METAL WIRE AND METAL NET

A tungsten or tungsten alloy wire with specific composition and manufacturing process addresses the challenge of maintaining high tensile strength and straightness, enabling applications such as screen printing and metal nets with improved performance.

DE112021007271B4Active Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
DE112021007271
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-12
Filing Date
2021-12-21
Publication Date
2024-12-05
Estimated Expiration
2041-12-21

AI Technical Summary

Technical Problem

Conventional tungsten wires with small diameters face a decrease in straightness while maintaining high tensile strength, leading to issues in applications requiring both properties.

Method used

A metal wire composed of tungsten or tungsten alloy with a tungsten content of at least 90% by weight, a diameter between 5 µm and 13 µm, and a tensile strength of at least 4.8 GPa, manufactured using a process that includes low-temperature hot drawing and room temperature drawing to achieve high straightness and tensile strength.

Benefits of technology

The metal wire achieves a balance of small diameter, high tensile strength, and excellent straightness, suitable for applications like screen printing and metal nets, with a natural hanging length of at least 800 mm per 1000 mm and diameter variation of at most 1.0 µm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Metal wire, including: Tungsten or a tungsten alloy, wherein the metal wire: a tungsten content of at least 90 wt.%; a diameter of at least 5 µm and at most 13 µm; a tensile strength of at least 4.8 GPa; and has a natural hanging length of at least 800 mm per 1000 mm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal wire and a metal mesh. [State of the art]

[0002] Conventionally, a tungsten wire with a small diameter and high tensile strength is known (see, for example, Patent Document (PTL) 1). [Document List][Patent Documents]

[0003] [PTL 1] Japanese unexamined patent application with publication number 2020-105548 [Summary of the invention][Technical problem]

[0004] However, the above-mentioned conventional tungsten wire has a problem that the straightness decreases as the diameter is reduced while maintaining high tensile strength.

[0005] Therefore, it is an object of the present invention to provide a metal wire having a small diameter and excellent tensile strength and straightness, and a metal net comprising the metal wire. [Solution to the problem]

[0006] A metal wire according to one aspect of the present invention comprises tungsten or a tungsten alloy. The metal wire has a tungsten content of at least 90 wt.%, a diameter of at least 5 µm and at most 13 µm, a tensile strength of at least 4.8 GPa, and a natural hanging length per 1000 mm of at least 800 mm.

[0007] A metal mesh according to one aspect of the present invention comprises the metal wire according to the one aspect as a warp or weft. [Advantageous effects of the invention]

[0008] The present invention can provide a metal wire having a small diameter and excellent tensile strength and straightness. [Brief description of the drawings] [ Fig. 1] Fig. 1 is a schematic diagram of a metal mesh including a metal wire according to one embodiment. [ Fig. 2A] Fig. 2A is a flowchart showing a method for manufacturing the metal wire according to the embodiment. [ Fig. 2B] Fig. 2B is a flowchart showing another example of the method for manufacturing the metal wire according to the embodiment. [ Fig. 3] Fig. 3 is a graph showing a relationship between the straightness and the tensile strength of the metal wire according to the embodiment. [ Fig. 4] Fig.4 is a graph showing a relationship between the diameter variation and the tensile strength of the metal wire according to the embodiment. [Description of embodiments]

[0009] Hereinafter, a metal wire and a metal net according to an embodiment of the present invention will be described in detail with reference to the drawings. It should be noted that each of the embodiments described below shows a specific example of the present invention. Therefore, the numerical values, shapes, materials, structural components, the arrangement and connection of the structural components, steps, the processing order of the steps, etc. shown in the following embodiments are merely examples and therefore do not limit the present invention. Of the structural components in the embodiments described below, those not specified in the independent claims are described as optional structural components.

[0010] Additionally, the figures are schematic representations and are not necessarily accurate illustrations. Accordingly, for example, the figures are not necessarily to scale. Furthermore, structural components that are substantially identical in the figures have the same reference numerals. Accordingly, duplicate descriptions are omitted or simplified.

