METHOD FOR PRODUCING A TACTICAL ADHESIVE USING A FIRST PLANETARY ROLLER EXTRUDER AND A STIRRINGLY ARRANGED SECOND DEGASING PLANETARY ROLLER EXTRUDER

DE502019012279D1Active Publication Date: 2024-10-31TESA SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012279
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-13
Filing Date
2019-08-20
Publication Date
2024-10-31
Estimated Expiration
2039-08-20

AI Technical Summary

Technical Problem

Current methods for producing thermally crosslinkable polymers in planetary roller extruders face challenges in achieving sufficient degassing, especially for highly viscous materials, which limits their use in producing reactive adhesives that can be crosslinked later, and existing degassing processes are not effective in reducing gas content to very low levels.

Method used

A method involving a first planetary roller extruder for compounding and a second degassing planetary roller extruder, where thermal crosslinkers are added and dispersed, followed by degassing in the second extruder to produce a thermally vulcanizable, meltable pressure-sensitive adhesive, allowing for efficient gas removal and processing within a temperature range of 130 °C to 230 °C.

Benefits of technology

This method enables the production of a thermally vulcanizable adhesive with adjustable adhesive strengths, suitable for automotive applications, by effectively reducing gas content and ensuring proper crosslinking, thus overcoming the limitations of existing degassing processes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for producing a particularly thermally vulcanizable, meltable, preferably pressure-sensitive adhesive, as well as an adhesive tape comprising the thermally vulcanizable adhesive.

[0002] Many units are known for the continuous production and processing of solvent-free and / or thermally crosslinkable polymer systems. Screw extruders such as single-screw, twin-screw, or planetary roller extruders of various lengths and configurations are commonly used. However, continuously operating kneaders of various designs, including combinations of kneaders and screw extruders, are also used for this task.

[0003] Extruders (single-screw and twin-screw extruders, planetary roller extruders, and ring extruders) are used primarily for plastics processing. The plastic is usually introduced in the form of granules, plasticized by the extruder, and extruded through a die, which forms the plasticized plastic into the desired shape.

[0004] In plastics processing, plasticization refers to the transformation of powdered or granular plastics through temperature and pressure, thus reducing the viscosity of the material. In this process, the plastics are heated above their specific melting temperatures in processing machines such as extruders, forming a hot, homogeneous plastic mass. Once the plastic is plasticized, it can be formed into pipes, sheets, films, or injection-molded parts in the subsequent process. Coating onto a substrate such as a carrier material is also possible.

[0005] In addition, plasticization refers to the addition of plasticizers (plasticizers, plasticizing agents, plasticizers) to plastics, i.e. chemical substances that influence the mechanical properties, for example the elasticity of the material.

[0006] In addition to plasticizing, the extruder's job is to homogenize the melt. Usually, additives and fillers need to be incorporated into the plastic matrix. In this case, the extruder's job is to evenly distribute the fillers and additives.

[0007] Planetary roller extruders were initially used in the processing of thermoplastics such as PVC, where they were primarily used to feed downstream units such as calenders or rolling mills. Due to their advantages of high surface renewal for material and heat exchange, which allows the energy introduced through friction to be dissipated quickly and effectively, as well as their short residence time and narrow residence time range, their application has recently expanded to include compounding processes that require particularly temperature-controlled operation.

[0008] Planetary roller extruders are available in various designs and sizes depending on the manufacturer. Depending on the desired throughput, the roller cylinder diameters typically range between 70 mm and 400 mm.

[0009] For processing plastics, planetary roller extruders usually have a filling section and a compounding section.

[0010] The filling section consists of a screw conveyor, into which the polymers to be plasticized, along with at least some of the other solid components if required, are continuously metered. The screw conveyor then transfers the material to the compounding section. Within the compounding section, additional solids can be added as needed, preferably via side-screw feeders, which convey the material into the planetary roller extruder through openings in the barrel shell, preventing the already plasticized polymers from escaping.

[0011] The addition of liquid formulation components usually does not occur via the filling section of the planetary roller extruder, but rather downstream in the compounding section, as the liquids often adversely affect the polymer plasticization process. The liquid components can be added via openings between the roller cylinders or via a special bore in the shell of a roller cylinder.

