Dielectric polymer thick-film paste composition

The dielectric polymer thick film paste composition addresses pinhole formation and moisture barrier issues by using titanium dioxide, boron nitride, and resin additives, ensuring improved adhesion and conductivity in electrical circuits.

DE112019003063B4Active Publication Date: 2024-11-07DU PONT CHINA LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
DE112019003063
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-18
Filing Date
2019-06-18
Publication Date
2024-11-07
Estimated Expiration
2039-06-18

AI Technical Summary

Technical Problem

Existing dielectric materials for in-mold electronics and wearable articles face challenges such as pinhole formation during screen printing, poor thermoformability, and inadequate moisture barrier properties, which affect the conductivity and durability of electrical circuits.

Method used

A dielectric polymer thick film paste composition comprising titanium dioxide and boron nitride powder, a resin mixture of polyol and phenoxy resin, and additives like linear aliphatic polyester and blocked aliphatic polyisocyanate, dissolved in polar aprotic solvents, which minimizes pinhole formation and enhances adhesion and moisture barrier properties.

Benefits of technology

The composition achieves reduced pinhole formation, improved adhesion to substrates, and maintains conductivity under washing and drying cycles, with enhanced dielectric properties and thermoformability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Dielectric polymer thick-film paste composition, comprising: (a) a mixture of titanium dioxide and boron nitride powder; (b) a resin mixture of polyol and phenoxy resin; (c) one or more additives selected from the group consisting of a linear aliphatic polyester, a block copolymer, a blocked aliphatic polyisocyanate and a wetting and dispersing agent; and (d) one or more polar, aprotic solvents, wherein the resin mixture and any additives are dissolved in the one or more solvents and the titanium dioxide and boron nitride powder are dispersed in the one or more solvents; wherein the paste composition comprises 40-65 wt% mixture of titanium dioxide powder, TiO2 powder, and boron nitride powder, BN powder, 5-20 wt% resin mixture and 15-40 wt% one or more solvents, and the resin mixture comprises 1-5 wt% polyol and 4-15 wt% phenoxy resin, the wt% referring to the total weight of the paste composition.
Need to check novelty before this filing date? Find Prior Art

Description

FIELD OF THE INVENTION

[0001] The present invention relates to dielectric polymer thick film paste compositions for use in forming polymer thick film dielectric layers for in-mold electronics and wearable articles. BACKGROUND OF THE INVENTION

[0002] There is an increasing demand for dielectrics in applications where thermoformable multilayer circuits are required and for use in garments where flexible dielectrics are required.

[0003] In the in-mold electronics (IME) industry, the dielectric layer serves to protect an electrically conductive layer, e.g., a silver layer, and must therefore be screen-printable with minimized pinhole formation, easily thermoformable, and must under no circumstances negatively impact the conduction properties of the conductive layer.

[0004] These dielectric layers must also provide a moisture barrier. Highly viscous polyurethane resin-based paste compositions can be problematic with regard to pinhole formation during the screen printing process.

[0005] Stretchable dielectrics are required to protect an electrically conductive layer in electrical circuits. Such dielectrics must be printable with minimal pinhole formation, and they must be stretchable moisture barriers and able to withstand washing and drying cycles.

[0006] US 2007 / 0 083 017 A1 generally relates to compositions comprising a polyimide component and a hydrophobic epoxy component, such compositions being useful as a binder component in a resistor, a resistor substrate, or other electronic substrate or a similar type application. [0006a] There is a continuing need for improved dielectric polymer thick film paste compositions. SUMMARY OF THE INVENTION

[0007] The present invention relates to a dielectric polymer thick film paste composition comprising: (a) a mixture of titanium dioxide and boron nitride powder; (b) a resin mixture of polyol and phenoxy resin; (c) one or more additives selected from the group consisting of a linear aliphatic polyester, a block copolymer, a blocked aliphatic polyisocyanate and a wetting and dispersing agent; and (d) one or more polar, aprotic solvents, wherein the resin mixture and any additives are dissolved in the one or more solvents and the titanium dioxide and boron nitride powders are dispersed in the one or more solvents;wherein the paste composition comprises 40-65 wt.% mixture of titanium dioxide powder, TiO2 powder, and boron nitride powder, BN powder, 5-20 wt.% resin mixture and 15-40 wt.% one or more solvents, and the resin mixture comprises 1-5 wt.% polyol and 4-15 wt.% phenoxy resin, wherein the wt.% is based on the total weight of the paste composition. DETAILED DESCRIPTION OF THE INVENTION

[0008] The invention relates to a dielectric polymer thick film paste composition.