[0011] Furthermore, in the present specification, terms representing shapes of structural components, such as circular, and numerical ranges include not only the exact meanings but also substantially identical ranges, such as a difference of about several percent. [Embodiment][Structure]

[0012] First, a metal wire according to an embodiment and a metal net comprising the metal wire are described with reference to Fig. 1 described.

[0013] The Fig.1 is a schematic diagram of a metal mesh 20 including a metal wire 10 according to the present embodiment. Fig. 1 schematically shows a mesh of only a portion of the metal mesh 20, but the entire metal mesh 20 has a mesh structure. The metal mesh 20 comprises a plurality of metal wires 10 as warp and weft. In other words, the metal mesh 20 is manufactured by weaving each of the plurality of metal wires 10 as warp or weft.

[0014] The metal mesh 20 is, for example, a screen mesh used for screen printing. The metal mesh 20 includes a plurality of openings 22. Each opening 22 is a part through which a printing ink passes during screen printing. By sealing a portion of the openings 22 with an emulsion or a resin (for example, a polyimide), a non-passage portion, which is a part through which a printing ink cannot pass, is formed. By structuring the shape of the non-passage portion into an arbitrary shape, screen printing with a desired shape can be performed.

[0015] When the metal mesh 20 is used for screen printing, the diameter of the metal wire 10 is gradually reduced to improve the accuracy of screen printing. As the diameter decreases, the absolute strength decreases significantly because the cross-sectional area of ​​the metal wire 10 decreases. For example, a typical tungsten wire with a diameter of 13 μm has a tensile strength of 3.4 GPa and an absolute strength of 0.45 N. In contrast, with a tungsten wire with a reduced diameter of 11 μm, the absolute strength is reduced to 0.32 N. To compensate for the decrease in absolute strength, an increase in strength per cross-sectional area, that is, an increase in tensile strength, is required. For example, a tensile strength of at least 4.8 GPa is required for the metal wire 10 with a diameter of 11 μm.

[0016] The metal wire 10 is a tungsten wire comprising tungsten (W) or a tungsten alloy wire comprising a tungsten alloy. The tungsten content is at least 90 wt% and may be at least 95 wt%, at least 99 wt%, at least 99.9 wt%, or at least 99.99 wt%.

[0017] It should be noted that the tungsten content is the proportion of tungsten relative to the weight of metal wire 10. The same applies to the content of other elements, such as rhenium (Re) and potassium (K), which will be described later. In addition, metal wire 10 may contain unavoidable elements that cannot be avoided during manufacturing.

[0018] The tungsten alloy is, for example, an alloy of rhenium and tungsten (ReW alloy). The rhenium content is, for example, at least 0.1 wt.% and at most 10 wt.%. The rhenium content can be at least 0.5 wt.% or at least 1 wt.%. Furthermore, the ruthenium content can be at least 5 wt.%.

[0019] When the rhenium content is high, the tensile strength of the metal wire 10 can be increased. On the other hand, when the rhenium content is too high, it is difficult to reduce the diameter while maintaining a high tensile strength of the metal wire 10. In particular, wire breakage is more likely to occur, making it difficult to draw a wire with a long length. By reducing the rhenium content and increasing the tungsten content to at least 90 wt%, the workability of the metal wire 10 can be improved. Furthermore, by reducing the content of rhenium, which is rare and expensive, a low-cost metal wire 10 with a long length can be mass-produced.

[0020] The diameter of the metal wire 10 is 13 µm at most. As the diameter decreases, a metal mesh 20 with a higher aperture ratio can be produced. For example, printing accuracy can be improved. The diameter of the metal wire 10 can be 12 µm at most, 10 µm at most, 8 µm at most, or 7 µm at most. The diameter of the metal wire 10 is at least 5 µm.

[0021] The diameter variation of the metal wire 10 is 1.0 µm at most. The diameter variation corresponds to an absolute difference between a maximum value and a minimum value of the diameter of the metal wire 10. Therefore, the diameter difference between any two points on the metal wire 10 is 1.0 µm at most. The diameter variation can be measured, for example, using a laser diameter gauge, a scanning electron microscope (SEM), or a laser microscope. The diameter variation can be 0.6 µm at most, 0.5 µm at most, 0.4 µm at most, or 0.3 µm at most.

