POWER STORAGE DEVICE
A polymer electrolyte layer with cyclic and chain polycarbonates and a high lithium salt concentration, combined with an alloy-forming layer, addresses the issue of short circuits in lithium-ion batteries by promoting uniform lithium deposition, thereby enhancing stability and conductivity.
Patent Information
- Application Number
- DE112023000643
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-01-19
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional lithium-ion batteries with a two-layer solid electrolyte layer are ineffective in preventing short circuits between electrodes due to lithium precipitation, which can lead to localized deposition and increased risk of short circuits.
Incorporating a polymer electrolyte layer containing cyclic polycarbonate and chain polycarbonate with a lithium salt concentration of 3 mol/L or more, along with an alloy-forming layer to facilitate uniform lithium deposition and reduce short circuits.
The solution enhances ionic conductivity and stabilizes lithium deposition, effectively reducing the occurrence of short circuits and enabling stable operation of the battery under repeated charging and discharging conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATION
[0001] This application is based on Japanese Patent Application No. 2022-006478 filed on January 19, 2022, the disclosure of which is incorporated herein by reference. TECHNICAL FIELD
[0002] The present disclosure relates to a chargeable and dischargeable power storage device. BACKGROUND
[0003] As a power storage device, lithium-ion batteries are known to be charged and discharged by the movement of lithium ions between a positive and a negative electrode. In lithium-ion batteries, repeated charging and discharging can cause lithium to precipitate on a surface of the negative electrode, potentially leading to a short circuit between the electrodes. In lithium-ion batteries that use a metallic lithium negative electrode and a solid electrolyte layer, an interface between the negative electrode and the solid electrolyte layer acts as a nucleus for lithium precipitation, and the precipitated lithium grows along the grain boundaries of the solid electrolyte, making them prone to short circuits.
[0004] Patent Literature 1 proposes that in a lithium-ion battery having a solid electrolyte layer, the solid electrolyte layer is divided into two layers to reduce a short circuit between the electrodes. LITERATURE ON THE STATE OF THE ART PATENT LITERATURE
[0005] Patent literature 1: WO 2014 / 010043 A1 SUMMARY OF THE INVENTION
[0006] However, the above-mentioned conventional technology only provides a two-layer solid electrolyte layer in a lithium-ion battery and is less effective in preventing short circuits between the electrodes.
[0007] In view of the above, an object of the present disclosure is to provide a power storage device capable of reducing a short circuit between electrodes.
[0008] A power storage device according to the present disclosure includes a negative electrode, a positive electrode, and a polymer electrolyte layer provided between the negative electrode and the positive electrode. The polymer electrolyte layer exhibits lithium ion conductivity. The polymer electrolyte layer contains cyclic polycarbonate and chain polycarbonate. The polymer electrolyte layer contains lithium salt, and a concentration of the lithium salt in the polymer electrolyte layer is 3 mol / L or more.
[0009] According to the present disclosure, by incorporating the chain polycarbonate into the polymer electrolyte layer, the lithium salt can be effectively concentrated and the ionic conductivity can be improved. As a result, a uniform lithium deposition reaction can take place on the electrode surface, and the occurrence of short circuits can be more effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a cross-sectional view showing a configuration of a power storage device according to the first and second embodiments. Fig. Figure 2 is a table showing non-short-circuit current density of examples and comparative examples. Fig. 3 is a table showing ionic conductivity of examples and comparative examples. Fig. 4 is a cross-sectional view showing a configuration of a power storage device according to a third embodiment. Fig. 5 is a cross-sectional view showing a configuration of a power storage device according to a fourth embodiment. Fig. 6 is a cross-sectional view showing a configuration of a power storage device according to a fifth embodiment. DETAILED DESCRIPTION
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to drawings. In each embodiment, parts corresponding to those described in a previous embodiment may be assigned the same reference numerals, and overlapping explanations may be omitted. While only a part of the configuration is described in each embodiment, the previously described other embodiments may also be applied to other parts of the configuration. The present disclosure is not limited to combinations of embodiments that combine parts that are expressly described as combinable. As long as there are no problems, the various embodiments may be partially combined with each other even if it is not expressly described. First embodiment
[0011] A first embodiment of the present disclosure will be described below with reference to the drawings. A power storage device 100 of the first embodiment is a secondary battery and can store and utilize electrical energy. The power storage device 100 is a lithium-ion battery that is charged and discharged by the movement of lithium ions between a negative electrode 102 and a positive electrode 104.