[0009] In one embodiment, the paste composition is used as a protective layer for a conductor in an electrical circuit to be thermoformed. The paste composition exhibits good flow through the screen mesh openings during the printing process, which minimizes or eliminates pinhole formation and achieves good dielectric insulation. The dried dielectric layer also adheres to the conductor or the plastic substrate.

[0010] In another embodiment, the paste composition is used to form protectable stretchable dielectric layers for electrical circuits in articles such as garments and seats.

[0011] The invention further provides articles containing such dielectrics.

[0012] The description of the present paste composition as “dielectric” is intended to indicate that the composition can be formed into a structure and subsequently processed to exhibit dielectric properties.

[0013] When the paste composition is used to form stretchable dielectric layers for articles such as garments and seats, the dielectric layer formed from the paste composition must adhere well to the substrate to which it has been dispensed. If the article is a garment, the layer must retain its conductive properties despite being subjected to washing and drying cycles.

[0014] The present dielectric polymer thick film paste composition comprises a mixture of titanium dioxide (TiO2) and boron nitride (BN) powder, a resin mixture of polyol and phenoxy resin, at least one additive selected from the group consisting of a linear aliphatic polyester, a block copolymer, a blocked aliphatic polyisocyanate, and a wetting and dispersing agent, and one or more polar, aprotic solvents, wherein the resin mixture and the one or more additives are dissolved in the one or more solvents and the inorganic powder is dispersed in the one or more solvents.

[0015] The paste composition is referred to as a polymer thick-film paste composition because the polymer remains as a component in the dielectric layer. The various components are discussed in detail in the following sections. Titanium dioxide and boron nitride powder

[0016] The paste composition includes a mixture of TiO2 and BN powder.

[0017] The TiO2 and BN powders used in the present paste composition can be supplied as finely divided particles of any morphology, including, but not limited to, one or more of the following morphologies: a flake shape, a spherical shape, a rod shape, a granule shape, a nodular shape, a platelet shape, a layered or coated shape, or other irregular shapes. Also contemplated are mixtures of particles of more than one of these types, or mixtures of particles of the same type having different size distributions.

[0018] The particle size of the powder is not subject to any specific restrictions, provided that the required functional properties can be achieved. In the present context, "particle size" shall refer to the "median particle size" or d, which means the 50% volume distribution size. The particle size distribution may further be characterized by other parameters, such as d, which means that 90 volume% of the particles are smaller than d, or d, which means that 10% of the particles are smaller than d. The volume distribution size may be determined by a variety of methods understood by those skilled in the art, including, but not limited to, laser diffraction and dispersion methods, which can be performed with a Microtrac X100 particle size analyzer (Montgomeryville, PA). Laser light scattering can, for example,using a Model LA-910 particle size analyzer, commercially available from Horiba Instruments Inc. (Irvine, CA), may also be used. In various embodiments, the median size of the inorganic particles is greater than 0.1 µm and less than 10 µm, as measured using the Microtrak X100 analyzer.

[0019] The TiO2 and BN powders comprise 40 wt.% to 65 wt.% of the paste composition, based on the total weight of the paste composition. In one embodiment, the ratio of the weight of the TiO2 powder to the weight of the BN powder, TiO2 / BN, ranges from about 2 to about 25. Resin mixture of polyol and phenoxy resin

[0020] The resin mixture is a mixture of polyol and phenoxy resin.

[0021] Polyol contains several hydroxyl groups and reacts with isocyanates to form polyurethanes.

[0022] The phenoxy resin with the following basic repeating form: -[O-C6H4-C(CH3)2-C6H4-O-CH2CHOHCH2]- and structure further contains hydroxy groups.

[0023] The resin mixture constitutes 5 wt% to 20 wt% of the paste composition, based on the total weight of the paste composition.