[0022] It should be noted that the cross-sectional shape of the metal wire 10 perpendicular to the axis of the metal wire 10 is, for example, round, but is not limited to this example. The cross-sectional shape of the metal wire 10 can be, for example, oval, square, or rectangular.

[0023] The tensile strength of the metal wire 10 is at least 4.8 GPa (= 4800 MPa). The tensile strength can be at least 4.9 GPa, at least 5.0 GPa, at least 5.1 GPa, or at least 5.2 GPa. The tensile strength can be measured, for example, according to the tensile test of the "Japanese Industrial Standard" (JIS H 4460 8).

[0024] The straightness of the metal wire 10 is expressed as the natural hanging length per 1000 mm. Specifically, the natural hanging length (i.e., the straightness) per 1000 mm of the metal wire 10 is at least 800 mm. The straightness of the metal wire 10 can be at least 900 mm, at least 950 mm, or at least 970 mm. The natural hanging length can be measured, for example, according to the straightness test of the "Japanese Industrial Standard" (JIS H 4460 15).

[0025] As described above, the metal wire 10 according to the present embodiment has a small diameter, high tensile strength, and high straightness. Furthermore, the metal wire 10 according to the present embodiment has a high tungsten content and excellent machinability. [Manufacturing process]

[0026] Next, a method for manufacturing the metal wire 10 will be described with reference to Fig. 2A and the Fig. 2B. The Fig. 2A is a flowchart showing the method for manufacturing the metal wire 10 according to the present embodiment. Fig. 2B is a flowchart showing another example of the method for manufacturing a metal wire 10 according to the present embodiment.

[0027] As it is in the Fig.As shown in Figure 2A, a tungsten ingot is first prepared (S10). Specifically, a tungsten ingot is prepared by preparing a tungsten powder aggregate and pressing and sintering the prepared tungsten powder aggregate.

[0028] It should be noted that when manufacturing the metal wire 10 containing a tungsten alloy, a mixture of a tungsten powder and a metal powder (for example, a rhenium powder) mixed in a predetermined ratio is prepared instead of the tungsten powder aggregate. The average particle size of the tungsten powder and the rhenium powder is in a range of, for example, at least 3 µm and at most 4 µm, but is not limited thereto.

[0029] Next, the produced tungsten ingot (S12) undergoes drop forging. Specifically, the tungsten ingot is press-forged and stretched from its edge to obtain a tungsten wire with a wire shape. The ingot can be subjected to rolling processing instead of drop forging.

[0030] For example, a tungsten ingot with a diameter of approximately 15 mm or more and 25 mm or less is formed into a tungsten wire with a diameter of approximately 3 mm by repeating the die forging process. Annealing during an intermediate step of the die forging process can ensure machinability in subsequent processing. For example, annealing at 2400 °C is performed in a range where the diameter is 8 mm or more and 10 mm or less. It should be noted that in order to achieve tensile strength through crystal grain refinement, annealing is not performed in the die forging process when the diameter is less than 8 mm.

[0031] Next, the tungsten wire is heated to 900 °C before hot drawing (S14). Specifically, the tungsten wire is heated directly, for example, by a torch. Heating the tungsten wire forms an oxide layer on its surface, preventing breakage of the tungsten wire during processing in the subsequent hot drawing step.

[0032] Next, hot drawing is performed (S16). Specifically, drawing of the tungsten wire, namely a wire drawing process (thinning) of the tungsten wire, is performed using one or more wire drawing dies while heating the metal wire. The heating temperature is, for example, 1000°C. Since the workability of the tungsten wire improves with increasing heating temperature, drawing can be easily performed. Hot drawing is repeatedly performed while changing the one or more wire drawing dies. The reduction in the area of ​​the tungsten wire by a wire drawing process using a single wire drawing die is, for example, at least 10% and at most 40%. In hot drawing, a lubricant comprising graphite dispersed in water can be used.

[0033] Hot drawing (S16) is repeated until the desired tungsten wire is obtained (no in S18). The desired diameter here is the diameter obtained when the remaining number of drawings is two. For example, the desired diameter is approximately 80 µm.