[0012] As in Fig. 1, the power storage device 100 includes a negative electrode current collector 101, the negative electrode 102, a positive electrode current collector 103, the positive electrode 104, and a solid electrolyte layer 105. Components of the power storage device 100, such as the negative electrode current collector 101, are stacked.
[0013] The negative electrode current collector 101 is connected to the negative electrode 102, and the positive electrode current collector 103 is connected to the positive electrode 104. Any material suitable as a current collector for a lithium-ion battery can be used for the negative electrode current collector 101 and the positive electrode current collector 103. In the present embodiment, copper (Cu) is used as the negative electrode current collector 101, and aluminum (Al) is used as the positive electrode current collector 103.
[0014] A negative electrode material forming the negative electrode 102 can be any material that can be used as a negative electrode active material for lithium-ion batteries, such as a carbon-based negative electrode material, an oxide-based negative electrode material, or a metal-based negative electrode material. In the present embodiment, metallic lithium is used as the negative electrode material.
[0015] A positive electrode material constituting the positive electrode 104 can be any material that can be used as a positive electrode active material for lithium-ion batteries. For example, a cobalt-based positive electrode material (LiCoO2), a nickel-based positive electrode material (LiNiO2), a manganese-based positive electrode material (LiMn2O4), an iron phosphate-based positive electrode material (LiFePO4), a ternary positive electrode material (NMC) composed mainly of nickel, manganese, and cobalt, and the like can be used as the positive electrode 104.
[0016] The solid electrolyte layer 105 is made of a solid electrolyte with lithium ion conductivity. The solid electrolyte layer 105 can be made of any solid electrolyte that can be used as an electrolyte layer in a lithium-ion battery. For example, an oxide-based solid electrolyte or a sulfide-based solid electrolyte can be used as the solid electrolyte. In the present embodiment, LLZO (Li7La3Zr2O 12 ), which is the oxide-based solid electrolyte. The solid electrolyte layer 105 corresponds to a solid electrolyte layer within the meaning of the present disclosure.
[0017] In the power storage device 100, an alloy-forming layer 106 capable of forming a lithium alloy and a polymer electrolyte layer 107 exhibiting lithium ion conductivity are provided on a surface of the solid electrolyte layer 105. The alloy-forming layer 106 and the polymer electrolyte layer 107 are provided as buffer layers to reduce the occurrence of a short circuit in the power storage device 100. The alloy-forming layer 106 and the polymer electrolyte layer 107 of the present embodiment are provided between the negative electrode 102 and the solid electrolyte layer 105, and between the positive electrode 104 and the solid electrolyte layer 105, respectively.
[0018] Since lithium metal is likely to precipitate during charging and discharging on the negative electrode side of a lithium-ion battery, the alloy-forming layer 106 and the polymer electrolyte layer 107 may be formed on at least one negative-electrode-facing surface of the solid electrolyte layer 105. In the present embodiment, the alloy-forming layers 106 and the polymer electrolyte layers 107 are provided on both a negative-electrode-facing surface and a positive-electrode-facing surface of the solid electrolyte layer 105. The alloy-forming layers 106 provided on the negative-electrode side and the polymer electrolyte layers 107 provided on the positive-electrode side have the same configuration as those provided on the negative-electrode side and those provided on the positive-electrode side.
[0019] The alloy-forming layer 106 and the polymer electrolyte layer 107 may have a multilayer structure in which each layer is formed separately, or they may have a mixed structure in which each layer is mixed and formed integrally. The alloy-forming layer 106 may be formed of two or more layers, and the polymer electrolyte layer 107 may be formed of two or more layers when the alloy-forming layer 106 and the polymer electrolyte layer 107 have a multilayer structure. In the present embodiment, the multilayer structure is formed in which one layer each of the alloy-forming layer 106 and the polymer electrolyte layer 107 is formed.
[0020] In the present embodiment, of the alloy-forming layer 106 and the polymer electrolyte layer 107, the alloy-forming layer 106 is close to the solid electrolyte layer 105, and the polymer electrolyte layer 107 is far from the solid electrolyte layer 105.
