COMPOSITE COPPER PARTICLES, METHOD FOR PRODUCING THE SAME AND METHOD FOR SHAPING A COMPOSITE COPPER FORM ITEM USING COMPOSITE COPPER PARTICLES

DE112021008564T5Pending Publication Date: 2024-10-02NIIMI SANGYO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE112021008564
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

Pure copper powder has a low light absorption rate, making it inefficient for 3D printing with low-output lasers like blue semiconductor or Yb fiber lasers, which results in reduced electrical and thermal conductivity and increased energy requirements.

Method used

Composite copper particles with light-absorbing substances like carbon or magnetite are dispersed in copper base particles, increasing light absorption and allowing for efficient 3D printing with Yb fiber lasers, maintaining conductivity and hardness.

Benefits of technology

The composite copper particles enable practical 3D printing with lower laser output, achieving electrical and thermal conductivity equivalent to pure copper while enhancing hardness through uniform dispersion of light-absorbing substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0001_ABST
    Figure 00000000_0001_ABST
  • Figure 00000000_0002_ABST
    Figure 00000000_0002_ABST
  • Figure 00000000_0003_ABST
    Figure 00000000_0003_ABST
  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A composite copper particle is provided that enables the practical shaping of copper objects using a 3D printer. Within this composite copper particle, particles of a light-absorbing substance are dispersed in a copper base particle. These light-absorbing particles have a diameter smaller than that of the base particle and an absorption coefficient of 40% or more for light with a wavelength of 1 µm. Because the light absorption coefficient of the composite copper particle itself is relatively high, it is possible, for example, to shape a copper object using a low-power 3D printer with a YB fiber laser.The composite copper particle is produced by i) producing a precursor particle in which small copper particles with a particle diameter smaller than that of the base particle and the particles of the light-absorbing substance are aggregated, and ii) spheroidizing the composite copper particle while melting the small copper particles to form the base particle by introducing the precursor particle into a thermal plasma flame.
Need to check novelty before this filing date? Find Prior Art

Description

Composite copper particles, their manufacturing method, and method for forming a composite copper shaped body using the same

[0001] The present invention relates to composite copper particles, a method for producing the same, and a method for forming a composite copper shaped body using the same.

[0002] Recently, 3D printing of metal powder materials (metal additive manufacturing) has been attracting attention, and in view of the good electrical and thermal conductivity of copper, 3D printing of a molded object using copper as a base material is also being considered. For example, the following Patent Document 1 describes a 3D printing method using Cu—Cr alloy powder as a material.

[0003] Japanese Patent Application Laid-Open No. 2018-070914

[0004] When copper is alloyed, it is generally inevitable that its electrical conductivity and thermal conductivity will deteriorate. Therefore, it is desirable to use pure copper powder as a material to produce a shaped object using a 3D printer. However, when pure copper powder is used as a material, a high-energy beam must be irradiated due to the extremely low light absorption rate of copper. For example, when using a relatively inexpensive 3D printer that irradiates a low-wavelength laser such as a blue semiconductor laser or employs a near-infrared laser (typically a Yb fiber laser), the shaping must be performed at a relatively high output. The present invention has been made in consideration of such circumstances, and aims to provide composite copper particles that can be used as a copper powder material that enables practical shaping using a 3D printer, a manufacturing method thereof, and a method for producing a composite copper shaped object using the same.

[0005] In order to solve the above problems, the composite copper particles of the present invention are characterized in that particles of a light-absorbing material having a particle diameter smaller than that of the base copper particle and an absorptivity of 40% or more for light with a wavelength of 1 μm are dispersed in the copper base particle.

[0006] Furthermore, the method for producing the composite copper particles of the present invention for producing the above-mentioned composite copper particles of the present invention is characterized by comprising: a step of preparing precursor particles in which copper particles having a particle size smaller than that of the base particles and particles of the light-absorbing material are aggregated or bonded to each other; and a step of introducing the precursor particles into a thermal plasma flame, melting the copper particles to produce the base particles, and spheroidizing the composite copper particles.

[0007] Furthermore, the method for manufacturing a composite copper shaped object of the present invention is characterized in that the composite copper particles of the present invention are used and shaped by irradiating Yb fiber laser light using a 3D printer.