[0034] It should be noted that when repeating the hot drawing, a wire drawing die with a smaller hole diameter is used than the hole diameter of the wire drawing die used in the immediately preceding hot drawing. Furthermore, when repeating the hot drawing, the tungsten wire is heated at a lower heating temperature than the heating temperature of the immediately preceding hot drawing. In other words, the heating temperature is gradually reduced. The final heating temperature, for example, is 400°C, which contributes to the refinement of crystal grains.

[0035] When a tungsten wire with the desired diameter is obtained and the remaining number of drawings is two (Yes in S18), drawing is carried out at room temperature (S20). It should be noted that, as stated in the Fig. 2B, electrolytic polishing (S19) may be performed prior to room-temperature drawing (S20). During room-temperature drawing, the tungsten wire is drawn without heating, thus achieving further refinement of crystal grains. Furthermore, room-temperature drawing also has the effect of aligning the crystal orientation in the processing axis direction (specifically, a direction parallel to the axis of the metal wire 10).

[0036] Room temperature, for example, is a temperature in the range of at least 0°C and at most 50°C. An example of room temperature is 30°C. Specifically, the tungsten wire is drawn using a plurality of wire drawing dies with different hole diameters. In room temperature drawing, a liquid lubricant such as a water-soluble lubricant is used. Since no heating is performed in room temperature drawing, a water-soluble lubricant is used. Since no heating is performed in room temperature drawing, liquid evaporation is prevented. Accordingly, a sufficient function as a lubricant can be exerted. Unlike hot drawing at 600°C or higher, which is the traditional tungsten wire processing method conventionally performed, the tungsten wire is not heated and is processed while being cooled with the liquid lubricant.As a result, dynamic recovery and dynamic recrystallization can be prevented, thereby contributing to the refinement of crystal grains without wire breakage and achieving high tensile strength.

[0037] For example, the processing rate during room temperature drawing is at least 70%. The processing rate is represented by the following expression (1) using the diameter Db immediately before room temperature drawing and the diameter Da immediately after room temperature drawing. Processing rate={1−(Da / Db)2}×100

[0038] As can be seen from expression (1), when the diameter decreases sharply due to room temperature drawing, the value of the processing rate increases. For example, even if the diameter Db immediately before room temperature drawing is the same, the diameter Da immediately after room temperature drawing decreases as the processing rate increases. By increasing the processing rate, the degree of thinning of the tungsten wire due to room temperature drawing increases, that is, a thinner tungsten wire is obtained. The processing rate of room temperature drawing is at least 70%, but may be at least 80%, at least 90%, or at least 95%. The diameter immediately after room temperature drawing is approximately in a range of at least 20 μm and at most 40 μm.

[0039] Next, low-temperature hot drawing (S22) is performed after room temperature drawing. In other words, the final drawing of the tungsten wire is performed while heating the tungsten wire at a low temperature. The temperature at this time is higher than the temperature (room temperature) for room temperature drawing (S20) and lower than the temperature for hot drawing (S16). Specifically, the temperature for low-temperature hot drawing is in a range of at least 100°C and at most 300°C. An example of the temperature for low-temperature hot drawing is 200°C or 300°C. The diameter after low-temperature hot drawing is approximately in a range of at least 10 μm and at most 16 μm.

[0040] Low-temperature hot drawing is a new processing method in which the heating temperature for processing is reduced by approximately 300°C compared to the heating temperature of 500°C to 600°C in normal drawing. This allows for increased tensile strength and improved straightness or diameter variation. On the other hand, if processing is carried out after drawing at room temperature at 500°C to 600°C, the tensile strength decreases and does not reach 4.8 GPa (Comparative Example 27 in Table 2, described below).

[0041] Finally, electrolytic polishing is performed on the tungsten wire resulting from low-temperature hot drawing to fine-tune its diameter (S24). For example, electrolytic polishing is performed by immersing the tungsten wire and a counter electrode in an electrolyte solution, such as a sodium hydroxide solution, and creating a potential difference between the tungsten wire and the counter electrode. The diameter after electrolytic polishing is 13 µm at most.