[0024] The polyol constitutes 1 wt% to 5 wt% of the paste composition, based on the total weight of the paste composition, and the phenoxy resin constitutes 4 wt% to 15 wt% of the paste composition, based on the total weight of the paste composition. additives

[0025] The paste composition comprises one or more additives selected from the group consisting of a linear aliphatic polyester, a block copolymer, a blocked aliphatic polyisocyanate and a wetting and dispersing agent.

[0026] A blocked aliphatic polyisocyanate is an isocyanate reaction product that is stable at room temperature but dissociates upon heating, regenerating the isocyanate functionality. The isocyanate functional group in a blocked polyisocyanate is masked by the use of a blocking agent, resulting in a compound that is apparently inert at room temperature but generates the reactive isocyanate functionality at elevated temperatures. For the blocked aliphatic isocyanates used in the present invention, curing temperatures of 110-160°C release the blocking agents. The resulting polyisocyanates can then react with the active hydroxy-containing compounds in the resin mixture.

[0027] Typical aliphatic polyisocyanates are hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI).

[0028] Typical blocking agents are 3,5-dimethylpyrazole (DMP), diethyl malonate (DEM), diisopropylamine (DIPA), 1,2,4-triazole (TRIA) and methyl ethyl ketone (MEKO).

[0029] Typical blocked aliphatic polyisocyanates are DMP-blocked HDI, (DEM) / (DIPA)-blocked HDI, and DEM-blocked polyisocyanate using both HDI and IPDI. MEKO-blocked polyisocyanate using H 12 MDI can also be used.

[0030] In one embodiment, the blocked aliphatic polyisocyanate comprises about 0.5 wt.% to about 5 wt.% of the paste composition, based on the total weight of the paste composition.

[0031] In one embodiment, the linear aliphatic polyester comprises about 1 wt.% to about 5 wt.% of the paste composition, based on the total weight of the paste composition. In one embodiment, the linear aliphatic polyester is a linear aliphatic polycarbonate polyester.

[0032] In one embodiment, the block copolymer comprises about 1 wt.% to about 5 wt.% of the paste composition, based on the total weight of the paste composition. In one embodiment, the block copolymer is a nonionic bifunctional block copolymer surfactant with terminal secondary hydroxy groups.

[0033] The wetting and dispersing agent is used to stabilize the TiO2 and BN particles. In one embodiment, the wetting and dispersing agent comprises about 0.1 wt.% to about 0.5 wt.% of the paste composition, based on the total weight of the paste composition. solvent

[0034] One or more polar, aprotic solvents are present in the paste composition. The resin mixture and the one or more additives are dissolved in the one or more solvents, and the TiO2 and BN powders are dispersed in the one or more solvents. A small amount of additional solvent may be added to the paste composition to adjust the final viscosity for dispensing or printing.

[0035] Typical solvents used are dipropylene glycol methyl ether, 2-butoxyethanol and triethyl phosphate.

[0036] The solvents constitute 15 wt% to 40 wt% of the paste composition, based on the total weight of the paste composition. Preparation of a dielectric polymer thick film paste composition

[0037] The resin mixture is dispersed in a solvent or mixed solvent to dissolve the resin mixture. For example, it can be heated to 70°C and stirred to dissolve the resin and form an organic medium. Portions of the resin mixture can be dissolved in different solvents or in the same solvent to form additional organic media. Alternatively, a single organic medium can be used. The one or more additives can be added to one of the organic media and stirred. The TiO2 and BN powders can be added to one of the organic media and stirred. The TiO2 and BN powders are typically added stepwise, with mixing after each addition to allow for better wetting. Typically, the BN powder was added first, followed by the TiO2 powder.If more than one organic medium is prepared, the media can be combined after any of the above steps, and the resulting paste composition is milled. Solvent can be added to adjust the viscosity before the paste composition is dispensed or printed. EXAMPLES, COMPARISON EXPERIMENTS EXAMPLES 1-4; COMPARISON EXPERIMENTS FROM

[0038] The dielectric paste compositions of Examples 1-4 were prepared in the following manner.

