METHOD FOR PRODUCING A SURFACE-FREE DISPERSION FROM FUNCTIONALIZED SEMICONDUCTOR OR CONDUCTOR MATERIAL
Patent Information
- Application Number
- DE502018015243
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-12-29
- Filing Date
- 2018-12-19
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2038-12-19
AI Technical Summary
Current methods for producing high-quality, surfactant-free dispersions of functionalized semiconductor or conductor materials face challenges such as high defect density, limited scalability, and difficulty in redispersing graphene layers after drying, due to the use of high-boiling solvents and the introduction of oxygen radicals during electrolytic exfoliation.
A method involving electrolytic exfoliation of a two-dimensionally layered carbon-based material in an aqueous or alcoholic electrolyte solution containing sulfuric acid and sulfate salts, with the addition of monomers of electrically conductive polymers or water-soluble vinyl monomers that polymerize at the anode, allowing for in-situ functionalization and dispersion without surfactants.
This method enables the production of stable, high-concentration dispersions of functionalized graphene in various solvents, including water and organic solvents, with reduced defect density and improved processing capabilities, avoiding the need for surfactants and environmentally less favorable solvents like DMF or NMP.
Description
[0001] The invention relates to a process for the production of surfactant-free dispersions of functionalized semiconductor or conductor material by electrolytic exfoliation of a base material and in-situ functionalization of the layers and / or monolayers formed thereby. State of the art
[0002] The isolation of individual layers of two-dimensionally structured or layered semiconductor or conductor materials has been of interest for several years, not least because the use of these materials in electronic components leads to enormous performance improvements and efficient applications.
[0003] An example of such an isolated layer of a two-dimensionally structured or layered material is graphene, which represents a monolayer—a single layer of graphite, a naturally occurring form of pure carbon, only one atom thick. Graphene also refers to materials in which several of these monolayers are arranged one above the other.
[0004] Graphene can be understood as a two-dimensional network of interconnected benzene rings, which, among other things, exhibits enormous electrical conductivity. Due to its electronic, thermal, optical, and mechanical properties, its use is of great interest in many fields of technology. Processes for the scalable and efficient production of high-quality conductive and semiconductor materials, such as graphene, ideally processable from solution, are therefore the subject of intensive research.
[0005] The production of graphene, for example, takes place under sometimes difficult process conditions, as high-boiling solvents such as DMF and NMP are used on a laboratory scale. Scaling up to an industrial scale is therefore extremely problematic and has so far prevented the large-scale production and application of this material.
[0006] A further challenge is the storage of freshly produced graphene, as it is difficult to redisperse after drying and the processability of the material monolayers or oligolayers is extremely difficult.
[0007] One of the most important, but still little-used technologies for producing monolayers or thin films of conductive materials such as graphene is the electrolytic exfoliation of two-dimensional, layered structured base material, such as graphite.
[0008] Exfoliation of graphite to produce graphene, for example in the form of flakes, represents a cost-effective and reliable strategy for its extraction.
[0009] Graphene layers as flakes have already been successfully prepared from graphite as a base material in the solid state (see for example i) KS Novoselov, AK Geim, SV Morozov, D. Jiang, Y. Zhang, SV Dubonos, IV Grigorieva, AA Firsov, Science 2004, 306, 666-669; ii) V. Leon, M. Quintana, MA Herrero, JLG Fierro, A. d. I. Hoz, M. Prato, E. Vazquez, Chem. Commun. 2011, 47, 10936-10938) or in liquid phase (see for example i) ZY Xia, S. Pezzini, E. Treossi, G. Giambastiani, F. Corticelli, V. Morandi, A. Zanelli, V. Bellani, V. Palermo, Adv. Funct. Mater. 2013, 23, 4684-4693; b) A. Ciesielski, P. Samori, Chem. Soc. Rev. 2014, 43, 381-398.) isolated.
[0010] Also by the reduction of graphene oxide, which is prepared, for example, by the so-called Hummers method (WS Hummers et al. J. Am. Chem. Soc. 1958, 80, 6, 1339 ) can be produced, graphene has been successfully produced.
[0011] Graphene oxide is highly dispersible in a wide variety of solvents, especially water, which greatly facilitates its implementation on a larger scale. It is also redispersible after complete drying.
[0012] However, the disadvantage of these reduction methods is that oxide groups and other defects, such as holes or non-six-fold rings, always remain within the material. These structural defects lead to severe limitations in the electronic and thermal properties of graphene produced from graphene oxide (C. Gómez-Navarro, RT Weitz, AM Bittner, M. Scolari, A. Mews, M. Burghard, K. Kern, Nano Lett. 2007, 7, 3499-3503).
[0013] The so-called liquid-phase exfoliation of graphite uses purely physical shear forces in primarily organic solvents and enables the production of graphene with significantly fewer defects (see, for example, a) F. Bonaccorso, A. Bartolotta, JN Coleman, C. Backes, Adv. Mater. 2016, 28, 6136-6166; b) A. Ciesielski, S. Haar, M. EI Gemayel, H. Yang, J. Clough, G. Melinte, M. Gobbi, E. Orgiu, MV Nardi, G. Ligorio, V. Palermo, N. Koch, O. Ersen, C. Casiraghi, P. Samorì, Angew. Chem. Int. Ed. 2014, 53, 10355-10361). However, the disadvantage is that this approach only results in low yields of exfoliated graphene and very small lateral layer sizes (JN Coleman, Acc. Chem. Res. 2013, 46, 14-22).
[0014] In addition, the small material platelets tend to re-aggregate (stack) after exfoliation. The use of surfactants or other additives to prevent this effect is therefore unavoidable. However, these additives are difficult to remove and significantly reduce the product's conductivity.
[0015] Anodic exfoliation has recently emerged as a very promising method to produce high-quality graphene on a large scale, at low cost, and in aqueous solution.
[0016] The two-dimensionally structured base material can be used either as an anode in aqueous solutions of ionic liquids (see, for example, X. Wang, PF Fulvio, GA Baker, GM Veith, RR Unocic, SM Mahurin, M. Chi, S. Dai, Chem. Commun. 2010, 46, 4487-4489) or mineral acids (see, for example, a) KS Rao, J. Sentilnathan, H.-W. Cho, J.-J. Wu, M. Yoshimura, Adv. Funct. Mater. 2015, 25, 298-305; b) K. Parvez, R. Li, SR Puniredd, Y. Hernandez, F. Hinkel, S. Wang, X. Feng, K. Müllen, ACS Nano 2013, 7, 3598-3606) or inorganic salts (e.g. (a) K. Parvez, Z.-S. Wu, R. Li, X. Liu, R. Graf, X. Feng, K. Müllen, J. Am. Chem. Soc. 2014, 136, 6083-6091; b) S. Yang, S. Brüller, Z.-S. Wu, Z. Liu, K. Parvez, R. Dong, F. Richard, P. Samorì, X. Feng, K. Müllen, J. Am. Chem. Soc. 2015, 137, 13927-13932). Under the influence of the electric current, electrons are transferred from the two-dimensionally structured base material, e.g.Graphite, for example, is split off, leaving a positive charge on the anode. The anions of the electrolyte can then easily be pushed between the individual layers of the base material, such as graphite, and split them off.
[0017] However, the disadvantage of this type of graphene is that it contains high levels of oxygen groups. This is due to oxygen radicals such as HO or O, which are formed during the manufacturing process by the splitting of water and add to the graphene layers (see KS Rao, J. Sentilnathan, H.-W. Cho, J.-J. Wu, M. Yoshimura, Adv. Funct. Mater. 2015, 25, 298-305).
[0018] Another problem is performing the process in high-boiling solvents such as DMF or NMP. Furthermore, the exfoliated layers tend to stick together again after drying, making it difficult to redisperse them.
[0019] One way to increase the dispersibility of graphene layers is to functionalize the graphene layers with small molecules or polymers.
