ROCN phase to all grain boundary phases can be calculated as the ratio of the number of pixels belonging to the ROCN phase when the number of pixels belonging to all grain boundary phases is set to 100%.
[0091] Furthermore, with regard to the CV value of the carbon concentration distribution in the element mapping data, information on the carbon detection amount is obtained by the EPMA for each measurement point (pixel). From the obtained information regarding the carbon detection amount, the standard deviation of the carbon detection amount and the mean value of the carbon detection amount at the measurement points are calculated, and the CV value can be calculated from the following expression. CV value = standard deviation of the detected carbon amount / average value of the detected carbon amount (2.3 Composition of an RTB-based magnet)
[0092] In the RTB-based magnet according to this embodiment, the content ratio a of the rare earth element (R) is 14 to 20 atomic%, the content ratio b of the transition metal element (T) is 70 to 82 atomic%, and the content ratio c of boron (B) is 4 to 7 atomic%.
[0093] In this embodiment, the ratio between M and T is within a predetermined range. Specifically, the ratio is 0.009 ≤ d / b ≤ 0.035. When d / b is within the above-described range, the ratio occupied by the RTMC phase in the RTB-based magnet tends to become appropriate, the main phase crystal grain is properly grown at a sintering temperature at which a dense sintered body is obtained, and D50 is thus adjusted within the above-described range. As a result, the flatness of the sub-curve tends to be improved.
[0094] d / b is preferably 0.014 or more. On the other hand, d / b is preferably 0.030 or less.
[0095] In a case where d / b is too large, the ratio occupied by the RTMC phase in the RTB-based magnet tends to become excessively large, and thus the ratio occupied by the main phase tends to decrease. As a result, the residual magnetic flux density Br tends to decrease.
[0096] In a case where d / b is too small, the RTMC phase tends to be less likely to form, making it difficult to control the crystal grain size of the main phase crystal grain. Abnormal grain growth and the formation of coarse main phase crystal grains occur, even at a temperature where a dense sintered body is not obtained. As a result, the flatness of the sub-curve tends to decrease.
[0097] Furthermore, in this embodiment, a ratio between C and T is within a predetermined range. Specifically, a ratio of 0.025 ≤ e / b ≤ 0.055 is established. When e / b is within the range, a ratio occupied by the RTMC phase in the RTB-based magnet becomes appropriate, and the main phase crystal grain tends to grow appropriately at a sintering temperature at which a dense sintered body is obtained, and D50 can be adjusted within the above-described range. As a result, the flatness of the sub-curve tends to be improved.
[0098] e / b is preferably 0.033 or more. On the other hand, e / b is preferably 0.050 or less.
[0099] In a case where e / b is excessively large, the sintering temperature at which a dense sintered body is obtained tends to become high. If the sintering temperature is too high, it is difficult to suppress abnormal grain growth even if the RTMC phase is formed. On the other hand, if sintering is carried out at a low firing temperature at which abnormal grain growth does not occur, voids tend to form in the sintered body. As a result, the residual magnetic flux density Br tends to decrease.
[0100] In a case where e / b is too small, the RTMC phase tends to be less likely to form, making it difficult to control the crystal grain size of the main phase crystal grain, and abnormal grain growth occurs, and coarse main phase crystal grains are formed even at a temperature where the dense sintered body cannot be obtained. As a result, the flatness of the sub-curve tends to decrease.
[0101] Furthermore, in this embodiment, from the viewpoint of obtaining a variable magnetic flux magnet with satisfactory properties, it is preferable that the rare earth element of the RTB-based magnet contains Nd and at least one or more types selected from Y, Ce, and Sm as described above. Furthermore, it is preferable that the rare earth element be divided into three groups of R1, R2, and Sm. Specifically, R1 represents one or more types of rare earth elements containing Nd and excluding Y, Ce, and Sm; R2 represents one or more types of elements selected from Y and Ce.
[0102] An anisotropy field of an R2T 14 B compound containing Y and Ce as R is smaller than that of an R2T 14 B compound containing R1, such as Nd. Since a Sm2T 14 B compound also has an in-plane anisotropy, the strong anisotropy field of the R2T14 B compound with a small amount of Sm2T 14 B compound can be drastically reduced. Here, if Nd is replaced with one or more species selected from Y, Ce, and / or Sm, the coercive force of the RTB-based magnet can be reduced. Furthermore, by controlling the substitution ratio of R1 to R2 and Sm, it is possible to further improve the magnetic properties suitable for the variable flux magnet in addition to reducing the coercive force of the RTB-based magnet.
[0103] In a case where the rare earth elements contained in the RTB-based magnet are composed of R1, R2 and Sm, if the total number of atoms of the rare earth elements is set to 1, a ratio of the number of atoms of R2 to the total number of atoms of the rare earth elements is set to “x”, and a ratio of the number of atoms of Sm to the total number of atoms of the rare earth elements is set to “y”, R indicating the rare earth element can be expressed as (R1 1-x-y R2 x Sm y ) can be expressed.
[0104] It is preferable that x and y lie on the straight side lines forming a pentagon having a point A (0.000; 0.050), a point B (0.000; 0.150), a point C (0.700; 0.100), a point D (0.700; 0.000) and a point E (0.300; 0.000) as vertices, or in the area (a hatched part in Fig. 3), which is surrounded by the pentagon, are as in Fig. 3. If x and y are within the Fig. 3, the coercive field strength of the magnet is further lowered, the magnetizing field is also lowered, and it is possible to obtain a satisfactory flatness of the sub-curve and a high residual magnetic flux density in the low magnetizing field.
[0105] In addition, it is preferable that x and y lie on straight lines connecting the points F (0.000; 0.075), G (0.000; 0.125), H (0.100; 0.125), I (0.200; 0.100), J (0.200; 0.050) and K (0.100; 0.075) located in Fig. 3 are shown in this order clockwise, or fall into the area (a hatched area in Fig. 3), which is surrounded by the straight side lines. If x and y are within the Fig. 3 shown above, the effect described above can be enhanced.
[0106] Furthermore, it is further preferable that x and y satisfy the relationship x = 0 and 0.075 ≤ y ≤ 0.125. That is, it is further preferable that R1 be replaced by Sm in the range described above. When x and y satisfy the relationships, the above-described effect can be further enhanced.
[0107] In this embodiment, from the standpoint of obtaining a magnet with variable magnetic flux and satisfactory properties, a proportion occupied by Fe or Fe and Co in the transition metal element of the RTB-based magnet is preferably 0.90 or more.