[0039] The polymer media used are as follows: Polymer Medium 1 (PM-1) - Prepared by blending a 30 wt.% phenoxy resin and polyester polyol blend (PKHM-301, Gabriel, Akron, OH) with 70 wt.% dipropylene glycol methyl ether (Dowanol™ DPM, Dow Chemical Co., Midland, MI). The manufacturer of PKHM-301 states that it has a hydroxyl content of 334 (OH equivalent weight, g / equiv.) and a molecular weight of 39,000 Daltons. This mixture was heated and stirred at 70-90°C for 3 hours or until all the resin dissolved, and then cooled to room temperature. Polymer Medium 2 (PM-2) - Prepared by mixing 20 wt% phenoxy resin (PKHH Gabriel, Akron, OH) with 80 wt% dipropylene glycol methyl ether (Dowanol™ DPM, Dow Chemical Co., Midland, MI). The manufacturer of PKHH states that it has a hydroxyl content of 280 (OH equivalent weight, g / equiv.) and a molecular weight of 52,000 Daltons. This mixture was heated and stirred at 70-90°C for 3 hours or until all the resin dissolved, and then cooled to room temperature. Polymer Medium 4 (PM-4) - Made by blending 5 wt.% phenoxy resin (PKHH Gabriel, Akron, OH) and 20 wt.% linear hydroxyl polyurethane (Desmocoll® 406, Covestro, Pittsburgh, PA) with 75 wt.% Dipropylene glycol methyl ether (Dowanol™ DPM, Dow Chemical Co., Midland, MI). The manufacturer of Desmocoll® 406 states that this polymer is primarily a linear hydroxyl polyurethane. It is a flexible polyurethane with a low crystallization rate. This mixture was heated and stirred at 70-90°C for 3 hours or until all the resin dissolved, and then cooled to room temperature. Polymer Medium 5 (PM-5) - Prepared by blending 20.5 wt% linear hydroxyl polyurethane (Desmocoll® 530, Covestro, Pittsburgh, PA) with 79.5 wt% dibasic esters (Flexisolv® DBE®-9 Esters, Invista, Wichita, KS). The manufacturer of Desmocoll® 530 states that this polymer is primarily linear hydroxyl polyurethane. It is a flexible polyurethane with a high crystallization rate and very low thermoplasticity. This mixture was heated and stirred at 70-90°C for 3 hours or until all the resin dissolved, and then cooled to room temperature. Polymer Medium 6 (PM-6) - Prepared by mixing 27 wt% phenoxy resin (PKHH Gabriel, Akron, OH) and 73% dibasic esters (Flexisolv® DBE®-9 Ester, Invista, Wichita, KS). This mixture was heated and stirred at 70-90°C for 3 hours or until all the resin dissolved, and then cooled to room temperature.

[0040] The following additives were used: A-1 - linear aliphatic polycarbonate polyester (Desmophen® C 1200, Covestro, Pittsburgh, PA) A-2 - nonionic bifunctional block copolymer surfactant with terminal secondary hydroxyl groups (Pluronic® 31R1, BASF) A-3 - blocked aliphatic H12MDI polyisocyanate (Desmodur BL 5375, Covestro, Pittsburgh, PA) A-4 - Wetting and dispersing agent (DISPERBYK-111, Palmerholland, North Olmsted, OH)

[0041] The inorganic powders used were the following: TiO2 - rutile titanium dioxide, approximately spherical, average particle size ~0.29 µm (Ti-Pure™ R-101, Chemours, Wilmington, DE) BN - boron nitride powder with platelet-shaped hexagonal crystal structure (CarboTherm™ CTF10 boron nitride powder, Saint-Gobain)

[0042] The solvents used were as follows: S-1 - Dipropylene glycol methyl ether (Dowanol™ DPM, Dow Chemical Co., Midland, MI) S-2 - Triethyl Phosphate (TEP) (Eastman Chemical Co., Kingsport, TN) S-3 - dibasic esters (DBE-9, Invista, Wichita, KS)

[0043] The required amounts of polymer medium, additives, and solvent for each sample in Table 1 were weighed and then mixed to form an organic vehicle. The TiO2 and BN powders were added to the organic vehicle and further mixed to form a paste composition. These inorganic powders were added gradually, mixing after each addition to allow for better wetting. Typically, the BN was added first, followed by the TiO2.

