Composite body and acoustic wave element

A multilayer film with alternating silicon and metal oxide layers in acoustic wave devices enhances the Q value, addressing the insufficient improvement in 5G frequency applications by optimizing refractive index differences.

DE112020003512B4Active Publication Date: 2024-11-07NGK INSULATORS LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE112020003512
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-22
Filing Date
2020-02-21
Publication Date
2024-11-07
Estimated Expiration
2040-02-21

AI Technical Summary

Technical Problem

Existing acoustic wave devices, particularly in the high frequency range for 5G applications, do not achieve sufficient improvement in the Q value despite the use of multilayer films like SiO2/Ta2O5 interposed between the supporting substrate and piezoelectric material substrate.

Method used

A composite body with a multilayer film structure comprising alternating layers of silicon oxides and metal oxides, where the refractive indices of the second and fourth layers differ, is used to enhance the Q value in acoustic wave devices.

Benefits of technology

The proposed multilayer film structure significantly improves the Q value in high frequency applications, achieving up to a 20% increase in Q value compared to standard configurations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Composite body, comprising: a carrier substrate; a substrate made of piezoelectric material; and a multi-layered film between the support substrate and the substrate made of piezoelectric material, the multilayered film has a lamination structure, the first layer, the second layer, the third layer and a fourth layer in this sequence; wherein the first layer and the third layer each contain silicon oxides; wherein the second layer and the fourth layer each contain metal oxides; where the refractive index of the second layer is higher than the refractive index of the first layer and the refractive index of the third layer; and where the refractive index of the second layer differs from the refractive index of the fourth layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a composite body comprising a substrate made of piezoelectric material and a carrier substrate, as well as to an acoustic wave device. TECHNICAL BACKGROUND

[0002] A surface acoustic wave device that functions as a filter device or oscillator and is used in mobile phones or the like is known, as is an acoustic wave device such as a Lamb wave device or a film bulk acoustic resonator (FBAR) that includes a piezoelectric thin film. As such an acoustic wave device, a device is known that is fabricated by bonding a support body and a piezoelectric substrate that conducts a surface acoustic wave, and providing interdigitated electrodes capable of oscillating the surface acoustic wave on a surface of the piezoelectric substrate.By adhering the support body whose thermal expansion coefficient is lower than that of the piezoelectric substrate to the piezoelectric substrate, the change in size of the piezoelectric substrate in response to a temperature change is reduced, so that the change in frequency characteristic of the surface acoustic wave device is reduced.

[0003] When the piezoelectric substrate and the silicon substrate are bonded together, it is known that a silicon oxide film is formed on the surface of the piezoelectric substrate, and the piezoelectric substrate and the silicon substrate are directly bonded together through the silicon oxide film (Patent Document 1). During bonding, the surfaces of the silicon oxide layer and the silicon substrate are irradiated with a plasma beam to activate the surfaces, and direct bonding is performed (plasma activation method).

[0004] Also known is the direct bonding process using the so-called FAB (Fast Atom Beam) system (Patent Document 2). In this process, a neutralized atom beam is irradiated at ambient temperature onto the respective bonding surfaces to activate them, which are then directly bonded to each other.

[0005] Furthermore, it is proposed to provide an intermediate layer of Ta2O5 or the like between the substrate of piezoelectric material and the support substrate, and to irradiate both the intermediate layer and the support substrate with neutralized rays to activate the respective surfaces that are directly bonded to each other (Patent Document 3).

[0006] According to Patent Document 4, the structure is proposed which includes a support substrate, a substrate made of piezoelectric material and a multilayer film having a plurality of SiO2 layers and Ta2O5 layers laminated together. (Prior art documents)(Patent documents) (Patent document 1] US 7 213 314 B2 (Patent document 2] JP 2014- 86 400 A (Patent document 3] WO 2017 / 163722 A1 (Patent document 4] WO 2018 / 154950 A1 DESCRIPTION OF THE INVENTION (Problems to be solved by the invention)

[0007] According to the acoustic wave device of Patent Document 3, the improvement in Q-value performance or the like is observed in mid-frequency applications (4G applications at 0.7 to 3.5 GHz or the like). However, in high-frequency applications (5G applications at 3.5 to 6 GHz or the like), the improvement in Q-value is proven to be small.

[0008] Furthermore, in an acoustic wave device in which a SiO2 / Ta2O5 multilayer film is sandwiched between the support substrate and the piezoelectric material substrate, as described in Patent Document 4, an acoustic wave emerging from the piezoelectric material substrate toward the support substrate is reflected by the multilayer film to reduce loss. However, in applications in the high-frequency range (5G at 3.5 to 6 GHz, etc.), it has been found that the improvement in Q value is not necessarily sufficient even in such an acoustic wave device.