[0042] Through the above-described processes, a metal wire 10 according to the present embodiment is manufactured. Through the above-described processes, the length of the metal wire 10 immediately after production is, for example, at least 50 km, and is thus industrially available. The metal wire 10 is cut to a suitable length according to the aspect in which the metal wire 10 is to be used, and can also be used, for example, in the form of a needle or a rod.

[0043] It should be noted that each of the processes described in the method for manufacturing the metal wire 10 is performed, for example, as an in-line process. Specifically, the plurality of wire drawing dies used in step S16 are arranged along the manufacturing line in order of decreasing hole diameter. Furthermore, heating devices, such as burners, are arranged between the wire drawing dies. Furthermore, an electrolytic polishing device may be arranged between the wire drawing dies.Furthermore, on the downstream side (post-processing side) of the wire drawing dies used in step S16, one or more wire drawing dies used in step S20 and one or more wire drawing dies used in step S22 are arranged in order of decreasing hole diameter, and the electrolytic polishing device is arranged on the downstream side of the wire drawing die with the smallest hole diameter. It should be noted that each of the operations can be performed individually.

[0044] Moreover, the above-described method for manufacturing the metal wire 10 is only an example, and the temperature and diameter in each process can be adjusted in an appropriate manner.

[0045] As described above, in the method for manufacturing the metal wire 10 according to the present embodiment, hot drawing is performed at a first temperature, which is a high temperature; room temperature drawing is performed at a second temperature, which is room temperature; and then low-temperature hot drawing is performed at a third temperature, which is a low temperature. The third temperature is higher than the second temperature (room temperature) and lower than the first temperature (high temperature).

[0046] As described above, a metal wire 10 is manufactured by implementing a novel process called low-temperature hot drawing (also referred to as low-temperature hot working). By performing low-temperature hot drawing, a metal wire 10 with a small diameter and a diameter deviation of 1.0 μm or less, as well as both high tensile strength and high straightness, can be obtained. [Work examples]

[0047] Hereinafter, working examples of the metal wire 10 according to the present embodiment will be described with reference to Table 1 and the Fig. 3 and Fig. 4, in comparison with metal wires according to comparative examples, which are produced without low-temperature hot drawing.

[0048] Table 1 shows the material, processing method (drawing method), diameter, tensile strength, straightness (natural hanging length per 1000 mm) and diameter variation of each of the working examples and comparative examples of metal wires comprising tungsten or tungsten alloy. [Table 1] Working example no. material Processing methods Diameter [µm] Tensile strength [GPa] Straightness [mm] Diameter variation [µm] Pulling at room temperature (processing rate) Low-temperature hot drawing (temperature) 1 ReW (Re: 1 wt%) Completed: 70% Performed: 300 °C 13 5,0 930 0,4 2 11 5,1 970 0,4 3 9 5,0 970 0,4 4 Completed: 70% Conducted: 200 °C 9 5,2 920 0,5 5 Completed: 80% Performed: 300 °C 9 5,2 960 0,4 6 7 5,2 960 0,4 7 W Completed: 70% Performed: 300 °C 13 4,9 820 0,5 8 11 4,9 950 0,3 9 9 4,9 950 0,4 10 7 4,9 970 0,6 11 Completed: 80% Performed: 300 °C 9 5,1 940 0,5 12 7 5,1 960 0,5 13 Completed: 80% Conducted: 200 °C 9 5,2 840 0,6 14 7 5,2 910 0,7 [Table 2] Comparison example no. material Processing methods Diameter [µm] Tensile strength [GPa] Straightness [mm] Diameter variation [µm] Pulling at room temperature (processing rate) Low-temperature hot drawing (temperature) 21 W Completed: 70% Not carried out 13 4,9 760 1,9 22 11 4,8 530 1,6 23 Not carried out Not carried out 13 3,4 950 0,5 24 11 3,7 940 0,5 25 13 4,4 940 0,5 26 8 4,5 900 0,4 27 Completed: 70% Normal warm-up 9 4,6 950 0,6 28 Straight annealing 13 4,5 920 1,9

[0049] The Fig. Figure 3 shows a relationship between the straightness and the tensile strength in each of the working examples shown in Table 1 and each of the comparative examples shown in Table 2. The Fig. 3 is a graph showing a relationship between the straightness and tensile strength of the metal wire 10 according to the present embodiment. Fig.3, the straightness (natural hanging length per 1000 mm) of the metal wire 10 is shown on the horizontal axis and the tensile strength of the metal wire 10 is shown on the vertical axis.