[0021] The positional relationship between the alloy forming layer 106 and the polymer electrolyte layer 107 is not particularly limited, but in order to exert short-circuit suppression effects of each layer, it is desirable that the alloy forming layer 106 is close to the solid electrolyte layer 105 and the polymer electrolyte layer 107 is far from the solid electrolyte layer 105.
[0022] The alloy-forming layer 106 is a layer capable of forming a lithium alloy and also exhibits lithium ion conductivity. In the alloy-forming layer 106, the lithium alloying reaction interferes with the nucleation of lithium precipitation.
[0023] The alloy-forming layer 106 may be made of M X N 1-X "M" is a metal element, "N" is a nitrogen element, and X ≦ 1.0. In particular, the alloy-forming layer 106 may be made of a metal nitride such as CuN or TiN, or of an elemental metal such as Ag or Au.
[0024] Lithium and the nitrogen contained in the metal nitride form an alloy to form LiN when the metal nitride is used as the alloy-forming layer 106. The simple metal and lithium form an alloy, for example, AgLi, when the simple metal is used as the alloy-forming layer 106. LiN has high ionic conductivity and can easily unify the current density, thus having a high short-circuit suppression effect. Therefore, it is desirable to use a metal nitride as the alloy-forming layer 106.
[0025] The alloy-forming layer 106 can be formed in any desired manner. For example, the alloy-forming layer 106 can be formed on the surface of the solid electrolyte layer 105 by atomic layer deposition (ALD) or by sputtering.
[0026] The thickness of the alloy-forming layer 106 is preferably 600 μm or less. If the thickness of the alloy-forming layer 106 exceeds 600 μm, the movement of lithium ions is hindered, resulting in a decrease in lithium ion conductivity. Furthermore, it is desirable that the thickness of the alloy-forming layer 106 be 200 μm or more. If the thickness of the alloy-forming layer 106 is less than 200 μm, it becomes difficult to form the alloy-forming layer 106 uniformly on the surface of the solid electrolyte layer 105, and durability is reduced.
[0027] The polymer electrolyte layer 107 exhibits lithium ion conductivity and is primarily composed of an ionic liquid made of lithium salt and a chain polyether. The chain polyether is a solvent. The polymer electrolyte layer 107 is also a layer with a low Young's modulus.
[0028] Ionic liquids are liquids at room temperature and are represented by liquid compounds consisting only of ions (anions and cations). Ionic liquids are non-volatile liquids with extremely low vapor pressure and relatively high ionic conductivity.
[0029] The lithium salt contained in the polymer electrolyte layer 107 may be at least one selected from LiN(SO2F)2, LiFSA, LiFSI, LiTFSI, Li((CF2SO2)2N), and LiBF4. By using these lithium salts, the concentration of the lithium salt in the polymer electrolyte layer 107 can be increased.
[0030] The chain polyether contained in the polymer electrolyte layer 107 is a polymer with an ether bond (-COC-) in a main chain. Examples of chain polyethers that can be used are DEME (N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium) or glyme. Examples of glymes that can be used are G3 (tetraglyme) and G4 (triglyme).
[0031] The polymer electrolyte layer 107 can be formed by any method. For example, the polymer electrolyte layer 107 can be formed by applying a mixture of the above-mentioned lithium salt and chain polyether to the surface of the previously formed alloy-forming layer 106.
[0032] By mixing the above-mentioned lithium salt with the chain polyether, a solvated ionic liquid is formed in which the chain polyether, which serves as the solvent, is coordinated with the lithium ions, and a gelled ionic liquid can be obtained. The higher the concentration of the lithium salt in the polymer electrolyte layer 107, the higher the viscosity of the polymer electrolyte layer 107 can be adjusted.
[0033] By using the lithium salt and the chain polyether in the present embodiment, the concentration of the lithium salt in the polymer electrolyte layer 107 can be increased. In the present embodiment, the concentration of the lithium salt in the polymer electrolyte layer 107 is set to 3 M (mol / L) or more. The lithium salt concentration in the electrolyte used in a typical lithium-ion battery is approximately 1 to 1.5 M, while the lithium salt in the polymer electrolyte layer 107 of the present embodiment has a higher concentration.
[0034] In the polymer electrolyte layer 107 of the present embodiment, the lithium salt is highly concentrated, so that the free solvent that is not coordinated with lithium ions can be reduced as much as possible. This can improve the electrochemical stability of the polymer electrolyte layer 107 and can also increase the ion transport number.