[0009] An object of the present invention is to provide a composite body capable of improving the Q value of an acoustic wave device. (Solution to the task)

[0010] The present invention provides a composite body comprising: a carrier substrate; a substrate made of piezoelectric material; and a multilayer film between the carrier substrate and the substrate made of piezoelectric material, wherein the multilayer film has a lamination structure comprising a first layer, a second layer, a third layer and a fourth layer in this order; wherein the first layer and the third layer each comprise silicon oxides; wherein the second layer and the fourth layer each comprise metal oxides; wherein a refractive index of the second layer is higher than a refractive index of the first layer and a refractive index of the third layer; and wherein the refractive index of the second layer differs from a refractive index of the fourth layer.

[0011] The present invention provides an acoustic wave device comprising: the composite body; and an electrode provided on the substrate made of piezoelectric material. (Effects of the invention)

[0012] As described in Patent Document 4, the inventors investigated why the improvement in the Q value in the acoustic wave device using a multilayer film made of SiO2 and Ta2O5 sandwiched between the support substrate and the piezoelectric material substrate is not necessarily sufficient for high-frequency applications (5G applications at 3.5 to 6 GHz or the like). Since the quality of the multilayer film suitable for medium frequencies (4G or similar) and the quality of the multilayer film suitable for high frequencies (5G or similar) are different, it is suspected that it is difficult to achieve the desired Q value in the high-frequency range.

[0013] Based on such speculations, the inventors attempted to provide the lamination structure including the first layer, the second layer, the third layer, and the fourth layer in the order of the multilayer film, forming the first layer and the third layer from silicon oxides, and forming the second layer and the fourth layer from metal oxides whose refractive indices are higher than those of the silicon oxides. Since the refractive index of the second layer and the refractive index of the fourth layer formed from the metal oxides are different, the Q value is further improved. In particular, a high Q value can be achieved even in the high frequency band (5G band). The present invention has thus been completed. BRIEF DESCRIPTION OF THE DRAWINGS Fig. Fig. 1(a) shows the state in which a multilayer film 22 is provided on a substrate of piezoelectric material 1, Fig. Fig. 1(b) shows the state where a bonding layer 4 is provided on the multilayer film 22, and Fig. Figure 1(c) shows the state where one surface of the interconnect layer 4 is activated. Fig. 2(a) shows the state in which a surface of a support substrate 6 is activated, and Fig. 2(b) shows a composite body 9 made of a carrier substrate and a substrate made of piezoelectric material. Fig. Fig. 3(a) shows the state in which a substrate of piezoelectric material 1A of a composite body 9A is thinned by machining, and Fig. 3(b) shows the state where an electrode is provided on the composite body 9A. Fig.Fig. 4(a) shows a composite body 9B obtained by directly bonding a bonding layer 4 provided on a multilayer film and a bonding layer 14 provided on the support substrate 6, and Fig. Fig. 4(b) shows an acoustic wave device 10B obtained by providing electrodes 11 on the piezoelectric material substrate 1A of the composite body 9B. Fig. Fig. 5(a) shows a composite body 9C obtained by directly bonding the multilayer film 22 and the support substrate 6, and Fig. Fig. 5(b) shows the state in which electrodes are provided on the piezoelectric material substrate 1A of the composite body 9C. Fig. Figure 6 is a diagram showing the refractive index distribution obtained by optical ellipsometry in the case where the refractive indices of the second and fourth layers are different. Fig.Figure 7 is a diagram showing the refractive index distribution obtained by optical ellipsometry for the case where the refractive indices of the second and fourth layers are equal and relatively low. Fig. 8 is a diagram showing the refractive index distribution obtained by optical ellipsometry for the case where the refractive indices of the second and fourth layers are equal and relatively high. EMBODIMENTS OF THE INVENTION

[0014] The present invention will be described in detail with reference to the drawings.

[0015] As in Fig.As shown in Figure 1(a), a piezoelectric material substrate 1 has a pair of surfaces 1a and 1b. A multilayer film 22 is deposited on one surface 1a. According to the present example, the multilayer film 22 is manufactured by providing, for example, two laminated structures on the piezoelectric material substrate 1. Each of the laminated structures 2 is configured such that a first layer 3A, a second layer 7A, a third layer 3B, and a fourth layer 7B are alternately provided from the piezoelectric material substrate 1 side.Although the first layer, the second layer, the third layer, and the fourth layer are laminated in order from the piezoelectric material substrate side according to the present example, the fourth layer, the third layer, the second layer, and the first layer may be laminated in order from the piezoelectric material substrate 1 side.