[0108] The RTB-based magnet may contain an element A that promotes a reaction of the main phase crystal grain in a powder metallurgy process. The element A is one or more types selected from the group consisting of copper (Cu), zirconium (Zr), and niobium (Nb). The total amount of these elements contained is preferably in a range of 0.05 to 1.00 atomic% when the total amount of elements contained in the RTB-based magnet is set to 100 atomic%. Note that the amount of Cu contained is preferably 0.20 atomic% or less.
[0109] When copper is added to the RTB-based magnet, a surface layer of the main phase crystal grain undergoes a reaction, which can remove distortion, defects, and the like. Furthermore, the addition of zirconium and / or niobium to the RTB-based magnet prevents coarsening of the main phase crystal grain during sintering, allowing the RTB-based magnet to be densified while maintaining a fine grain size.
[0110] In addition, the RTB-based magnet may contain titanium (Ti), tantalum (Ta), vanadium (V), silver (Ag), germanium (Ge), or the like. Furthermore, the RTB-based magnet may contain unavoidable impurities, such as impurities derived from the raw material and impurities added during manufacturing. In this embodiment, the total amount of elements such as Ti and unavoidable impurities in the RTB-based magnet is preferably 1 atomic% or less.
[0111] Furthermore, the RTB-based magnet may contain oxygen (O) within a predetermined range. The amount of oxygen (O) contained is preferably 1000 to 8000 ppm. If the amount of O contained is too small, the corrosion resistance of the magnet will be insufficient. If the amount of O contained is too large, a liquid phase will not form sufficiently in the magnet, resulting in a decrease in coercive force. To obtain more satisfactory corrosion resistance and coercive force, a range of 1500 to 3000 ppm is preferable.
[0112] Furthermore, the RTB-based magnet can contain nitrogen (N) within a predetermined range. The amount of N contained is preferably 8000 ppm or less. If the amount of N contained is too large, the coercive force tends to become insufficient.
[0113] The composition of the RTB-based magnet after sintering can be measured, for example, by inductively coupled plasma atomic emission spectroscopy (ICP-AES).
[0114] In addition, a method commonly known as the standard method can be used to measure the amount of oxygen, carbon, and nitrogen contained in the RTB-based magnet after sintering. The amount of oxygen is measured using, for example, an inert gas melt non-dispersive infrared absorption method; the amount of carbon is measured using, for example, an oxygen flow combustion infrared absorption method; and the amount of nitrogen is measured using, for example, an inert gas melt thermal conductivity method. (3. Method for manufacturing an RTB-based magnet)
[0115] Next, an example of a method for manufacturing the RTB-based magnet according to this embodiment will be described below. (3.1 Processes for producing alloys)
[0116] First, raw material metals are prepared for the production of the RTB-based magnet according to this design. The raw material metals are melted in a vacuum or inert gas atmosphere to produce a raw material alloy with a specified composition.
[0117] Examples of raw material metals include rare earth metals or rare earth alloys, pure iron, ferroboron, and their alloys. The composition of the raw material alloy can be adjusted according to the desired composition of the RTB-based magnet. Additionally, the raw material metal of element M can be added during melting.
[0118] A method for obtaining the raw material alloy by melting the raw material metals is not particularly limited as long as it is a known melting method, and examples include a strip casting method and high-frequency induction melting. The atmosphere at the time of melting is preferably set to a vacuum or an inert gas, and more preferably to an argon (Ar) atmosphere.
[0119] In the strip casting process, a molten metal of the raw material alloy, obtained by melting the raw material metals in a non-oxidizing atmosphere such as an Ar atmosphere, is discharged onto the surface of a rotating roller. The molten metal, rapidly cooled on the roller, rapidly solidifies into a thin plate or flake. The rapidly solidified alloy has a homogeneous structure with a crystal grain size of 1 to 50 µm. In addition, an alloy obtained by a reducing diffusion process can be used as the raw material alloy.
[0120] In this embodiment, as a method for manufacturing a magnet using the raw material alloy, a so-called single alloy method using one kind of raw material alloy is used, however, a so-called mixed method using a main phase forming raw material alloy (low-R alloy) mainly having an R2T 14 B compound, which is a main phase crystal grain, and a grain boundary phase-forming raw material alloy (high-R alloy) which contains more R than the low-R alloy and effectively contributes to the formation of a grain boundary phase. (3.1.1 HDDR treatment)
[0121] In this embodiment, it is preferable to subject the raw material alloy to hydrogenation-disproportionation-desorption-recombination (HDDR) treatment. HDDR treatment is a process for chemically obtaining a fine crystal grain by sequentially performing hydrogenation, disproportionation, desorption, and recombination of the raw material alloy. When the RTB-based magnet is manufactured using the raw material alloy obtained by HDDR treatment, the crystal grain size of the main phase crystal grain after sintering can be reduced and its grain size distribution can be narrowed.
[0122] In HDDR treatment, the raw material alloy is kept at 700°C to 900°C in an H2 gas atmosphere or a mixed atmosphere of H2 gas and an inert gas to hydrogenate the raw material alloy. Then, the raw material alloy is subjected to dehydrogenation treatment at 700°C to 900°C until the partial pressure of the H2 gas in the atmosphere reaches 13 Pa or less, and then the raw material alloy is cooled. This produces a fine-structure HDDR alloy. (3.2 Pulverization process)
[0123] The produced raw material alloy (the HDDR alloy or a raw material alloy not subjected to HDDR treatment) undergoes a pulverization process. In the case of the mixed process, a low-R alloy and a high-R alloy are pulverized individually or in combination. The pulverization process can be divided into a coarse and a fine grinding process. First, the raw material alloy is coarsely pulverized until a particle size of several hundred µm is achieved.
[0124] Hydrogen crushing is effective as coarse crushing, in which crushing is carried out by dehydrogenation after hydrogen is absorbed into the raw material alloy. The dehydrogenation treatment is carried out to reduce hydrogen, which becomes an impurity in a sintered rare earth magnet. The temperature at the time of hydrogen absorption is room temperature. The holding temperature for dehydrogenation after hydrogen absorption is set at 200°C to 400°C or higher, preferably 300°C. The holding time varies depending on the relationship to a holding temperature, the composition and weight of the raw material alloy, etc., and is set to at least 30 minutes or longer per 1 kg, preferably one hour or longer. The dehydrogenation treatment is carried out in a vacuum or in an Ar gas stream.