[0035] The polymer electrolyte layer 107 can be mixed with a solvent such as sulfolane or an ionic liquid such as [EMI][FSI], [EMI][FTI], [EMI][TFSI], or [BMI][TFSI]. As a result, the lithium salt in the polymer electrolyte layer 107 can have a higher concentration.
[0036] In addition, additives such as a binder or a diluent, e.g., polyvinylidene fluoride (PVDF), may be added to the polymer electrolyte layer 107.
[0037] The results of a short-circuit resistance test performed on the power storage device 100 of the present embodiment will be described using an example and a comparative example shown in Fig. 2 are shown. In Fig. 2, Examples 1A to 1C and Comparative Examples 1A to 1F correspond to the first embodiment. Example 2 corresponds to a second embodiment, which will be described later, and will be described in the second embodiment.
[0038] In Examples 1A to 1C, a power storage device in which an alloy-forming layer 106 and a polymer electrolyte layer 107 are formed is used. In Comparative Examples 1A to 1F, a power storage device in which at least one of the alloy-forming layer 106 and the polymer electrolyte layer 107 is not formed is used. In the power storage devices of Examples 1A to 1C and Comparative Examples 1A to 1F, metallic lithium is used as the negative electrode 102 and LLZO is used as the solid electrolyte layer 105. The thickness of the solid electrolyte layer 105 is 900 μm.
[0039] In Examples 1A and 1B, the alloy-forming layer 106 is formed by sputtering Ag to a thickness of 600 µm. In Example 1C, the alloy-forming layer 106 is formed by ALD with TiNx to a thickness of 100 µm. In Examples 1A to 1C, LiFSI (lithium salt) and G4 (chain polyether) are mixed and gelled for use as the polymer electrolyte layer 107. In Examples 1A and 1C, the lithium salt concentration in the polymer electrolyte layer 107 is set to 4.5 M, and in Example 1B, the lithium salt concentration is set to 7.0 M.
[0040] In Comparative Example 1A, a power storage device in which neither the alloy-forming layer 106 nor the polymer electrolyte layer 107 is formed is used.
[0041] Comparative Examples 1B to 1E use power storage devices in which the alloy-forming layer 106 is formed and the polymer electrolyte layer 107 is not formed. In Comparative Example 1B, AlOx is formed as the alloy-forming layer 106 with a thickness of 100 µm by ALD. In Comparative Example 1C, the alloy-forming layer 106 is formed by sputtering Ag with a thickness of 600 µm. In Example 1D, the alloy-forming layer 106 is formed by ALD with TiNx with a thickness of 100 µm. In Comparative Example 1E, CuNx is formed as the alloy-forming layer 106 with a thickness of 300 µm by ALD.
[0042] Comparative Example 1F uses a power storage device in which no alloy-forming layer 106 is formed and the polymer electrolyte layer 107 is formed. In Comparative Example 1F, a polymer electrolyte gelled by mixing LiFSI (lithium salt) and G4 (chain polyether) is used as the polymer electrolyte layer 107. In Comparative Example 1F, the lithium salt concentration in the polymer electrolyte layer 107 is set to 1.0 M.
[0043] In the short-circuit resistance test, an HS cell (sealed bipolar cell) manufactured by Hohsen Corporation is used, and the power storage devices of Examples and Comparative Examples are assembled under a load of 5 kgf. Before the short-circuit resistance test, alternating current is applied to the devices of Examples and Comparative Examples while heating them to 60 degrees Celsius to ensure interfacial stability.
[0044] In the short-circuit resistance test, the power storage devices of the examples and comparative examples are charged three times at an arbitrary current density for 30 minutes and then discharged. The current density is adjusted in the order of 0.02 mA / cm 2 , 0.2 mA / cm 2 , 0.5 mA / cm 2 , 1.0 mA / cm 2 , 1.5 mA / cm 2 , 2.0 mA / cm 2 increased until a short circuit occurs. An upper limit of the current density at which no short circuit occurs is determined as the non-short-circuit current density.