[0016] As in Fig. 1(b), a bonding layer 4 may further be provided on the surface 22a of the multilayer film 22. In this case, as shown in Fig. 1(c), a neutralized beam is irradiated onto the surface of the bonding layer 4 as shown by arrows A, so that the surface of the bonding layer 4 is activated to provide an activated surface 5.

[0017] As in Fig.As shown in Figure 2(a), a neutralized beam is irradiated onto the surface of the support substrate 6, as shown by arrows B, so that the surface of the support substrate 6 is activated to provide an activated surface 6a. Then, as shown in Fig. 2(b), the activated surface 5 of the first connecting layer 4 and the activated surface 6a of the carrier substrate 6 are directly contacted under pressure to form a Fig. 2(b) to obtain the composite body 9. An arrow C indicates a bonding interface.

[0018] According to a preferred embodiment, the surface 1b of the substrate of piezoelectric material 1 of the composite body 9 is further subjected to a polishing process to reduce the thickness of a substrate of piezoelectric material 1A to obtain a composite body 9A as shown in Fig. 3(a). 1c shows a polished surface. As in Fig.As shown in Fig. 3(b), predetermined electrodes 11 are formed on the polished surface 1c of the piezoelectric material substrate 1A to manufacture an acoustic wave device 10A.

[0019] According to a preferred embodiment, a connecting layer 14 is provided on the carrier substrate, so that the connecting layer 14 is directly connected to the connecting layer on the multilayer film. In this way, it is possible to Fig. 4(C) to obtain the composite body 9B. As shown in Fig. As shown in Fig. 4(b), an acoustic wave device 10B can be obtained by providing the electrodes 11 on the piezoelectric material substrate 1A of the composite body.

[0020] According to a preferred embodiment, the carrier substrate and the multilayer film are further bonded directly to each other. This creates the Fig. 5(a) shown composite body 9C. As in Fig.As shown in Fig. 5(b), an acoustic wave device 10C can be obtained by providing the electrodes 11 on the piezoelectric material substrate 1A of the composite body.

[0021] According to the present invention, the multilayer film provided between the support substrate and the piezoelectric material substrate comprises a first layer, a second layer, a third layer, and a fourth layer in order, the first layer and the third layer are formed of silicon oxides, the second layer and the fourth layer are formed of metal oxides, the refractive index of the second layer is higher than the refractive index of the first layer and the refractive index of the third layer, and the refractive index of the second layer is different from the refractive index of the fourth layer.The first layer, the second layer, the third layer, and the fourth layer may be arranged in order from the support substrate side to the piezoelectric material substrate side, or alternatively, they may be arranged in order from the piezoelectric material substrate side to the support substrate side.

[0022] The silicon oxides forming the first layer and the third layer may preferably have a composition of SiOx (1.80 ≦ x ≦ 2.50).

[0023] Although the metal oxides constituting the second and fourth layers are not specifically limited, the metal oxides may preferably be hafnium oxide, tantalum oxide, or zirconium oxide from the viewpoint of improving the Q value.

[0024] The composition of the hafnium oxide can preferably be HfO z (1.80 ≦ z ≦2.50]. The composition of the tantalum oxide may preferably be Ta2Oy (4.60 ≦ y ≦ 5.50]. Furthermore, the composition of the zirconium oxide may preferably be ZrO z (1.80 ≦ z ≦ 2.50]

[0025] In a preferred embodiment, the multilayer film has a plurality of lamination structures. This enables the modulation of the refractive indices, so that the Q value can be reduced more effectively. The number of lamination structures of the multilayer film can preferably be 2 or more. However, if the number of lamination structures is too large, the effect of the support substrate constraining the piezoelectric material substrate is reduced, so the number of lamination structures can preferably be 5 or fewer, and more preferably 3 or fewer.

[0026] For the purposes of the present invention, the difference between the refractive index of the second layer and the refractive index of the first layer or the refractive index of the third layer may preferably be 0.2 or greater, and more preferably, it may be 0.3 or greater. Furthermore, the difference between the refractive index of the second layer and the refractive index of the first layer or the refractive index of the third layer may preferably be 0.8 or less, and more preferably, it may be 0.6 or less.

[0027] For the purposes of the present invention, the difference between the refractive index of the fourth layer and the refractive index of the second layer can preferably be 0.02 or greater, and particularly preferably 0.03 or greater. Furthermore, the difference can preferably be 0.10 or less.