[0020] Previous work dealt with the cathodic exfoliation of graphite in organic solvents and the simultaneous in-situ functionalization of the graphene sheets with diazonium salts (see, among others, (a) Ejigu, A.; Kinloch, IA; Dryfe, RAW, Single Stage Simultaneous Electrochemical Exfoliation and Functionalization of Graphene. ACS Applied Materials & Interfaces 2017, 9 (1), 710-721; (b) Zhong, YL; Swager, TM, Enhanced Electrochemical Expansion of Graphite for in Situ Electrochemical Functionalization. Journal of the American Chemical Society 2012, 134 (43), 17896-17899; (c) Ossonon, BD; Bélanger, D., Functionalization of graphene sheets by the diazonium chemistry during electrochemical exfoliation of graphite. Carbon 2017, 111, 83-93.)
[0021] Carbon 2017, 111, 83-93 shows the functionalization of exfoliated graphene with diazonium compounds (diazonium-substituted anthraquinone), i.e. with -N 2 +< .
[0022] The diazonium salts generate free radicals and functionalize the surface through a reduction reaction at the cathode.
[0023] Weitere Publikationen beschäftigen sich mit der anodischen Exfolierung von Graphit unter Verwendung verschiedener organischer Salze als Elektrolyt wie Phytinsäure (Feng, X.; Wang, X.; Cai, W.; Qiu, S.; Hu, Y.; Liew, K. M., Studies on Synthesis of Electrochemically Exfoliated Functionalized Graphene and Polylactic Acid / Ferric Phytate Functionalized Graphene Nanocomposites as New Fire Hazard Suppression Materials. ACS Applied Materials & Interfaces 2016, 8 (38), 25552-25562), Hex(4-carboxylphenoxy)cyclotriphosphazen (Cai, W.; Feng, X.; Wang, B.; Hu, W.; Yuan, B.; Hong, N.; Hu, Y., A novel strategy to simultaneously electrochemically prepare and functionalize graphene with a multifunctional flame retardant. Chemical Engineering Journal 2017, 316, 514-524), Tetracyanoquinodimethan (Khanra, P.; Lee, C.-N.; Kuila, T.; Kim, N. H.; Park, M. J.; Lee, J. H., 7,7,8,8-Tetracyanoquinodimethaneassisted one-step electrochemical exfoliation of graphite and its performance as an electrode material.Nanoscale 2014, 6 (9), 4864-4873.), 9-Anthrazen-Carbonsäure (Khanra, P.; Kuila, T.; Bae, S. H.; Kim, N. H.; Lee, J. H., Electrochemically exfoliated graphene using 9-anthracene carboxylic acid for supercapacitor application. Journal of Materials Chemistry 2012, 22 (46), 24403-24410), Tetranatriumtetrasulfonsäure (Mensing, J. P.; Kerdcharoen, T.; Sriprachuabwong, C.; Wisitsoraat, A.; Phokharatkul, D.; Lomas, T.; Tuantranont, A., Facile preparation of graphene-metal phthalocyanine hybrid material by electrolytic exfoliation. Journal of Materials Chemistry 2012, 22 (33), 17094-17099), oder organische Natriumsulfonate (Munuera, J. M.; Paredes, J. I.; Villar-Rodil, S.; Ayan-Varela, M.; Martinez-Alonso, A.; Tascon, J. M. D., Electrolytic exfoliation of graphite in water with multifunctional electrolytes: en route towards high quality, oxide-free graphene flakes. Nanoscale 2016, 8 (5), 2982-2998).
[0024] These publications describe the intercalation of the salt between the individual layers of graphite and the functionalization of the layers through pp interactions.
[0025] The thus functionalized graphene layers exhibit high ID / IG ratios in the RAMAN spectrum. The conductivity of the layers and their dispersibility are not considered.
[0026] Some examples describe the use of functionalized graphene as an electrode material in batteries or supercapacitors.
[0027] Other publications demonstrate the exfoliation of graphite with mixed electrolytes such as ammonium sulfate / ammonia or glycine and ammonia. Na 2 S 2 O 3 / H 2 SO 4 systems and potassium halides have also been used to dope graphene with heteroatoms or halogens.
[0028] Chen et al. (Chen, CH et al., Nanoscale, 2015, 7, 15362–15373) published a graphene exfoliation process using small-molecule additives such as melamine to obtain melamine-functionalized graphene layers. The exfoliation yield was increased. No statements were made regarding the temporal stability of the resulting dispersions. A method is described for the production of highly crystalline graphene by electrolytic exfoliation in 0.65 M sulfuric acid with the addition of melamine in high concentrations of 10 to 200 g / 100 ml of electrolyte solution. At voltages of 20 V, with a periodic reversal of polarity every 10 minutes, graphene layers are exfoliated from the graphite electrode and coated with melamine molecules. These in-situ applied protective layers prevent further oxidation of the graphene layer and thus lead to larger graphene crystallites.The remaining melamine is then washed off the collected graphene with water, which, after drying, exhibits a high C / O ratio of 26.17, indicating a low defect density of oxygen defects. The authors assume that covalent functionalization of the graphene platelets does not occur. The graphene produced in this way is readily dispersible in DMF or NMP. Among other things, the use of a graphene dispersion in DMF for processing on quartz substrates is reported.
[0029] Another possibility for producing functionalized graphene is the use of ionic liquids, i.e. salts that are liquid at temperatures below 100°C without the salt being dissolved in a solvent such as water.
[0030] A publication by Liu et al. (Adv. Funct. Mater. 2008, 18, 1518–1525) describes the electrolytic exfoliation of graphite in an aqueous electrolyte solution containing ionic liquids. The cations of the ionic liquids intercalate between the individual graphite layers, thus driving them apart. In this case, imidazolium hexafluorophosphate was used as the ionic liquid. XPS measurements revealed that the two nitrogen atoms of the imidazolium group interact with the graphene surface, thus binding the salt to the graphene. The thus functionalized graphene is not dispersible in water, but is dispersible in aprotic solvents such as DMF or NMP.
[0031] In 2014, Ouhib et al. published a method for producing functionalized graphene from a few layers (Ouhib et al. J. Mater. Chem. A, 2014, 2, 15298). They describe cathodic graphene exfoliation using acrylonitrile and tetraethylammonium perchlorate in an organic electrolyte (DMF) for use in batteries. The resulting products are dispersed in dimethylformamide. Highly ordered pyrolytic graphite (HOPG) is introduced as the cathode into an electrolysis cell with an electrolyte containing an ammonium salt and vinyl monomers, and graphene layers are exfoliated. In parallel, the vinyl monomers were electropolymerized, forming a chemisorbed polymer layer around the graphene layers. Disadvantageously, the electrolysis was carried out in anhydrous, high-boiling organic solvents such as DMF, and exfoliation only occurs with the aid of ultrasonic treatment.The cathodic exfoliation also ensures that no monolayers of graphene can be formed, but rather graphite nanoplatelets with >20 to 50 atomic layers are formed, as shown in the Raman spectrum of the sample in . Fig. 2 the publication. Few-layer graphene, in contrast to graphite, would show a symmetric 2D peak without a shoulder at -2700 cm -1< in the spectrum, but this is Fig. 2 clearly visible.
[0032] WO 2012 / 064292 discloses a process for producing polymer-graphene composites, wherein graphene layers are electrolytically exfoliated from graphite electrodes. The exfoliation takes place in a polymer solution, preferably using PDOT-PSS as the polymer. Composites with conductive polymers that are easily dispersible are formed. A disadvantage of this process is that it only uses pre-polymerized electrolyte additives, which are more dispersible than the corresponding monomers. It can be assumed that the polymers used in the electrolyte solution play both the role of an exfoliating agent that intercalates into the graphite layers and that they also function as graphene functionalizers. Due to the voluminous size of the polymer molecules, a kinetically inhibited and correspondingly slow intercalation process can be assumed, which is also indicated by the long exfoliation times of up to 40 hours.
