METHOD FOR PRODUCING AN ADHESIVE-FREE WOUND CONTACT COMPOSITE MATERIAL

DE502018015273D1Active Publication Date: 2024-11-14COVESTRO DEUTSCHLAND AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502018015273
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-02-16
Filing Date
2018-02-13
Publication Date
2024-11-14
Estimated Expiration
2038-02-13
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing a composite material for wound dressings, comprising the steps of (I) providing a first film, (II) mixing an NCO-terminated polyurethane prepolymer with at least water to obtain a polyurethane prepolymer-water mixture, (III) applying the polyurethane prepolymer-water mixture to at least a portion of the first film surface to form a layer, (IV) covering at least a portion of the second layer surface of the still liquid layer with a further film, wherein the adhesive strength between the first film and the layer and between the layer and the further film is in each case greater than the breaking stress of the layer,wherein the composite material between the first film and the layer and between the further film and the layer does not contain any further material, and wherein the first film and / or the further film contains a material selected from the group consisting of a thermoplastic polyurethane, a polyurethane or a mixture thereof.

[0002] The prior art describes composite materials for wound dressings that have an adhesive, for example in the form of an adhesive layer, between the films used and the foam layer, which serves to absorb fluid in the wound dressing. The material of the adhesive differs from that of the films or layer. This adhesive is required to ensure sufficient adhesion between the layer and the films. Applying this adhesive between the films and the layer requires separate production steps during the composite material production. This results in additional time, material, and cost expenditure, as well as increased complexity in the construction of the composite material.

[0003] EP 0 097 517 discloses a wound dressing consisting of a laminate of a deformable hydrophilic foam between two layers of deformable meshes. The meshes are preferably formed from a thermoplastic polyurethane. Preferred hydrophilic foams are hydrophilic polyurethane foams.

[0004] An object of the present invention is to at least partially improve at least some of the disadvantages of the prior art.

[0005] It is a further object of the invention to provide a method for producing a composite material which is as cost- and time-saving as possible and has as few process steps as possible.

[0006] At least one of the objects is achieved by a method for producing a composite material according to the subject matter of claim 1. Particular embodiments are described in the dependent claims.

[0007] The invention relates to a method for producing a composite material for wound dressings, comprising the steps: (I) Providing a first film having a first film surface and a second film surface running almost parallel to the first film surface; (II) Mixing an NCO-terminated polyurethane prepolymer with at least water to obtain a polyurethane prepolymer-water mixture; (III) Applying the polyurethane prepolymer-water mixture to at least a portion of the first film surface to form a layer, wherein the layer has a first layer surface that is in contact with the first film over at least a portion of the first film surface and has a second layer surface that runs almost parallel to the first layer surface; (IV) Covering at least a portion of the second layer surface of the still-liquid layer with at least one further film surface of a further film to obtain the composite material; wherein the adhesive force between the first film and the layer and between the layer and the further film is in each case greater than the breaking stress of the layer, so that when an attempt is made to peel a film off the layer, the layer tears, and wherein the composite material between the first film and the layer and between the further film and the layer has no further material and wherein the first film and / or the further film contains a material selected from the group consisting of a thermoplastic polyurethane, a polyurethane or a mixture thereof.

[0008] According to the invention, the adhesive strength is higher than the breaking stress of the layer if the layer cannot be separated from the first or the further film without leaving residue. This means that when the first or the further film is separated from the layer, the layer suffers a cohesive failure and not an adhesive failure in which the adhesive strength would be lower than the breaking stress of the layer. In contrast to an adhesive failure, which would represent a separation of the bond at the adhesive surface between the respective film and the layer and would enable a residue-free separation of the films from the layer, the cohesive failure occurs inside the layer and leaves residues of the layer material on the respective film to be separated.

[0009] In the process according to the invention, no further material is applied to the first film, the layer or the further film between steps (I) and (IV) in such a way that further material would be located between the layer and the films. The composite material as produced in the process according to the invention contains no further adhesive-containing materials between the materials provided and processed in steps (I) to (IV). According to the invention, the materials for the first film and the further film are selected such that the adhesive strength between the films and the layer is greater than the breaking stress of the layer. The adhesive strength is preferably in a range from 10 to 500%, or preferably in a range from 20 to 450%, or preferably in a range from 50 to 400%, or preferably in a range from 100 to 300% greater than the breaking stress of the layer.

[0010] Preferably, after application and covering in steps (III) and (IV), the layer formed has sufficient adhesive strength between the first film and the layer as well as between the layer and the further film to hold the composite together even under load.

[0011] In the context of the invention, sufficient adhesive strength or an adhesive strength between the films and the layer that is greater than the breaking stress of the layer means that when an attempt is made to peel at least one of the two films, such as the first film or the further film, from the layer, a visible or tangible residue of material from the layer remains or remains behind on at least part of the first film surface of the first film or the further film surface of the further film. As a result, when an attempt is made to separate at least one of the films from the layer, a cohesive failure occurs in the layer. When attempting to separate at least one of the films from the layer, it is not possible to peel the films from the layer without leaving any residue. Regardless of the force required to tear the composite apart, the adhesive strength is always greater than the breaking stress of the foam.The ultimate stress is the maximum force, for example, in the form of mechanical stress, that the material can withstand before breaking. It is expressed as force per cross-sectional area. The ultimate stress of the layer, measured according to DIN EN ISO 527-2, is preferably at least 0.04 MPa.

[0012] Preferably, the adhesive strength of the layer to the films is sufficient to hold the composite together for application in a wound material for its usual use in the medical or wound care environment. The cohesion of the composite means that disassembly or pulling apart of the composite material into its original minimum components such as the first film, the layer and the further film is not possible without destroying the composite material, in particular the layer material. As a result, the minimum components cannot be returned as originally used without residues of the layer material being left on at least one of the films. Thus, an attempt to peel the first or the further film from the layer would result in the first or further films having parts of the layer on their surface.Furthermore, after the composite has been produced according to the method of the invention, the layer preferably exhibits no adhesive strength to other materials that are subsequently brought into contact with it. Preferably, the breaking stress of the first and / or the further film is greater than the breaking stress of the layer. Preferably, the breaking stress of the first and / or the further film is greater than the adhesive strength between the respective film and the layer.

[0013] Even if the composite material itself is constructed without adhesive within the composite, a further material, such as a third film, can be glued to the composite via an adhesive layer on the outside of the composite, i.e. on the surface of the first film or the further film, which is arranged facing away from the layer.