[0028] The first layer and the third layer are formed of silicon oxides, and the refractive indices are usually 1.40 to 1.58. It is preferable that the refractive index of the first layer and the refractive index of the third layer are substantially the same, and from this point of view, the difference between the first layer and the refractive index of the third layer may preferably be 0.01 or less. Since the Q value can be further improved by providing a difference between the refractive index of the first layer and the refractive index of the third layer, from this point of view, the difference between the refractive indices of the first layer and the third layer may preferably be 0.02 or more, and more preferably 0.03 or more. However, the difference may preferably be 0.10 or less.

[0029] The refractive indices of the respective layers shall be measured under the following conditions.

[0030] The measurement is carried out with a high-speed spectroscopic ellipsometer using the following system under the following measurement conditions. "System"

[0031] “M-2000” (JA Woollam Corporation), rotation compensation type “measurement conditions” Angle of incidence: 65,70,75 degrees Wavelength for measurement: 195 to 1680 nm Beam size: 2mm × 8mm The following analysis is then carried out.

[0032] “Analytical model” Metal oxide / silicon oxide / metal oxide / silicon oxide / metal oxide / silicon oxide / metal oxide / silicon oxide / substrate

[0033] “Analytical methods”

[0034] The measured Δ (phase difference) and φ (amplitude reflection) spectrum is compared with (Δ, φ) calculated based on the analytical model described above, and the dialectical function and layer thickness are adjusted to approximate the measured value (Δ, φ). Regarding the optical constants of the respective films, the value obtained from the formation of a single layer using the reference is used as the initial value. The wavelength dispersion of the refractive index is determined as the result where the measured value and the theoretical value best agree (the root mean square error converges to the minimum value).

[0035] The thickness of the first layer, the second layer, the third layer, and the fourth layer may preferably be 20 nm or more, and more preferably 100 nm or more. Since the thickness of each layer is too large, the confinement of the piezoelectric material substrate by the support substrate is weak. From this point of view, the thickness of each layer may preferably be 300 nm or less.

[0036] Although the method for forming the first layer, second layer, third layer, and fourth layer constituting the multilayer film is not limited, sputtering, chemical vapor deposition (CVD), and vapor deposition can be cited. For example, in the case of sputtering, the refractive index of the second layer and the refractive index of the fourth layer can be changed depending on the presence or absence of a bias voltage. That is, the refractive indices of the metal oxide layers can be made relatively high by applying a bias voltage, and the refractive indices of the metal oxide layers can be lowered by not applying a bias voltage. In ion-assisted vapor deposition, the refractive index of each layer can be adjusted by adjusting the assist energy.That is, the refractive index of the metal oxide layer can be made relatively high by increasing the auxiliary energy, and the refractive index of the metal oxide layer can be lowered by decreasing the auxiliary energy.

[0037] The specific production conditions for the respective layers forming the multilayer film are selected according to the chamber specifications. In a preferred embodiment, the total pressure is 0.28 to 0.34 Pa, and the oxygen partial pressure is 1.2 × 10 -3 up to 5.7 × 10 -2 Pa, and the film forming temperature is set to ambient temperature.

[0038] According to a preferred embodiment, one or more connecting layers may be provided between the substrate made of piezoelectric material and the carrier substrate. The material of such a connecting layer may be as follows. Si (1-v) O v , Ta2O5, Al2O3, Nb2O5, TiO2

[0039] In a preferred embodiment, the connecting layer provided between the carrier substrate and the substrate made of piezoelectric material has a composition of Si (1-v) O v [0.008 ≦ v ≦ 0.408].

[0040] The oxygen ratio of the composition is significantly lower than the oxygen ratio of SiO2 (corresponding to v with 0.667]. The insulating property of the compound layer can be further improved by coating the compound layer consisting of silicon oxide with such a composition of Si (1-v) O v is formed and is further inserted between them.

[0041] In the composition Si (1-v) O v, which forms each layer, the electrical resistance of the interconnect layer becomes low when v is less than 0.008. Therefore, v may preferably be 0.008 or higher, more preferably 0.010 or higher, particularly preferably 0.020 or higher, and most preferably 0.024 or higher. Since the interconnect strength is further improved by making v 0.408 or lower, v may preferably be 0.0408 or lower, and particularly preferably 0.225 or lower.

[0042] Although the thickness of each compound layer is not specifically limited, the thickness may preferably be 0.01 to 10 µm, and more preferably 0.01 to 0.5 µm from the viewpoint of production cost.

[0043] Although the film formation method of the respective compound layers is not limited, sputtering, chemical vapor deposition, and vapor deposition can be cited. Particularly preferred is the adjustment of the oxygen gas content in a chamber during reactive sputtering with Si as the sputtering target, so that the oxygen ratio (v) of the respective compound layer can be controlled.