[0008] The composite copper particles of the present invention have a relatively high degree of light absorption due to the particles of the light-absorbing material dispersed in the base particles. Therefore, the method for manufacturing a composite copper object of the present invention using such composite copper particles allows for the object to be manufactured at a relatively low output. Furthermore, the composite copper object manufactured by this method has electrical conductivity and thermal conductivity equivalent to that of a pure copper object, and, because the particles of the light-absorbing material are uniformly dispersed in the copper matrix, has a higher hardness than a pure copper object. Furthermore, the method for manufacturing composite copper particles of the present invention allows for the easy production of spherical composite copper particles of the present invention in which the particles of the light-absorbing material are uniformly dispersed.

[0009] 1 is a schematic diagram for explaining the spheroidization of precursor particles by a thermal plasma flame; 2 is a photograph showing an SEM image of composite copper particles of an example, and a graph showing particle size distribution; 3 is a schematic diagram of an apparatus for measuring the degree of light absorption of composite copper particles of an example; and 4 is a graph showing the calorific value of composite copper particles of an example.

[0010] The composite copper particles of the present invention are composed of a single copper base particle in which a plurality or a large number of particles of a light-absorbing material are dispersed. The particles have a particle diameter smaller than that of the base particle and an absorptivity of 40% or more for light with a wavelength of 1 μm. The "base particle" can also be called a matrix particle or a base material particle. Considering that the composite copper particles of the present invention are used for shaping using a Yb fiber laser, the "light-absorbing material" used has an absorptivity of 40% or more for light with a wavelength of 1 μm. The "light-absorbing material particles" have a particle diameter smaller than that of the base particle because they are dispersed in the base particle. When the composite copper particles of the present invention are melted by a Yb fiber laser during shaping, the interior of the base particle is melted and exposed. Therefore, it is desirable that the light-absorbing material particles be dispersed not only on the surface of the base particle but also inside it.

[0011] The "light-absorbing material" is preferably one that does not form a compound with copper. Specifically, for example, one or more materials selected from carbon (C), magnetite (Fe3O4), wustite (FeO), chromia (Cr2O3), and hematite (Fe2O3) can be used. In particular, when carbon is used, the electrical conductivity of the shaped body can be maintained high. Furthermore, when magnetite is used, spherical composite copper particles can be easily obtained.

[0012] In consideration of shaping using a Yb fiber laser, the particle diameter of the composite copper particles of the present invention is desirably 10 μm or more and 100 μm or less. In order to be dispersed in composite copper particles of that particle diameter, the particle diameter of the light-absorbing substance is desirably 0.01 μm or more and 1 μm or less.

[0013] With regard to particle shape, the composite copper particles of the present invention preferably have a ratio of the major axis to the minor axis of 1 or more and 1.5 or less, and in short, preferably have a spherical shape.

[0014] Considering that the composite copper particles of the present invention can be used for shaping using a Yb fiber laser and that the electrical conductivity and thermal conductivity are not reduced compared to pure copper shaped bodies, the composite copper particles of the present invention preferably contain a light-absorbing substance in an amount of 1 wt % to 10 wt % inclusive, and the weight composition ratio of copper to the light-absorbing substance is preferably in the range of 99:1 to 90:10.

[0015] The method for producing composite copper particles of the present invention comprises: i) a precursor particle preparation step of preparing precursor particles in which a plurality or a large number of copper particles (sometimes referred to as "small copper particles" for convenience) having a particle size smaller than that of the base particle and a plurality or a large number of particles of a light-absorbing material are aggregated or bonded to each other; and ii) a spheroidization step of introducing the precursor particles into a thermal plasma flame to melt the small copper particles to produce the base particle and to spheroidize the composite copper particles. Incidentally, it is preferable to use small copper particles having a particle size of 0.1 μm or more and 10 μm or less.

[0016] The precursor particle preparation step may be carried out by mixing the copper small particle powder and the light absorbing material particle powder in a ball mill, mortar, or the like while adding a binder and water as a medium to prepare a paste or slurry, drying and calcining the slurry, and then pulverizing and classifying the dried and calcined product, or spray-drying the slurry with a spray dryer and calcining the dried product, etc. Incidentally, it is desirable to prepare precursor particles having a particle diameter of 15 μm or more and 105 μm or less.

[0017] The spheroidizing step may be performed by introducing precursor particles into a thermal plasma flame generated by a high-frequency induction coil in an Ar atmosphere or an Ar—H atmosphere, using, for example, an apparatus such as that described in Japanese Patent No. 3639279.

