COMPOSITE MATERIAL FOR A TRANSFORMER
Patent Information
- Application Number
- DE502017016468
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2017-03-03
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2037-03-03
Description
Technical area
[0001] The present application relates to a composite material, in particular for use in a transformer, a method for producing the composite material according to the invention and a use of such a composite material. Technical background
[0002] In state-of-the-art transformers, grain-oriented electrical steel is installed in the form of laminations. Due to the effect of magnetostriction, these laminations vibrate when an alternating current is applied, resulting in the typical hum of a transformer. Since transformers are often installed in or near residential areas, additional soundproofing measures must be taken to reduce noise pollution. These are very costly.
[0003] Other known means for reducing noise pollution are structure-borne sound-damping composite sheets installed in transformers. For example, US Pat. No. 6,499,209 B1 discloses a transformer made from a multitude of composite sheets. The individual composite sheets consist of two outer magnetic layers and an approximately 25 µm thick viscoelastic film based on a cross-linked acrylic polymer arranged between them.
[0004] While such systems exhibit the required acoustic properties and, due to the correspondingly thick layers, suitable adhesion values, the known systems still lack the magnetic properties required for transformer applications, nor the iron fill factors achievable using these composite sheets in an iron core. Therefore, there is further potential for the development of these composite sheets.
[0005] In addition to the prior art discussed above, EP 0 305 966 A1 discloses a process in which an organic insulating coating is applied to a grain-oriented electrical steel sheet to create an insulating film, which is then baked at 250-350 °C. The organic insulating coating is an acrylic-like coating or a coating made of styrene, polyvinyl, melamine, phenol, silicon, vinyl acetate, epoxy, or similar. The organic coating is intended to improve the punching properties of the grain-oriented electrical steel sheet.
[0006] Furthermore, WO 2009 / 101129 A2 discloses a process for producing a grain-oriented electrical steel coated with a phosphate layer. A phosphate solution containing a colloidal component and at least one colloid stabilizer is applied to the electrical steel. Lamellas are punched from the thus coated electrical steel, each comprising a single layer of electrical steel and any layers applied thereto. Summary of the invention
[0007] The invention is based on the object of providing a composite material which is improved compared to the prior art, in particular to provide a composite material for use in a transformer which has improved properties compared to a monolithic electrical steel strip.
[0008] This problem is solved by a composite material having the features of patent claim 1.
[0009] Advantageous embodiments and variants of the invention emerge from the dependent claims and the following description.
[0010] According to the invention, the composite material, in particular for use in a transformer, comprises a first and a second grain-oriented electrical steel layer and a polymeric layer arranged therebetween, wherein the polymeric layer consists of a crosslinked high-molecular-weight acrylate-based copolymer and has a layer thickness in the range of 3 to 10 µm, wherein the crosslinked high-molecular-weight acrylate-based copolymer is composed of a copolymerized mixture of at least one alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, both of which have an alkyl group having 1 to 12 carbon atoms, a glycidyl monomer unit, an unsaturated carboxylic acid monomer unit, and a crosslinker, and the copolymerized mixture has an average molar mass of 500 kDa to 1500 kDa.
[0011] Surprisingly, it has been found that the composite material according to the invention, in comparison to composite materials known from the prior art, has defined soft magnetic properties which are in the range of monolithic electrical steel sheets.
[0012] Preferably, the composite material has a loss at P1.7; 50 Hz in the range of 0.60 to 1.0 W / kg, more preferably 0.60 to 0.90 W / kg, most preferably 0.60 to 0.8 W / kg and / or a field strength at J800 in the range of 1.88 to 1.96 T, more preferably 1.90 to 1.96 T, determined according to DIN EN 60404-2.
[0013] Furthermore, it has surprisingly been shown that the composite material according to the invention has a comparable iron fill factor in the later application area of transformers as in the current state of the art and thus shows no loss of performance.
[0014] Preferably, the iron fill factor in a transformer using the composite material according to the invention is 96.0 to 99.0%, more preferably 98.0 to 99.0%, even more preferably 98.3 to 99.0%.
[0015] By using the composite material according to the invention, not only can the structure-borne noise generated in the transformer be significantly reduced, but increased efficiency can also be generated, for example, by varying the thickness of the electrical steel sheet used.
[0016] Because the polymer layer is made of a cross-linked, high-molecular-weight acrylate-based copolymer, vibrations and / or oscillations can be absorbed more effectively and converted into thermal energy. This significantly reduces structure-borne sound, significantly reducing or even completely eliminating the need for secondary acoustic measures.