[0044] Each of the above mixing steps can be performed in a planetary centrifugal mixer. A Thinky® mixer (available from Thinky® USA, Inc., Laguna Hills, CA), operated at 1000 rpm for 30 s, was suitable. After being thoroughly mixed, the paste composition was repeatedly passed through a three-roll mill with a 25 µm gap at pressures progressively increased from 0 to 150 psi (-1.04 MPa). A suitable mill is available from Charles Ross and Son, Hauppauge, NY.

[0045] The degree of dispersion of each paste composition can be determined using commercially available fineness of grind (FOG) measuring instruments (e.g., instruments available from Precision Gage and Tool, Dayton, Ohio) according to ASTM Standard Test Method D 1210-05, published by ASTM International, West Conshohocken, PA, and incorporated herein by reference. The data obtained are usually reported as FOG values, represented as X / Y, meaning that the size of the largest particle detected is X µm and the median size is Y µm. In one embodiment, the FOG values ​​of the present paste compositions are typically 20 / 10 or less, which has typically been found to be sufficient for good printability.

[0046] Typically, the processed paste composition is adjusted before printing by adding a small amount of solvent as needed to achieve a viscosity suitable for dispensing, stencil, or screen printing. Viscosity values ​​can be obtained using a Brookfield viscometer (Brookfield Inc., Middleboro, MA) with a 14-gauge spindle and a 6-gauge cup. Typically, a final viscosity of approximately 60-90 Pa s (measured at 10 rpm / 3 min) is found to achieve good dispensing printing results, and a final viscosity of 25-70 Pa s (measured at 10 rpm / 3 min) is found to achieve good screen printing results. However, some variation, for example, ±30 Pa s or more, would be acceptable depending on the specific printing equipment and parameters.

[0047] The amounts in grams (g) for each of the components used in the examples and comparative experiments are shown in Table I. TABLE I sample Organic vehicle filler Example 1 60g PM - 1, 51g PM-2, 8.25g A-2, 0.75g A-4, 25.2g S-1 135 g TiO2, 45 g BN Example 2 45g PM-1, 66g PM-2, 8.25g A-2, 0.75g A-4, 24g S-1 135 g TiO2. 45 g BN Example 3 86.9g PM-3, 7.5g A-1, 0.63g A-4, 31.5g S-1, 3.75g S-2 125 g TiO2 6.25 g BN Example 4 86.9g PM-3, 7.5g A-1, 2.5g A-3, 0.63g A-4, 28.5g S-1, 3.75g S-2 125 g TiO2, 6.25 g BN See Exhibit A 79.5g PM-4, 67.5g PM-2, 8.25g A-2, 0.75g A-4, 22g S-1 108 g TiO2, 36 g BN See Exhibit B 70.2g PM-5. 98.1 g Medium F. 19.5 grams DBE-9 112.2 g TiO2 Pressure characterization

[0048] The printing performance of the dielectric paste compositions from Examples 1-2 and Comparative Experiments AB in Table I were evaluated by the following procedure. 1. 20 mil thick polycarbonate from Tekra was cut to a size of 3x4 inches and run through a Natgraph belt dryer. 2. A first silver conductor (DuPont™ ME603, Silver Conductor, DuPont Co., Wilmington, DE) was printed using an 80-durometer diamond blade and a 325 / 1.1 s / s mesh screen (s / s - stainless steel), followed by drying in the Natgraph belt dryer. 3. Two dielectric layers were printed onto the first conductor using the dielectric paste compositions from Examples 1-2 and Comparative Experiments AB, using a 60-durometer diamond blade and a 280 s / s mesh screen to form a composite dielectric over the first conductor. Each dielectric layer was dried in the Natgraph belt dryer after printing. 4. A second silver conductor (DuPont™ ME603, Silver Conductor, DuPont Co., Wilmington, DE) was printed onto the dielectric composite layer using an 80 durometer diamond blade and a 325 / 1.1 s / s mesh screen (s / s - stainless steel), followed by drying in the Natgraph belt dryer. 5. The thickness of the dielectric composite layer was measured using a handheld micrometer. 6. The breakdown voltage (BDV) was measured using a HiPot tester. Eight such measurements were taken for each sample.