[0012] The area of ​​the filling section with the screw is preferably cooled to prevent material from sticking to the screw. However, there are also versions without a screw section, in which the material is fed directly between the central and planetary spindles.

[0013] The compounding section consists of a driven central spindle and several planetary spindles that rotate around the central spindle within one or more roller cylinders with internal helical gearing. The rotational speed of the central spindle, and thus the rotational speed of the planetary spindles, can be varied, making it an important parameter for controlling the compounding process.

[0014] The surrounding housing features a contemporary double shell design. The inner shell is formed by a bushing with internal gearing. The critical cooling system for the planetary roller extruder is located between the inner and outer shells.

[0015] The planetary spindles do not require any circumferential guidance. The toothing ensures that the distance between the planetary spindles remains constant in the circumferential direction. This can be described as self-guiding.

[0016] The materials are circulated between central and planetary spindles or between planetary spindles and helical gearing of the roller part, so that under the influence of shear energy and external temperature control the materials are dispersed into a homogeneous compound.

[0017] The number of planetary spindles rotating in each roller cylinder can be varied and thus adapted to the process requirements. The number of spindles influences the free volume within the planetary roller extruder, the material residence time in the process, and also determines the surface area for heat and material exchange. The number of planetary spindles influences the compounding result via the introduced shear energy. With a constant roller cylinder diameter, a larger number of spindles can achieve better homogenization and dispersion performance and a higher product throughput.

[0018] The maximum number of planetary spindles that can be installed between the central spindle and the roll cylinder depends on the diameter of the roll cylinder and the diameter of the planetary spindles used. When using larger roll diameters, as required to achieve production-scale throughput rates, or smaller diameters for the planetary spindles, the roll cylinders can be equipped with a larger number of planetary spindles. Typically, up to seven planetary spindles are used for a roll diameter of D=70 mm, while ten planetary spindles can be used for a roll diameter of D=200 mm, for example, and 24 for a roll diameter of D=400 mm, for example.

[0019] Compared to the other extruders mentioned, planetary roller extruders have an extremely high plasticizing effect. This opens up the possibility of processing raw materials that are not suitable or only poorly suited to other extruders. Planetary roller extruders can also be used to significantly increase production output.

[0020] All extruders have the problem that gaseous components can occur in the melt, which are undesirable or which negatively influence the quality of the product being manufactured during further processing.

[0021] Such components can include water, air, or (residual) solvents. Some polymers or fillers absorb water. These polymers or fillers must either be pre-dried, or the steam generated in the extruder must be vented.

[0022] Powdered bulk materials, in particular, can sometimes introduce large amounts of air into the compounding process due to their large surface area and often low bulk density. Here, too, degassing is usually necessary to achieve the desired product quality.

[0023] Gaseous components that are initially desirable but subsequently undesirable include organic solvents, water, air, reaction accelerators or inhibitors, or inert gases such as nitrogen, argon, or carbon dioxide. If these gases are not completely chemically converted, residues containing monomeric and oligomeric degradation products and decomposition products remain.

[0024] The proportion of volatile liquid components in plasticized polymers can often be up to 3 to 4 wt.%, but in extruded polymers must usually not exceed 0.1 wt.%.

[0025] There are various reasons that require degassing.

[0026] This includes: Improving product quality Avoiding health damage Reducing costs Preventing chemical degradation Carrying out further process steps

[0027] Various devices are available for degassing. Degassing is usually performed at the extruder. First, a degassing zone is defined on the extruder, which is usually located at the end of the process length, immediately before the polymers exit the extruder. The disadvantage of this degassing position is that even easily evaporated liquid components that are supposed to remain in the polymers in defined quantities, such as crosslinkers, plasticizers, etc., can be removed from the polymers in an undefined manner through unwanted evaporation.

[0028] Various solutions are available for degassing. All of them are based on the release of the volatile components dissolved in the melt by reducing the pressure. The pressure drop can be to ambient pressure or below it. The gas then inevitably releases from the melt. The gas bubbles can then be removed.