[0017] The core losses of electrical steel sheets depend heavily on the thickness of the sheets used. As a general rule, the smaller the thickness of the electrical steel sheet, the lower the loss. By using the composite sheet according to the invention, two electrical steel sheets of correspondingly better quality with a thickness of 0.20 mm can be bonded together – compared to an electrical steel sheet with a thickness of, for example, 0.40 mm. For a particular transformer type, this can either significantly increase the efficiency of the transformer or enable the construction of a smaller transformer with the same efficiency.
[0018] In practice, the composite materials themselves and the components produced from them occasionally come into contact with various, sometimes very aggressive, oils that can attack the polymer layer and thus lead to delamination. It is therefore desirable for the polymer layer to be resistant to such technical oils. It has been shown that when the crosslinked, high-molecular-weight acrylate-based copolymer is composed of a copolymerized mixture of at least one alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, both of which contain an alkyl group with 1 to 12 carbon atoms, a glycidyl monomer unit, an unsaturated carboxylic acid monomer unit, and a crosslinker, no swelling of the polymer layer or delamination of the composite is detectable.
[0019] In a more preferred embodiment, the crosslinked high molecular weight acrylate-based copolymer consists exclusively of the two components, the copolymerized mixture and the crosslinker.
[0020] According to the invention, the copolymerized mixture consists of at least one alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, both of which have an alkyl group having 1 to 12 carbon atoms, a glycidyl monomer unit and an unsaturated carboxylic acid monomer unit.
[0021] Preferably, the glycidyl monomer unit is selected from the group consisting of allyl glycidyl ether, glycidyl acrylate ester, glycidyl methacrylate ester and / or mixtures thereof.
[0022] Preferably, the alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit has an alkyl group having 4 to 12 carbon atoms.
[0023] If the polymeric layer has a glass transition temperature of higher than -15 °C, according to a preferred embodiment, an alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit having an alkyl group with 1 to 4 carbon atoms can be added to the mixture to be copolymerized.
[0024] According to a preferred embodiment, the crosslinked high molecular weight acrylate-based copolymer is composed of a copolymerized mixture of at least 55 to 85 wt% of an alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, both having an alkyl group with 4 to 12 carbon atoms, 0 to 35 wt% of an alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, both having an alkyl group with 1 to 4 carbon atoms, 0.01 to 2 wt% of a glycidyl monomer unit, 1 to 15 wt%, more preferably 3 to 13 wt% of an unsaturated carboxylic acid monomer unit, and 0.05 to 1 wt% of a crosslinker.
[0025] The copolymerized mixture has an average molar mass in the range of 500 to 1500 kDa, more preferably 600 to 1000 kDa, even more preferably 700 to 900 kDa, and most preferably 800 kDa ± 20 kDa. The average molar mass is determined by GPC. A polystyrene standard was used for calibration.
[0026] Preferably, the alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit having an alkyl group with 4 to 12 carbon atoms is selected from 2-ethylhexyl acrylate, isooctyl acrylate, butyl acrylate, 2-methylbutyl acrylate, 4-methyl-2-pentyl acrylate, isodecyl methacrylate, methyl acrylate, ethyl acrylate, methyl methacrylate and / or a mixture thereof.
[0027] The unsaturated carboxylic acid monomer unit is preferably selected from acrylic acid, methacrylic acid, fumaric acid, and / or a mixture thereof. Preferred mixtures consist of acrylic acid and methacrylic acid, acrylic acid and fumaric acid, or methacrylic acid and fumaric acid.
[0028] According to a preferred embodiment, the copolymerization is carried out using a solvent mixture, preferably a mixture of ethyl acetate and acetone. The solvent mixture preferably has a ratio that allows reflux in the range of 68 to 78°C.
[0029] Preferably, the solids content during copolymerization is in the range of 40 to 60 wt.%.
[0030] AIBN is preferably used as a radical initiator for copolymerization.
[0031] Furthermore, the copolymerization is preferably carried out under a nitrogen atmosphere so that a high molecular weight copolymer, preferably with an average molecular weight of ≥ 500 kDa, is obtained.
[0032] Preferably, the crosslinker is selected from aluminum acetylacetonate (AIACA), iron acetylacetonate (FeACA), titanium acetylacetonate (TiACA) or zirconium acetylacetonate (ZrACA).