[0018] The method for manufacturing a composite copper shaped object of the present invention can be carried out by using the composite copper particles of the present invention and irradiating them with Yb fiber laser light using a 3D printer, and the specific device and manufacturing method are not limited. Generally, the method can be carried out using a powder bed method, but it can also be carried out using a metal deposition method.

[0019] [A] Production of Composite Copper Particles Three types of composite copper particles (sample numbers #11, #21, and #22) using carbon (C) as the light-absorbing material, and three types of composite copper particles (sample numbers #31, #32, and #33) using magnetite (Fe3O4) as the light-absorbing material were produced. Neither carbon nor magnetite forms compounds with copper. The production process can be divided into (a) blending of raw materials and preparation of precursor particles, and (b) spheroidization and classification. Each process is described below.

[0020] (a) Blending of raw materials and preparation of precursor particles The blending ratio of raw materials in the production of each composite copper particle, that is, in the production of each precursor particle, is as shown in the table below.

[0021] i) Sample No. 11: Copper powder AFS-Cu 7 μm (average particle size 7.2 μm) manufactured by Nippon Atomize Co., Ltd. was prepared as copper, and FW200 (average particle size 0.013 μm) manufactured by COLOUR BLACK was prepared as carbon. These were mixed in a mortar with the addition of methanol and pure water as a medium according to the blending ratio in the table above to prepare a paste.

[0022] The paste was dried at room temperature and then compacted using a die with a diameter of 50 mm at a pressure of 1 ton to obtain pellets. The pellets were then calcined in an Ar atmosphere at 600°C for 8 hours, and the calcined pellets were crushed in a mortar and classified to produce precursor particles with particle sizes of 20 to 80 μm.

[0023] ii) Sample Nos. 21 and 22: For copper, ATP-Cu 1.5 μm copper powder (average particle size 1.54 μm) manufactured by Nippon Atomized Processing Co., Ltd. was prepared, and for carbon, Nerox 505 carbon powder (average particle size approximately 0.015 μm) manufactured by Orion Engineered Carbons Co., Ltd. was prepared. These were mixed according to the blending ratios in the table above, and pure water having the blending ratios in the table above was used as a medium. Special polyvinyl alcohol PVA JMR-10M manufactured by Nippon Vinyl Acetate & Poval Co., Ltd. was added as a binder so that the solid content met the blending ratio in the table above. The mixture was dispersed and mixed in a ball mill to prepare a slurry.

[0024] The slurry was spray-dried using a spray dryer (TRS-2W) manufactured by Sakamoto Giken Co., Ltd. to obtain granulated powder having an average particle size of 35 μm. The granulated powder was calcined by holding it in an Ar atmosphere at 600° C. for 12 hours, and a debindered solid powder was produced as precursor particles.

[0025] iii) Sample Nos. 31, 32, and 33: Copper powder ATP-Cu 1.5 μm (average particle size 1.54 μm) manufactured by Nippon Atomize Co., Ltd. was used as the copper, and magnetite powder Bayferrox® (registered trademark) manufactured by LANXESS (average particle size approximately 0.2 μm) was used as the magnetite. These were mixed according to the blending ratios shown in the table above, and pure water was used as the medium in the blending ratios shown in the table above. Special polyvinyl alcohol PVA JMR-10M manufactured by Nippon Vinyl Acetate & Poval Co., Ltd. was added as a binder so that the solid content met the blending ratio shown in the table above. The mixture was dispersed and mixed in a ball mill to prepare a slurry.

[0026] The slurry was dried in a rotary evaporator and compacted using a die with a diameter of 50 mm at a pressure of 1 ton to obtain pellets. The pellets were crushed and sieved through a 200-mesh (74 μm) stainless steel mesh to obtain powder, which was then calcined at 600° C. for 12 hours in an Ar atmosphere to produce a debindered solid powder as precursor particles.

[0027] (b) Spheroidization and Classification The precursor particles prepared as described above are composed of a plurality of relatively small copper particles (hereinafter, sometimes referred to as "small copper particles") and a plurality of light-absorbing material particles, which are aggregated or bonded together. The spheroidization process involves heating and melting such precursor particles in a thermal plasma flame to spheroidize them. Schematically, as shown in FIG. 1 , precursor particles 16 are introduced from a supply pipe 14 into a plasma flame 12 generated by a high-frequency induction coil 10, thereby obtaining spheroidized composite copper particles 18. The precursor particles 16 are composed of an aggregate of a plurality of copper particles of 10 μm or less and a plurality of light-absorbing material particles of 0.01 μm to 1 μm. This spheroidization process melts the plurality of copper particles into a single base particle. As a result, the composite copper particles obtained by the spheroidization process are composed of a single base particle dispersed with light-absorbing material particles having a particle size smaller than that of the base particle.