[0044] Although the specific production conditions for each compound layer are appropriately selected depending on the specification of the chamber, according to a preferred example, the total pressure is set to 0.28 to 0.34 Pa, the oxygen partial pressure to 1.2 × 10 -3 up to 5.7 × 10 -2 Pa, and the film formation temperature is set to ambient temperature. Furthermore, B-doped Si can be specified as the Si target.

[0045] The oxygen concentration of the compound layer is measured by EDS under the following conditions.

[0046] Measuring system: The elemental analysis is carried out using the elemental analysis system “JEM-ARM200F” from JEOL Ltd.

[0047] Measurement conditions: A sample of a thinned piece is examined using the FIB (Focused Ion Beam) method at an accelerating voltage of 200 kV.

[0048] According to the present invention, the carrier substrate can be formed from a monocrystalline or polycrystalline material. The material of the carrier substrate can preferably be selected from the group consisting of silicon, sialon, sapphire, cordierite, mullite, and aluminum oxide. The aluminum oxide can preferably be translucent aluminum oxide.

[0049] Silicon can be monocrystalline silicon, polycrystalline silicon or high-resistance silicon.

[0050] Sialon is a ceramic material obtained by sintering a mixture of silicon nitride and aluminum oxide and has the following composition. Si 6-w Al w N 8-w

[0051] That is, Sialon has the composition of mixed alumina with silicon nitride, and w indicates the ratio of mixed alumina. w can preferably be 0.5 or more. Furthermore, w can preferably be 4.0 or less.

[0052] Sapphire is a single crystal with the composition Al2O3, and alumina is a polycrystal with the composition Al2O3. Cordierite is a ceramic material with the composition 2MgO · 2Al2O3 · 5SiO2. Mullite is a ceramic material with a composition ranging from 3Al2O3-2SiO2 to 2Al2O3-SiO2.

[0053] Although the material of the piezoelectric substrate is not limited as long as it has the required piezoelectricity, the material can preferably be a single crystal with the composition LiAO3. A represents one or more elements from the group consisting of niobium and tantalum. LiAO3 can therefore be lithium niobate, lithium tantalate, or lithium niobate-lithium tantalate solid solution.

[0054] The respective components of the present invention are described in more detail below.

[0055] The application of the composite body of the present invention is not specifically limited and, for example, it can preferably be used as an acoustic or optical device.

[0056] A surface acoustic wave device, a Lamb wave device, a thin film resonator (FBAR), or the like is known as an acoustic wave device. For example, the surface acoustic wave device is constructed by providing input-side IDT (Interdigital Transducer) electrodes (also called comb electrodes or interdigital electrodes) for oscillating surface acoustic waves and output-side IDT electrodes for receiving the surface acoustic waves on the surface of the piezoelectric substrate. By applying a high-frequency signal to the input-side IDT electrodes, an electric field is generated between the electrodes, causing the surface acoustic wave to oscillate and propagate on the piezoelectric substrate.The propagating surface acoustic wave is then derived as an electrical signal from the IDT electrodes on the output side, which are provided in the propagation direction.

[0057] A metal film may be provided on a bottom surface of the piezoelectric material substrate. After the Lamb device is fabricated as the acoustic wave device, the metal film plays a role in improving the electromechanical coupling factor near the bottom surface of the piezoelectric material substrate. In this case, the Lamb device has the structure that interdigitated electrodes are formed on the surface of the piezoelectric material substrate, and that the metal film on the piezoelectric material substrate is exposed through a cavity provided in the support body. Materials such as such metal layers include, for example, aluminum, an aluminum alloy, copper, gold, or the like. When fabricating the Lamb wave device, a composite substrate including the single-crystal piezoelectric substrate without the metal layer on the bottom surface may also be used.

[0058] A metal layer and an insulating layer may be provided on the underside of the piezoelectric material substrate. The metal film plays the role of electrodes when the thin-film resonator is fabricated as an acoustic wave device. In this case, the thin-film resonator has the structure that electrodes are formed on the upper and lower surfaces of the piezoelectric material substrate, and the insulating film is made into a cavity to expose the metal film on the piezoelectric material substrate. Materials for such metal layers include, for example, molybdenum, ruthenium, tungsten, chromium, aluminum, or the like. Other materials for the insulating layers include silicon dioxide, phosphosilicate glass, borophosphosilicate glass, or the like.

[0059] Furthermore, the optical device may be an optical switching device, a wavelength conversion device, or an optical modulation device. Furthermore, a periodic domain inversion structure may be formed in the substrate made of piezoelectric material.

[0060] When the subject matter of the present invention is an acoustic wave device and the substrate of piezoelectric material is formed of lithium tantalate, it is preferable to use the substrate rotated from the Y-axis to the Z-axis by 123 to 133° (e.g., 128°) around the X-axis, which is a propagation direction of a surface acoustic wave, because the propagation loss is small.