[0014] The first film can be provided in any manner that a person skilled in the art would choose. Preferably, provision in step (I) is carried out using a roll-to-roll process. However, it is also conceivable for cut films to be provided on a preferably flat surface that is at least as large as the first film. Preferably, the first and / or the further film has cutouts, preferably in the form of holes.

[0015] The mixing in step (II) can be carried out in any manner that a person skilled in the art would select for this purpose. Mixing in step (II) is preferably carried out using a two-component low-pressure mixing unit with a dynamic, static-dynamic, or static stirrer, or a stirrer selected from the group consisting of a magnetic stirrer, a laboratory dissolver, a Dispermat, or another device suitable for mixing liquids known to a person skilled in the art. The polyurethane prepolymer-water mixture is preferably prepared in an amount of 0.1 l to 10,000 l in step (II). The polyurethane prepolymer-water mixture is preferably prepared by combining at least one NCO-terminated polyurethane prepolymer and water. The NCO-terminated polyurethane prepolymer and water react to form urea groups and release CO2, thus obtaining a polyurethane foam. The prepolymer is usually in liquid form.

[0016] The NCO-terminated polyurethane prepolymer is preferably obtainable from the reaction of a reaction mixture comprising a polyisocyanate and a polyol. The polyisocyanate preferably has an NCO functionality in a range from >1.5 to 6, or preferably from 1.8 to 5, or preferably from 2 to 4, in particular from 2. Suitable polyisocyanates are aliphatic, aromatic, araliphatic, or cycloaliphatic polyisocyanates.Examples of such suitable polyisocyanates are 1,4-butylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 2,2,4- and / or 2,4,4-trimethylhexamethylene diisocyanate, the isomeric bis-(4,4'-isocyanatocyclohexyl)methanes or their mixtures of any isomer content, 1,4-cyclohexylene diisocyanate, 4-isocyanatomethyl-1,8-octane diisocyanate (nonane triisocyanate), 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate, 1,5-naphthylene diisocyanate, 2,2'- and / or 2,4'- and / or 4,4'-diphenylmethane diisocyanate, 1,3- and / or 1,4-bis-(2-isocyanato-prop-2-yl)-benzene (TMXDI), 1,3-bis(isocyanato-methyl)benzene (XDI) and alkyl-2,6-diisocyanatohexanoates (lysine diisocyanates) with C1-C8 alkyl groups.

[0017] The polyisocyanate is preferably an aliphatic polyisocyanate. Preferred aliphatic diisocyanates are hexamethylene diisocyanate and isophorone diisocyanate, as well as mixtures thereof.

[0018] The polyol preferably has an OH functionality of >1.5 to 6, or preferably from 1.8 to 5, or preferably from 2 to 4, in particular from 3. The polyol is preferably selected from the group consisting of a polyether polyol, a polycarbonate polyol, a polyether polycarbonate polyol, a polyester polyol, or a mixture of at least two thereof. The polyol is preferably a polyether polyol. The polyol preferably comprises a polyol containing polyoxyethylene groups. With regard to the polyols, copolymers of ethylene oxide and propylene oxide with an ethylene oxide content, based on the total amount of oxyalkylene groups present, of 60 to 85 mol% are preferred.

[0019] Alternatively, both water or an aqueous mixture can be added to the prepolymer or a prepolymer mixture, or conversely, the prepolymer or the prepolymer mixture can be added to water or the aqueous mixture. It is also possible to combine two material streams (prepolymer / prepolymer mixture and water / aqueous mixture) in one mixing element.

[0020] Preferably, step (II) is further carried out in the presence of a base. The base preferably has a pK b value of > 6, more preferably > 7. A CO2-releasing base such as bicarbonate is particularly preferred.

[0021] The application in step (III) can be carried out in any manner that a person skilled in the art would select for this purpose. Preferably, the application in step (III) is selected from the group consisting of pouring, coating, whereby preferably any type of coating is suitable, contactless printing, screen printing, application by means of a brush, spraying, or a combination of at least two thereof. Preferably, the application is carried out by means of an applicator in a coating process, preferably a roller coating process or a doctor blade coating process. The doctor blade as applicator is preferably selected from a metal doctor blade, a wooden doctor blade, a plastic doctor blade, a rubber doctor blade, or a combination of at least two thereof. Instead of a doctor blade, one or more rollers or rolls can also be used as an applicator.The gap between the film to be coated and the applicator, such as the doctor blade gap or the gap between the roller and the first film, preferably has a thickness in a range from 100 µm to 1 cm, or preferably in a range from 250 µm to 5 mm. The applicator, for example the doctor blade or the roller, is preferably moved at a speed in a range from 0.1 to 30 m / min, or preferably in a range from 1 to 20 m / min, or preferably in a range from 2 to 10 m / min, or when using a stationary applicator such as a doctor blade or roller, the web is moved under the doctor blade or roller at a speed in the previously specified speed ranges. The elimination of CO2 after mixing the polyurethane prepolymer water mixture in step (II) produces the layer from the applied mixture in step (III), preferably in the form of an open-cell foam.The polyurethane prepolymer-water mixture preferably has a density in a range from 900 g / l to 1200 g / l, or preferably in a range from 950 g / l to 1150 g / l, or preferably in a range from 1000 to 1100 g / l. The layer in the form of a foam preferably has an average pore size in a range from 100 to 700 µm, preferably in a range from 120 to 400 µm, or preferably in a range from 150 to 250 µm. The resulting layer in the form of the foam preferably has a lower density than the polyurethane prepolymer-water mixture during its production. Preferably, the layer has a density which is in a range of 3 to 10 times, or preferably in a range of 3.5 to 9.5 times, or preferably in a range of 4 to 9 times greater than the density of the polyurethane prepolymer-water mixture.Preferably, the layer has a density in a range of 90 g / l to 350 g / l, or preferably in a range of 100 g / l to 280 g / l, or preferably in a range of 110 to 180 g / l.

[0022] Covering at least part of the second layer surface of the still-liquid layer with another film in step (IV) is preferably carried out by a method selected from the group consisting of deposition, lamination, or a combination thereof. Preferably, the additional film is deposited from roll to roll onto the still-liquid layer formed in step (III).

[0023] The first film and / or the further film contain a material selected from the group consisting of a thermoplastic polyurethane, a polyurethane or a mixture thereof.