[0028] The spheroidizing treatment may be carried out using, for example, an apparatus such as that described in Japanese Patent No. 3639279. Specifically, the spheroidizing treatment for the composite copper particles of this example was carried out using an apparatus in which a high-temperature plasma generator YPK-70 manufactured by Nippon High Frequency Co., Ltd. was connected to a homemade stainless steel reaction vessel, and a thermal plasma flame was generated in an Ar—H atmosphere using 30 kW of electric power.

[0029] The classification was carried out by a general method using a mesh. As described in Japanese Patent No. 3639279, spheroidization treatment may be carried out while removing fine particles. As a result of classification, composite copper particles having a particle size of 10 μm to 100 μm were produced for all sample numbers.

[0030] Scanning electron microscope photographs (SEM images) of the produced composite copper particles and particle size distributions for sample numbers #22 and #32 are shown in Figure 2. The microscope used was a Hitachi TM400 tabletop microscope, and the particle size distributions were obtained using free software Image J. For all sample numbers, the ratio of the major axis to the minor axis of each composite copper particle was 1 or more and 1.5 or less, and in short, all composite copper particles were approximately spherical.

[0031] [B] Evaluation of Light Absorption i) Light Absorption Rate of Each Constituent Material The composite copper particles of the examples are intended for use in, for example, modeling using a Yb fiber laser 3D printer. In this application, the absorption rate of light at approximately 1.1 μm, which is the wavelength of the laser light from the Yb fiber laser, becomes an issue. The absorption rates of the materials constituting the composite copper particles of the examples are as shown in the table below. The table also lists Inconel 718, a type of nickel alloy, because it has high high-temperature strength and is widely used in 3D printers. Since the absorption rate for 1 μm light is roughly similar to that for 1.1 μm light, the table below lists the absorption rate for 1 μm light.

[0032] ii) Method for measuring the degree of light absorption The degree of light absorption of each composite copper particle was measured using a measuring device shown in Fig. 3. The measuring device includes a stage 22 on which a beaker 20 is placed, a halogen spot heater 24 disposed below the stage 22, a stirrer 26 for stirring the inside of the beaker 20, and a thermometer 28 for measuring the temperature inside the beaker 20. The stage 22 has openings at the top and bottom that are covered with quartz glass 30, and light from the halogen spot heater 24 is irradiated into the beaker 20 through the stage 22. An infrared filter 32 is disposed inside the stage 22, and the infrared filter 32 is cooled by cooling water 34 that flows inside the stage 22.

[0033] A predetermined amount of methanol 36 is placed in the beaker 20, and the methanol 36 is stirred by the stirrer 26. The composite copper particles 38 of the example are allowed to settle to the bottom of the beaker 20. The halogen spot heater 24 is an irradiation device for near-infrared rays (approximately 1 μm), and light with wavelengths of less than 1 μm, at which copper has a high light absorption rate, is cut by the infrared filter 32 and does not reach the beaker 20. Incidentally, the light from the halogen spot heater 24 is focused on the composite copper particles 38 that have settled in the beaker 20.

[0034] Light is irradiated from halogen spot heater 24, and the amount of heat generated by composite copper particles 38 over time is measured by the change in temperature measured by thermometer 28. Methanol 36, cooling water 34, beaker 20 itself, and quartz glass 30 transmit almost all light and can therefore be considered not to contribute to heat generation. It can be considered that the higher the degree to which composite copper particles 38 absorb light, that is, the higher the light absorptivity of the composite copper particles themselves, the greater the heat generated.

[0035] As a result of measuring the degree of light absorption, the calorific value versus time from the start of irradiation with light from the halogen spot heater is shown in a graph in Figure 4 for each composite copper particle of the Examples. For comparison with each composite copper particle of the Examples, the graph also shows the calorific values ​​for comparative particles: a) Sample No. 41: tough pitch copper particles (average particle size 30 μm), and b) Sample No. 42: Inconel 718 particles (average particle size 35 μm).