[0125] In this embodiment, the coarse crushing process is preferably hydrogen crushing, but mechanical coarse crushing may be further performed on the raw material alloy by using a punch mill, a jaw crusher, a brown mill, or the like.
[0126] After the coarse crushing process, a fine crushing process is carried out. A jet mill is mainly used for fine crushing. After coarse crushing, powder with a particle size of approximately several hundred µm is pulverized until an average particle size of 1.2 to 4 µm, preferably 1.5 to 3 µm, is achieved. The jet mill generates a high-speed gas flow by releasing a high-pressure inert gas from a narrow nozzle. The coarsely pulverized powder is accelerated by the high-speed gas flow, causing it to collide with the coarsely pulverized powder or collide with a target or container wall for pulverization. The pulverized powder is classified by a classifying rotor embedded in a pulverizer and a cyclone downstream of the pulverizer.
[0127] Wet grinding can be used for fine grinding. In wet grinding, a ball mill, wet attritor, or similar equipment can be used. The coarsely ground powder, with a particle size of approximately several hundred µm, is pulverized until an average particle size of 1.5 to 4 µm, or preferably 2 to 3 µm, is achieved. Since wet grinding pulverizes an alloy without contacting the alloy powder with oxygen, selecting a suitable dispersion medium results in a fine powder with a low oxygen concentration.
[0128] In this embodiment, as a carbon source of the RTMC phase and for the purpose of lubrication in a molding process to be described later, improving the orientation of a magnet, or the like, a fatty acid or a derivative of the fatty acid, hydrocarbons, or the like may be added to the powder in an amount of about 0.5 to 2.0 wt% at the time of fine grinding and / or after fine grinding.
[0129] Examples of the fatty acid or fatty acid derivative are zinc stearate, calcium stearate, aluminum stearate, stearic acid amide, oleic acid amide, ethylenebisisostearic acid amide and lauric acid amide, and examples of the hydrocarbons are paraffin and naphthalene. (3.3 Forming process)
[0130] Next, the powder is shaped after fine grinding. In this design, the shaping takes place under the application of a magnetic field. The forming pressure in the magnetic field can be adjusted to a range of 0.3 to 3 tons / cm 2 (30 to 300 MPa). The molding pressure can be constant from the beginning to the end of the molding process, gradually increased or decreased, or vary irregularly. Since the molding pressure is low, the orientation remains satisfactory. However, if the molding pressure is too low, the strength of a green compact is insufficient, causing a problem in handling. Accordingly, the molding pressure can be adjusted taking this situation into account. A final relative density of the green compact achieved by the magnetic field molding process is typically 40% to 60%.
[0131] The applied magnetic field can be adjusted to approximately 960 to 1600 kA / m. The applied magnetic field is not limited to a static magnetic field and can be a pulsed magnetic field. Furthermore, the static magnetic field and the pulsed magnetic field can be used in combination. (3.4 Sintering process)
[0132] The green compact undergoes a sintering process. Sintering takes place in a vacuum or in an inert gas atmosphere. The holding temperature and holding time can be adjusted depending on the composition of the magnet, the pulverization method of the alloy powder, the average crystal grain size, the grain size distribution of the main phase crystal grains, and the like. In this embodiment, the holding temperature is preferably 800°C to 1000°C, and the holding time is preferably 1 minute to 20 hours. The holding period is preferably 4 to 20 hours.
[0133] In this design, the RTMC phase is formed in a grain boundary phase at the time of sintering, and thus a fine R2T 14 B crystal grains are shaped to a certain extent, suppressing abnormal grain growth. As a result, the crystal grain size of the main phase crystal grain can be adjusted to within the range of D50.
[0134] After sintering, the resulting sintered body can be subjected to aging treatment. The aging treatment conditions can be adjusted appropriately, taking into account the microstructure of the sintered body. For example, the treatment temperature can be set within a temperature range of 400°C to 900°C. (4th engine)
[0135] A configuration of a motor according to this embodiment is not particularly limited as long as the motor includes the RTB-based magnet. However, in this embodiment, the RTB-based magnet is incorporated into a rotor of the motor. Fig. 4 shows an example of a motor 10 according to this embodiment.
[0136] Fig. Fig. 4 is a cross-sectional view of the motor 10 according to this embodiment from the direction of the rotation axis, and since the motor has a 90-degree rotational symmetry, symmetrical parts are omitted. As in Fig. 4, the motor 10 includes a rotor 11 and a stator 16.
[0137] The rotor 11 includes a rotor iron core 12 and a stacked magnet 15. The rotor iron core 12 is made of stacked electromagnetic steel plates. The stacked magnet 15 includes a variable magnetic flux magnet 13 formed by the RTB-based magnet according to this embodiment, and fixed magnetic flux magnets 14a and 14b formed by a permanent magnet with a coercive force and magnetization greater than those of the variable magnetic flux magnet 13. Furthermore, the stacked magnet 15 is embedded in the rotor iron core 12.
[0138] As in Fig. 4, the fixed flux magnets 14a and 14b are arranged to overlap the two main surfaces of the variable flux magnet 13 in the thickness direction of the stacked magnet 15 and are integrated therewith. In addition, as shown in Fig.As shown in Figure 4, the magnetization directions of the variable flux magnet 13 and the fixed flux magnets 14a and 14b are arranged parallel to the thickness direction of the stacked magnet 15. That is, the variable flux magnet 13 and the fixed flux magnets 14a and 14b are magnetically arranged in series, so that the magnetization directions of the variable flux magnet 13 and the fixed flux magnets 14a and 14b are the same. The magnetization direction (center axis direction) of the stacked magnet 15 becomes the d-axis, and the center axis direction between the stacked magnets becomes the q-axis.
[0139] The stator 16 is arranged on an outer peripheral side of the rotor 11 through an air gap. The stator 16 includes an armature iron core 17 and an armature winding 18. A magnetic field is generated by briefly applying a large d-axis current to the armature winding 18, and the magnetization of the variable magnetic flux magnet 13 is reversibly changed to reversibly change the magnitude of the magnetic flux.
[0140] In the variable magnetic flux magnet, the difference between the magnetization at the time of magnetization and the magnetization at the time of demagnetization increases, and the rate of change of the induced voltage of a motor increases at the time of magnetization and demagnetization. As a result, the torque variation rate of the variable magnetic flux motor increases, which can increase the motor's efficiency.