[0024] The first film preferably comprises a material capable of building up an adhesive force to the layer that is greater than the breaking elongation of the layer. The first film preferably comprises a material capable of building up an adhesive force between the layer and the first film that is above 0.5 N / 20 mm, or preferably above 1 N / 20 mm, or preferably above 2 N / 20 mm, or preferably in a range from 0.5 N / 20 mm to 30 N / 20 mm, or preferably in a range from 1 N / 20 mm to 25 N / 20 mm, or preferably in a range from 2 N / 20 mm to 15 N / 20 mm.

[0025] The first film preferably has a total surface area in a range from 1 cm 2 to 1000 m 2 , or preferably in a range from 10 cm 2 to 500 m 2 , or preferably in a range from 50 cm 2 to 100 m 2 , with possible recesses being included in the calculation or measurement of the total surface area of ​​the first film. The recesses in the film preferably occupy an area in a range from 5 to 50%, or preferably in a range from 10 to 45%, or preferably from 15 to 40% of the total surface area of ​​the first film.

[0026] Preferably, the proportions of the materials for the further film are the same as stated for the first film. Furthermore, the total area of ​​the further film is preferably in the same range as stated for the first film. In a preferred embodiment of the process according to the invention, at least steps (III) and (IV) taken together, preferably steps (II) to (IV) taken together, are carried out in a period of less than 120 seconds, preferably less than 90 seconds, or preferably less than 60 seconds or preferably less than 40 seconds. Preferably, no more than 120 seconds, preferably no more than 90 seconds, or preferably no more than 60 seconds or preferably no more than 40 seconds elapse between stirring the polyurethane-water mixture in step (II) and applying this mixture to the first film in step (III).Preferably, no more than 120 seconds, preferably no more than 90 seconds, or preferably no more than 60 seconds or preferably no more than 40 seconds elapse between the mixing of the polyurethane-water mixture in step (II) and the application of the further film in step (IV) to the polyurethane-water mixture applied to the first film in step (III).

[0027] In the process according to the invention, the composite material comprises no further material between the first film and the layer, nor between the further film and the layer. However, as already mentioned, the composite material may comprise further materials, such as adhesives, on its outer surface, i.e., on a surface of the first film or the further film that is not connected to the layer.

[0028] Preferably, the polyurethane prepolymer-water mixture is applied in step (III), preferably in the form of a wet layer, with a wet layer thickness determined by the doctor blade gap in a range from 50 to 5000 µm, preferably in a range from 100 to 3000 µm, or preferably in a range from 300 to 2000 µm. The wet layer is preferably covered by the further film within 1 to 90 seconds, or preferably from 2 to 80 seconds, or preferably within 5 to 60 seconds. The wet layer cures preferably within 1 to 10 minutes, preferably within 2 to 8 minutes, or preferably within 3 to 6 minutes to at least 50%, or preferably to at least 60%, or preferably to at least 70%, based on the total amount of liquid that escapes during the entire curing process.

[0029] In a preferred embodiment of the process according to the invention, the layer has a thickness after curing that is 1.5 to 30 times, or preferably 2 to 10 times, or preferably 2.5 to 5 times greater than the thickness upon application of the polyurethane prepolymer-water mixture in step (III). Preferably, the layer after curing has a thickness in a range from 70 µm to 10 cm, or preferably in a range from 100 µm to 5 cm, or preferably in a range from 200 µm to 10 cm, or preferably in a range from 500 µm to 1 cm.

[0030] In a preferred embodiment of the process according to the invention, the NCO-terminated polyurethane prepolymer has a weight fraction of low molecular weight, aliphatic diisocyanates with a molecular weight of ≥ 140 to ≤ 278 g / mol of ≤ 1.0 wt.%, based on the prepolymer, and is obtainable as component A) by reacting A1) low molecular weight, aliphatic diisocyanates with a molecular weight of ≥ 140 to ≤ 278 g / mol with A2) di- to hexafunctional polyalkylene oxides with an OH number of ≥ 22.5 to ≤ 112 mg KOH / g and an ethylene oxide content of ≥ 50 to ≤ 100 mol%, based on the total amount of the oxyalkylene groups contained.

[0031] The NCO-terminated polyurethane prepolymer is preferably obtainable from the reaction of a reaction mixture comprising a low-molecular-weight, aliphatic diisocyanate and a polyol containing polyoxyethylene groups. With regard to the low-molecular-weight, aliphatic diisocyanates, hexamethylene diisocyanate and isophorone diisocyanate, as well as mixtures thereof, are preferred. With regard to the polyols, copolymers of ethylene oxide and propylene oxide with an ethylene oxide content, based on the total amount of oxyalkylene groups present, of 60 to 85 mol% are preferred.

[0032] Preferably, the NCO-terminated polyurethane prepolymer further comprises: H1) one or more low molecular weight, aliphatic diisocyanates having a molar mass of ≥ 140 to ≤ 278 g / mol, preferably ≥ 168 to ≤ 258 g / mol and / or polyisocyanates preparable therefrom having an isocyanate functionality of ≥ 2 to ≤ 6; and / or H2) one or more monofunctional polyalkylene oxides having an OH number of ≥ 10 to ≤ 250 and an ethylene oxide content of ≥ 50 to ≤ 100 mol%, based on the total amount of oxyalkylene groups present; and / or a hydrophilic isocyanate component obtainable by reacting components mentioned under H1) with components mentioned under H2).

[0033] The NCO-terminated polyurethane prepolymer preferably comprises: A) isocyanate-functional prepolymers with a weight fraction of low molecular weight, aliphatic diisocyanates with a molecular weight of ≥ 140 to ≤ 278 g / mol, preferably ≥ 168 to ≤ 258 g / mol of ≤ 1.0 wt.% based on the prepolymer, obtainable by reacting A1) low molecular weight, aliphatic diisocyanates with a molecular weight of ≥ 140 to ≤ 278 g / mol, preferably > 168 to ≤ 258 g / mol with A2) di- to hexafunctional polyalkylene oxides with an OH number of ≥ 22.5 to ≤ 112 mg KOH / g and an ethylene oxide content of ≥ 50 to ≤ 100 mol%, based on the total amount of the oxyalkylene groups present, B) optionally heterocyclic, 4-ring or 6-ring oligomers of low molecular weight, aliphatic diisocyanates with a molecular weight of ≥ 140 to ≤ 278 g / mol, preferably ≥ 168 to ≤ 258 g / mol, D) optionally catalysts, E) optionally alkali metal salts of weak inorganic acids, F) optionally surfactants, G) optionally mono- or polyhydric alcohols,H) the following components: H1) one or more low molecular weight, aliphatic diisocyanates with a molecular weight of ≥ 140 to ≤ 278 g / mol, preferably ≥ 168 to ≤ 258 g / mol and / or polyisocyanates preparable therefrom with an isocyanate functionality of ≥ 2 to ≤ 6; and / or H2) one or more monofunctional polyalkylene oxides with an OH number of ≥ 10 to ≤ 250 and an ethylene oxide content of ≥ 50 to ≤ 100 mol%, based on the total amount of oxyalkylene groups present; and / or a hydrophilic isocyanate component obtainable by reacting components mentioned under H1) with components mentioned under H2).