[0036] As can be seen from the graph, tough pitch copper particles (#41) have the lowest calorific value and the lowest degree of light absorption. In contrast, the composite copper particles (#11-#33) of the examples all have higher calorific values ​​and higher degrees of light absorption than tough pitch copper particles. Specifically, the composite copper particles (#11, #21, #22) containing carbon as the light-absorbing material exhibited higher light absorption levels the higher the carbon content, regardless of the precursor particle preparation method. Similarly, the composite copper particles (#31, #32, #33) containing magnetite as the light-absorbing material exhibited higher light absorption levels the higher the magnetite content. Furthermore, by increasing the carbon / magnetite content to a certain extent, it became possible to achieve a higher degree of light absorption than Inconel 718 particles (#42).

[0037] [C] 3D Printing Among the composite copper particles of the above examples, sample number #32 was used and modeled using an EOS 3D additive manufacturing device (EOS M280). This 3D additive manufacturing device used a Yb fiber laser with a maximum output of 400 W and a laser diameter of approximately 100 μm. As a comparative example, modeling was also performed using tough pitch copper particles of sample number #41. The dimensions of the model were length 100 mm, width 50 mm, and thickness 20 mm. The composite copper particles of sample number #32 were modeled at an output of 200 W, and the tough pitch copper particles of sample number #41 were modeled at an output of 380 W, with both models having a layer pitch of 30 μm. In the following, the body made using the composite copper particles of sample number #32 will be referred to as a magnetite composite copper body, and the body made using the tough pitch copper particles of sample number #41 will be referred to as a tough pitch copper body.

[0038] The hardness (Vickers hardness), electrical conductivity, and thermal conductivity of these molded bodies were measured as their properties, and the measurement results are shown in the table below.

[0039] As can be seen from the above table, the magnetite composite copper shaped body exhibits physical properties in terms of electrical conductivity and thermal conductivity that are approximately equivalent to those of the tough pitch copper shaped body. In other words, by using the composite copper particles of the examples, it is possible to produce a shaped body with physical properties equivalent to those of a shaped body using pure copper particles, even with a low-output Yb fiber laser.

[0040] Furthermore, the magnetite composite copper shaped body is harder than the tough pitch copper shaped body. This is thought to be because the composite magnetite particles are uniformly dispersed in the copper matrix, exhibiting physical properties similar to those of alumina dispersion strengthened copper. Therefore, the magnetite composite copper shaped body is expected to maintain high hardness and high conductivity without softening even at relatively high temperatures.

[0041] 10: High frequency induction coil 12: Plasma flame 14: Supply pipe 16: Precursor particles 18: Composite copper particles 20: Beaker 22: Stand 24: Halogen spot heater 26: Stirrer 28: Thermometer 30: Quartz glass 32: Infrared filter 34: Cooling water 36: Methanol 38: Composite copper particles

Claims

1. Composite copper particles in which particles of a light-absorbing substance with a particle size smaller than the base particles and an absorption rate of 40% or more for light with a wavelength of 1 μm are dispersed in copper base particles.

2. Composite copper particles according to claim 1, wherein the light-absorbing substance is one or more selected from the group consisting of carbon, magnetite, wustite, chromia, and hematite.

3. Composite copper particles according to claim 2, wherein the light-absorbing material is carbon.

4. Composite copper particles according to claim 2, wherein the light-absorbing material is magnetite.

5. Composite copper particles according to any one of claims 1 to 4, wherein the particle diameter of the composite copper particles is 10 μm or more and 100 μm or less.

6. Composite copper particles according to claim 5, wherein the particle diameter of the light-absorbing material particles is 0.01 μm or more and 1 μm or less.

7. Composite copper particles according to any one of claims 1 to 6, wherein the composite copper particles are spherical.

8. Composite copper particles according to any one of claims 1 to 7, wherein the light-absorbing substance is contained in the composite copper particles in an amount of 1 wt% to 10 wt%.

9. A method for producing composite copper particles according to any one of claims 1 to 8, comprising the steps of: preparing precursor particles in which copper particles having a particle size smaller than that of the base particles and particles of the light-absorbing material are aggregated or bonded together; and introducing the precursor particles into a thermal plasma flame, melting the copper particles to produce the base particles, and spheroidizing the composite copper particles.

10. A method for manufacturing a composite copper object using the composite copper particles according to any one of claims 1 to 8, by irradiating Yb fiber laser light using a 3D printer.

Citation Information

Patent Citations

  • Shading correction system

    JP1988009279A

  • Manufacturing method of laminate molded article and laminate molded article

    JP2018070914A