[0033] According to a further preferred embodiment, the electrical steel layer has a layer thickness in the range of 50 to 1500 µm, more preferably in the range of 100 to 500 µm, even more preferably in the range of 150 to 350 µm and most preferably in the range of 180 to 270 µm.
[0034] To produce the composite material according to the invention, two electrical steel layers of equal or different thicknesses can be used.
[0035] According to another preferred embodiment, the grain-oriented electrical steel layer has one or preferably 2 to 5, more preferably 2 to 3 surface layers, each with a layer thickness in the range of 0.3 to 5 µm, more preferably 1 to 2.5 µm. The surface layer exerts a tensile stress on the iron silicate portion of the grain-oriented electrical steel layer, so that the difference between the magnetic loss of the individual sheets and the finished transformer (so-called construction factor) is minimized.
[0036] Each layer may consist of a silicate, preferably a magnesium silicate, alternatively a phosphate compound, preferably a phosphosilicate compound.
[0037] According to another preferred embodiment, the polymeric layer has a layer thickness in the range of 4 to 8 µm, more preferably in the range of 4.5 to 7.5 µm.
[0038] According to a further aspect, the present invention relates to a process for the continuous production of a composite material comprising the process steps: Providing a first grain-oriented electrical steel layer, coating the first grain-oriented electrical steel layer with a polymeric agent consisting of a high-molecular acrylate-based copolymer and a crosslinker, heating the coated first grain-oriented electrical steel layer, providing and heating a second grain-oriented electrical steel layer, laminating the two grain-oriented electrical steel layers to obtain a composite material having a polymeric layer consisting of a crosslinked high-molecular acrylate-based copolymer with a layer thickness in the range of 3 to 10 µm.
[0039] Preferably, the first grain-oriented electrical steel layer as well as the second grain-oriented electrical steel layer are provided as a coil, so that a continuous process for producing the composite material according to the invention can be realized.
[0040] Preferably, the first grain-oriented electrical steel layer is coated using a coater. This applies a homogeneous layer of the polymeric agent to the first grain-oriented electrical steel layer. The application is carried out such that, after the lamination step, the composite material has a polymeric layer with a layer thickness in the range of 3 to 10 µm, preferably 4 to 8 µm, more preferably in the range of 4 to 8 µm, and most preferably in the range of 4.5 to 7.5 µm.
[0041] According to another preferred embodiment, a pretreatment of the first electrical steel layer takes place between the step of providing the first electrical steel layer and the application of the polymer layer. Preferably, the pretreatment is a cleaning step. This removes any adhering dirt particles and oils from the surface of the electrical steel layer, thus preparing it for application of the polymeric agent.
[0042] In a preferred embodiment, the high molecular weight acrylate-based copolymer is formed from a copolymerized mixture of at least one alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, both of which have an alkyl group having 1 to 12 carbon atoms, a glycidyl monomer unit, and an unsaturated carboxylic acid monomer unit.
[0043] The electrical steel layers are preferably heated to a temperature in the range of 150 to 250°C, more preferably in the range of 160 to 190°C, and even more preferably in the range of 175 to 185°C. The electrical steel layers can be heated using conventional furnaces or by induction. Corresponding techniques are known to those skilled in the art.
[0044] The lamination of the two tempered electrical steel layers is preferably carried out using a duplicating station. Here, the first electrical steel layer, to which the polymeric agent has been applied, is combined with the second electrical steel layer to form the composite material according to the invention.
[0045] The still hot composite material usually passes through a cooling section, where it cools down to room temperature and is then wound into a coil.
[0046] According to a particularly preferred embodiment, in a next process step, a thermally activatable adhesive is applied to one, more preferably both, sides of the composite material by means of a coil coating process.
[0047] According to a further aspect, the present invention relates to a composite material produced by the method according to the invention.
[0048] Preferably, a composite material produced in this way has, in comparison to composite materials known from the prior art, soft magnetic properties which are in the range of monolithic grain-oriented electrical steel sheets.
[0049] Preferably, the composite material has a loss at P1.7; 50 Hz in the range of 0.60 to 1.0 W / kg, more preferably 0.60 to 0.90 W / kg, most preferably 0.60 to 0.8 W / kg and / or a field strength at J800 in the range of 1.88 to 1.96 T, more preferably 1.90 to 1.96 T, determined according to DIN EN 60404-2.
[0050] In a further aspect, the present invention relates to an iron core containing a plurality of lamellae of the composite material according to the invention.
[0051] In a further aspect, the present invention relates to a transformer comprising an iron core according to the invention.