[0034] The prepolymers A) used preferably have a residual monomer content (monomers correspond to low-molecular-weight, aliphatic diisocyanates) of less than 0.5 wt.% based on the prepolymer. This content can be achieved by appropriately selecting the amounts of diisocyanates A1) and polyalkylene oxides A2). However, it is preferred to use excess diisocyanate A1) and subsequently remove unreacted monomers, preferably by distillation.

[0035] In the preparation of the isocyanate-functional prepolymers A), the ratio of the polyalkylene oxides A2) to the low molecular weight, aliphatic diisocyanates A1) is typically adjusted so that 1 mol of OH groups of the polyalkylene oxides A2) is present in 2 to 20 mol, preferably 2 to 10 mol and particularly preferably 5 to 10 mol of NCO groups of the low molecular weight, aliphatic diisocyanates A1).

[0036] The hydrophilic polyisocyanates mentioned under H) are typically prepared by reacting 1 mol of OH groups of the monofunctional polyalkylene oxide component H2) with 1.25 to 15 mol, preferably with 2 to 10 mol, and particularly preferably 2 to 6 mol, of NCO groups of a polyisocyanate H1) having an isocyanate functionality of 2 to 6, based on aliphatic diisocyanates. Examples of such polyisocyanates H1) are biuret structures, isocyanurates, or uretdiones based on aliphatic diisocyanates. The polyisocyanate H1) and the polyalkylene oxide H2) are preferably linked to one another via a urethane group or a urea group, respectively, with linkage via urethane groups being particularly preferred.

[0037] The NCO content of the isocyanate-functional prepolymers A) is preferably 1.5 to 4.5 wt.%, particularly preferably 1.5 to 3.5 wt.% and very particularly preferably 1.5 to 3.0 wt.%.

[0038] Examples of low-molecular-weight, aliphatic diisocyanates of component A1) are hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), butylene diisocyanate (BDI), bisisocyanatocyclohexylmethane (HMDI), 2,2,4-trimethylhexamethylene diisocyanate, bisisocyanatomethylcyclohexane, bisisocyanatomethyltricyclodecane, xylene diisocyanate, tetramethylxylylene diisocyanate, norbornane diisocyanate, cyclohexane diisocyanate, or diisocyanatododecane, with hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), butylene diisocyanate (BDI), and bis(isocyanatocyclohexyl)methane (HMDI) being preferred. Particular preference is given to BDI, HDI, and IPDI, with hexamethylene diisocyanate and isophorone diisocyanate being most preferred.

[0039] Polyalkylene oxides of component A2) are preferably copolymers of ethylene oxide and propylene oxide with an ethylene oxide content, based on the total amount of oxyalkylene groups present, of 50 to 100 mol%, preferably 60 to 85 mol%, initiated with polyols or amines. Suitable initiators of this type are glycerol, trimethylolpropane (TMP), sorbitol, pentaerythritol, triethanolamine, ammonia, or ethylenediamine.

[0040] The polyalkylene oxides of component A2) typically have number-average molecular weights of 1000 to 15000 g / mol, preferably of 3000 to 8500 g / mol.

[0041] Furthermore, the polyalkylene oxides of component A2) have OH functionalities of 2 to 6, preferably of 3 to 6, particularly preferably of 3 to 4.

[0042] Compounds of component B) which may optionally be used are heterocyclic, 4-ring or 6-ring oligomers of low molecular weight, aliphatic diisocyanates having a molecular weight of 140 to 278 g / mol, preferably ≥ 168 to ≤ 258 g / mol, such as isocyanurates, iminooxadiazinediones or uretdiones of the aforementioned low molecular weight, aliphatic diisocyanates.

[0043] If excess low-molecular-weight diisocyanate was used, the excess low-molecular-weight aliphatic diisocyanate is subsequently removed, preferably by thin-film distillation. Acidic or alkylating stabilizers such as benzoyl chloride, isophthaloyl chloride, methyl tosylate, chloropropionic acid, HCl, or antioxidants such as di-tert-butylcresol or tocopherol can be added before, during, and after the reaction or the distillative removal of the excess diisocyanate. The NCO content of the hydrophilic polyisocyanates H) is preferably 0.3 to 20 wt.%, more preferably 2 to 10 wt.%, and most preferably 3 to 6 wt.%.

[0044] To accelerate the formation of urea or urethane, catalysts can be used in component D). These are typically compounds familiar to those skilled in the art from polyurethane technology. Preferred compounds are those from the group consisting of catalytically active metal salts not included in component E), amines, amidines, and guanidines. Examples include tin dibutyl dilaurate (DBTL), tin acetate, 1,8-diazabicyclo[5.4.0]undecen-7 (DBU), 1,5-diazabicyclo[4.3.0]nonen-5 (DBN), 1,4-diazabicyclo[3.3.0]octen-4 (DBO), N-ethylmorpholine (NEM), triethylenediamine (DABCO), pentamethylguanidine (PMG), tetramethylguanidine (TMG), cyclotetramethylguanidine (TMGC), n-decyltetramethylguanidine (TMGD), n-dodecyltetramethylguanidine (TMGDO), dimethylaminoethyltetramethylguanidine (TMGN), 1,1,4,4,5,5-hexamethylisobiguanidine (HMIB), phenyltetramethylguanidine (TMGP) and hexamethyleneoctamethylbiguanidine (HOBG).

[0045] Preference is given to using amines, amidines, guanidines or mixtures thereof as catalysts of component D). Preference is also given to using 1,8-diazabicyclo[5.4.0]undecene-7 (DBU).