[0033] KR 20160072535 A describes a process for producing graphene nanofilms by electrochemical exfoliation in a persulfate electrolyte solution. For this purpose, the washed and dried electrodes are immersed in a corresponding electrolyte solution and exfoliated at a voltage of 1 to 20 V, forming graphene nanofilms. These are then separated from the electrolyte solution by filtration and washed with distilled water. To produce a nanoink, the nanofilm particles are dispersed in an organic solvent such as N-methylpyrrolidinone (NMP) or DMF at a concentration of 0.5 to 20 mg / ml using ultrasound, which is intended to prevent the nanofilm particles from reattaching to one another. The disadvantage of this process is that it can produce more or less strongly oxidized, but not specifically functionalized, graphene films.
[0034] WO 2017 / 050689 A1 demonstrates the exfoliation of graphite in the presence of radical scavengers. The radical scavengers used are TEMPO, which was replaced with ascorbic acid, NaBH 3 , gallic acid, H 2 N-NH 2 *H 2 O, or HI for control purposes. The dispersions are prepared in a separate dispersion step with additives such as polyvinylpyrrolidone or poly(sodium 4-styrenesulfonate). No statements are made regarding the stability of the dispersions.
[0035] WO 2016 / 203388 A1 shows the functionalization of graphene with the help of biomolecules such as glutathione with the aim of preserving or restoring paper.
[0036] Biosensors and Bioelectronics (2017, 87, 195-202) describes the functionalization of graphite or graphene electrodes with polyaniline for use in bioelectrochemical systems (BES), for example, in bioremediation or the biodegradation of contaminants. Such BES utilize electroactive microorganisms for extracellular electron transfer.
[0037] Journal of Power Sources 2014, 249, 48-58, deals with the electropolymerization of pyrrole on partially exfoliated graphene. Detachment from the electrodes does not occur and is not desired.
[0038] A method to covalently chemically functionalize the exfoliated layers of conductor or semiconductor materials, such as graphene, in situ, for example to protect them from attack by hydroxyl radicals (oxidation) and / or to simultaneously increase the dispersibility of the layers in environmentally friendly, for example aqueous, solvents without the addition of surface-active additives, is not yet known from the state of the art.
[0039] The object of the invention is to provide a process for producing a surfactant-free dispersion of functionalized semiconductor or conductor materials by electrolytic exfoliation in environmentally friendly solvents that are easy to use on an industrial scale, with simultaneous and / or direct functionalization of the monolayers or thin layers of the material for better dispersibility and easier processing.
[0040] The object is achieved by a process for producing a surfactant-free dispersion of functionalized semiconductor or conductor materials from a two-dimensionally layered, carbon-based base material by electrolytic exfoliation, in an electrolysis cell comprising at least one electrode pair consisting of a first and a second electrode, and an aqueous and / or alcoholic electrolyte solution containing sulfuric acid and / or at least one sulfate and / or hydrogen sulfate salt and / or a perchlorate and / or a persulfate, with the steps: a) bringing the electrodes into contact with the electrolyte solution, b) electrolytic exfoliation of the base material, for example in the form of particles of functionalized conductor or semiconductor material, by applying a voltage between the first and second electrodes, c) separating the functionalized semiconductor or conductor material from the electrolyte solution, and d) dispersing the functionalized material after separation in inorganic and / or organic liquid media, without the addition of surfactants, wherein at least the first of the electrodes of the electrode pair contains the two-dimensionally layered, carbon-based base material, and the first electrode is connected as an anode, and at least one organic compound is added to the electrolyte solution before and / or during the electrolytic exfoliation, wherein the organic compound is selected from a.Monomers of electrically conductive polymers which are anodically oxidatively polymerized, and / or b. freely radically polymerizable, water-soluble vinyl monomers which have in their structure at least one amide group (e.g. isopropylacrylamide) and / or one anionic functional group (e.g. SO 3 -< , NO 2 -< , CO 2 -2< , PO 3 -3< , O -< ) (e.g. styrenesulfonate) and which polymerize freely radically at the anode.
[0041] For the purposes of the invention, a conductor or semiconductor material is an electrically conductive material with a highly ordered, layered structure consisting of a monolayer of the material or of several superimposed layers of the material. The semiconductor material has a specific band gap, which is formed by the energy difference between the valence band and the conduction band.
[0042] For the purposes of the invention, "functionalized" means that the material is coated with functional groups or polymer chains that adhere to the surface of the material by chemical reaction or at least chemisorption.
[0043] According to the invention, the semiconductor or conductor material is a carbon-based material, i.e. its basic structure contains mainly carbon.
[0044] In one embodiment, the functionalized semiconductor or conductor material is in the form of particles with dimensions in the nanometer to micrometer range.
[0045] In one embodiment, the semiconductor or conductor material is selected from graphene, carbon-based semiconductor or conductor polymers.
[0046] In one embodiment, the two-dimensionally layered structured base material is selected from semiconducting or conductive carbon modifications, carbon-based semiconductor or conductor polymers in the form of two-dimensionally structured base material.
[0047] In one embodiment, the semiconducting or conductive carbon modifications are selected from graphite, non-graphitic carbon, carbon nanofoam, glassy carbon, carbon black, activated carbon, carbon fibers, tar and pitch, and their derivatives.
[0048] Graphite can be naturally occurring or synthetically produced graphite.
[0049] The exfoliation of the semiconductor or conductor material from or from the two-dimensional, layered, structured base material takes place electrolytically in an electrolysis cell containing at least one pair of electrodes. An electrode pair comprises a first electrode E1 and a second electrode E2.
[0050] In one embodiment, at least the first electrode E1 contains the base material in the form of flakes, powder, fibers, foils, pieces, pastes, or a mixture thereof. The electrode can also be a single flake of the base material or several of these flakes, either pressed together or connected by a conductive material.
[0051] According to the invention, the electrode E1 is connected as an anode during exfoliation.
[0052] In one embodiment, the second electrode comprises a metal. In one embodiment, the metal is a noble metal selected from Cu, Au, Ag, Pt, and Pd.
[0053] In a further embodiment, the metal is a non-noble metal or an alloy selected from Fe, steel, Al, Pb, brass, Ti, Zn, Sn, Ni, Hg, Mg.
[0054] In one embodiment, the metal-containing electrode is connected as a cathode during exfoliation.
[0055] In one embodiment, the second electrode comprises a non-elemental metallic conductive material. In one embodiment, the non-elemental metallic material is selected from graphite, carbon, and / or conductive polymers.
[0056] In one embodiment, the non-elemental metallic electrode is connected as a cathode during exfoliation. According to the invention, the electrolyte solution is an aqueous and / or alcoholic solution
[0057] In one embodiment, the solution is aqueous-alcoholic, meaning it contains a mixture of water and alcohol.
[0058] In one embodiment, the water / alcohol ratio is 100:0 to 0:100, preferably 99:1 to 1:99, particularly preferably 20:80 to 80:20.
[0059] In one embodiment, the alcohol comprises only one alcoholic component. In another embodiment, the alcohol comprises several different alcoholic components.
[0060] In one embodiment, the alcohol is selected from ethanol and / or ethylene glycol.
[0061] According to the invention, the electrolyte solution contains sulfuric acid and / or at least one salt selected from sulfate and / or hydrogen sulfate and / or perchlorate and / or persulfate salt.
[0062] For the purposes of the invention, the salt comprises either only one salt component or a mixture of several salt components.
[0063] In one embodiment, the salt is an inorganic salt.
[0064] In one embodiment, the inorganic salt is selected from (NH 4 ) 2 SO 4 and / or K 2 SO 4 and / or Na 2 SO 4 and / or KHSO 4 and / or NaHSO 4 and / or a persulfate.
[0065] In one embodiment, the salt is an organic salt. In one embodiment, the organic salt is selected from tetraalkylammonium sulfates and / or tetraalkylammonium hydrogen sulfates.
[0066] The cation of the salt therefore corresponds to the general formula NR 4 +< , with R = H and / or C1- to C5-alkyl, where all R can be the same or different.
[0067] In step a), the electrodes are brought into contact with the electrolyte solution.
[0068] In one embodiment, the electrodes are immersed in the electrolyte solution. In another embodiment, the electrolyte solution is added to the electrodes in the electrolysis cell.
[0069] In step b), the base material is electrolytically exfoliated by applying a voltage between the first and second electrode.