[0052] A further aspect of the present invention further relates to a method for producing an iron core comprising the steps: Providing a composite material according to the invention, separating a plurality of lamellae from the composite material, and connecting the lamellae to form an iron core.
[0053] The slats can be separated from the composite material, which is preferably in coil form, using a suitable punching or cutting tool, for example. The separated slats are then stacked into a package and joined together.
[0054] The fact that a composite material, preferably in the form of a coil, is already provided results in a process advantage during separation compared to the production of the iron core using a monolithic electrical steel sheet, since only half the separation steps are required to provide an iron core with the same number of laminations.
[0055] The slats are preferably joined by means of punched stacking, which creates a mechanical connection between the individual slats. This connection is formed by raised portions that are punched into the individual slats.
[0056] According to a more preferred embodiment, the individual slats are glued together. Preferably, a thermally activated adhesive is used for bonding. This can be activated before, during, or after stacking the slats. Thus, the thermally activated adhesive can be activated throughout the various process steps and thus brought into a sticky state, ensuring temporal and / or spatial separation.
[0057] Alternatively, a so-called baking varnish or a point-like adhesive connection can be used to glue the slats together.
[0058] In a further aspect, the present invention relates to the use of the composite material according to the invention for producing an iron core for a transformer.
[0059] The invention is explained in more detail below using examples. Examples
[0060] Various polymeric agents have been produced: Solution 1:
[0061] For this purpose, a monomer solution was prepared from 207 g of butyl acrylate, 61.2 g of 2-ethylhexyl acrylate, 23.1 g of acrylic acid, and 0.1 g of 2,3-epoxypropyl methacrylate. 68.5 g of the monomer solution was then taken and fed into a 1.5-liter reactor purged with nitrogen. The reactor was equipped with a stirrer, a reflux condenser, and a thermistor. 29.7 g of ethyl acetate and 18 g of acetone were then added to the monomer solution. The solution was heated to reflux. 0.05 g of AIBN (Dupont) was then dissolved in 4.5 g of ethyl acetate and added to the refluxing solution. The solution was then kept under vigorous reflux for 15 minutes. The remaining monomer solution was mixed with 195 g of ethyl acetate, 40 g of acetone and 0.24 g of AIBN and added as a solution to the solution boiling under reflux in the reactor constantly over 3 hours.After the addition was complete, the solution was refluxed for an additional hour. A solution of 0.12 g of AIBN, 9 g of ethyl acetate, and 4 g of acetone was then added to the reactor, and the solution was refluxed for another hour. This process was repeated two more times. After the addition was complete, the solution was refluxed for another hour. 178 g of toluene and 27 g of n-heptane were then added. The crude product obtained had a solids content of 36 wt.% and a viscosity of 8000 Pa s. The viscosity was determined using a Brookfield viscometer (#4 spindle, 12 rpm). The resulting copolymer consisted of 71 wt.% butyl acrylate, 21 wt.% 2-ethylhexyl acrylate, 8 wt.% acrylic acid, and 0.03 wt.% 2,3-epoxypropyl methacrylate. The copolymer was then mixed with 0.1 wt% aluminum acetylacetonate to obtain the polymeric agent. Solution 2:
[0062] For this purpose, a monomer solution was prepared from 30 g of butyl methacrylate, 150 g of butyl acrylate, 27 g of ethyl methacrylate, 55 g of 2-ethylhexyl acrylate, 18.7 g of methacrylic acid, and 0.1 g of 2,3-epoxypropyl acrylate. 75.5 g of the monomer solution was then taken and fed into a 1.5-liter reactor purged with nitrogen. The reactor was equipped with a stirrer, a reflux condenser, and a thermistor. 32 g of ethyl acetate and 20 g of acetone were then added to the monomer solution. The solution was heated to reflux. 0.05 g of AIBN (Dupont) was then dissolved in 4.5 g of ethyl acetate and added to the refluxing solution. The solution was then kept under vigorous reflux for 15 minutes. The remaining monomer solution was mixed with 195 g of ethyl acetate, 40 g of acetone and 0.24 g of AIBN and added as a solution to the solution boiling under reflux in the reactor constantly over 3 hours.After the addition was complete, the solution was refluxed for an additional hour. A solution of 0.12 g of AIBN, 9 g of ethyl acetate, and 4 g of acetone was then added to the reactor, and the solution was refluxed for another hour. This process was repeated two more times. After the addition was complete, the solution was refluxed for another hour. 183 g of toluene and 27 g of n-heptane were then added. The crude product obtained had a solids content of 38 wt% and a viscosity of 7500 Pa.s. The viscosity was determined using a Brookfield viscometer (#4 spindle, 12 rpm). The resulting copolymer consisted of 10 wt% butyl methacrylate, 53 wt% butyl acrylate, 10 wt% ethyl methacrylate, 20 wt% 2-ethylhexyl acrylate, 6.5 wt% methacrylate, and 0.03 wt% 2,3-epoxypropyl acrylate. The copolymer was then blended with 0.1 wt% aluminum acetylacetonate to obtain the polymeric agent. Solution 3 (Reference):