[0046] However, catalysts of component D) can also be omitted; this is preferred.

[0047] Component E) uses alkali metal salts of weak inorganic acids. These are alkali metal salts of inorganic acids whose corresponding free acids have a pKa value of > 4.0 in water at 25 °C. Examples of particularly suitable alkali metal salts of weak inorganic acids are potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, and sodium bicarbonate, including any mixtures of these salts.

[0048] To improve foam formation, foam stability, or the properties of the resulting polyurethane foam, compounds of component F) can be used. Such additives can, in principle, be any known anionic, cationic, amphoteric, and nonionic surfactants, as well as mixtures thereof. Preference is given to using alkyl polyglycosides, EO / PO block copolymers, alkyl or aryl alkoxylates, siloxane alkoxylates, esters of sulfosuccinic acid, and / or alkali or alkaline earth metal alkanoates. Particular preference is given to using EO / PO block copolymers. Preferably, the EO / PO block copolymers alone are used as component F).

[0049] In addition, compounds of component G) can be used to improve certain foam properties of the resulting polyurethane foam. These are, in principle, all mono- and polyhydric alcohols known to the person skilled in the art, as well as mixtures thereof. These are mono- or polyhydric alcohols or polyols, such as ethanol, propanol, butanol, decanol, tridecanol, hexadecanol, ethylene glycol, neopentyl glycol, butanediol, hexanediol, decanediol, trimethylolpropane, glycerin, pentaerythritol, monofunctional polyether alcohols and polyester alcohols, polyetherdiols, and polyesterdiols.

[0050] In the preparation of the hydrophilic polyisocyanates listed under H), which, as mentioned, are used optionally, the ratio of the monofunctional polyalkylene oxides H2) to the low molecular weight, aliphatic diisocyanates H1) is preferably adjusted such that 1.25 to 15 mol, preferably 2 to 10 mol, and particularly preferably 2 to 6 mol of NCO groups of the low molecular weight, aliphatic diisocyanate H1) are present per 1 mol of OH groups of the monofunctional polyalkylene oxides. This is followed by allophanatization or biuretization and / or isocyanurate formation or uretdione formation. If the polyalkylene oxides H2) are bonded to the aliphatic diisocyanates H1) via urethane groups, allophanatization preferably takes place subsequently. Furthermore, it is preferred that isocyanurate structural units are formed.

[0051] The reaction can be carried out in the presence of urethanization catalysts such as tin compounds, zinc compounds, amines, guanidines or amidines, or in the presence of allophanatization catalysts such as zinc compounds.

[0052] The reaction of the components for the preparation of the hydrophilic polyisocyanates listed under H) typically takes place at 25 to 140 °C, preferably 60 to 100 °C.

[0053] However, catalysts can also be omitted in the preparation of H); this is preferred.

[0054] Examples of low-molecular-weight, aliphatic diisocyanates of component H1) are hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), butylene diisocyanate (BDI), bisisocyanatocyclohexylmethane (HMDI), 2,2,4-trimethylhexamethylene diisocyanate, bisisocyanatomethylcyclohexane, bisisocyanatomethyltricyclodecane, xylene diisocyanate, tetramethylxylylene diisocyanate, norbornane diisocyanate, cyclohexane diisocyanate, or diisocyanatododecane, with hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), butylene diisocyanate (BDI), and bis(isocyanatocyclohexyl)methane (HMDI) being preferred. Particular preference is given to BDI, HDI, and IPDI, and very particular preference is given to hexamethylene diisocyanate and isophorone diisocyanate.Examples of higher molecular weight polyisocyanates H2) are polyisocyanates with an isocyanate functionality of 2 to 6 with isocyanurate, urethane, allophanate, biuret, iminooxadiazinetrione, oxadiazinetrione and / or uretdione groups based on the aliphatic and / or cycloaliphatic diisocyanates mentioned in the previous section.

[0055] Higher molecular weight compounds containing biuret, iminooxadiazinedione, isocyanurate, and / or uretdione groups based on hexamethylene diisocyanate, isophorone diisocyanate, and / or 4,4'-diisocyanatodicyclohexylmethane are preferably used as component H1). Isocyanurates are further preferred. Structures based on hexamethylene diisocyanate are most preferred.

[0056] The monofunctional polyalkylene oxides H2) have an OH number of 15 to 250, preferably 28 to 112, and an ethylene oxide content of 50 to 100 mol%, preferably 60 to 100 mol%, based on the total amount of oxyalkylene groups contained.

[0057] Monofunctional polyalkylene oxides in the sense of the invention are understood to mean compounds which have only one isocyanate-reactive group, i.e. a group which can react with an NCO group.

[0058] The preparation of polyalkylene oxides (H2) by alkoxylation of suitable starter molecules is known from the literature (e.g., Ullmann's Encyclopedia of Industrial Chemistry, 4th edition, Volume 19, Verlag Chemie, Weinheim, pp. 31-38). Suitable starter molecules are, in particular, saturated monoalcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, diethylene glycol monobutyl ether, as well as aromatic alcohols such as phenol or monoamines such as diethylamine. Preferred starter molecules are saturated monoalcohols of the type mentioned above. Particular preference is given to using diethylene glycol monobutyl ether or n-butanol as starter molecules. The monofunctional polyalkylene oxides (H2) typically have number-average molecular weights of 220 to 3700 g / mol, preferably of 500 to 2800 g / mol.

[0059] The monofunctional polyalkylene oxides H2) preferably have an OH group as isocyanate-reactive group.

[0060] Typically, components A) to H) are used in the following amounts (for reaction with 0.1 to 200 parts by weight of water in step (II) of the process according to the invention): 100 parts by weight of isocyanate-functional prepolymers A) 0 to 30 parts by weight of heterocyclic oligomers B) 0 to 1 part by weight of catalysts D) 0 to 5 parts by weight of alkali metal salts of weak inorganic acids E) 0 to 10 parts by weight of surfactants F) 0 to 20 parts by weight of alcohols G) 0 to 250 parts by weight of one or more of the components mentioned under H).

[0061] Components A) to H) are preferably used in the following amounts (for reaction with 0.1 to 100 parts by weight of water): 100 parts by weight of isocyanate-functional prepolymers A) 1 to 30 parts by weight of heterocyclic oligomers B) 0 to 1 part by weight of catalysts D) 0.01 to 5 parts by weight of alkali metal salts of weak inorganic acids E) 0 to 5 parts by weight of surfactants F) 0 to 10 parts by weight of alcohols G) 10 to 100 parts by weight of one or more of the components mentioned under H).