[0070] In one embodiment, the voltage is 1 to 30 V, preferably 5 to 15 V, particularly preferably 8 to 12 V, in particular 10 V.
[0071] According to the invention, at least the first electrode E1 contains the two-dimensionally structured, layered, carbon-based base material. This electrode E1 is connected as the anode. By applying a voltage, oxygen-containing radicals such as HO or O2 initially form in the anode region, which attack the interfaces or intrinsic defects of the base material and add thereto, forming oxides of the base material. At the same time, the surface layers of the base material are forced apart, allowing the anions of the electrolyte, i.e., sulfate and / or hydrogen sulfate ions, to intersperse them and expand the distance between the individual layers of the base material.
[0072] The intercalation of the electrolyte's anions leads to an expansion of the distance between the layers to such an extent that the intermolecular forces can be overcome, causing individual layers to separate from the electrode. This results in the exfoliation of a monolayer, multiple layers, or a thin layer of the base material from the electrode.
[0073] These monolayers or multilayers or layers of the base material are coated or functionalized in situ with the organic compound contained in or added to the electrolyte solution.
[0074] According to the invention, at least one organic compound is added to the electrolyte solution before and / or during the electrolytic exfoliation.
[0075] According to the invention, the at least one organic compound is selected from a. monomers of electrically conductive polymers which are anodically oxidatively polymerized, and / or b. freely radically polymerizable, water-soluble vinyl monomers which have in their structure at least one amide group (e.g. isopropylacrylamide) and / or at least one anionic functional group (e.g. SO 3 -< , NO 2 -< , CO 2 -2< , PO 3 -3< , O -< ) (e.g. styrenesulfonate) and which polymerize freely radically at the anode.
[0076] Variants a. and b. can be combined with each other as desired.
[0077] By applying a voltage between electrodes E1 and E2, the anodically oxidizable organic molecules, due to their partially negative charge, migrate / diffuse into the anode region, where they are electrolytically oxidized, i.e., an electron is abstracted. Radicals are formed according to the following equations:
[0078] These radicals react with the surface of the semiconductor and / or conductor material and functionalize it by forming a coating of molecules.
[0079] According to the invention, the organic compound in variant a is selected from anodically oxidatively polymerizable monomers of electrically conductive polymers.
[0080] In one embodiment, the monomers of the electrically conductive polymers in variant a are selected from aromatic amines, aniline, pyrrole, and thiophene.
[0081] In one embodiment, the electrically conductive polymers in variant a are selected from substituted and / or unsubstituted polyanillins, polypyrroles, and / or polythiophenes.
[0082] In one embodiment, a substituted polyaniline is sulfonated polyaniline.
[0083] The functionalization of the conductor or semiconductor material is carried out with the compounds according to variant a. by oxidative polymerization.
[0084] Just as with functionalization with small organic anodically oxidizable molecules, during electrolysis the anions of the electrolyte initially intercalate between the individual layers of the base material, forcing them apart until they split off. At the same time, the monomers of the electrically conductive polymers are anodically oxidized, meaning they lose an electron, forming radical cations.
[0085] These react with the surface of the exfoliated semiconductor or conductor material and polymerize further there. This forms a polymer coating on the mono- and / or multilayers or layers of the conductor material and functionalizes them.
[0086] The electrochemical exfoliation process creates free radicals on the surface of the graphene, which are stabilized by the extensive network of conjugated electrons. These radicals and anions can be used as starting points for free-radical and oxidative polymerization reactions to covalently functionalize the graphene surface. Another possible mechanism is the activation of oxygen-containing groups (especially epoxide) on the graphene surface by electrochemical exfoliation.
[0087] According to the invention, the organic compound in variant b. is selected from free-radically polymerizable, water-soluble vinyl monomers which have at least one amide group and / or one anionic functional group in their structure and which polymerize free-radically at the anode (Table 1).
[0088] In one embodiment, the anionic functional group is selected from SO 3 -< , NO 2 -< , CO 2 -2< , PO 3 -3< , O -< (e.g. isopropylacrylamide or styrenesulfonate). Table 1 Functional group Time of addition of the molecule Notes / Examples / Functionalization mechanisms "Vinyl-Verbindungen" R:aromatic and aliphatic before / during Polymerization (free radical, cationic) e.g.: N-isopropylacrylamide, methylenebisacrylamide, sodium 4-vinylbenzenesulfonate
[0089] In variant b. of the process according to the invention, the free radical polymerization of the water-soluble vinyl monomers takes place.
[0090] Vinyl monomers would normally polymerize at the cathode based on the reduction reaction of the vinyl group (anionic polymerization mechanism). For such reactions, anhydrous organic solvents are typically used in the prior art under a protective gas atmosphere.
[0091] However, if such monomers contain functional groups that oxidize faster than the vinyl group is reduced, or if they contain anionic groups such as SO 3 -< , NO 2 -< , CO 2 -< , PO 3 -<, they move to the anode and, activated by free radicals from water splitting, can undergo free radical polymerization (see Figure 1 ).
[0092] This type of polymerization has been successfully carried out, for example, for monomers such as isopropylacrylamide and vinyl monomers (see, for example, Fig. 1 b) containing anionic groups (such as sodium 4-vinylbenzenesulfonate, Fig. 1 b).
[0093] Surprisingly, it was found that polymerization in the presence of the exfoliated conductor or semiconductor material led to polymer-functionalized conductor or semiconductor material.
[0094] In step c) of the process according to the invention, the functionalized semiconductor or conductor material, for example in the form of particles, is separated from the electrolyte solution. Separation methods are known to the person skilled in the art.
[0095] In one embodiment, the functionalized material is dried and dispersed after separation.
[0096] The production of highly concentrated and stable dispersions has so far only been possible with the use of additives such as surfactants. Surfactants can be used to adjust the filler content of the dispersions to virtually any desired level in various solvents or media.
[0097] However, surfactants have a detrimental effect on interactions with the matrix (e.g., in polymer composites) and reduce the conductivity and stability of the applied semiconductor or conductor layers, for example, in printed circuit applications. The surfactants must be subsequently washed out or thermally removed in a complex process. This complicates processing and is also extremely costly and energy-intensive.
[0098] Furthermore, dispersion is currently known in ecologically and economically less advantageous solvents such as DMF or NMP.
[0099] Advantageously, the dispersion of the material functionalized according to the invention is possible not only in organic, anhydrous solvents, but in particular also in water or aqueous solvents without the addition of surfactants, thus enabling significantly better environmental compatibility and lower costs.
[0100] Aqueous solvents within the meaning of the invention are homogeneous solvents which also contain a proportion of water.
[0101] Advantageously, dispersion is possible not only in water or aqueous solvents or organic solvents, but also in a wide range of reactants, for example polymerization precursors, epoxides, silicones without the use of additives such as surfactants.
[0102] Advantageously, the dispersions prepared according to the invention are stable over a long period of time even without the addition of such additives. Contrary to the state of the art, this stability can even be achieved exclusively in water. The dispersions thus formed can be easily processed, which is advantageous, for example, in the coating of substrates with the functionalized conductor or semiconductor material.
[0103] In one embodiment, the dispersion takes place in a solvent selected from water and / or alcohols.
[0104] In one embodiment, the solvent is aqueous-alcoholic, meaning it contains a mixture of water and alcohol.
[0105] In one embodiment, the volume ratio of water to alcohol is 0:100 to 100:0, preferably 99:1 to 1:99, particularly preferably 80:20 to 20:80.
[0106] In one embodiment, the alcohol comprises only one alcoholic component. In another embodiment, the alcohol comprises several different alcoholic components.
[0107] In one embodiment, the alcohol is selected from ethanol and / or ethylene glycol.
[0108] In one embodiment, the concentration of the functionalized material in aqueous and / or alcoholic dispersions is 0.1 to 100 g / l, preferably 0.1 to 10 g / l, particularly preferably 0.1 to 2 g / l, in particular 0.1 to 1 g / l.
[0109] Advantageously, dispersions with a significantly higher concentration than previously known from the state of the art can be realized without the use of additives that modify the interfacial tension, such as surfactants.