[0141] In particular, the efficiency of the motor can be further increased by using the stacked magnet 15 in which the fixed flux magnets 14a and 14b and the variable flux magnet 13 are stacked in series.
[0142] In a case where the variable flux magnet 13 is embedded instead of the stacked magnet 15 alone, an operating point of the motor during typical operation lies in an irreversible demagnetization region beyond a reversal point of a magnetization curve of the variable flux magnet 13 with a small coercive force. Therefore, it is difficult to effectively utilize an inherent residual magnetic flux density Br of the variable flux magnet 13 and a magnetic flux in a maximum magnetization state. A variation amount of the magnetic flux between a magnetic flux in a magnetization state and a demagnetization state also decreases. As a result, the efficiency of a motor corresponding to the inherent performance of the variable flux magnet 13 is not achieved.
[0143] In contrast, when using the stacked magnet 15, the operating point of the variable magnetic flux magnet 13 is shifted in a positive magnetic field direction during typical operation and can be maintained within a reversible range that does not exceed the inversion point of the magnetization curve. Furthermore, the magnetic flux in the maximum magnetized state and the fluctuation range of the magnetic flux between the magnetized state and the demagnetized state can be increased.
[0144] Furthermore, in a case where a magnet with fixed and a magnet with variable magnetic flux, as in Fig. 4, are stacked in series, it is preferable that the fixed magnetic flux magnets 14a and 14b are arranged so that the two main surfaces of the variable magnetic flux magnet 13 are located therebetween. Instead of the Fig.4, in the case of the variable magnetic flux magnet 13 alone or in a case where the fixed magnetic flux magnet 14 is arranged to be stacked on a single surface of the variable magnetic flux magnet 13, a direction of magnetic field lines passing through the interior of the variable magnetic flux magnet 13 caused by the d-axis current deviates from a magnetization direction as it moves away from the air gap. As a result, a magnetic field acting on the interior of the variable magnetic flux magnet 13 becomes non-uniform, and a magnetization state within the variable magnetic flux magnet 13 also becomes non-uniform.
[0145] In contrast, in the Fig.With the arrangement shown in Figure 4, the direction of the magnetic field lines passing through the interior of the variable flux magnet 13 is aligned with the magnetization direction, thus making the magnetic field acting on the interior of the variable flux magnet 13 uniform, and the magnetization state inside the variable flux magnet 13 also uniform. Consequently, the magnetic flux in the maximum magnetization state and the fluctuation range between the magnetic flux in the magnetization state and the magnetic flux in the demagnetization state can be increased.
[0146] Note that the RTB-based magnet according to this embodiment is also appropriately applied to a generator, but a configuration of the generator is the same as the configuration of the motor, and therefore, its description is omitted. (5. Effect in this embodiment)
[0147] In this embodiment, in order to obtain the RTB-based magnet as a suitable variable magnetic flux magnet, the RTMC phase in which the R concentration, the M concentration and the C concentration are higher than that in the main phase crystal grain and the T concentration is lower than that in the main phase crystal grain is between the main phase crystal grains consisting of the R2T 14 B compound is present. The RTMC phase is formed at the grain boundary phase during sintering, and thus, the grain growth of the main phase crystal grain can be controlled, and abnormal grain growth of the main phase crystal grain can be suppressed, while the main phase crystal grain can grow to a certain extent, thereby obtaining a dense sintered body.
[0148] As a result, the single-domain structure of the main-phase crystal grain is stabilized, and deviations in the nucleation magnetic field of the main-phase crystal grain are suppressed. Accordingly, problems of magnetization properties in low magnetic fields and steep slopes of the sub-loop, which were difficult to solve due to the mechanism of the nucleation magnet, are solved. The properties required for variable-flux magnets, especially the flatness of the sub-loop, can be achieved satisfactorily when using the RTB-based magnet as a variable-flux magnet.
[0149] In addition, when D50 of the main phase crystal grain is set within the range described above, the single-domain structure of the main phase crystal grain can be further stabilized, so that the flatness of the sub-curve becomes further satisfactory.
[0150] Furthermore, when the structure of the grain boundary phase is controlled as described above, it is possible to suppress a decreasing rate of coercive force at high temperature while satisfactorily maintaining the flatness of the sub-curve.
[0151] If R1 is replaced by a rare earth element capable of generating a high anisotropy field of the R12T 14 B compound formed by a Nd2T 14B compound, it is possible to realize a low coercive force while maintaining the properties required for the variable magnetic flux magnet because the rare earth element is contained in the RTB-based magnet. Specifically, by controlling a substitution ratio of Y and / or Ce with respect to R1 and a substitution ratio of Sm with respect to R1, it is possible to lower the magnetizing field while reducing the coercive force, and it is possible to achieve satisfactory residual magnetic flux density and sub-curve flatness at the low magnetizing field.
[0152] The embodiment of the invention has been described above. The invention is not limited to the embodiment and can be modified in various aspects within the scope of the invention. EXAMPLES
[0153] The invention is described in more detail below using examples. However, the invention is not limited to the following examples. (Experiment Example 1)
[0154] First, raw materials were mixed to obtain an RTB-based magnet having the composition shown in Table 1, the raw materials were melted, and the resulting molten metal was cast by a strip casting method to obtain a raw material alloy having a flake shape.
[0155] Next, HDDR treatment was performed on raw material alloys of samples according to Experimental Examples 1-1 to 1-17. During the HDDR treatment, each of the raw material alloys was kept at 800°C in an H2 gas atmosphere to be hydrogenated, then subjected to dehydrogenation treatment at 800°C until the partial pressure of the H2 gas in the atmosphere was 1 Pa or less, and then cooled to obtain an HDDR alloy. HDDR treatment was not performed on raw material alloys of samples according to Experimental Examples 1-18 to 1-21.
[0156] Next, the following hydrogen pulverization was performed. Specifically, hydrogen was absorbed into the HDDR alloy at room temperature, the HDDR alloy was subjected to heat treatment at 300°C in an Ar atmosphere for one hour, and then cooled to room temperature. Heat treatment was then performed again in a vacuum atmosphere at 300°C for one hour. The resulting pulverized product was then cooled to room temperature in the Ar atmosphere.