[0061] When the piezoelectric material substrate is made of lithium niobate, it is further preferable to rotate the substrate from the Y-axis to the Z-axis by 86 to 94° (e.g., 90°) around the X-axis, which is the propagation direction of the surface acoustic wave, to achieve lower propagation loss. Although the size of the piezoelectric material substrate is not specifically limited, the diameter can be, for example, 50 to 150 mm, and the thickness can be 0.2 to 60 µm.

[0062] The following method is preferred to obtain the composite body of the invention.

[0063] First, the respective surfaces to be bonded (the surface of the multilayer film, the surface of the bonding layer, the surface of the piezoelectric material substrate, and the surface of the support substrate) are smoothed to obtain flat surfaces. The method for smoothing the respective surfaces here includes lapping, chemical mechanical polishing (CMP), and the like. Furthermore, the flat surfaces may preferably have Ra of 1 nm or less, and more preferably 0.3 nm or less.

[0064] To remove the residue of a polishing agent and treat the denatured layer, the respective surfaces of the respective bonding layers are cleaned. The surface cleaning method includes wet cleaning, dry cleaning, scrubbing, or the like, with scrubbing being preferred from the viewpoint of easy and effective maintenance of the cleaned surface. At this time, it is particularly preferable to use "Sun Wash LH540" as the cleaning agent and then perform cleaning using a scrubbing machine with a mixed solution of acetone and IPA.

[0065] Then a neutralized beam is irradiated onto the respective surfaces to activate the respective surfaces.

[0066] When the surfaces are activated by the neutralized beam, a system for generating the neutralized beam, which is irradiated, is preferably used as described in Patent Document 2. That is, a high-speed saddle-field type atomic beam source is used as the beam source. An inert gas is then introduced into the chamber, and a high voltage is applied to the electrodes from a direct current source. This creates a saddle-field type electric field between the electrode (positive electrode) and a housing (negative electrode), causing the electrons to move, e, so that atomic and ion beams are obtained from the inert gas. Of the beams that reach a grid, the ion beam is neutralized at the grid, and the beam of neutral atoms is emitted from the high-speed atomic beam source.The atomic species providing the beam may preferably be an inert gas (argon, nitrogen or similar).

[0067] When activated by radiation irradiation, the voltage may preferably be 0.5 to 2.0 kV and the current may preferably be 50 to 200 mA.

[0068] The activated bonding surfaces are then brought into contact with each other and bonded under a vacuum atmosphere. The temperature at this time is ambient temperature, particularly and preferably 40°C or lower, and particularly preferably 30°C or lower. Furthermore, the temperature during bonding is preferably 20°C or higher and 25°C or lower. The pressure during bonding is preferably 100 to 20,000 N. EXAMPLES (Preliminary Experiment)

[0069] First, a silicon oxide layer or a hafnium oxide layer was formed on a piezoelectric material substrate to record the film formation conditions under which the layers described below were obtained. However, the bias voltages were adjusted as follows to adjust the refractive index of the hafnium oxide layer. Silicon oxide layer (SiO2): thickness; 150 nm, refractive index; 1.52 Hafnium oxide layer (HfO2): bias voltage; 100 V, thickness; 150 nm, refractive index; 2.07 Hafnium oxide layer (HfO2): bias voltage; 200 V ; thickness; 150 nm, refractive index; 2.12 Hafnium oxide layer (HfO2): bias voltage; 400 V ; thickness; 150 nm, refractive index 2.15 (Inventive Example A1]

[0070] Then, a surface acoustic wave device was constructed according to the Fig. 1 to 3 described processes.

[0071] Specifically, a lithium tantalate (LT) substrate with an OF portion, a diameter of 4 inches, and a thickness of 250 μm was used as the piezoelectric material substrate 1. A 128° Y-cut LT substrate was used as the LT substrate, in which the surface acoustic wave (SAW) propagation direction was in the X direction and the cutting angle was in the Y direction. The surface 1a of the piezoelectric material substrate 1 was subjected to mirror polishing so that the arithmetic average surface roughness Ra reached 0.3 nm. Furthermore, Ra was measured with an atomic force microscope (AFM) in a field of view of 10 μm × 10 μm.