[0045] As in Fig. 2, the non-short-circuit current density in Comparative Examples 1A to 1F is 0.2 to 1.0 mA / cm 2 . In the power storage devices of Comparative Examples 1A to 1F, the current density fluctuated, and it is believed that repeated charging and discharging causes local deposition of lithium, resulting in a decrease in the non-short-circuit current density.
[0046] As in Fig. 2, the high non-short-circuit current density in Examples 1A to 1C is 2.0 to 3.0 mA / cm 2 . In the power storage devices of Examples 1A to 1C in which the alloy-forming layer 106 and the polymer electrolyte layer 107 are formed, a high short-circuit suppression effect is achieved.
[0047] In the power storage devices of Examples 1A to 1C, nucleation of lithium precipitation is prevented by the lithium alloying reaction in the alloying layer 106, and the current density is made uniform by the polymer electrolyte layer 107, which has high ionic conductivity. As a result, a uniform lithium deposition reaction is enabled during charging and discharging of the power storage device, reducing the occurrence of a local lithium deposition reaction and increasing the effectiveness of the short-circuit suppression effect.
[0048] It is assumed that the metal nitride or elemental metal constituting the alloy-forming layer 106 diffuses to the lithium metal side forming the electrode during charging and discharging, forming a mixed ion / electron conduction interface with lithium ion conductivity and electronic conductivity on the lithium metal surface. It is assumed that the lithium deposition reaction occurs uniformly, which improves the short-circuit suppression effect.
[0049] It is also assumed that in the alloy-forming layer 106, lithium ions are guided in a direction along the electrode surface due to the lithium alloy, and the lithium ions move evenly toward the electrode in the polymer electrolyte layer 107, which has a high ion transport number. Therefore, it is assumed that the lithium deposition reaction occurs evenly, which improves the short-circuit suppression effect.
[0050] In the above-described embodiment, the alloy-forming layer 106, which can form a lithium alloy, and the polymer electrolyte layer 107, which has lithium ion conductivity, are provided on the surface of the solid electrolyte layer 105. As a result, the uniform lithium deposition reaction can take place on the electrode surface, and the occurrence of localized lithium deposition reactions can be reduced, thereby reducing the occurrence of short circuits.
[0051] Furthermore, the power storage device 100 of the present embodiment is configured using the negative electrode 102 made of lithium metal and the solid electrolyte layer 105, and is prone to short circuits. Therefore, by forming the alloy-forming layer 106 and the polymer electrolyte layer 107 on the surface of the solid electrolyte layer 105, the short-circuit suppression effect can be more effectively achieved.
[0052] In addition, the volume of the alloy-forming layer 106 fluctuates due to alloying reactions during charging and discharging. Since the polymer electrolyte layer 107 of the present embodiment is a low Young's modulus layer, the polymer electrolyte layer 107 is capable of absorbing the volume fluctuations of the alloy-forming layer 106. As a result, the power storage device 100 can be used stably and continuously even when the power storage device is repeatedly charged and discharged.
[0053] In the present embodiment, the polymer electrolyte layer 107 uses a polymer electrolyte with a lithium salt concentration of 3 M or more. This can improve the electrochemical stability and the ion transport number.
[0054] Furthermore, since the polymer electrolyte layer 107 in the power storage device 100 of the present embodiment is in a gel state, the polymer electrolyte layer 107 is less likely to volatilize. Therefore, the power storage device 100 of the present embodiment can be used in applications with large air pressure fluctuations, such as eVTOLs (electric vertical takeoff and landing aircraft) and submarines. Second embodiment
[0055] Next, a second embodiment of the present disclosure will be described. Only portions different from the first embodiment will be described below.
[0056] A power storage device 100 of the second embodiment has a similar configuration to that described above with reference to Fig. 1 and includes a negative electrode current collector 101, a negative electrode 102, a positive electrode current collector 103, a positive electrode 104, a solid electrolyte layer 105, an alloy-forming layer 106, and a polymer electrolyte layer 107. In the second embodiment, the solvent of a polymer electrolyte constituting the polymer electrolyte layer 107 is different from that in the first embodiment. In the second embodiment, a chain polycarbonate and a cyclic polycarbonate are used as the solvent for the polymer electrolyte. The lithium salt of the polymer electrolyte can be the same as in the first embodiment.
[0057] The chain polycarbonate and the cyclic polycarbonate are the main components of the polymer electrolyte and account for 50 wt% or more of the polymer electrolyte. The polymer electrolyte may contain at least one chain polycarbonate. The polymer electrolyte may contain additives such as a binder and a diluent.