[0050] The Fig. Figure 4 shows a relationship between the diameter variation and the tensile strength in each of the working examples shown in Table 1 and each of the comparative examples shown in Table 2. The Fig. Fig. 4 is a graph showing a relationship between the diameter variation and the tensile strength of the metal wire 10 according to the present embodiment. Fig. 4, the diameter variation of the metal wire 10 is shown on the horizontal axis and the tensile strength of the metal wire 10 is shown on the vertical axis. It should be noted that in the Fig. 3 and Fig.4 The number adjacent to a plotted point represents each of the numbers assigned to the working examples and the comparative examples, namely, the working examples 1 to 14 in Table 1 and the comparative examples 21 to 28 in Table 2.

[0051] The metal wire in each of Working Examples 1 to 14 is a metal wire manufactured according to the flow chart shown in the Fig. 2A. The metal wire in each of Working Examples 1 to 14 is a metal wire obtained by performing both room temperature drawing (S20) and low-temperature hot drawing (S22) while appropriately adjusting processing conditions such as the material, the target diameter, the processing rate of room temperature drawing, and the low-temperature hot drawing temperature.

[0052] The metal wire in each of Comparative Examples 21 and 22 is a metal wire obtained without performing the low-temperature hot drawing (S22) after the room temperature drawing (S20). As shown in Table 2 and the Fig. 3, the straightness is low, although high tensile strength is obtained by drawing at room temperature. In addition, as shown in the Fig. 4, the diameter variation is large and the straightness is low.

[0053] The metal wire in each of Comparative Examples 23 to 26 is a metal wire produced without either room temperature drawing (S20) or low temperature hot drawing (S22). As shown in Table 2 and the Fig. 3 and Fig.As shown in Figure 4, high tensile strength cannot be obtained if drawing is not performed at room temperature. To increase the tensile strength, drawing at room temperature is necessary, but in this case, the straightness decreases as in Comparative Examples 21 and 22.

[0054] It should be noted that the metal wire in Comparative Example 27 is a metal wire obtained by performing room temperature drawing (S20) and normal hot drawing at a temperature of 500 °C to 600 °C instead of low-temperature hot drawing (S22). As shown in Table 2 and the Fig. As shown in Figure 3, the tensile strength does not reach 4.8 GPa, although high straightness is achieved.

[0055] Accordingly, high tensile strength and high straightness cannot both be achieved without low-temperature hot drawing. There is a trade-off between the tensile strength and straightness of a thin metal wire with a diameter of 13 µm or less, such as the metal wire according to Comparative Examples. In other words, straightness decreases as tensile strength increases, and tensile strength decreases as straightness increases.

[0056] In contrast, as shown in Table 1 and the Fig. 3, high tensile strength and high straightness are achieved in working examples 1 to 14. In addition, as shown in the Fig.4, high tensile strength and small diameter variation or high straightness are achieved. In other words, by performing low-temperature hot drawing, a metal wire 10 having both high tensile strength and high straightness can be obtained, even when the diameter is 13 μm or less and is small. The metal wire 10 is a tungsten wire containing no rhenium or a rhenium-tungsten alloy wire with a rhenium content of 10 wt% or less, and thus is a metal wire 10 with excellent workability.

[0057] It should be noted that the metal wire in each of Working Examples 1 to 6 is a rhenium-tungsten alloy wire containing 1 wt% rhenium, and the metal wire in each of Working Examples 7 to 14 is a tungsten wire containing no rhenium. As can be seen from Table 1, when comparing tungsten wires with the same diameter and under the same drawing conditions, the tensile strength of the rhenium-tungsten alloy wire is slightly improved compared to the tensile strength of the tungsten wire. This is due to the solid solution strengthening mechanism. In addition, dispersion strengthening by deposition at grain boundaries in an oxide state also contributes to an improvement in tensile strength to some extent.