[0049] The average breakdown voltage (kV / mil) data measured in this way are presented in Table II along with observations regarding the number of pinholes. TABLE II sample BDV (kV / mil) Print quality Example 1 1,45 Few pinholes Example 2 1,19 Few pinholes See Exp. A 0,44 Many pinholes See Exp. B 0,07 Large pinholes and rough surface Thermoforming

[0050] The thermoforming performance of the dielectric paste compositions from Examples 3-4 and Comparative Experiment B in Table I were evaluated by the following procedure. 1. 15 mil thick polycarbonate (Makrofol Clear G / M, Covestro DE1-4) was cut to a size of 12x12 inches and passed through a Natgraph belt dryer. 2. A first silver conductor (DuPont™ ME603, Silver Conductor, DuPont Co., Wilmington, DE) was printed using an 80-durometer diamond blade and a 325 / 1.1 s / s mesh screen (s / s - stainless steel), followed by drying in the Natgraph belt dryer. 3. Two dielectric layers were printed onto the first conductor using the dielectric paste compositions from Examples 3-4 and Comparative Experiment B, using a 60-durometer diamond blade and a 280 s / s mesh screen to form a composite dielectric over the first conductor. Each dielectric layer was dried in the Natgraph belt dryer after printing. 4. A second silver conductor (DuPont™ ME603, Silver Conductor, DuPont Co., Wilmington, DE) was printed onto the dielectric composite layer using an 80-durometer diamond blade and a 325 / 1.1 s / s mesh screen (s / s - stainless steel), followed by drying in the Natgraph belt dryer. 5. The printed samples were then thermoformed using a Formec thermoforming machine. 6. The breakdown voltage (BDV) was measured using a HiPot tester. There were 49 such measurements for each sample.

[0051] The average breakdown voltage data (kV / mil) measured in this way are shown in Table III. TABLE II sample BDV (kVimil) Example 3 0,78 Example 4 1,12 See Exhibit B 0

[0052] The BDV data in Table II reveal that the dielectric layers printed with the paste compositions of Examples 1-2, which contain the resin blend of polyol and phenoxy resin and a mixture of flexible block copolymer additives and wetting and dispersing agents, have a desirably higher BDV than the dielectric layers printed with pastes of Comparative Experiments AB, which contain polyurethane and phenoxy resins but no polyol.The BDV in Table III show that Example 3, which contains the resin mixture of polyol and phenoxy resin and a mixture of additives of flexible polyester and wetting and dispersing agent, and Example 4, which contains the resin mixture of polyol and phenoxy resin and a mixture of additives of flexible polyester, blocked aliphatic polyisocyanate and wetting and dispersing agent, have good flexibility and accordingly have a high BDV even after thermoforming, unlike that observed for Comparative Experiment B.

Claims

[1] Dielectric polymer thick film paste composition comprising: (a) a mixture of titanium dioxide and boron nitride powder; (b) a resin mixture of polyol and phenoxy resin; (c) one or more additives selected from the group consisting of a linear aliphatic polyester, a block copolymer, a blocked aliphatic polyisocyanate and a wetting and dispersing agent; and (d) one or more polar, aprotic solvents, wherein the resin mixture and any additives are dissolved in the one or more solvents and the titanium dioxide and boron nitride powders are dispersed in the one or more solvents; wherein the paste composition comprises 40-65 wt.% mixture of titanium dioxide powder, TiO2 powder, and boron nitride powder, BN powder, 5-20 wt.% resin mixture and 15-40 wt.% one or more solvents, and the resin mixture comprises 1-5 wt.% polyol and 4-15 wt.% phenoxy resin, wherein the wt.% is based on the total weight of the paste composition. [2] Paste composition according to claim 1, wherein the ratio of the weight of the TiO2 powder to the weight of the BN powder, TiO2 / BN, is in the range of 2 to 25. [3] Paste composition according to claim 1, wherein the one or more additives are present in amounts of 1-5 wt% linear aliphatic polyester, 1-5 wt% block copolymer, 0.5-5 wt% blocked aliphatic polyisocyanate and 0.1-0.5 wt% wetting and dispersing agent, wherein the wt% are based on the total weight of the paste composition.

Citation Information

Patent Citations

  • Compositions comprising polyimide and hydrophobic epoxy, and methods relating thereto

    US20070083017A1