[0157] Subsequently, 0.5 to 2.0 mass% of lauric acid amide was added to a coarsely pulverized powder as a carbon source in a grain boundary phase and as a pulverization aid, and fine grinding was performed using a jet mill. For fine grinding, the speed of a classifying rotor of the jet mill was adjusted so that the average particle size of a finely pulverized powder was 1.5 µm for the samples according to Experimental Examples 1-1 to 1-18 and 1-20, and the average particle size of the finely pulverized powder was 2.0 µm for the samples according to Experimental Examples 1-19 and 1-21.
[0158] The obtained finely pulverized powder was filled into a mold placed in an electromagnet and molded in a magnetic field in which a pressure of 120 MPa was applied while a magnetic field of 1200 kA / m was applied, thereby forming a green compact.
[0159] Subsequently, the obtained green compact was kept in a vacuum at a temperature specified in Table 2 for 4 hours for sintering and rapidly cooled to obtain a sintered body (RTB-based magnet). Furthermore, the obtained sintered body was subjected to aging treatment in an Ar atmosphere at 590 °C for 1 hour, thereby obtaining a sample of the RTB-based magnet of each of Test Examples 1-1 to 1-21.
[0160] It should be noted that in this embodiment, the respective processes from HDDR treatment to sintering were carried out in an inert gas atmosphere in which the oxygen concentration is less than 50 ppm.
[0161] The results of composition analysis with respect to the obtained samples of Experimental Examples 1-1 to 1-21 are shown in Table 1. Note that the amount of each element shown in Table 1 was measured by ICP atomic emission spectroscopy (ICP-AES). In addition, x and y were calculated from the composition analysis results, and a relationship of x and y was established in Fig. 3 applied.
[0162] Regarding the obtained samples, D50 of the main phase crystal grains was measured as follows.
[0163] First, a 10 µm square area on a cross-sectional surface of each sample was observed with an SEM to obtain a backscattered electron image. The obtained backscattered electron image was input into image analysis software, the contours of 200 main-phase crystal grains were extracted, and a main-phase crystal grain area was obtained. An equivalent circle diameter in a region where the accumulated area distribution of the main-phase crystal grains is 50% was defined as D50. The results are shown in Table 2. (Calculation of the area share of cavities)
[0164] First, a cross-sectional area of each of the obtained samples was ground by ion milling to exclude the influence of oxidation of an outermost surface layer. Then, the cross-section after ion milling was analyzed with an electron probe microanalyzer (EPMA) to obtain a backscattered electron image with respect to a 40 μm square area. The obtained backscattered electron image was binarized at a predetermined level, a void fraction was identified, and an area of the void fraction was calculated. The calculated area of the void fraction was divided by the sum of an area of the main phase crystal grain, an area of the grain boundary phase, and the area of the void fraction to calculate an area ratio that the void occupies in a total area. The results are shown in Table 2. (Identification of the phase that forms the grain boundary phase)
[0165] After obtaining a backscattered electron image in the same manner as described above, elemental mapping (256 points × 256 points) of the region was performed. From the backscattered electron image and the obtained elemental mapping data, the RTMC phase, the ROCN phase, and the RTBC phase occupying the grain boundary phase were identified in the following order.
[0166] A backscattered electron image from which the void portion was removed was binarized, a main phase crystal grain region and a grain boundary phase region were identified, and the main phase crystal grain area and the grain boundary phase area were calculated. Note that the binarization was performed based on the signal intensity of the backscattered electron image.
[0167] From the backscattered electron image and the obtained element mapping data, different contrast regions were specified, which constitute the main phase crystal grain and the grain boundary phase. Next, spot analysis was performed in the main phase crystal grain region using the EPMA to calculate the mean and standard deviation of the characteristic X-ray intensity of the respective elements R, T, M, B, C, O, and N. For each of the respective elements, a value obtained by adding three times the standard deviation to the mean of the characteristic X-ray intensity in the main phase crystal grain region was calculated, and this was defined as the content ratio (atomic %) of each element in the main phase crystal grain region. Note that the content ratios of the rare earth element, the transition metal element, the element M, and carbon in the main phase crystal grain region are referred to as R. MP , T MP, M MP and C MP were determined.
[0168] It is important to note that C MP in the sample of Experimental Example 1-12 with respect to five different main phase crystal grains, C MP and T MP measured using the 3DAP and C MP / T MP calculated. C MP / T MP was 0.0048.
[0169] Next, with respect to various contrast regions constituting the grain boundary phase, spot analysis was performed with the EPMA, and regions in which the value of the characteristic X-ray intensity is larger than the value (mean + 3 × standard deviation) of the characteristic X-ray intensity in the main phase crystal grain region, and regions in which the value of the characteristic X-ray intensity is smaller than the value (mean + 3 × standard deviation) of the characteristic X-ray intensity in the main phase crystal grain region were specified with respect to the respective elements (R, T, M, B, C, O and N).
[0170] In the different contrast regions constituting the grain boundary phase, a region in which the concentrations of elements R, M and C are larger than those in the main phase crystal grain and a region in which a concentration of T is smaller than that in the main phase crystal grain are determined as the RTMC phase in the grain boundary phase.
[0171] In addition, in the different contrast regions constituting the grain boundary phase, a region was defined as RCON phase in the grain boundary phase, in which regions where the concentrations of the elements R, C, O and N are larger than in the main phase of the crystal grain overlap each other.
[0172] In addition, in the different contrast regions constituting the grain boundary phase, a region where regions where the concentrations of elements R, B, and C are larger than those in the main phase crystal grain and a region where the concentration of T is smaller than that in the main phase crystal grain overlap each other was determined as the RTBC phase in the grain boundary phase.
[0173] It should be noted that in the RTMC phase identified as described above, a quantitative analysis was performed to determine the compositional proportions (R RC , T RC , M RC and C RC ) of the respective elements. The quantitative analysis was performed at three points in the RTMC phase, and the values of M RC / R RC and C RC / R RC The values of the samples were calculated from an average of the measured values. The results are presented in Table 2.
[0174] Furthermore, the number of pixels is calculated with respect to a single closed region belonging to the R-rich phase. A phase was specified in which the number of pixels in the RTMC phase and the RTBC phase is the largest. Furthermore, an area of one pixel was calculated from a scale bar of the backscattered electron image, and the maximum area of the R-rich phase was calculated from the product of the number of pixels and the area of the one pixel. In the examples, the R-rich phase that had the maximum area was the RTMC phase or the RTBC phase. The results are shown in Table 2.