[0029] A suitable gas vent is an opening on the extruder's shell / housing located in the pressure drop area, optionally connected to a suction line. In cascade extruder systems, venting usually takes place between the primary and secondary extruders.

[0030] During operation, it becomes clear that the degassing zone is a relatively sensitive area. The goal here is to achieve the best possible separation of gas and polymer melt and to prevent the plasticized materials from escaping.

[0031] It is known that degassing in planetary roller extruders takes place in the area of ​​the thrust rings. However, degassing at this position is only sufficiently effective for a few materials: Materials with higher viscosities, such as most plasticized polymers, can usually not be degassed, or not in the desired manner or completely, because the venting opening often becomes clogged with material after a very short time, which can even lead to a complete loss of degassing capability.

[0032] Planetary roller extruders are modular in design, composed of individual roller cylinders. Each module consists of a central spindle common to all modules, planetary spindles rotating around the central spindle, and a housing. The number and type of planetary spindles can vary in each module and be adapted to the specific process task of the module. The module housings are provided with flanges at the ends, via which the modules can be coupled together. The end faces of the modules are connected to each other via spacer rings, which are available in various designs. For example, there are spacer rings that reduce the free cross-section at the end of a roller cylinder, thus influencing the residence time in the upstream roller cylinder and thus influencing, for example, the dispersion process.There are also designs of intermediate rings that do not influence the conveying characteristics of the material within the planetary roller extruder.

[0033] For degassing in a planetary roller extruder, the intermediate rings are selected so that they have at least one radial bore at the desired degassing point through which the gaseous components can escape.

[0034] One degassing variant, according to DE 198 56 235 A1, proposes reverse degassing of the melt, either alone or in addition. Reverse degassing occurs by venting gas before material compaction, which prevents gas passage, occurs in the compression zone of the filling section. Depending on the distance of the material compaction preventing gas passage, the reverse degassing can be located up to 80 cm from the material feed, for example, in the material feed direction.

[0035] Backward degassing also includes the fact that released gas flows back through the material feed or that backward degassing takes place on the extruder in the axial direction and conveying direction before the feed material is fed in.

[0036] Preferably, the reverse degassing takes place as part of a multi-stage degassing process and the reverse degassing in the area where the feed material is introduced forms the first degassing step in which, in particular, air is removed.

[0037] For reverse degassing, it is advantageous if the extruder is designed as a planetary roller extruder section in the gas flow area. The planetary roller extruder section offers particularly favorable gas passages between the rotating planetary spindles.

[0038] For degassing, it may be sufficient to simply provide openings through which the gas or drawn-in air can escape. However, degassing can also be enhanced by applying an induced draft.

[0039] However, it turns out that the known degassing processes are not sufficient to reduce the gas content in the polymer melts to very low values.

[0040] It is not yet possible to produce thermally crosslinkable polymers in a planetary roller extruder in such a way that a very reactive, often highly viscous mass can be sufficiently degassed from the planetary roller extruder, which can only be crosslinked at a later time.

[0041] The compounding and degassing of adhesives with thermal crosslinkers is limited by the process temperatures. This is particularly true for setups with a compounding PWE followed by a twin-screw extruder (DSE). The cooling effect of the DSE is severely limited; typically, additional energy is introduced, resulting in a temperature increase in this unit.

[0042] DE 10 2008 004 388 A1 discloses a particularly pressure-sensitive adhesive containing expanded microballoons. The adhesive strength of the adhesive containing the expanded microballoons is reduced by a maximum of 30% compared to the adhesive strength of an adhesive of identical basis weight and formulation, which is defoamed by destroying the cavities created by the expanded microballoons. Various extruders, including a planetary roller extruder, can be used as mixing units for production.

[0043] DE 10 2010 062 669 A1 discloses a process in which two mixing units are connected in series. It is disclosed that extruders, such as twin-screw extruders and / or planetary roller extruders, are particularly suitable as mixing units. Thus, a combination of two planetary roller extruders is described, although it is not disclosed whether these extruders are vented.