[0062] Components A) to H) are particularly preferably used in the following amounts (for reaction with 1 to 60 parts by weight of water): 100 parts by weight of isocyanate-functional prepolymers A) 5 to 15 parts by weight of heterocyclic oligomers B) 0 to 0.5 parts by weight of catalysts D) 0.1 to 1 part by weight of alkali metal salts of weak inorganic acids E) 0 parts by weight of surfactants F) 0 parts by weight of alcohols G) 20 to 80 parts by weight of one or more of the components mentioned under H).

[0063] In a preferred embodiment of the process according to the invention, component A1) is selected from the group consisting of hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate) or a mixture of at least two thereof.

[0064] In a preferred embodiment of the method according to the invention, the layer has at least one of the following properties: i. A water vapor transmission rate (MVTR) of ≥ 1500 g / m 2 < / 24h, preferably > 2500 g / m 2 < / 24h; ii. A retention (determined using a 6 kg weight for 20 seconds) of at least 25%, preferably at least 35% (g / g), based on maximum absorption according to DIN EN 13726-1:2002, Part 3.2 / 3.3; iii. A thickness of at least 0.1 mm, preferably in a range from 0.1 to 50 mm, or preferably in a range from 1 to 25 mm, or preferably in a range from 1.5 to 15 mm; iv. A density in a range from 70 to 200 g / l, preferably in a range from 80 to 170 g / l, or preferably in a range from 100 to 150 g / l.

[0065] In the method according to the invention, the first film and / or the further film comprises a material selected from the group consisting of a thermoplastic polyurethane, a polyurethane, or a mixture thereof. The material of the first and / or the further film and / or an optional third film preferably differs from the material of the layer by at least one property, preferably selected from the group consisting of a higher density, a lower water vapor permeability, a lower elongation at break, a lower thickness, or a combination of at least two thereof.

[0066] In a preferred embodiment of the method according to the invention, the first film and / or the further film has at least one of the following properties: EF1 EF1 A thickness in a range of 15 to 75 µm, or preferably in a range of 20 to 50 µm, or preferably in a range of 25 to 45 µm; EF2 A water vapor permeability of ≥ 1000 g / dm 2< , or preferably of ≥1500 g / dm 2< , or preferably in a range of 1000 to 20000 g / dm 2< , or preferably in a range of 1500 to 10000 g / dm 2< (determined according to DIN 13726-2:2002, Part 3.2); EF3 An elongation at break of ≥ 200%, preferably ≥ 400%, or preferably in a range of 200 to 4000%, or preferably in a range of 500 to 3000% (determined according to DIN EN ISO 527-2); EF4 Contains recesses which preferably amount to at least 3%, or preferably at least 5%, or preferably at least 10%, or preferably in a range of 3 to 30%, or preferably in a range of 5 to 25%, or preferably in a range of 10 to 20%, based on the total area of ​​the respective film; EF5 If a bacterial and viral barrier is required according to ASTM F1671 (American standard), the first or subsequent films should preferably have no cutouts.

[0067] Preferably, the first film and / or the further film has the features EF1 and EF2, or EF2 and EF3, or EF1 and EF4, or EF1 and EF5, or EF2 and EF3, or EF2 and EF4, or EF2 and EF5, or EF3 and EF4, or EF4 and EF5, or EF3 and EF4, or EF3 and EF5, or EF4 and EF5, or EF1 and EF2 and EF3, or EF1 and EF2 and EF4, or EF1 and EF2 and EF5, or EF1 and EF3 and EF4, or EF1 and EF3 and EF4, or EF1 and EF3 and EF5, or EF2 and EF3 and EF4, or EF2 and EF4 and EF5, or EF3 and EF4 and EF5, or EF1 and EF2 and EF3 and EF4, or EF1 and EF2 and EF3 and EF5, or EF1 and EF2 and EF4 and EF5, or EF1 and EF3 and EF4 and EF5, or EF2 and EF3 and EF4 and EF5, or EF1 and EF2 and EF3 and EF4 and EF5. Also preferred are films that have combinations of features, wherein feature EF4 does not occur together with feature EF5.

[0068] In a preferred embodiment of the method according to the invention, at least the first film and / or the further film has cutouts which have a diameter in a range from 1 to 8 mm, preferably from 1.5 to 7 mm, or preferably from 2 to 5 mm. The cutouts are preferably regularly distributed over the respective film. Preferably, the respective film with cutouts has a number of cutouts in a range from 1 to 10 cutouts per cm², or preferably in a range from 2 to 8 cutouts per cm², or preferably in a range from 3 to 7 per cm². The cutouts can have any shape that a person skilled in the art would select for this purpose. Preferably, the cutouts have a circular shape. Preferably, the cutouts are formed by punching out the corresponding area from the first film or the further film.

[0069] The layer of the composite material produced in the process according to the invention preferably contains a polyurethane that is formed from the NCO-terminated polyurethane prepolymer together with the water. In step (II), further NCO-terminated polyurethane prepolymers can preferably be produced simultaneously or sequentially and applied simultaneously or sequentially to the first film in step (III). After application in step (III), the at least one prepolymer-water mixture forms the layer that contains at least one layer containing a polyurethane. If more than one layer of a polyurethane-prepolymer-water mixture is applied to the first film, the at least two layers have either the same or different polyurethanes, i.e. at least one first polyurethane and optionally at least one further polyurethane after curing of the mixture.The at least one further polyurethane preferably has at least one different property, preferably selected from the group consisting of water vapor permeability, thickness, retention, and density, compared to the first polyurethane. Preferably, at least one of the aforementioned properties of the first polyurethane differs from the further polyurethane by at least 10% of the respective value of the property of the first polyurethane.

[0070] According to the invention, after application in step (III), no additional material other than the polyurethane applied in step (III) is located between the first film and the layer. According to the invention, after application in step (III), no further material other than the polyurethane applied in step (III) is located between the layer and the further film. According to the invention, after application in step (III), no further material other than the polyurethane applied in step (III) is located between the layer and the first film or between the layer and the further film. In the context of the invention, the feature that the composite material has no additional material between the layer and the films is understood to mean that, apart from the materials used to form the first film under I., the layer under II. and the further film under III.No further or additional materials are used that are arranged between the first film and the layer, or between the layer and the further film, and preferably contribute to the bonding of the films to the layer. However, there may be further layers inside the composite material that do not contain polyurethane. However, these further layers do not come into direct contact with the first or the further film.