[0110] The functionalization of the semiconductor or conductor material according to the invention makes it possible for the first time to process or process the material, for example on electrodes or substrates, from a wide variety of media.
[0111] For example, stable dispersions of graphene functionalized with polyaniline (EG-PANI) according to the invention could be produced at high concentrations in water or ethylene glycol. Dispersions of graphene functionalized with sulfonated polyaniline (EG-SPANI) were also successfully produced in water, ethanol, and ethylene glycol. Further examples are listed in Table 2. Entry Product Solvent Stable Concentration (mg / mL) 1a EC-SPAIN Water 0.4 to 2 1b EC-SPAIN Water 100* 2a EC-SPAIN Ethanol 0.5 to 1 2b EC-SPAIN Ethanol 80* 3 EC-SPAIN Ethylene glycol 1 4 EC-SPAIN DMF 1 5 EC-PANI Water 0.1-0.2 6 EC-PANI Ethanol 0.3-0.4 7 EC-PANI Ethylene glycol 0.5-0.6 8 EC-PPy Water 0.1-0.2 9 EC-PPy Ethanol 0.3-0.4 10 EC-PPy Ethylene glycol 0.5-0.6 11 EC-PNIPAM water 0.3-0.4 12 EC-PSS water 0.4 13 EC-PAM water 0.25 *: Dispersion in paste form with significantly higher viscosity than that of the base solvent
[0112] Table 2: Examples of stable dispersions of various materials prepared according to the invention in different media and different concentrations: EG-SPANI = Exfoliated graphene functionalized with sulfonated polyaniline, EG-PANI = Exfoliated graphene functionalized with polyaniline, EG-PPy = Exfoliated graphene functionalized with polypyrrole, EG-PNIPAM = Exfoliated graphene functionalized with poly(N-isopropylacrylamide), EG-PSS = Exfoliated graphene functionalized with poly(styrenesulfonate), EG-PAM = Exfoliated graphene functionalized with poly(methylenebisacrylamide).
[0113] For the purposes of the invention, inorganic and / or organic liquid media are understood to mean both pure and multi-component solvents or monomers or silicones or mixtures thereof.
[0114] It is sensible to keep the dispersion free of compounds that modify the interfacial tension, such as surfactants, detergents or emulsifiers.
[0115] Advantageously, the conductor or semiconductor material produced according to the invention exhibits a particularly low defect density. RAMAN measurements demonstrate that by functionalizing the exfoliated material with small organic molecules or polymers, the surface of the base material is protected from oxygen radicals during exfoliation. This is evident in the particularly low ID -IG ratios.
[0116] For example, EG-PANI produced according to the invention shows an ID -IG ratio of 0.12 or EG-PPy produced according to the invention shows an ID -IG ratio of 0.13.
[0117] For the realization of the invention, it is also expedient to combine the above-described inventive embodiments, embodiments and features of the claims in an expedient manner.
[0118] The following exemplary embodiments are intended to explain the invention in more detail, but without limiting it thereto: Examples of implementation
[0119] The present invention is described in more detail by the following figures and exemplary embodiments, without this being intended to limit the scope of the claims defined above: Fig. 1: Schematic illustration of the in-situ exfoliation and functionalization of graphite, Fig. 2: Proposed mechanism of in-situ functionalization, Fig. 3: RAMAN spectra of a) EG and b) PPy-functionalized EG, Fig. 4: a) XPS overview spectra of EG and EG-PPy, b) high-resolution XPS spectrum of the C1s region of EG, c) high-resolution XPS spectrum of the C1s region of EG-PPY and d) high-resolution XPS spectrum of the N1s region of EG-PPY, Fig. 5: RAMAN spectrum of PANI-functionalized EG, Fig. 6: a) high-resolution XPS spectrum of the C1s region of EG-PANI and b) high-resolution XPS spectrum of the N1s region of EG-PANI, Fig. 7:a) TGA, b) AFM and c) RAMAN analyses of SPANI-functionalized EG (EG-SPANI), Fig. 8: XPS analysis of EG-SPANI: a) overview spectrum and high-resolution XPS spectra b) of the C1s region, c) of the S2p region and d) of the N1s region, Fig. 9: Schematic illustration of the mass production of EG-SPANI (= exfoliated graphene functionalized with sulfonated polyaniline) through a continuous flow system, Fig. 10: a) TGA and b) AFM analyses of PNIPAM-functionalized EG (EG-PNIPAM), Fig.11: XPS analysis of EG-PNIPAM a) overview spectrum and b) high-resolution spectrum of the N1s region, Fig. 12: TGA analyses of a) EG functionalized with polymethylenebisacrylamide (PAM) b) EG functionalized with sulfonated polystyrene, Fig. 13: a) TGA, b) XPS overview spectrum and c) XPS N1s region analyses of a butylamine-functionalized EG d) increased degree of butylamine functionalization detected by TGA, Fig. 14:a) TGA and b) XPS spectra of valeric acid-functionalized EG, Fig. 15: Proposed mechanism for the direct post-functionalization of EG immediately after exfoliation, Fig. 16: a, b) RAMAN and c) TGA spectra of polypyrrole-functionalized EG by direct post-functionalization, Fig. 17: XPS analysis of polypyrrole-functionalized EG using direct post-functionalization, a) overview spectrum, b) C1s region and c) N1s region, Fig. 18: TGA analysis of EG after direct post-functionalization with a) valeric acid, b) butylamine and tert-octylamine, Fig. 19: Zeta potential measurements of aqueous dispersions of functionalized graphene, Fig. 20: Charge and discharge curve of a half-cell lithium-ion battery with LiCoO 2 / EG-SPANI (90 / 10) as cathode material, Fig. 21:Cyclic voltammetry measurements of 3-electrode cell supercapacitors with a freestanding film of functionalized graphene (EG-SPANI) as electrode. Characterization of the manufactured materials
[0120] SEM images were obtained using a field emission scanning electron microscope (Gemini 1530 LEO) with an accelerating voltage of 10 keV. AFM characterization was performed on a Veeco Nanoscope-IIla Multimode Picoforce (Digital Instruments). Raman spectroscopy and mapping were performed using a Bruker RFS 100 / S spectrometer (laser wavelength 532 nm). XPS analyses were performed on a Thermo Scientific K-Alpha X-ray photoelectron spectrometer with a base chamber pressure between ~10 -8 < -10 -9 < mbar and an Al anode as the X-ray source (X-ray radiation of 1496 eV). Spot sizes of 400 µm were used. Survey spectra were recorded with an average of 10 scans, a pass energy of 200.00 eV, and a step size of 1 eV. High-resolution spectra were recorded with an average of 10 scans, a pass energy of 50.00 eV, and a step size of 0.1 eV.The sheet resistances of the EG films were measured with a four-point resistance measurement system using a Keithley 2700 multimeter (probe spacing: 0.635 mm, Rs = 4.532 V / I). Example 1 Electrochemical exfoliation and in situ functionalization of graphite with polypyrrole and preparation of a dispersion of polypyrrole-functionalized graphene (EG-PPy)
[0121] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes with a fixed spacing of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.8 g) in 60 mL of deionized water. Pyrrole (7 µL, reagent grade, 98% purity) was dissolved in 10 mL of water to obtain a 0.01 M monomer solution. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the solution), a constant potential of 10 V was applied to start the exfoliation process, while the monomer solution was added at a rate of 20 ml / h using a syringe pump.
[0122] After exfoliation was complete and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3×400 mL) to remove any residues such as ammonium sulfate and pyrrole monomers. The light gray product (polypyrrole-functionalized graphene, EG-PPY, 60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.1–0.2 mg / mL and was stable for over one week, meaning no particle sedimentation occurred.
[0123] For dispersions in other solvents, the product (polypyrrole-functionalized graphene, EG-PPY, 60 mg) was washed with water, then dispersed in ethanol or ethylene glycol (30 ml each) using mild ultrasonication and allowed to stand for 24 h. The resulting supernatants yielded stable dispersions with a graphene content of 0.2–0.3 mg / ml (ethanol) and 0.5–0.6 g / ml (ethylene glycol).