[0063] A viscoelastic vibration damping material ISD 110 from 3M was used as a reference. Application was carried out according to the data sheet using a 1 and 2 mil film, corresponding to a minimum thickness of 25 and 50 µm, respectively. The adhesive was supplied in 25 and 50 µm thicknesses with a paper liner and contained no solvents. Upon heating, 5 to 30 µg / cm² of volatile substances (hydrocarbons, organic esters, esters, alcohols, acrylates, acetates, etc.) were released. Application was carried out according to the data sheet. Air inclusions were avoided. Solution 4 (Reference):
[0064] A general-purpose adhesive from UHU® was also used. This was a colorless, crystal-clear gel with a gel-like, thixotropic consistency. The formulation had a solids content of 32 wt.% based on a polyvinyl ester with a density of 0.95 g / cm³. A mixture of low-boiling esters and alcohols was used as the solvent. The formulation consisted of 50 to 70 wt.% methyl acetate and 5 to 10 wt.% each of ethanol and acetone. Example 1
[0065] A total of 20 transformer cores were constructed. In all examples shown in Table 1, a composite material was manufactured using two grain-oriented electrical steel grades, 23HP85D (nominal thickness 230 µm) and 27HP85D (nominal thickness 270 µm), and the respective polymeric agent.
[0066] For solutions 1, 2, and 4, grain-oriented electrical steel strips were coated with the adhesive system in the specified layer thicknesses using a coater. For solution 3, the correspondingly thick, solid adhesive layer was applied to the grain-oriented electrical steel strips using a roller to ensure that there were no bubbles. The material was then pre-dried for 1 minute at 110 °C to remove the solvent. For the lamination process with solutions 1 to 4 according to Table 1, the corresponding electrical steel strips were then heated to approximately 180 °C in a continuous oven (oven time approximately 50 s). Immediately after reaching the PMT (peak metal temperature), they were laminated under pressure in a roller mill with grain-oriented electrical steel sheets that had also been heated to 180 °C. For solution 3, a layer thickness of approximately 50 µm was achieved by laminating two coated grain-oriented electrical steel strips together.
[0067] State-of-the-art transformers with three legs were constructed from 0.8 t (for the 230 µm thick sheets) or 48 t (for the 270 µm thick sheets) of the composite material and characterized for noise performance according to EN60076-10.
[0068] The durability of the polymer layer was also investigated. For this purpose, appropriately cut test specimens (2.5 x 10 cm) from the resulting composite materials were placed in a suitable test fluid (Shell ATF 134 FE gear oil; Nynas Nytro Taurus (IEC 60296) Ed. 4 - Standard Grade) for 164 hours at 120 °C. After the exposure time, the test specimens were visually inspected. Neither delamination nor swelling of the polymer layer could be detected. Short description of the drawings
[0069] The invention is explained in more detail below with reference to the drawings. In detail: Fig. 1 shows a first embodiment of the composite material according to the invention, Fig. 2 shows a second embodiment of the composite material according to the invention, Fig. 3 shows a multi-layer structure using the composite material according to the second embodiment, and Fig. 4 shows a process diagram for producing the composite material according to the invention. Description of the preferred embodiments
[0070] In Fig. 1 A three-layer structure of a composite material 1 according to the invention is shown according to a first embodiment. The composite material 1 comprises a first electrical steel layer 2, a second electrical steel layer 4, and a polymer layer 3 arranged therebetween.
[0071] Fig. 2shows a second embodiment of the composite material 5 according to the invention with a first and second electrical steel layer 2, 4 and a polymer layer 3 arranged therebetween. On the side opposite the polymer layer 3, the two electrical steel layers 2, 4 each have an insulation layer 6. According to a preferred embodiment, this is formed by a thermally activatable adhesive.
[0072] In Fig. 3 A multilayer structure 7 using the composite material 5 according to the second embodiment is shown. The individual layers of the composite material 5 are arranged one above the other in a stack. If the insulation layer 6 is formed by a thermally activated adhesive, the multilayer structure 7 has a homogeneous insulation layer 6 between the individual lamellae (not shown).