[0058] Chain polycarbonate and cyclic polycarbonate can be prepared by polymerizing cyclic monomers with a dielectric constant of 80 or more. Cyclic monomers with a relative dielectric constant of 80 or more tend to open the ring during polymerization and produce chain polymers.
[0059] In the second embodiment, vinylene carbonate (VC) is used as the cyclic monomer, which has a relative dielectric constant of 80 or more. Therefore, the chain polycarbonate and the cyclic polycarbonate are obtained as vinylene carbonate-derived polymers. The polymer electrolyte of the second embodiment contains polycarbonate produced by polymerizing vinylene carbonate and decomposition products produced from unpolymerized vinylene carbonate. Hereinafter, the vinylene carbonate-derived polymer is also referred to as the "VC polymer."
[0060] The polymer electrolyte of the second embodiment can be obtained by adding a polymerization initiator to a mixture of a lithium salt and vinylene carbonate, followed by heating or irradiating the mixture with ultraviolet light. The polymerization initiator can be any solvent-soluble polymer, and the polymerization initiator used can include azobisisobutyronitrile (AIBN), benzoyl peroxide (BPO), and cumene hydroperoxide. The polymerization initiator can be added in an amount of about 1 mg per 1 ml of vinylene carbonate.
[0061] During the polymerization of vinylene carbonate, a ring-opening reaction occurs, resulting in the production of chain polycarbonate. A portion of the vinylene carbonate does not undergo ring opening, resulting in the production of cyclic polycarbonate when vinylene carbonate is polymerized. Therefore, the polymer electrolyte of the second embodiment contains chain polycarbonates and cyclic polycarbonates.
[0062] In the polymer electrolyte of the second embodiment, the chain polycarbonate enhances the electrostatic force with the lithium ions, so that the concentration of the lithium salt can be improved. In the second embodiment, the concentration of the lithium salt in the polymer electrolyte layer 107 is set to 3 M (mol / L) or more.
[0063] In addition, high ionic conductivity is obtained in the polymer electrolyte of the second embodiment. In a typical polymer electrolyte, the ionic conductivity in the room temperature range is about 10 -5 S / cm, while in the polymer electrolyte of the second embodiment, the ionic conductivity in the room temperature range is about 10 -3 S / cm.
[0064] In the following, the ionic conductivity of the power storage device 100 of the second embodiment will be described by means of examples and comparative examples shown in Fig. 3. The ionic conductivity in Fig. 3 is a value measured in the room temperature range, and the measured value is given in logarithm.
[0065] In Examples 2A to 2C, the polymer electrolyte is prepared using LiFSI as the lithium salt and VC polymer as the solvent. In Comparative Example 2A, LiClO4 is used as the lithium salt and polyethylene oxide (PEO) as the solvent to obtain a polymer electrolyte. In Comparative Example 2B, LiN(CF3CO2)2 is used as the lithium salt and ethylene oxide (CH2CH2O) is used. n used as a solvent to obtain a polymer electrolyte.
[0066] In Example 2A, the lithium salt concentration is 3 M, in Example 2B, the lithium salt concentration is 7 M, and in Example 2C, the lithium salt concentration is 10 M. In Comparative Examples 2A and 2B, the lithium salt concentration is 1 M. In Examples 2A to 2C, higher lithium salt concentrations are obtained than in Comparative Examples 2A and 2B.
[0067] As in Fig. 3, the ionic conductivity of Comparative Example 2A is -5.2, and the ionic conductivity of Comparative Example 2B is -5.0. In contrast, the ionic conductivity of Example 2A is -4.0, the ionic conductivity of Example 2B is -3.5, and the ionic conductivity of Example 2C is -3.2. The power storage devices of Examples 2A to 2C have significantly improved ionic conductivity compared to the power storage devices of Comparative Examples 2A and 2B. Furthermore, in the power storage devices 100 of Examples 2A to 2C, the higher the lithium salt concentration, the higher the ionic conductivity is achieved.
[0068] Next, the results of a short-circuit resistance test performed on the power storage device 100 of the second embodiment will be described with reference to Example 2 in Fig. 2. The short-circuit resistance test of Example 2 is the same as the short-circuit resistance test described in the first embodiment with reference to Fig. 2 was described.