[0175] Next, the CV value of the carbon concentration distribution was calculated from the obtained element mapping data in the following order. Based on the information of the detected carbon amount (carbon concentration) obtained by surface analysis, the standard deviation of the detected carbon amount and the average value of the detected carbon amount were calculated, and the CV value was calculated from the following formula. The results are shown in Table 2. CV value (%) = standard deviation of the detected carbon amount / average value of the detected carbon amount (Magnetic properties)
[0176] Next, the magnetizing field Hmag of the obtained samples as well as the coercive field strength HcJ and the residual magnetic flux density Br in the magnetizing field Hmag were measured using a BH meter as follows.
[0177] First, the sub-loop was measured while the maximum magnetic field was measured at constant intervals from a value of the same magnetic field as the coercive field strength Hcj _2387kA / m (corresponds to HcJ _30kOe ) of a JH hysteresis curve (main loop) measured at the maximum magnetic field of 2390 kA / m, and then a magnetic field was obtained in which the sub-loop is closed and has a symmetrical shape, and this magnetic field was defined as the magnetizing field Hmag. The measurement results of the sub-loop with respect to Experimental Example 1-9 are shown in Fig. 5. In Fig.5, a closed sub-loop was obtained even in a case where the magnetic field was 240 kA / m, 280 kA / m, and 320 kA / m, but a sub-loop with a symmetrical shape was only achieved at a magnetic field of 320 kA / m. Accordingly, the magnetizing field Hmag of Experimental Example 1-9 was 320 kA / m. In the examples, a sample in which Hmag was 800 kA / m or less was determined to be "satisfactory." The results are shown in Table 3.
[0178] Next, the coercive field strength at the time of applying the magnetizing field Hmag was expressed as HcJ _Hmag and a residual magnetic flux density at the time of application of the magnetizing field Hmag as Br _Hmag In the examples, a sample in which HcJ _Hmag 576 kA / m or less was determined as "satisfactory". In addition, a sample in which Br_ Hmag0.91 T or more is determined as "satisfactory." The results are presented in Table 3.
[0179] A temperature coefficient of coercivity of the obtained sample was measured as follows. First, the coercivity in a minimum magnetizing field of a sample was measured at room temperature (23°C), and this was expressed as HcJ. _23°C Next, the sample was heated to 180 °C and held for about five minutes. In a state where the sample temperature was stabilized, the coercive field strength was measured in the minimum magnetization field and expressed as HcJ. _180°C Then, a temperature coefficient β (% / °C) of the coercive field strength was expressed by the following expression. β=(HcJ_180°C−HcJ_23°C) / HcJ_23°C / (180−23)*100
[0180] For use as a variable magnetic flux magnet, the temperature coefficient β of the coercive field strength is preferably at least -0.45% / °C or more, and more preferably -0.40% / °C or more.
[0181] Next, the flatness of the sub-curve was measured as follows. Fig. Figure 6 shows a group of sub-loops measured during the change of a negative reversal magnetic field Hrev in relation to Experimental Example 1-9. Among the magnetization curves obtained from a plurality of negative reversal magnetic fields Hrev, a magnetization curve (a bold line in Fig. 6), which, starting from an operating point (-HcJ _Hmag , 0) was obtained, which corresponds to the coercive field strength of the secondary loop in the second and third quadrants, a ratio of the coercive field strength of the secondary loop HcJ _Hmag and H _50%Js, which is a magnetic field that is 50% of the magnetic polarization Js at the time of application of the magnetizing field Hmag, as the flatness of the sub-curve (100 × H _50%Js / HcJ _Hmag ). In the examples, a sample with a flatness of the secondary curve of 63% or more was determined to be "satisfactory." The results are shown in Table 3. (Evaluation of the engine's idle characteristics)
[0182] The motor characteristics in case of using magnets of test examples 1-1 to 1-21 as magnet 13 with variable magnetic flux of a Fig.The results of the motor shown in Figure 4 were evaluated at room temperature. An NdFeB magnet (HcJ = 2000 kA / m, Br = 1.26 T) was used as the fixed flux magnets 14a and 14b. The thickness of the variable flux magnet 13 in the magnetization direction was set to 5 mm, the thickness of each of the fixed flux magnets 14a and 14b in the magnetization direction was set to 0.5 mm, and the thickness of the entire stacked magnet 15 in the magnetization direction was set to 6 mm. At this time, the allowable range of the d-axis current was -60 to 60 A, and the range of the magnetic field acting on the variable flux magnet by the d-axis current was -130 to 130 kA / m.
[0183] In the JH curve of the variable flux magnet of the Fig.In Experimental Example 1-9 shown in Figure 5, the magnetizing field Hmag required for the magnetization of the magnet to exhibit a symmetrical hysteresis from a positive region to a negative region is 320 kA / m. On the other hand, the magnetic field range due to the d-axis current applied by the motor is -130 to 130 kA / m, which is lower than the magnetizing field Hmag. As shown in Fig. However, as shown in Figure 7, if the magnetization variation range of the variable flux magnet is limited to the positive magnetization range, even at 130 kA / m, which is less than half of the magnetizing field Hmag, the magnetization variation amount between a magnetized state and a demagnetized state can be made relatively large. By utilizing this property, it became possible to evaluate the motor characteristic with respect to a magnet whose Hmag is 130 kA / m or more.
[0184] Each of the variable flux magnets from Experimental Examples 1-1 to 1-21 was mounted on a motor evaluation device, and the induced voltage characteristics at no-load conditions after magnetization and demagnetization were measured as follows. First, the variable flux magnet was adjusted to a maximum magnetized state by applying a positive maximum d-axis current of 60 A, and an induced voltage between UV phases was measured at an no-load speed of 600 rpm. Next, an induced voltage at no-load conditions was measured after applying the d-axis current while increasing a negative d-axis current at constant intervals up to -60 A. This resulted in a variation of the induced voltage in the second quadrant during demagnetization.Next, an induced voltage under no-load conditions was measured after applying the d-axis current while increasing a positive d-axis current at constant intervals up to 60 A. Accordingly, a change in the induced voltage in the first quadrant during magnetization was obtained. A change rate between the maximum value and the minimum value of the induced voltages obtained during the measurement was derived as the change rate of the induced voltage after magnetization and demagnetization of a magnet. In the examples, a sample in which the change rate of the induced voltage was 30% or more was determined to be "satisfactory." The results are shown in Table 3. In addition, the induced voltage characteristics of the motor evaluation device on which the variable flux magnet of Experimental Example 1-9 was mounted are shown in . Fig. 8 shown.