[0124] The reaction was scaled up by using thicker graphite foils while maintaining the electrode area in the electrolyte and increasing the pyrrole concentration (in a constant ratio to the weight of the graphite electrode).
[0125] The successful functionalization was confirmed by X-ray photoelectron spectroscopy (XPS). The oxygen content was 11.46 atom% for EG and 9.52 atom% for EG-PPy.
[0126] In the case of EG-PPy, in contrast to EG, nitrogen was also detected in a concentration of 2.79 atom-%, which can be assigned to the polypyrrole groups ( Fig. 4a ).
[0127] The high-resolution spectrum of the N1s region ( Fig. 4d ) shows a main band at 400 eV which can be assigned to the -NH groups, as well as a band at 401 eV which can be assigned to the polaron structure (CN +< ) of polypyrrole.
[0128] The high-resolution spectrum of the C1s region ( Fig. 4c ) shows three main bands at 284.35 eV, 285.4 eV and 287.2 eV, which can be assigned to the C=C, C-OH and C=O bonds.
[0129] In contrast, unfunctionalized EG shows five different bands ( Fig. 4b ).In addition to the bands at 284.4 eV, 285.2 eV and 287.2 eV (C=C, C-OH and C=O bonds), two further bands at 286.5 eV and 290.2 eV occur, which are assigned to epoxide (COC) and carboxylate groups (OC=O) ( Fig. 4b The absence of epoxy groups in the case of the functionalized EG indicates that the graphene is subject to less severe oxidation during exfoliation, which is attributed to a protective effect of the PPy functionalization of the basal plane.
[0130] The high quality of the functionalized graphene can be demonstrated by RAMAN spectroscopy. While the spectrum of EG shows a relatively high intensity ratio of the D and G peaks of 0.52 ( Fig. 3a )indicates a significant degree of defect sites (due to the attack of hydroxyl radicals on the exposed graphene surfaces), the addition of the 0.01M aqueous pyrrole solution during exfoliation can protect the graphene surface by the formed polypyrrole functionalities, which is illustrated by a low ID -IG ratio of 0.13. ( Fig. 3b ).
[0131] A thin film of EG-PPy was prepared by filtration of a dispersion on PC filter paper. The film's sheet resistance was measured using a four-point resistivity measurement system, and the film thickness was measured using SEM, yielding a conductivity of approximately 500 S / cm.
[0132] Zeta potential measurements of aqueous dispersions showed the stability of EG-PPy dispersions over a wide pH range ( Fig. 19 ) Example 2 Electrochemical exfoliation and in situ functionalization of graphite with polyaniline and preparation of a dispersion of polyaniline-functionalized graphene (EG-PANI)
[0133] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes with a fixed spacing of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.8 g) in 60 mL of deionized water. Aniline (10 µL, Acros organics, 99.8% purity) was dissolved in 26 µL of H 2 SO 4 and 10 mL of water to obtain a 0.01 M monomer solution. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the solution), a constant potential of 10 V was applied to start the exfoliation process, while the monomer solution was added at a rate of 15 ml / h using a syringe pump.
[0134] After exfoliation was complete and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3×400 mL) to remove any residues such as ammonium sulfate and aniline monomers. The light gray product (polyaniline-functionalized graphene, EG-PANI, 60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.1–0.2 mg / mL and was stable for over one week.
[0135] For dispersions in other solvents, the product (polyaniline-functionalized graphene, EG-PANI, 60 mg) was washed with water, for example, in ethanol or ethylene glycol (30 ml each) using mild ultrasonication, and then dispersed in the same way. The resulting supernatants yielded stable dispersions with a graphene content of 0.2–0.3 mg / ml (ethanol) and 0.5–0.6 g / ml (ethylene glycol).
[0136] The reaction was scaled up by using thicker graphite foils while maintaining the electrode area in the electrolyte and increasing the aniline concentration (in a constant ratio to the weight of the graphite electrode).
[0137] The successful functionalization was demonstrated by X-ray photoelectron spectroscopy (XPS).
[0138] The oxygen content was 11.46 atom% for EG and 6.68 atom% for EG-PANI. In contrast to EG, nitrogen was also detected in EG-PANI at a concentration of 2.02 atom%, which is attributable to the polyaniline groups. ( Fig. 6a , 6b ).
[0139] The high-resolution spectrum of the N1s region ( Fig. 6b ) shows three bands at 399eV, 400 eV and 401 eV which can be assigned to the C=N, -NH and -NH +< groups of polyaniline.
[0140] The high-resolution spectrum of the C1s region ( Fig. 6a ) shows three main bands at 284.4 eV, 285.2 eV and 286.5 eV, which can be assigned to the C=C, C-OH and C=O bonds, while the proportion of epoxy groups is low.
[0141] The high quality and low defect density of the functionalized graphene can be demonstrated by RAMAN spectroscopy. By adding the 0.01M aqueous aniline solution during exfoliation, the graphene surface can be protected by the formed polyaniline functionalities, which is demonstrated by a low ID -IG ratio of 0.12. ( Fig. 5 ).
[0142] A thin film of EG-PANI was produced by filtration of a dispersion on PC filter paper. The film's sheet resistance was measured using a four-point resistivity measurement system, and the film thickness was measured using SEM, yielding a conductivity of approximately 400 S / cm.
[0143] Zeta potential measurements of aqueous dispersions showed the stability of EG-PANI dispersions in the neutral pH range and low stability under acidic conditions ( Fig. 19 ) Example 3 Electrochemical exfoliation and in situ functionalization of graphite with sulfonated polyaniline and preparation of a dispersion of EG-SPANI (= exfoliated graphene functionalized with sulfonated polyaniline)
[0144] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes with a fixed spacing of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.8 g) in 60 mL of deionized water. Anilinesulfonic acid (18 mg, Sigma-Aldrich, 95% purity) was dissolved in 26 µL of H 2 SO 4 and 10 mL of water to obtain a 0.01 M monomer solution. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the solution), a constant potential of 10 V was applied to start the exfoliation process, while the monomer solution was added at a rate of 15 ml / h using a syringe pump.
[0145] After exfoliation was complete and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3×400 mL) to remove any residues such as ammonium sulfate and aniline monomers. The dark gray product (polyaniline sulfonate-functionalized graphene, EG-SPANI, 60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.3–0.4 mg / mL and was stable for over one week.
[0146] For dispersions in other solvents, the product (polyanilinesulfonate-functionalized graphene, EG-SPANI, 60 mg) was washed with water and dispersed analogously in ethanol or ethylene glycol (30 ml each) using mild ultrasonication and allowed to stand for 24 h. The resulting supernatants yielded stable dispersions with a graphene content of 0.4–0.5 mg / ml (ethanol) and 0.8–1.0 g / ml (ethylene glycol).
[0147] The reaction was scaled up by using thicker graphite foils while maintaining the electrode area in the electrolyte and increasing the aniline concentration (in a constant ratio to the weight of the graphite electrode).
[0148] The successful functionalization was demonstrated by thermogravimetry (TGA), where the functionalized EG-SPANI showed an almost 5 wt.% higher mass loss compared to unfunctionalized EG ( Fig. 7a ).
[0149] The AFM investigations showed a layer thickness of 4 nm and 1.2 nm for the edges and basal planes of the platelets, respectively ( Fig. 7b ). RAMAN measurements showed a low ID / IG ratio of 0.12 and thus a low defect density ( Fig. 7c ).
[0150] X-ray photoelectron spectroscopy (XPS) revealed a nitrogen content of 2.15 atom% and a sulfur content of 0.62 atom%, which can be attributed to the polyanilinesulfonate groups ( Fig. 8a ).
[0151] The high-resolution spectrum of the N1s region shows a main band at 400 eV, which can be assigned to the -NH groups, as well as the band at 401 eV, which can be assigned to the polaron structure (CN +< ) of polyanilinesulfonate. The high-resolution spectrum of the C1s region ( Fig. 8b )shows three main bands at 284.35 eV, 285.4 eV, and 287.2 eV, which can be assigned to the C=C, C-OH, and C=O bonds, respectively. The high-resolution spectrum of the sulfur region ( Fig. 8c ) shows two bands at 167.4 eV and 168.6 eV which can be assigned to the sulfonic acid and sulfonate groups of the polyanilinesulfonate, respectively.