[0069] In Example 2, the alloy-forming layer 106 is formed by sputtering Ag to a thickness of 300 µm. In Example 2, a mixed solution of LiFSI (lithium salt), vinylene carbonate (solvent), and azobisisobutyronitrile (polymerization initiator) is heated to 60 degrees Celsius to polymerize, thereby obtaining a polymer electrolyte. In Example 2, the lithium salt concentration of the polymer electrolyte is set to 5.0 M. In Example 2, the non-short-circuit current density is 5.0 mA / cm 2 , which is a higher value than in Examples 1A to 1C of the first embodiment.
[0070] In the second embodiment described above, the polymer electrolyte layer 107 contains the chain polycarbonate and the cyclic polycarbonate, and the concentration of the lithium salt in the polymer electrolyte layer 107 is set to 3 M or more. By including the chain polycarbonate in the polymer electrolyte layer 107, the lithium salt can be effectively concentrated and the ionic conductivity can be improved. As a result, a uniform lithium deposition reaction can take place on the electrode surface, and the occurrence of short circuits can be more effectively reduced. Third embodiment
[0071] Next, a third embodiment of the present disclosure will be described. Only portions different from the above embodiments will be described below.
[0072] As in Fig. 4, a power storage device 100 of the third embodiment includes a negative electrode current collector 101, a negative electrode 102, a positive electrode current collector 103, a positive electrode 104, a polymer electrolyte layer 107, and a separator 108. In the power storage device 100 of the third embodiment, a solid electrolyte layer 105 and an alloying layer 106 are not provided.
[0073] The separator 108 has a porous structure and functions to separate the negative electrode 102 and the positive electrode 104 and to allow ions to pass through. The separator 108 can be made of, for example, polypropylene, polyethylene, nonwoven fabric, or the like.
[0074] In the third embodiment, similar to the second embodiment, a chain polycarbonate and a cyclic polycarbonate are used as the main components for the polymer electrolyte layer 107. More specifically, a VC polymer derived from vinylene carbonate is used.
[0075] In Fig. In Figure 4, the separator 108 and the polymer electrolyte layer 107 are shown separately for simplicity, but in reality, the separator 108 and the polymer electrolyte layer 107 are provided integrally. Specifically, the polymer electrolyte layer 107 is provided by impregnating it into the pores of the separator 108.
[0076] In the power storage device 100 according to the third embodiment described above, a uniform lithium deposition reaction can take place on the electrode surface, and the occurrence of short circuits can be more effectively reduced.
[0077] Moreover, in the third embodiment, the polymer electrolyte layer 107 is provided by impregnating the pores of the separator 108, but this is not limitative, and the polymer electrolyte layer 107 may also be provided by applying the polymer electrolyte layer 107 to the electrode surface. Fourth embodiment
[0078] Next, a fourth embodiment of the present disclosure will be described. Only portions different from the above embodiments will be described below.
[0079] As in Fig. 5, a power storage device 100 of the fourth embodiment includes a negative electrode current collector 101, a positive electrode current collector 103, a positive electrode 104, a solid electrolyte layer 105, and a polymer electrolyte layer 107. In the power storage device 100 of the fourth embodiment, a negative electrode 102 and an alloying layer 106 are not provided.
[0080] In the fourth embodiment, similar to the second embodiment, a chain polycarbonate and a cyclic polycarbonate are used as the main components for the polymer electrolyte layer 107. Specifically, a VC polymer derived from vinylene carbonate is used.
[0081] In the fourth embodiment, the polymer electrolyte layer 107 is provided on the negative electrode current collector 101 side of the solid electrolyte layer 105.
[0082] In Fig. In FIG. 5, the solid electrolyte layer 105 and the polymer electrolyte layer 107 are shown separately for simplicity, but in reality, the solid electrolyte layer 105 and the polymer electrolyte layer 107 are provided integrally. The solid electrolyte layer 105 is a porous body, and the polymer electrolyte layer 107 is in a state of penetrating the pores of the solid electrolyte layer 105 on the negative electrode current collector 101 side.