[0185] Each of the variable flux magnets of Experimental Examples 1-1 to 1-21 was mounted on the motor evaluation device, and torque characteristics were measured with respect to a current phase β for a magnetization state by a d-axis current of 60 A and a demagnetization state by a d-axis current of -60 A, respectively. A torque variation rate after magnetization and demagnetization of the magnet was derived from a maximum torque value in each state. In the examples, a sample in which the torque variation rate was 15% or more was determined to be "satisfactory." The results are shown in Table 3. In addition, the torque characteristics of the motor evaluation device on which the variable flux magnet of Experimental Example 1-9 was mounted are shown in Fig. 9 shown. [Table 3] RTB-based magnet Engine idle characteristics magnetic characteristics Magnetization field Hmag (kA / m) Coercive field strength HcJ _Hmag (kA / m) Temperature coefficient b of the coercive field strength (% / °C) residual magnetic flux density Br _Hmag (T) Flatness of the secondary curve H _50%Js / HCJ _Hmag (%) Rates of change of induced voltage after magnetization and demagnetization (%) Torque variation rate after magnetization and demagnetization (%) Experimental example 1-1 400 80 -0,60 1,29 15 0 0 Comparison example Experimental example 1-2 320 150 -0,37 1,23 67 42 20 Example Experimental example 1-3 280 176 -0,36 1,15 80 45 25 Example Experimental example 1-4 280 208 -0,38 1,13 85 47 27 Example Experimental example 1-5 380 271 -0,43 1,11 86 45 25 Example Experimental example 1-6 480 320 -0,50 0,99 87 44 21 Example Experimental example 1-7 560 368 -0,53 0,82 90 12 6 Comparison example Experimental example 1-8 400 160 -0,45 1,20 52 29 14 Comparison example Experimental example 1-9 320 176 -0,45 1,12 69 38 19 Example Experimental example 1-10 300 184 -0,44 1,11 80 45 25 Example Experimental example 1-11 290 192 -0,41 1,11 81 46 26 Example Experimental example 1-12 280 200 -0,39 1,11 83 47 26 Example Experimental example 1-13 300 216 -0,39 1,10 87 47 27 Example Experimental example 1-14 310 224 -0,40 0,99 90 44 21 Example Experimental example 1-15 360 240 -0,47 0,81 92 29 14 Comparison example Experimental example 1-16 280 208 -0,38 1,14 86 47 27 Example Experimental example 1-17 273 192 -0,39 1,11 78 46 26 Example Experimental example 1-18 244 172 -0,39 1,10 75 43 25 Example Experimental example 1-19 227 160 -0,39 1,12 70 41 23 Example Experimental example 1-20 288 192 -0,38 1,12 79 44 25 Example Experimental example 1-21 264 176 -0,40 1,13 74 40 22 Example
[0186] Experimental Example 1-2 lies outside the scope of claim 1.
[0187] From Tables 2 and 3, it was confirmed that the properties required for the variable magnetic flux magnet in the formation of the RTMC phase are satisfactory.
[0188] Furthermore, in a case where the RTB-based magnet according to the example was incorporated into a motor, it was confirmed that the change rates of induced voltage and torque increase after magnetization and demagnetization of a magnet. (Experimental Example 2)
[0189] The samples were prepared according to the same method as in Experimental Example 1, except that the raw materials were mixed to obtain RTB-based magnets with the compositions shown in Tables 4 and 5, and the samples were evaluated according to the same method as in Experimental Example 1. The results of composition analysis on the samples of Experimental Examples 2-1 to 2-55 are shown in Tables 4 and 5. In addition, x and y were calculated from the composition analysis results, and a relationship of x and y was established in Fig. 3. In addition, the evaluation results of samples 2-1 to 2-55 are shown in Tables 6 to 9.
[0195] [Table 8] RTB-based magnet magnetic characteristics Magnetization field Hmag (kA / m) Coercive field strength HcJ _Hmag (kA / m) Temperature coefficient b of the coercive field strength (% / °C) residual magnetic flux density Br _Hmag (T) Flatness of the secondary curve H _50%Js / HcJ _Hmag (%) Experimental example 2-1 800 576 -0,38 1,11 70 Example Experimental example 2-2 480 312 -0,40 1,08 73 Example Experimental example 2-3 360 248 -0,39 1,06 73 Example Experimental example 2-4 240 128 -0,41 1,02 71 Example Experimental example 2-5 160 96 -0,40 0,95 63 Example Experimental example 2-6 640 528 -0,39 1,16 80 Example Experimental example 2-7 480 320 -0,41 1,09 73 Example Experimental example 2-8 440 288 -0,40 1,07 72 Example Experimental example 2-9 360 256 -0,41 1,05 70 Example Experimental example 2-10 240 168 -0,40 0,94 67 Example Experimental example 2-11 480 320 -0,41 1,16 84 Example Experimental example 2-12 440 304 -0,40 1,14 82 Example Experimental example 2-13 384 280 -0,38 1,13 81 Example Experimental example 2-14 344 224 -0,39 1,07 79 Example Experimental example 2-15 224 144 -0,38 1,04 76 Example Experimental example 2-16 200 104 -0,39 1,02 74 Example Experimental example 2-17 160 72 -0,41 0,98 71 Example Experimental example 2-18 360 240 -0,38 1,14 84 Example Experimental example 2-19 320 224 -0,39 1,13 83 Example Experimental example 2-20 280 208 -0,38 1,13 85 Example Experimental example 2-21 264 192 -0,38 1,12 85 Example Experimental example 2-22 240 168 -0,39 1,10 84 Example Experimental example 2-23 224 128 -0,40 1,04 82 Example Experimental example 2-24 184 96 -0,41 1,03 79 Example Experimental example 2-25 160 72 -0,41 1,00 71 Example Experimental Example 2-26 144 40 -0,41 0,96 69 Example Experimental Example 2-27 224 160 -0,39 1,12 83 Example