[0152] A thin film of EG-SPANI was produced by filtration of a dispersion on PC filter paper. The film's sheet resistance was measured using a four-point resistance measurement system, and the film thickness was measured using SEM, yielding a conductivity of approximately 800 S / cm.
[0153] Zeta potential measurements of aqueous dispersions showed the stability of EG-SPANI dispersions in a wide pH range (3-10) with a zeta potential below -40 mV ( Fig. 19 ) Example 4 Mass production of EG-SPANI (= exfoliated graphene functionalized with sulfonated polyaniline) by a continuous flow system and dispersion
[0154] Graphite exfoliation was carried out in a continuous flow system, using graphite foils (5 cm x 30 cm, 2.3 g per foil) (Alfa Aesar, 99.99% purity) as working anodes and copper foils of the same size as cathodes. The copper electrodes were attached to the reactor wall, where the graphite electrodes were immersed in the electrolyte from above. ( Fig.9 ). The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1M, 46.2g), anilinesulfonic acid (1g, Sigma-Aldrich, 95% purity), and 1.4mL H2SO4 in 3.5L of deionized water and continuously flowed into the system via a pump at a constant rate. After the electrodes were immersed in the electrolyte (150cm2< active electrode area in the solution), a constant potential of 10V was applied to initiate the exfoliation and polymerization processes.
[0155] After exfoliation was complete and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (2 L) to remove any residues such as ammonium sulfate and aniline monomers. The dark gray product (polyaniline sulfonate-functionalized graphene, EG-SPANI, 2.2 g) was then dispersed in deionized water (150 ml) using mild ultrasonication (30 min, 30% amplitude, 2 watts). This dispersion was allowed to stand for 24 hours to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.5 mg / ml and was stable for several weeks. Example 5 Electrochemical exfoliation and in situ functionalization of graphite with poly-N-isopropylacrylamide and preparation of a dispersion of EG-PNIPAM (= poly-N-isopropylacrylamide-functionalized graphene)
[0156] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes with a fixed spacing of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.8 g) in 60 mL of deionized water. N-isopropylacrylamide (30 mg, 0.25 mmol, Sigma, 97% purity) was dissolved in 10 mL of water to obtain a 0.02 M monomer solution. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the electrolyte solution), a constant potential of 10 V was applied to start the exfoliation process, while the monomer solution was added at a rate of 20 ml / h using a syringe pump.
[0157] After exfoliation was complete and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3×400 mL) to remove any residues such as ammonium sulfate and aniline monomers. The dark gray product (poly-N-isopropylacrylamide-functionalized graphene, EG-PNIPAM, 60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed. The resulting aqueous dispersion contained functionalized graphene at a concentration of 0.3–0.4 mg / mL and was stable for over one week.
[0158] The successful functionalization was demonstrated by TGA, where the functionalized EG-PNIPAM showed over 40 wt.% mass loss compared to unfunctionalized EG ( Fig. 10a ).
[0159] The AFM investigations showed a layer thickness of 3 nm, which illustrates the presence of functional groups on the surface ( Fig. 10b ).
[0160] X-ray photoelectron spectroscopy (XPS) revealed a nitrogen content of 0.86 atom% and an increase in the C / O ratio, which are attributable to the PNIPAM functionalization ( Fig. 11a ). The high-resolution spectrum of the N1s region shows a main band at 400 eV which can be assigned to the -NH groups, as well as the band at 401 eV which can be assigned to the amide structure of PNIPAM ( Fig. 11b ).
[0161] A thin film of EG-PNIPAM was grown by filtration of a dispersion on PC filter paper. The relatively high sheet resistance of the film of -140 Ω / □ (determined using a four-point resistance measurement system) is due to the presence of the insulator PNIPAM on the graphene surface.
[0162] The process was also successfully carried out in an analogous manner with other vinyl monomers, such as methylenebisacrylamide and sodium 4-vinylbenzenesulfonate, which could be polymerized on the surface of the graphene. The successful functionalization with poly(methylenebisacrylamide) (PAM) and poly(sodium 4-vinylbenzenesulfonate) (PSS) was demonstrated by TGA analogously to Example 4 ( Fig. 12a and 12b ).
[0163] In addition, stable aqueous dispersions with EG-PAM (0.25 mg / ml) and EG-PSS (0.4 mg / ml) were prepared. Comparison example 6 Electrochemical exfoliation and in situ functionalization of graphite with butylamine
[0164] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes with a fixed spacing of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.93 g) and butylamine (30 mg, 0.41 mmol, Aldrich, 99.5% purity) in 70 mL of deionized water. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the electrolyte solution), a constant potential of 10 V was applied to start the exfoliation process. After exfoliation was completed and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water.The washing process was repeated three times (3 x 400 mL) to remove any residues such as ammonium sulfate and butylamine. The dark gray product (60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed. The resulting aqueous dispersion contained functionalized graphene at a concentration of 0.1 mg / mL and was stable for over one week.
[0165] In TGA measurements, a residual mass of 66 wt.% was determined, with the loss being mainly due to the cleavage of the butyl groups at 374°C ( Fig. 13a ).
[0166] X-ray photoelectron spectroscopy (XPS) revealed a nitrogen content of 1.11 atom-%, which can be attributed to the butylamine groups ( Fig. 13b ). The high-resolution spectrum of the N1s region shows three main bands which can be assigned to the amide, amine and NH 3 +< groups ( Fig. 13c ).
[0167] The degree of functionalization could be increased by increasing the butylamine concentration (150 mg, 2 mmol) under otherwise identical conditions as above. This was also demonstrated by an increased mass loss in the TGA to a residual mass of 51 wt.%. ( Fig. 13d ).
[0168] The process was successfully carried out in an analogous manner with other amines, such as tert-octylamine, melamine and 2-amino-2-(hydroxymethyl)-1,3-propanediol (TRIS). Comparison example 7 Electrochemical exfoliation and in situ functionalization of graphite with valeric acid + Dispersal
[0169] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes at a fixed distance of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.93 g) and valeric acid (30 mg, 0.3 mmol, Alfa Aesar, 99% purity) in 70 mL of deionized water. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the electrolyte solution), a constant potential of 10 V was applied to start the exfoliation process.
[0170] After exfoliation was complete and the graphite foil was consumed, the suspended graphene flakes were separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3×400 mL) to remove any residues such as ammonium sulfate and valeric acid. The dark gray product (60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.1 mg / mL and was stable for over one week.
[0171] The successful functionalization was demonstrated by TGA, where the functionalized EG showed a 4 wt.% greater mass loss compared to unfunctionalized EG ( Fig. 14a ).
[0172] At the same time, an increase in the C / O ratio to ~9 was detected by X-ray photoelectron spectroscopy (XPS) (compared to unfunctionalized EG: ~7.3). ( Fig. 14b ) which can be explained by the attack and functionalization with pentyl radicals on the graphene surface ( Fig. 2 ). Comparison example 8 Electrochemical exfoliation of graphene and subsequent functionalization with polypyrrole + dispersion
[0173] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes at a fixed distance of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.93 g) in 70 ml of deionized water. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the electrolyte solution), a constant potential of 10 V was applied to start the exfoliation process.
[0174] After exfoliation was complete and the graphite foil was consumed, pyrrole (100 µL, 1.5 mmol, Sigma-Aldrich, 98% purity) was added, and the mixture was homogenized for 5 min in an ultrasonic bath and then stirred for 30 min. The suspended graphene flakes were then separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3 × 400 mL) to remove any residues such as ammonium sulfate and pyrrole. The dark gray product (60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min in an ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant dispersion was then removed.The resulting aqueous dispersion contained functionalized graphene at a concentration of 0.2 mg / ml and was stable for over one week.