[0083] The power storage device 100 of the fourth embodiment is configured as an anode-less battery in which the negative electrode 102 is not formed on the negative electrode current collector 101 in an initial state. In the anode-less battery, lithium metal is deposited on the negative electrode current collector 101 by lithium ions that migrate from the positive electrode 104 during charging and form the negative electrode 102. During discharge, the lithium metal forming the negative electrode 102 migrates to the positive electrode 104 as lithium ions.
[0084] In the power storage device 100 according to the fourth embodiment described above, a uniform lithium deposition reaction on the electrode surface is possible, and the occurrence of short circuits can be more effectively reduced. Fifth embodiment
[0085] Next, a fifth embodiment of the present disclosure will be described. Only portions different from the above embodiments will be described below.
[0086] As in Fig. 6, a power storage device 100 of the fifth embodiment includes a negative electrode current collector 101, a negative electrode 102, a positive electrode current collector 103, a positive electrode 104, a polymer electrolyte layer 107, and a base membrane 109. The polymer electrolyte layer 107 is provided to cover both surfaces of the base membrane 109.
[0087] In the fifth embodiment, similar to the second embodiment, a chain polycarbonate and a cyclic polycarbonate are used as the main components for the polymer electrolyte layer 107. More specifically, a VC polymer derived from vinylene carbonate is used.
[0088] The base membrane 109 is a foil-like element. The base membrane 109 can be formed using at least one of the materials constituting the solid electrolyte layer 105 and the material constituting the alloy-forming layer 106. The base membrane 109 can be formed by pulverizing the materials constituting the solid electrolyte layer 105 and the alloy-forming layer 106 into a foil-like element.
[0089] In the power storage device 100 according to the fifth embodiment described above, a uniform lithium deposition reaction can take place on the electrode surface, and the occurrence of short circuits can be more effectively reduced.
[0090] The present disclosure is not limited to the above-described embodiments and can be modified in various ways as follows within the scope of protection that does not deviate from the gist of the present disclosure. The means disclosed in the individual embodiments can be combined as appropriate, as long as the combination is feasible.
[0091] Although the present disclosure has been described in accordance with the embodiments, the present disclosure is not limited to the embodiments and structures disclosed therein. The present disclosure is intended to cover various modifications and equivalent arrangements. While the various elements are shown in various combinations and configurations for illustrative purposes, other combinations and configurations, including more, fewer, or only a single element, are also within the spirit and scope of the present disclosure. QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] 2022-006478
[0001] WO 2014 / 010043 A1
[0005]
Claims
[1] Power storage device comprising: a negative electrode (102); a positive electrode (103); and a polymer electrolyte layer (107) provided between the negative electrode and the positive electrode and having lithium ion conductivity, wherein the polymer electrolyte layer contains cyclic polycarbonate and chain polycarbonate, the polymer electrolyte layer contains lithium salt, and a concentration of the lithium salt in the polymer electrolyte layer is 3 mol / L or more. [2] The power storage device according to claim 1, wherein the cyclic polycarbonate and the chain polycarbonate are main components of the polymer electrolyte layer. [3] The power storage device according to claim 1 or 2, wherein the cyclic polycarbonate and the chain polycarbonate are formed of a material having a relative dielectric constant of 80 or more. [4] The power storage device according to claim 1 or 2, wherein the cyclic polycarbonate and the chain polycarbonate are formed from vinylene carbonate. [5] The power storage device according to any one of claims 1 to 4, wherein the lithium salt is at least one selected from the group consisting of LiN(SO2F)2, LiFSA, LiFSI, LiTFSI, Li((CF2SO2)2N) and LiBF4 [6] A power storage device according to any one of claims 1 to 5, further comprising: an electrolyte layer (105) having lithium ion conductivity provided between the positive electrode and the negative electrode; and an alloy-forming layer (106) capable of forming an alloy with lithium, wherein the polymer electrolyte layer and the alloy-forming layer are formed at least on one surface of the electrolyte layer facing the negative electrode. [7] The power storage device according to claim 6, wherein the alloy-forming layer contains a metal nitride. [8] The power storage device according to claim 6 or 7, wherein the alloy-forming layer has a thickness of 600 nm or less. [9] The power storage device according to any one of claims 6 to 8, wherein the solid electrolyte layer is made of solid electrolyte. [10] A power storage device according to any one of claims 1 to 9, wherein the negative electrode contains Li metal.
Citation Information
Patent Citations
All-solid-state battery, and production method therefor
WO2014010043A1
JP2022006478A