[0196] [Table 9] RTB-based magnet magnetic characteristics Magnetization field Hmag (kA / m) Coercive field strength HcJ _Hmag (kA / m) Temperature coefficient b of the coercive field strength (% / °C) residual magnetic flux density Br _Hmag (T) Flatness of the secondary curve H _50%Js / HcJ _Hmag (%) Experimental Example 2-28 184 128 -0,41 1,11 82 Example Experimental Example 2-29 184 96 -0,41 1,11 77 Example Experimental example 2-30 184 80 -0,38 1,09 69 Example Experimental Example 2-31 160 56 -0,41 1,03 69 Example Experimental example 2-32 120 40 -0,41 0,97 68 Example Experimental Example 2-33 104 24 -0,38 0,91 63 Example Experimental Example 2-34 80 24 -0,39 1,10 68 Example Experimental Example 2-35 344 232 -0,39 1,14 82 Example Experimental Example 2-36 280 200 -0,38 1,13 84 Example Experimental Example 2-37 360 240 -0,39 1,15 82 Example Experimental Example 2-38 280 208 -0,38 1,14 83 Example Experimental Example 2-39 320 208 -0,38 1,12 82 Example Experimental example 2-40 280 192 -0,38 1,14 83 Example Experimental Example 2-41 264 192 -0,38 1,13 84 Example Experimental Example 2-42 344 216 -0,40 1,13 83 Example Experimental Example 2-43 280 184 -0,38 1,12 83 Example Experimental example 2-44 360 224 -0,39 1,14 84 Example Experimental example 2-45 280 208 -0,38 1,12 84 Example Experimental Example 2-46 280 192 -0,38 1,15 83 Example Experimental Example 2-47 280 184 -0,39 1,16 82 Example Experimental example 2-48 320 232 -0,39 1,07 72 Example Experimental Example 2-49 320 256 -0,38 1,08 72 Example Experimental example 2-50 320 224 -0,38 1,07 71 Example Experimental Example 2-51 320 192 -0,38 1,02 73 Example Experimental Example 2-52 264 208 -0,38 1,14 83 Example Experimental Example 2-53 264 192 -0,38 1,15 84 Example Experimental example 2-54 264 216 -0,38 1,15 86 Example Experimental example 2-55 264 168 -0,38 1,11 81 Example
[0190] From Tables 6 to 9, it was confirmed that the coercive field strength can be reduced, and the properties required for the variable magnetic flux magnet can be met by replacing part of Nd with Y or Ce. INDUSTRIAL APPLICABILITY
[0191] Since the RTB-based magnet of the present invention satisfies the characteristics required for the variable magnetic flux magnet, the RTB-based magnet is suitable for the variable magnetic flux magnet. LIST OF REFERENCE SYMBOLS 1 RTB-BASED MAGNET 2 MAIN PHASE CRYSTAL GRAIN 4 GRAIN BOUNDARY PHASE 4a Two-grain grain boundary 4b TRIPLE JOINT
Claims
[1] RTB-based magnet comprising: one or more rare earth elements; one or more of the transition metal elements, including iron, or two or more of the transition metal elements, including iron and cobalt; Boron; an element M which is gallium or gallium and aluminum; and Carbon, where when a content fraction of rare earth elements is defined as "a", a content fraction of transition metal elements as "b", a content fraction of boron as "c", a content fraction of element M as "d", and a content fraction of carbon as "e", where the sum of the elements contained in the RTB-based magnet is set to 100 atomic%, a, b, c, d, and e satisfy the following relationships: 14 atom%≤a≤20 atom%, 70 atom%≤b≤82 atom%, 4 atom%≤c≤7 atom%, 0.010≤d / b≤0.035, and 0.033≤e / b≤0.055, the RTB-based magnet contains: main phase crystal grains consisting of a compound with a tetragonal structure of R2T 14 B-type, and a grain boundary phase that is present between the main phase crystal grains, the grain boundary phase contains an RTMC phase which includes the rare earth elements, the transition metal elements, the element M and carbon, the RTMC phase satisfies the relationships: R RC > R MP , T RC < T MP , M RC > M MP , and C RC > C MP and R RC and M RC satisfy the relationship: 0.07 ≤ M RC / R RC ≤ 0.65, when the content proportions of the rare earth elements, the transition metal elements, the element M and the carbon included in the main phase crystal grains are each expressed as R MP , T MP , M MP , and C MPand the content proportions of the rare earth elements, the transition metal elements, the element M and the carbon contained in the RTMC phase are each defined as R RC , T RC , M RC , and C RC are defined. [2] The RTB-based magnet according to claim 1, wherein an average crystal grain size D50 of the main phase crystal grains is 2.50 µm or less. [3] RTB-based magnet according to claim 1 or 2, wherein the grain boundary phase contains an ROCN phase in which the content proportions of the rare earth elements, oxygen, carbon and nitrogen are higher than the content proportions of the rare earth elements, oxygen, carbon and nitrogen contained in the main phase crystal grains, an area fraction of the ROCN phase is 10% or more when the area of the grain boundary phase is set to 100%, and a maximum area of a phase in which the content of rare earth elements is higher than the content of rare earth elements contained in the main phase crystal grains, in the grain boundary phase 70 µm 2 or less. [4] The RTB-based magnet according to any one of claims 1 to 3, wherein a CV value of a concentration distribution of carbon in the RTB-based magnet is 0.85 or less. [5] The RTB-based magnet according to any one of claims 1 to 4, wherein the rare earth elements comprise Nd and one or more species selected from the group consisting of Y, Ce and Sm. [6] RTB-based magnet according to any one of claims 1 to 5, wherein the rare earth elements are composed of R1, R2 and Sm, R1 is one or more rare earth elements including Nd and not including Y, Ce and Sm, and R2 is one or more elements selected from Y and Ce, and in an (x, y) plane, x and y lie on straight lines forming a pentagon having a point A (0.000; 0.050), a point B (0.000; 0.150), a point C (0.700; 0.100), a point D (0.700; 0.000), and a point E (0.300; 0.000) as vertices, or lie in a region surrounded by the pentagon when the total number of atoms of the rare earth elements included in the RTB-based magnet is set to 1, wherein a ratio of the number of atoms of R2 to the total number of atoms of the rare earth elements is defined as "x" and a ratio of the number of atoms of Sm to the total number of atoms of the rare earth elements is defined as "y". [7] A motor comprising the RTB-based magnet according to any one of claims 1 to 6. [8] A generator comprising the RTB-based magnet according to any one of claims 1 to 6.
Citation Information
Patent Citations
Permanent magnet, method of manufacturing the same, permanent magnet for motor, and permanent magnet motor
JP2010034522A
Permanent magnet and method for manufacturing permanent magnet
JP2010074084A
R-Fe-B-BASED FINE CRYSTAL HIGH-DENSITY MAGNET
JP2012099852A
Magnetic body
WO2012090765A1
Permanent magnet on RTB base
DE102017203059A1