[0044] DE 10 2013 224 774 A1 and DE 10 2012 212 883 A1 also do not disclose a process in which a first planetary roller extruder in which no degassing takes place and a second degassing planetary roller extruder arranged downstream is used.

[0045] The object of the invention is to provide a process for producing a preferably pressure-sensitive adhesive which can be thermally vulcanised within a temperature range of 130 °C to 230 °C and with process-technically limited residence times, so that it can be used in the automotive industry both in the body shop on oiled sheets and in the paint shop on cathodic dip-coated or otherwise painted sheets for bonding and / or sealing, for example for hem seam bonding, hem seam sealing, seam sealing, underlining bonding, hole sealing and much more.

[0046] This object is achieved by a method for producing a particularly thermally vulcanizable, meltable, preferably pressure-sensitive adhesive using a first planetary roller extruder and a second vented planetary roller extruder arranged downstream, as set forth in the main claim. The subclaims relate to advantageous embodiments of the subject matter of the invention.

[0047] Accordingly, the invention relates to a method according to claim 1 for producing a particularly thermally vulcanizable, meltable, preferably pressure-sensitive adhesive using a first planetary roller extruder and a second vented planetary roller extruder arranged downstream, wherein a) the first planetary roller extruder consists of an atmospherically operated filling and dispersing zone comprising at least one roller cylinder, b) the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive-forming polymers are fed to the planetary roller extruder in a plasticized state, c) the plasticized polymers are fed into the at least one roller cylinder of the filling and dispersing zone, specifically within the first third of the roller cylinder, d) downstream of the addition of the plasticized polymers in the filling and dispersing zone, solids such as thermal crosslinkers are added to the plasticized polymers, in particular with the aid of a side-screw feeder, via an opening in the at least one roller cylinder, e) the solids are dispersed in the plasticized polymers in the filling and dispersing zone, f) the solids contain at least thermal crosslinkers,which can crosslink the plasticized polymers for the purpose of increasing the molecular weight of the polymers, g) the feed temperatures of the central spindle and of the at least one roller cylinder within the filling and dispersing zone are adjusted so that no gelling of the plasticized polymers blended with the thermal crosslinkers occurs, h) the mixture of plasticized polymers and solids, preferably thermal crosslinkers, is fed to a second vented planetary roller extruder, more preferably inline, i) the second vented planetary roller extruder consists of a vent zone of at least one roller cylinder, j) the mixture of plasticized polymers and solids, preferably thermal crosslinkers, is degassed in the vented planetary roller extruder, k) the degassed mixture of plasticized polymers and solids, preferably thermal crosslinkers, is fed to a coating unit, more preferably inline,That is, without intermediate filling or transferring with subsequent remelting. Furthermore, feeding to the coating unit preferably takes place without any additional processing.

[0048] Dispersing is a process step in the production of formulations, such as those commonly found in paints, printing inks, plastics, or pigment preparations. A dispersion is created, i.e., a solid phase is dispersed in a liquid phase. In addition to uniform distribution in the liquid phase, dispersion also describes the wetting of the solid to be dispersed with the liquid phase and the comminution of the solid to be dispersed.

[0049] According to the invention, a vacuum is understood to mean a pressure of less than 300 mbar, preferably 200 mbar, more preferably a pressure of less than 100 mbar.

[0050] According to a further preferred embodiment of the invention, a single-screw conveying part is provided upstream of the first planetary roller extruder, which enables atmospheric reverse degassing.

[0051] If necessary, non-plasticized polymers can also be fed into the single-screw conveying section, which are plasticized before entering the at least one roller cylinder of the filling and dispersing zone.

[0052] The plasticized polymers are fed into the first planetary roller extruder through at least one opening in the wall of at least one roller cylinder, specifically within the first third of the filling and dispersing zone.

[0053] Alternatively, the plasticized polymers can be fed into the first planetary roller extruder via an intermediate ring which is located between the single-screw conveyor part and the first roller cylinder and which has at least one radial bore for the purpose of feeding the plasticized polymers.