[0058] Therefore, a similar effect can be obtained if other metal elements with different atomic radii are used instead of rhenium as elements causing such a strengthening mechanism. That is, if the metal wire 10 comprises a tungsten alloy, the metal included in the tungsten alloy does not have to be rhenium. In other words, the tungsten alloy can be an alloy of tungsten and at least one type of metal other than tungsten.

[0059] Metals other than tungsten include transition metals and elements with atomic radii close to that of rhenium, such as molybdenum (Mo), iridium (Ir), ruthenium (Ru), or osmium (Os). The content of each of these metals is, for example, at least 0.1 wt.% and at most 10 wt.%, but is not limited to this. For example, the content of the metal in the tungsten alloy can be less than 0.1 wt.% or more than 1 wt.%.

[0060] Furthermore, as can be seen from a comparison of Working Example 3 and Working Example 4, lowering the temperature of low-temperature hot drawing can increase the tensile strength while maintaining high straightness even when the diameter is identical. As can be seen from a comparison of Working Example 3 and Working Example 5, by increasing the processing rate of room temperature drawing, it is possible to increase the tensile strength while maintaining high straightness even when the diameter is identical. A tungsten wire containing no rhenium exhibits a similar relationship, as can be seen from a comparison of Working Examples 9 to 14.

[0061] As can be seen from a comparison of Working Examples 3 and 4, by increasing the temperature of low-temperature hot drawing, it is possible to increase straightness while maintaining high tensile strength even when the diameter is identical. A tungsten wire containing no rhenium exhibits a similar relationship, as can be seen from a comparison of Working Examples 9 to 14. [Beneficial effects, etc.]

[0062] As described above, the metal wire 10 according to the present embodiment comprises tungsten or a tungsten alloy. The metal wire has a tungsten content of at least 90 wt%, a diameter of at least 5 µm and at most 13 µm, a tensile strength of at least 4.8 GPa, and a natural hanging length per 1000 mm of at least 800 mm. Furthermore, the metal wire has a diameter variation of, for example, at most 1.0 µm.

[0063] This makes it possible to obtain a metal wire 10 with a small diameter and excellent tensile strength and straightness.

[0064] It should be noted that the straightening annealing process is generally known as a treatment for improving straightness. In the straightening annealing process, a metal wire is heated at a high temperature of about 1000°C after the wire drawing process or electrolytic polishing. However, for example, when the straightening annealing process is performed on the metal wire in Comparative Example 21, the tensile strength is reduced although the straightness is increased. For example, the metal wire in Comparative Example 28 in Table 2 is a metal wire obtained by subjecting the metal wire in Comparative Example 21 to the straightening annealing process. As can be seen from a comparison with Comparative Example 21, the straightness can be improved by performing the straightening annealing process, but instead the tensile strength is reduced to less than 4.8 GPa.In other words, the straight annealing process cannot provide both high straightness and high tensile strength. Furthermore, the diameter variation remains virtually unchanged in the straight annealing process. Therefore, the diameter variation cannot be reduced.

[0065] In contrast, the metal wire 10 according to the present embodiment is a metal wire without the straightening annealing process. By using low-temperature hot drawing without the straightening annealing process, both high straightness and high tensile strength can be achieved.

[0066] In addition, the metal wire, for example, has a natural hanging length of at least 900 mm per 1000 mm.

[0067] This increases the straightness and therefore the metal wire 10 is better suited for weaving a metal net 20, for example.

[0068] For example, if a metal wire with a diameter variation of more than 1.0 µm is used for weaving, uneven weaving is likely to occur during weaving. Therefore, the unevenly woven metal mesh may exhibit height variations. If this metal mesh is used for a screen mesh, problems such as reduced accuracy during screen printing may occur when the metal mesh is pressed or squeezed through a squeegee.