[0071] In a preferred embodiment of the method according to the invention, the wound dressing has at least one of the following properties: WA1. A thickness in a range of 1 mm to 10 cm, preferably 1.2 mm to 2.5 cm, or preferably in a range of 1.4 to 10 mm; WA2. A swelling behavior upon absorption of water of less than 200 vol.%, preferably less than 180 vol.%, preferably less than 150 vol.%; WA3. An extension in each of the spatial directions lying in the plane corresponding to the largest surface area of ​​the wound dressing of < 50%, preferably < 35%, or preferably < 20%, based on the extension of the wound dressing in the third spatial direction, upon contact with a liquid; WA4. A combination of at least two of the properties WA1 to WA3, preferably the properties WA1 and WA2, or WA1 and WA3, or WA2 and WA3, or WA1 and WA2 and WA3. Methods:

[0072] Unless otherwise indicated, all percentages refer to the weight and total quantity or to the total weight of the compositions.

[0073] Unless otherwise stated, all analytical measurements refer to measurements at temperatures of 23 °C. Determination of the breaking stress;

[0074] The breaking stress was determined using DIN EN ISO 527-2. Thickness measurement:

[0075] The layer thickness is determined using a pneumatic probe and a display connected to the layer thickness output by DR. JOHANNES HEIDENHAIN GmbH, Germany (MT25P). Density measurement:

[0076] To determine the volume, a sample piece measuring 5 x 5 cm² (with rounded corners and a curve radius of 3 mm) is punched out using a punch. The height / thickness is measured from the average of a 5-fold determination using the method described above. To subsequently calculate the density, the mass of the sample piece is determined on a Mettler Toledo XS603S balance. Retention:

[0077] To determine retention, a 5 x 5 cm2 foam piece is lifted with tweezers after complete absorption, allowed to drain for 30 seconds, and weighed. The foam piece is then placed on a metal pedestal and weighted down with a 6 kg weight for 20 seconds. After removing the weight, the foam piece is weighed again, and the remaining moisture content is determined as a percentage of the maximum absorption. Determination of the MVTR (moisture vapor transmission rate)

[0078] The MVTR is determined based on DIN EN13726-2:2002 (Part 3.2). A metal cylinder is filled with water as described in the DIN standard and sealed at the top with the film or layer to be tested. The total weight (beaker with water and film) is then determined using a balance. The test setup is stored at 37°C for 24 hours, and the weight is again determined. The water loss evaporating through the film can be determined by subtraction. The MVTR is expressed in g / (m 2 < * 24 h) or g / m 2 < / 24 h. Determination of the maximum absorption capacity of water:

[0079] The maximum absorption capacity was determined according to DIN EN 13726-1:2002 Part 3.2 on a flat piece of foam measuring 5 * 5 cm2. Examples: Inventive production of an adhesive-free wound contact material (Example B 1)

[0080] 125 g of Baymedix FP505 were mixed with 25 g of an aqueous solution of 1.32 wt% sodium bicarbonate, 4.8 wt% Pluronic PE6800, and 0.4% citric acid monohydrate under vigorous stirring for 7 s using a stirrer with an anchor blade (Labordissolver green 037 from Pendraulik GmbH) at 930 rpm. The mixture was then applied to a PU film of type VPT9101 (Covestro Deutschland AG) using a doctor blade with a 1.5 mm gap in the xy direction. The surface of the reaction mixture, which extends in the xy direction, was then covered with another PU film of type VPT9101. The cover film has circular holes with a diameter of 4 mm and a distance of 5 mm between the hole centers, arranged in rows, with the rows offset from one another. After a waiting time of 30 minutes at the latest, the resulting composite according to the invention was ready to be used as a wound contact material.

[0081] The layer in the form of dry foam (8 mm thick) showed a maximum absorption of 1100%, a swelling of 30 vol% at an extension of 3 mm in the xy direction (starting from a 100 cm 2< measuring piece in the xy direction).

[0082] When attempting to separate the composite back into its original components, namely the two PU films of type VPT9101 and the foam, such a high force had to be applied due to the high adhesive strength between the PU films and the foam that the foam suffered a cohesive failure and consequently foam residues remained on the PU films. Comparison example (VB 1) Manufacture as in comparative example 1 except:

[0083] The reaction mixture was applied to a release paper of type Y 05200 from the Felix Schöller Group, Osnabrück and the covering was done using the release paper of the same type but in a needled variant: The dry foam (5 mm thick) showed a maximum absorption of 1500%, a swelling of 180 vol% and 40 mm in the xy direction (starting from a 100 cm 2< measuring piece in the xy direction).

[0084] When attempting to separate the composite back into its original components, namely the two release papers of type Y 05200 and the foam, the adhesive strength between the release papers and the foam was so low that it was easy to separate the release paper without leaving any residue of the foam, which is equivalent to an adhesive failure without the layer being destroyed or cracked. Figures

[0085] The following description of the figures shows the process for producing the composite material as well as the arrangement of the films and the layer in the composite material according to the invention. Figure 1: a schematic representation of the method according to the invention with steps (I) to (IV); Figure 2: a schematic representation of a composite material; Figure 3: a schematic representation of a wound dressing.

[0086] In Figure 1In step (I), corresponding to step (I) of the process according to the invention, the first film 100 is provided. This film 100 is preferably a polyurethane film with a thickness of 20 to 50 µm. The first film 100 has a first film surface 102 and a second film surface 104 opposite the first film surface 102. In step (II), corresponding to step (II) of the process according to the invention, an NCO-terminated polyurethane prepolymer is mixed with water in a mixer 106 to obtain a polyurethane prepolymer-water mixture 110. The weight ratio of the NCO-terminated polyurethane prepolymer to water is between 100:10 and 100:50, preferably 100:20. The mixture 110 is applied in step (III), corresponding to step (III) of the process according to the invention, using a steel doctor blade (Film Applicator System Wasag Model 288 from ERICHSEN GmbH & Co.KG, Germany, with a doctor blade gap height of 1.5 mm) to the first film surface 102 of the provided film 100 in a wet film thickness of 1500 µm. Within a few seconds to a few minutes, a layer 200 of the mixture 110 forms on the film 100. Before the layer 200 is completely foamed, in step (IV), corresponding to step (IV) of the method according to the invention, a further film 120 with its further film surface 130 is applied to the layer 200. This is preferably carried out via a roll-to-roll process directly after the application of the mixture 110 to the first film 100, which is also provided in the form of a roll-to-roll arrangement. The film 120 is preferably applied immediately, i.e., as quickly as technically possible, after the application of the reaction mixture 200.In this example, the film 120 is applied to the mixture 110 applied in step (III) within a few seconds, preferably within a period of 1 to 90 seconds, or preferably within a period of 2 to 60 seconds. The composite 10 formed in step (IV) corresponds to a composite material 10 according to the invention, which can be further processed into a wound dressing 20.