[0054] The addition of the solids, preferably the addition of the thermal crosslinkers forming the solids, lime or TiO2, is advantageously carried out within the first two-thirds, preferably within the first half of the filling and dispersing zone.

[0055] In addition to the thermal crosslinkers, other solids such as dyes, color pigments or other fillers that modify the polymers can be added via the solids addition opening.

[0056] Heat exchange in planetary roller extruders preferably takes place via the central spindle and / or the roller cylinders, which are operated via heating / cooling devices with a temperature control medium.

[0057] In order to be able to run a wide range of formulations and to specifically adjust the properties of the polymers, flexible temperature control is necessary; therefore, it is advantageous to use separate temperature control circuits for the central spindle and the roller cylinders and, if necessary, to equip the roller cylinders with more than one temperature control circuit.

[0058] For thermodynamic reasons, water or pressurized water is preferred as the tempering medium, but the process is not limited to this.

[0059] According to a further preferred variant of the invention, each roller cylinder in the degassing zone has at least one liquid temperature control circuit. These circuits establish a decreasing temperature gradient during roller cylinder temperature control, which prevents gelling of the thermally sensitive polymers.

[0060] Preferably, the plasticized polymers are fed into the first planetary roller extruder by means of a single-screw conveyor, by means of a melt pump, by means of a single-screw or multi-screw extruder or by means of a barrel or tank melting unit.

[0061] Further preferably, the thermally sensitive polymer mixture is discharged from the first planetary roller extruder by means of a melt pump coupled to the end of the last roller cylinder area.

[0062] According to a preferred variant, the roller cylinder region of the degassing zone consists of at least two, more preferably exactly three or exactly four coupled roller cylinders, which are connected to one another in particular via toothed intermediate rings and which each have at least one opening in the shell through which the plasticized polymers mixed with the solids, in particular the thermal crosslinkers, can be freed from air and optionally other volatile substances by means of a vacuum.

[0063] The roller cylinder openings of the at least two roller cylinders forming the degassing zone are advantageously each equipped with a product hold-down device which prevents the plasticized polymers from escaping from the planetary roller extruder, wherein the product hold-down device is preferably designed as a meshing twin-screw pair, via whose free flanks air and optionally other volatile components are extracted from the thermally sensitive polymers under the influence of heat and vacuum.

[0064] In the preferred variant of the vented planetary roller extruder with three or four coupled roller cylinders, the plasticized polymers mixed with the solids, in particular the thermal crosslinkers, are fed into the second roller cylinder.

[0065] The second roller cylinder is then separated in a vacuum-tight manner from the evacuated part of the vented planetary roller extruder by means of appropriately designed intermediate rings.

[0066] In addition to degassing, compounding takes place in the degassing planetary roller extruder.

[0067] Further preferably, the planetary spindles of the at least one roller cylinder of the filling and dispersing zone and the planetary spindles of the at least one roller cylinder of the downstream degassing zone are each driven by a common central spindle.

[0068] Further preferably, the at least one roller cylinder, in particular all roller cylinders of the filling and dispersing zone, are equipped with a number of planetary spindles which amounts to more than 70%, preferably more than 80% of the maximum possible number of planetary spindles.

[0069] The maximum possible number of planetary spindles is a process-related parameter. Beyond a certain number of planetary spindles, no change in the process can be detected. The maximum possible number of planetary spindles corresponds to the number of planetary spindles up to which the influence of each individual planetary spindle on the process can be detected.

[0070] In extreme cases, increasing the maximum possible number of planetary spindles may even lead to a deterioration in process control.

[0071] Further preferably, the at least one roller cylinder, in particular all roller cylinders of the degassing zone, are equipped with a number of planetary spindles which amounts to less than 75%, preferably less than 60% of the maximum possible number of planetary spindles.

[0072] According to a particularly preferred variant, the two above features are fulfilled for all roller cylinders simultaneously.

[0073] Further preferably, the coating unit is a calender or a nozzle through which the thermally sensitive polymer mixture is applied to a carrier material.

[0074] According to the invention, the coating of the preferably produced adhesive compositions is carried out using a multi-roller applicator. This can be an applicator consisting of at least two rolls with at least one roll gap up to five rolls with three roll gaps.