[0072] Then, two laminated structures were sequentially formed on the piezoelectric material substrate 1 by sputtering to obtain the multilayer film 22. The first layer of silicon oxide was first formed on the piezoelectric material substrate, and the second layer, third layer, and fourth layer were formed in this order. The thickness and refractive index of each layer were adjusted as follows based on the preliminary experiment. First layer (SiO2): thickness; 150nm, refractive index; 1.53 Second layer (HfO2): thickness 150nm, refractive index; 2.12 Third layer (SiO2): thickness; 150nm, refractive index; 1.53 Fourth layer (HfO2): thickness; 150nm, refractive index 2.07

[0073] The interconnect layer 4 was deposited on the multilayer film 2. Specifically, the direct current sputtering method was applied, and boron-doped Si was used as a target. Furthermore, oxygen gas was introduced as an oxygen source. At this time, the amount of oxygen gas introduced was adjusted to control the total atmospheric pressure and the oxygen partial pressure in a chamber. The thickness of the interconnect layer 4 was 50 nm. The arithmetic average roughness Ra of the surface of the interconnect layer 4 was 0.2 to 0.6 nm. Subsequently, the interconnect layer 4 was subjected to chemical mechanical polishing (CMP) until the layer thickness was adjusted to 80 to 190 nm and Ra to 0.08 to 0.4 nm.

[0074] Furthermore, the support substrate 6 was manufactured with a flat orientation part (OF), a diameter of 4 inches, and a thickness of 500 µm, and made of silicon. The surface of the support substrate 6 was processed by chemical mechanical polishing (CMP) so that the arithmetic average roughness Ra was 0.2 nm.

[0075] Then, the neutralized beam was irradiated onto the surface of the interconnect layer 4 and onto the Si substrate as the supporting substrate 6 to activate the surfaces, which were directly bonded to each other.

[0076] In particular, the surface of the connecting layer 4 and the surface of the carrier substrate 6 were cleaned to remove impurities and then placed in a vacuum chamber. After evacuation to 10 -6Pa, the surfaces were irradiated with a high-speed atom beam (acceleration voltage of 1 kV and Ar flow rate of 27 sccm) for 120 seconds. After the irradiated surface (activated surface) of the bonding layer 4 and the activated surface of the supporting substrate 6 were brought into contact with each other, the substrates were bonded together by applying a pressure of 10,000 N for 2 minutes. Then, the resulting composite bodies of the respective examples were heated at 100 °C for 20 hours. The resulting composite bodies were measured by optical ellipsometry to obtain a refractive index chart, which is shown in Fig. 6 is shown.

[0077] Then, the surface of the piezoelectric material substrate 1 was ground and polished from an original thickness of 250 µm to 1 µm. Electrode patterns were then formed for measurement to obtain surface acoustic wave devices. The Q value was then measured at a frequency of 5.5 GHz and presented in Table 1.

[0078] In addition, the Q value was measured as follows.

[0079] A surface acoustic wave resonator was fabricated on a wafer, and the frequency characteristics were measured using a network analyzer. The resonance frequency f r and its half-width Δf r were calculated on the basis of the frequency characteristics thus obtained, and f r / Δf r was determined as Q-value. (Inventive Example A2]

[0080] The composite body and the surface acoustic wave device were manufactured using the same method as in Inventive Example A1. However, the respective layers constituting the multilayer film were adjusted as follows. The Q value of the resulting device at a frequency of 5.5 GHz was measured and shown in Table 1. First layer (SiO2): thickness; 150 nm, refractive index; 1.53 Second layer (HfO2): thickness; 150 nm, refractive index; 2.15 Third layer (SiO2): thickness; 150 nm, refractive index; 1.53 Fourth layer (HfO2): thickness; 150 nm, refractive index; 2.05 (Comparison example A1]

[0081] The composite body and the surface acoustic wave device were obtained by the same method as in Inventive Example A1. Furthermore, the respective layers constituting the multilayer film were adjusted as follows. The thus-obtained composite body was measured by optical ellipsometry to obtain a refractive index chart shown in Fig. 7. Furthermore, the Q value of the thus obtained device was measured at a frequency of 5.5 GHz and shown in Table 1. First layer (SiO2): thickness: 150 nm, refractive index 1.53 Second layer (HfO2): thickness: 150 nm, refractive index 2.07 Third layer (SiO2): thickness: 150 nm, refractive index: 1.53 Fourth layer (HfO2): thickness; 150 nm, refractive index 2.07 (Comparison example A2]