[0073] Fig. 4shows a process diagram for the continuous production of the composite material 1, 5 according to the invention using a coil coating system 10. The system 10 has a first and a second coil unwinding station 11, 12, with which a first and a second grain-oriented electrical steel layer 2, 4 is provided. Furthermore, the system 10 has a stitching device 13 and a first and a second strip storage device 14, 20, which allow a coil to be changed without having to interrupt the process. The first electrical steel layer 2 is, if necessary, first fed to a pretreatment stage 15 in order to free the surface of the electrical steel layer 2 from adhering dirt particles and oils. Subsequently, the polymeric agent (not shown) is applied to one side via an application roller 16. The electrical steel layer 2 coated with the polymeric agent then passes through a 2-zone oven 17, in which the applied coating is pre-dried at 100-120°C.The solvent is removed during this process. In the second zone of the furnace 17, the electrical steel layer 2 is heated to the PMT (170-190°C). Furthermore, a second electrical steel layer 4 is provided from the second unwinding station 12 and initially fed to a heating station 17, where the second electrical steel layer 4 is also heated to the PMT. In a doubling station 18, the two electrical steel layers 2, 4 are laminated together to form the composite material 1, 5 under a pressure of 5 kN and at a temperature of 150-170°C. The still-hot composite material 1, 5 then passes through a cooling station, where it cools to room temperature and is subsequently wound into a coil on a steel winding station 21. List of reference symbols
[0074] 1Composite material 2First electrical steel layer 3Polymer layer 4Second electrical steel layer 5Composite material 6Insulation layer 7Multi-layer structure 10Strip coating system 11Strip unwinding station 12Strip unwinding station 13Stapling device 14Strip storage 15Pretreatment stage 16Applicator roller 17Heating station 18Duplicating station 19Cooling station 20Strip storage 21Strip winding station
Claims
1. Composite material, comprising - a first and a second grain-oriented electrical steel strip layer, and-a polymer layer arranged therebetween, wherein the polymer layer consists of a cross-linked high-molecular acrylate-based copolymer and has a layer thickness of 3 µm to 10 µm, wherein the cross-linked high-molecular acrylate-based copolymer is composed of - a copolymerized mixture of at least - an alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, wherein both of which have an alkyl group which has 1 to 12 carbon atoms, - a glycidyl monomer unit, - an unsaturated carboxylic acid monomer unit, and - a cross-linking agent and the copolymerized mixture has an average molar mass of 500 kDa to 1500 kDa.
2. Composite material according to any of the preceding claims, characterized in that the grain-oriented electrical steel strip layers each have a layer thickness of 50 µm to 1500 µm.
3. Composite material according to any of the preceding claims, characterized in that the electrical steel strip layers each have an insulation layer having a layer thickness of 0.5 µm to 2 µm.
4. Composite material according to any of the preceding claims, characterized in that its loss P1.7; 50 Hz , determined according to DIN EN 60404-2, is 0.60 W / kg to 1.0 W / kg.
5. Composite material according to any of the preceding claims, characterized in that its field strength J800, determined according to DIN EN 60404-2, is 1.88 T to 1.96 T.
6. Use of a composite material according to any of the preceding claims for producing an iron core for a transformer.
7. Method for the continuous production of a composite material, the method comprising the following method steps: - providing a first grain-oriented electrical steel strip layer, - coating the first electrical steel strip layer with a polymeric agent consisting of a high-molecular acrylate-based copolymer and a cross-linking agent, - heating the coated first grain-oriented electrical steel strip layer, - providing and heating a second grain-oriented electrical steel strip layer, - laminating the two grain-oriented electrical steel strip layers to obtain a composite material having a polymer layer consisting of the cross-linked high-molecular acrylate-based copolymer, which is composed as claimed in claim 1, having a layer thickness of 3 µm to 10 µm.
8. Method according to claim 7, characterized in that the high-molecular acrylate-based copolymer is formed by a copolymerized mixture of at least - an alkyl acrylate ester monomer unit and / or alkyl methacrylate ester monomer unit, wherein both of which have an alkyl group which has 1 to 12 carbon atoms, - a glycidyl monomer unit, and - an unsaturated carboxylic acid monomer unit.
9. Method according to claim 7 or 8, characterized in that the grain-oriented electrical steel strip layers are heated to a temperature of 150 °C to 250 °C.