[0069] In addition, if a metal wire with a straightness of less than 800 mm is woven, the wire may be kinked and cause problems such as wire breakage during weaving. If secondary processing of a wire other than weaving, such as twisted wire processing, is performed using a metal wire with a straightness of less than 800 mm, wire breakage or other problems may occur.

[0070] On the other hand, the metal mesh 20 according to the present embodiment includes the metal wire 10 as a warp or weft. Furthermore, the metal mesh 20 is used, for example, as a mesh for screen printing.

[0071] As a result, the metal mesh 20 can be easily manufactured because the metal wire 10 has a small diameter and excellent tensile strength and straightness. Because the diameter is small, the metal mesh 20 can be manufactured with a high opening ratio.

[0072] In addition, the metal wire has a tungsten content of at least 90 wt.%.

[0073] For example, by reducing the content of other elements such as rhenium and increasing the tungsten content, the metal wire 10 having excellent workability can be obtained. [Miscellaneous]

[0074] Although the metal wire and the metal net according to the present invention have been described based on the above-described embodiment, the present invention is not limited to the above-described embodiment.

[0075] For example, in the above-described embodiment, an example was described in which the metal mesh 20 is a sieve mesh, but the present invention is not limited to this example. The metal mesh 20 can also be used, for example, as a filter or protective clothing. All strands of the warp and weft of the metal mesh 20 can be the metal wire 10. Alternatively, at least a single strand of the warp or weft can be the metal wire 10, and the remaining strands of the warp or weft can be another metal wire, such as stainless steel.

[0076] Additionally, the metal wire 10 can be used, for example, in applications other than wire rods for weaving metal meshes 20. For example, the metal wire 10 can be used as saw wires, medical needles, ropes, or strings.

[0077] Furthermore, the metal wire 10 may comprise, for example, tungsten doped with potassium (K). Doped potassium is present at the crystal grain boundaries of tungsten. Potassium (K) dispersed at grain boundaries inhibits grain coarsening during heating at high temperature and during hot drawing, but no grain coarsening occurs during drawing at room temperature. Therefore, the amount of potassium (K) may be, for example, at most 0.010 wt%. However, the presence of potassium (K) at grain boundaries has the effect of slightly increasing the strength in the processes up to drawing at room temperature. With such a potassium-doped tungsten wire, a tungsten wire with a higher tensile strength than the general tensile strength of a piano wire can be achieved, as is the case with the tungsten alloy wire.A similar effect can be achieved not only with the oxides of potassium, but also with oxides of other substances, such as cerium or lanthanum.

[0078] A potassium-doped tungsten wire can be manufactured by the same manufacturing method as the present embodiment using potassium-doped tungsten powder instead of tungsten powder.

[0079] In addition, for example, the surface of the metal wire 10 may be coated with an oxide film or a nitride film or may be plated.

[0080] In addition, embodiments obtained by one skilled in the art by making modifications to the above embodiment, as well as embodiments obtained by combining structural components and functions described in the above embodiment without substantially departing from the teachings of the present invention, are also intended to be within the scope of the present invention. [List of reference symbols] 10 metal wire 20 metal net

Claims

[1] Metal wire, comprising: Tungsten or a tungsten alloy, where the metal wire: a tungsten content of at least 90% by weight; a diameter of at least 5 µm and at most 13 µm; a tensile strength of at least 4.8 GPa; and has a natural hanging length of at least 800 mm per 1000 mm. [2] The metal wire according to claim 1, wherein the metal wire has a diameter variation of at most 1.0 µm. [3] Metal wire, comprising: Tungsten or a tungsten alloy, where the metal wire: a tungsten content of at least 90% by weight; a diameter of at least 5 µm and at most 9 µm; a tensile strength of at least 4.8 GPa; and has a diameter variation of no more than 1.0 µm. [4] Metal wire according to any one of claims 1 to 3, wherein the metal wire has a natural hanging length per 1000 mm of at least 900 mm. [5] A metal mesh comprising the metal wire according to any one of claims 1 to 4 as a warp or weft. [6] The metal mesh according to claim 5, wherein the metal mesh is used as a mesh for screen printing.

Citation Information

Patent Citations

  • Tungsten wire and saw wire

    JP2020105548A