[0082] The composite body and the surface acoustic wave device were obtained by the same method as in Inventive Example A1. However, the respective layers constituting the multilayer film were adjusted as follows. The thus-obtained composite body was measured by optical ellipsometry to obtain a refractive index chart shown in Fig. 8. Furthermore, the Q value of the thus obtained device was measured at a frequency of 5.5 GHz and shown in Table 1. First layer (SiO2): thickness: 150 nm, refractive index 1.53 Second layer (HfO2): thickness: 150 nm, refractive index 2.12 Third layer (SiO2): thickness: 150 nm, refractive index: 1.53 Fourth layer (HfO2): thickness; 150 nm, refractive index 2.12 Table 1 Refractive index of hafnium oxide layer 7A (lamination structure on the bottom side) / (lamination structure on the top side) Refractive index of hafnium oxide layer 7B (lamination structure on the bottom side) / (lamination structure on the top side) Result of the Q-value assessment Comparison example A1 2,07 / 2,07 2,07 / 2,07 Standard (± 0%) Comparison example A2 2,12 / 2,12 2,12 / 2,12 ± 0% Inventive Example A1 2,12 / 2,12 2,07 / 2,07 + 20% Inventive Example A2 2,15 / 2,15 2,05 / 2,05 + 8%

[0083] As shown in Table 1, the refractive indices of the second layer and the fourth layer according to Comparative Example A1 were in the same order of magnitude as in the Fig. 7, because the refractive indices of the second layer and the fourth layer were set to lower values. In Comparative Example A2, the refractive indices of the second layer and the fourth layer were set to higher values, so that the refractive indices of the second layer and the fourth layer were in the same order of magnitude as the refractive indices obtained in the preliminary experiment, as shown in Fig. 8. In addition, the Q value was the same as in Comparative Example A1, and the effect of increasing the refractive indices was not observed.

[0084] According to the inventive example A1, the Fig. The refractive index distribution shown in Figure 6 was obtained.

[0085] As shown in Table 1, it was also demonstrated that the Q-value was improved by up to 20% compared to the standard value.

[0086] According to the inventive example A2, when changing the refractive index of the second layer and the refractive index of the fourth layer, a modulation of the refractive index in the thickness direction was observed, which was similar to that in Fig. 6 is similar.

[0087] As shown in Table 1, it was also demonstrated that the Q-value was significantly improved compared to the standard value. (Inventive Examples B1, B2 and Comparative Examples B1 and B2]

[0088] In Inventive Examples A1 and A2 and Comparative Examples A1 and A2, the material of the second layer was changed from HfO2 to Ta2O5. When the Q value of the resulting devices was measured, similar results were obtained as in Inventive Examples A1 and A2 and Comparative Examples A1 and A2. (Inventive Examples C1 and C2 and Comparative Examples C1 and C2]

[0089] In Inventive Examples A1 and A2 and Comparative Examples A1 and A2, the material of the second layer was changed from HfO2 to ZrO2. When the Q value of the resulting device was measured, similar results were obtained as in Inventive Examples A1 and A2 and Comparative Examples A1 and A2.

Claims

[1] Composite body, comprising: a carrier substrate; a substrate made of piezoelectric material; and a multilayer film between the carrier substrate and the substrate made of piezoelectric material, wherein the multilayer film has a lamination structure, which has a first layer, a second layer, a third layer and has a fourth layer in this order; wherein the first layer and the third layer each comprise silicon oxides; wherein the second layer and the fourth layer each comprise metal oxides; wherein a refractive index of the second layer is higher than a refractive index of the first layer and a refractive index of the third layer; and wherein the refractive index of the second layer differs from a refractive index of the fourth layer. [2] The composite body according to claim 1, wherein the multilayer film has a plurality of the lamination structures. [3] Composite body according to claim 1 or 2, wherein the metal oxides comprise hafnium oxide, tantalum oxide or zirconium oxide. [4] The composite body according to any one of claims 1 to 3, wherein a difference between the refractive index of the second layer and the refractive index of the first layer is 0.3 to 0.

8. [5] The composite body according to any one of claims 1 to 4, wherein a difference between the refractive index of the second layer and the refractive index of the fourth layer is 0.02 or more. [6] The composite body according to any one of claims 1 to 5, wherein a thickness of the first layer, a thickness of the second layer, a thickness of the third layer and a thickness of the fourth layer are each 20 nm or more and 300 nm or less. [7] Composite body according to one of claims 1 to 6, further comprising a bonding layer having a composition of Si (1-v) O v [0.008 ≦ v ≦ 0.408] between the substrate of piezoelectric material and the support substrate. [8] Acoustic wave device, comprising: the composite body according to one of claims 1 to 7; and an electrode provided on the substrate of piezoelectric material. [9] An acoustic wave device according to claim 8, which is used for an acoustic wave having a frequency of 3.5 to 6 GHz.

Citation Information

Patent Citations

  • High speed atom beam source and normal temperature bonding device including the same

    JP2014086400A

  • Method of forming a surface acoustic wave (SAW) filter device

    US7213314B2

  • Bonding method

    WO2017163722A1

  • Elastic wave device, high-frequency front end circuit, and communication device

    WO2018154950A1