[0175] The proposed mechanism for direct functionalization is described in Fig. 15 The electrochemical exfoliation process creates free radicals on the surface of the graphene, which are stabilized by the extensive network of conjugated electrons. These radicals and anions can be used as starting points for free-radical and oxidative polymerization reactions to covalently functionalize the graphene surface. Another possible mechanism is the activation of oxygen-containing groups (especially epoxide) on the graphene surface by electrochemical exfoliation.
[0176] The RAMAN spectrum showed an ID / IG ratio of 0.3. In addition, the RAMAN spectrum indicated three bands at 848.5 cm -1< , 994.9 cm -1< and 1050.1 cm -1< ( Fig. 16a ). which can be attributed to the functionalization of EG with polypyrrole (EG-PPy) and are not observed in unfunctionalized EG ( Fig. 16b )
[0177] Furthermore, the successful functionalization was demonstrated by TGA, where the functionalized EG showed a 19 wt.% higher mass loss compared to unfunctionalized EG ( Fig. 16c ).
[0178] XPS measurements showed an oxygen content of 10.92 atom% (EG) and 8.43 atom% (EG-PPy) as well as a nitrogen content of 3.37 atom% for EG-PPy which is due to the polypyrrole functionalization ( Fig. 17a )
[0179] The high-resolution spectrum of the N1s region shows a main band at 400 eV which can be assigned to the -NH group, as well as the band at 401 eV which can be assigned to the polaron structure (CN +< ) of polypyrrole ( Fig. 17c ). The high-resolution spectrum of the C1s region ( Fig. 17b ) shows a band at 285.5 eV, which is assigned to the CN bond, which is not detectable in unfunctionalized EG. Comparison example 9 Electrochemical exfoliation of graphene and direct functionalization with valeric acid + dispersion
[0180] Through the effects of electrochemical exfoliation on the surface of the graphene and the generation of active / reactive centers (see Fig. 15 ) The surface can also be functionalized with various other agents containing, for example, amine or carboxylate groups, as will be illustrated in the following example.
[0181] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes at a fixed distance of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.93 g) in 70 ml of deionized water. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the electrolyte solution), a constant potential of 10 V was applied to start the exfoliation process.
[0182] After exfoliation was complete and the graphite foil was consumed, valeric acid (100 mg, 0.98 mmol, Alfa-Aesar, 99% purity) was added, and the mixture was homogenized for 5 min in an ultrasonic bath and then stirred for 30 min. The suspended graphene flakes were then separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3 × 400 mL) to remove any residues such as ammonium sulfate and pyrrole. The dark gray product (60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min in an ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.1 mg / ml and was stable for over one week.
[0183] The successful functionalization was demonstrated by TGA, where the functionalized EG showed a residual mass of almost 63 wt.% compared to unfunctionalized EG.
[0184] In addition, the step at approximately 200°C, which is usually attributed to the conversion of epoxy groups, is significantly weaker than in unfunctionalized EG, indicating a reaction between the epoxy groups in EG and the valeric acid ( Fig. 18a ). Comparison example 10 Electrochemical exfoliation of graphene and direct functionalization with amines
[0185] Graphite exfoliation was performed in a two-electrode system, using graphite foils (2 cm × 3 cm, 100 mg per foil) (Alfa Aesar, 99.99% purity) as working anodes and gold foils of the same size as cathodes. The gold electrodes were arranged parallel to the graphite electrodes at a fixed distance of 2 cm. The electrolyte for exfoliation was prepared by dissolving ammonium sulfate (0.1 M, 0.93 g) in 70 ml of deionized water. After the electrodes were immersed in the electrolyte (6 cm 2 < active electrode area in the electrolyte), a constant potential of 10 V was applied to start the exfoliation process.
[0186] After exfoliation was complete and the graphite foil was consumed, butylamine (100 mg, 1.37 mmol, Sigma-Aldrich, 99.5% purity) was added to the electrolyte, and the mixture was homogenized for 5 min in an ultrasonic bath and then stirred for 30 min. The suspended graphene flakes were then separated using a 0.2 µm PC (polycarbonate) filter and washed with deionized water. The washing process was repeated three times (3 × 400 mL) to remove any residues such as ammonium sulfate. The dark gray product (60 mg) was then dispersed in deionized water (30 mL) using mild ultrasonication (30 min in an ultrasonic bath). This dispersion was allowed to stand for 24 h to allow non-exfoliated, non-functionalized platelets and larger particles to settle. The supernatant was then removed. The resulting aqueous dispersion contained graphene at a concentration of 0.1 mg / ml and was stable for over one week.
[0187] The successful functionalization was demonstrated by TGA. In Fig. 18 a It is evident that the step at approximately 200°C, which is usually associated with the conversion of epoxy groups, is significantly less pronounced than in unfunctionalized EG. This indicates a reaction between the epoxy groups in EG and the butylamine. Similarly, functionalization with tert-octylamine was detected using TGA. ( Fig. 18 b) . Example 11 Functionalized graphene powder as a cathode additive in lithium-ion batteries
[0188] Functionalized graphene (EG-SPANI) was added as a conductive additive to typical cathode materials such as LiFePO 4 and LiCoO 2 using a solution-mixing method to prepare electrodes for lithium-ion batteries.
[0189] For this purpose, the dispersion prepared according to Example 3 was mixed with commercially available cathode material (LiFePO4 / LiCoO2) in a mass ratio of 1:1 using ultrasound. After filtration and drying of the mixture, it was filled into a half-cell as the cathode material, in which lithium foil was arranged as the anode.
[0190] At a constant current rate of 0.1 C (1C=170 mAh / g), the material showed a charge and discharge capacity of 120 mAh / g ( Fig. 20 ). Example 12 Functionalized graphene as freestanding electrode films in supercapacitor cells
[0191] Freestanding films of functionalized graphene (EG-SPANI) were used as an electrode in a three-electrode supercapacitor cell, with platinum wire as the counter electrode, AgCl as the reference electrode, and 0.1 M sulfuric acid as the electrolyte. The functionalized graphenes showed a good capacitance of up to 312 F / g, while unfunctionalized EG exhibited a capacitance of less than 20 F / g. ( Fig. 21 ).
Claims
1. Method for producing a surfactant-free dispersion of functionalised semiconductor or conductor material from a two-dimensionally layered structured, carbon-based base material by electrolytic exfoliation, in an electrolytic cell, comprising at least one electrode pair of a first and second electrode, and an aqueous and / or alcoholic electrolyte solution, containing sulphuric acid and / or at least one salt, selected from sulphate and / or hydrogen sulphate and / or perchlorate and / or persulphate salt, comprising the steps: a) bringing the electrodes into contact with the electrolyte solution, b) electrolytic exfoliation of the base material by applying a voltage between the first and second electrode, c) separating the functionalized conductor or semiconductor material from the electrolyte solution, and d) dispersing the functionalized material after separation in inorganic and / or organic liquid media, without the addition of surfactants, wherein at least the first of the electrodes of the electrode pair contains the two-dimensionally layered structured, carbon-based base material, and the first electrode is connected as an anode, and at least one organic compound is added to the electrolyte solution before and / or during the electrolytic exfoliation, wherein the organic compound is selected from a. monomers of electrically conductive polymers which are polymerised by anodic oxidation, and / or b. freely radical-polymerizable, water-soluble vinyl monomers which have at least one amide group and / or at least one anionic functional group in their structure and which undergo free radical polymerisation at the anode.
2. Method according to claim 1, characterised in that the semiconductor or conductor material is selected from graphene, carbon-based semiconductor or conductor polymers.
3. Method according to claim 1 or 2, characterised in that the two-dimensionally layered structured, carbon-based base material is selected from semiconductive or conductive carbon modifications, carbon-based semiconductor or conductor polymers in the form of two-dimensionally structured base material.
4. Method according to any of claims 1 to 3, characterised in that the second electrode comprises a metal.
5. Method according to any of claims 1 to 4, characterised in that the voltage is 1 to 20 V.
6. Method according to any of claims 1 to 5, characterised in that the functionalised material is dried and dispersed after the separation.