[0087] In Figure 2A composite material 10 is shown schematically. The composite material 10 is constructed from a first film 100, which is connected via a first film surface 102 to a layer 200 via its first layer surface 202. On the second layer surface 204 of the layer 200, located on the first layer surface 202, the layer is connected to a further film 120. The first film 100, which in this case is designed to come into contact with the skin of the user and thus with the wound, can preferably have recesses 108 (as in Figure 3shown) in the first film 100, but also in the further film 120 (not shown here). However, preferably only the film which is designed to come into contact with the skin has recesses 108. The roughness of the films 100 and 120 can differ greatly on the inward-facing (102, 130) and outward-facing film surfaces (104, 140). Furthermore, the composite 10 can have a bacterial and / or viral barrier. This can be achieved either by at least one of the films 100 and / or 120 being designed as such a barrier with properties according to ASTM F1671, or by the foam 200 containing active ingredients which enable such a barrier.

[0088] Figure 3 shows schematically a wound dressing 20 containing the composite material 10, which as in Figure 2 described and as described in Figure 1described. In addition to the composite material 10, the wound dressing 20 optionally has an additional material 300, preferably in the form of a third film, on the film surface 104 of the further film 120 opposite the layer 200. This additional material 300, or the third film 300, serves primarily to protect the composite material 10 against external influences. The third film preferably protects the composite material 10 from tearing or tearing when the wound dressing 20 is in use. Optionally or alternatively, the thickness of the further film 120 can also be adjusted, i.e. preferably increased, so that rapid tearing under high stress is avoided. However, due to the choice of material for the additional material 300, an undesirable thickness of the composite material 10 can also be avoided.Recesses 108 have been incorporated into the first film 100, which in this case comes into contact with the user's skin and thus with the wound.

Claims

1. Method for producing a composite material (10) for wound dressings (20), comprising the following steps: (I) providing a first film (100), having a first film surface (102) and a second film surface (104) running virtually parallel to the first film surface (102); (II) mixing an NCO-terminated polyurethane prepolymer with at least water to give a polyurethane prepolymer / water mixture (110), (III) applying the polyurethane prepolymer / water mixture to at least one part of the first film surface (102) to form a layer (200), the layer (200) having a first layer surface (202) which is in contact with the first film (100) via at least one part of the first film surface (102), and having a second layer surface (204) which runs virtually parallel to the first layer surface (202) ; (IV) covering at least one part of the second layer surface (204) of the still-liquid layer (200) with at least one part of a further film surface of a further film (120) to give the composite material (10), wherein the bond strength between the first film (100) and the layer (200) and also between the layer (200) and the further film (120) is greater in each case than the tensile strain at break of the layer (200), wherein the composite material (10) has no further material between the first film (100) and the layer (200) and also between the further film (120) and the layer (200), and wherein the first film (100) and / or the further film (120) comprises a material selected from the group consisting of a thermoplastic polyurethane, a polyurethane or a mixture thereof.

2. Method according to Claim 1, wherein the further film (120) is preferably deposited from roll to roll onto the still-liquid layer (200) in step (IV).

3. Method according to Claim 1 or 2, wherein at least steps (III) and (IV) take place within a period of less than 120 seconds.

4. Method according to any of the preceding claims, wherein the layer (200) has a thickness after curing which is greater by 1.5 to 30 times than the thickness on application of the polyurethane prepolymer / water mixture in step (III).

5. Method according to any of the preceding claims, wherein the NCO-terminated polyurethane prepolymer has a weight fraction of low molecular mass, aliphatic diisocyanates having a molar mass of ≥ 140 to ≤ 278 g / mol of ≤ 1.0 wt%, based on the prepolymer, and is obtainable as component A) by reaction of A1) low molecular mass, aliphatic diisocyanates with a molar mass of ≥ 140 to ≤ 278 g / mol with A2) di- to hexa-functional polyalkylene oxides with an OH number of ≥ 22.5 to ≤ 112 mg KOH / g and an ethylene oxide fraction of ≥ 50 to ≤ 100 mol%, based on the total amount of the oxyalkylene groups present.

6. Method according to the preceding claim, wherein component A1) is selected from the group consisting of hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate) or a mixture of at least two thereof.

7. Method according to any of the preceding claims, wherein the layer (200) has at least one of the following properties: i. a water vapour transmissibility (MVTR) of ≥ 1500 g / m2 / 24h, ii. a retention (determined using a 6 kg weight over 20 seconds) of at least 25% (g / g), based on maximum absorption, iii. a thickness of at least 0.1 mm, iv. a density in a range from 70 to 200 g / l.

8. Method according to any of the preceding claims, wherein the first film (100) and / or the further film (120) have / has at least one of the following properties: EF1 a thickness in a range from 15 to 75 µm; EF2 a water vapour transmissibility of ≥ 1000 g / m2 / 24h; EF3 an elongation at break of ≥ 200%, preferably ≥ 500% elongation at break; EF4 contains apertures (108) which make up preferably at least 3%, based on the total area of the respective film (100, 120); EF5 exhibit a bacterial barrier and viral barrier in accordance with ASTM F1671.

9. Method according to any of the preceding claims, wherein at least the first film (100) and / or the further film (120) have / has apertures (108) which have a diameter in a range from 2 to 10 mm.

10. Method according to any of the preceding claims, wherein the wound dressing has at least one of the following properties: WA1. a thickness in a range from 1 mm to 10 mm; WA2. a swelling on contacting with water of less than 200 vol%, based on the volume before contacting with water; WA3. an extent in one of the spatial directions that lies within the plane corresponding to the largest areal extent of the wound dressing of < 50%, based on the extent of the wound dressing in the third spatial direction, on contacting with a fluid; WA4. a combination of at least two of the properties WA1. to WA3.