[0075] Coating units such as calenders (I, F, L-calenders) are also conceivable, so that the preferred adhesive mass is formed to the desired thickness as it passes through one or more roll gaps.

[0076] To improve the transfer behavior of the formed adhesive layer from one roller to another, anti-adhesive rollers or anilox rollers can also be used. To produce a sufficiently precisely formed adhesive film, the peripheral speeds of the rollers may differ.

[0077] The preferred 4-roll applicator consists of a metering roll, a doctor roll that determines the thickness of the layer on the carrier material and is arranged parallel to the metering roll, and a transfer roll located below the metering roll. The compound and the web-like material are brought together on the application roll, which together with the transfer roll forms a second nip.

[0078] Depending on the type of web-like carrier material to be coated, the coating can be carried out using the synchronous or counter-rotating process.

[0079] The also preferred two-roller applicator consists of a metering roller and a stationary or very slowly rotating doctor roller. The thickness of the layer on the substrate is determined by the gap between the two rollers.

[0080] The forming unit can also be formed by a gap that occurs between a roller and a fixed doctor blade.

[0081] The fixed doctor blade can be a knife blade or a fixed (half) roller.

[0082] According to a preferred embodiment of the invention, the plasticized polymers are polymers from the group of non-thermoplastic elastomers, thermoplastic synthetic rubbers, polyacrylates, polyurethanes, polyepoxides and mixtures thereof in any ratios.

[0083] Further preferably, the plasticized polymers are mixed with, for example, tackifying resins, fillers, plasticizers, oils, thixotropic agents, powdered thermal crosslinkers, dyes and optionally other additives.

[0084] In addition to other liquids such as oils or plasticizers, thermal crosslinkers and / or crosslinking accelerators as well as dye dispersions are used as liquids.

[0085] Particularly preferably, the mixtures coming out of the planetary roller extruders are self-adhesive or curable structural adhesives. Adhesive tape rolls are preferably produced from the ACX plus< -range manufactured by tesa.

[0086] Another adhesive that can be produced particularly advantageously is disclosed in detail in WO 2018 / 059931 A1. This comprises a meltable polybutadiene polyurethane, ground sulfur, and optionally at least one vulcanization accelerator, at least one filler, at least one epoxy resin, at least one tackifier resin, at least one plasticizer, and other auxiliaries and additives.

[0087] The adhesive can be used as an adhesive tape or sealing tape or as part of an adhesive or sealing tape in the automotive industry in the body shop for application to oiled sheets or in the painting process for application to painted sheets, especially on cathodic dip-coated sheets, but also in other areas where process temperatures between 130 °C and 230 °C are available.

[0088] Of the optional substance classes vulcanization accelerator, filler, epoxy resin, tackifier resin, bitumen, plasticizer, and other auxiliaries and additives, only one or any combination of several substance classes may be included. Likewise, within a substance class, one compound or any number of different compounds may be included.

[0089] The invention particularly relates to a thermally vulcanizable adhesive that has a solid or at least very highly viscous consistency at room temperature and is preferably pressure-sensitively adhesive. It can be processed as a melt in a compounding and extrusion process within a temperature range between approximately 40°C and 100°C, and is thermally vulcanizable and thus curable within a temperature range between 130°C and 230°C. The resulting curing involves chemical crosslinking.

[0090] The bond strengths achievable with the adhesive should be freely adjustable within wide limits and according to requirements. This range includes tensile shear strengths from greater than 0 to at least 30.0 N / mm². The adhesive should be capable of being manufactured within a temperature range of 40 °C to 100 °C using a compounding and extrusion process. The base elastomer of this adhesive must therefore be present as a melt within this latter temperature range.

[0091] During melt processing or during subsequent storage at temperatures up to 40 °C, the vulcanization reaction or any other crosslinking reaction must not initiate. In the temperature range from room temperature (20 °C to 25 °C, ideally 23 °C) to 30 °C, the adhesive must be sufficiently strong or highly viscous so that it can be wound into a roll as a release liner or film coated onto a carrier material without flowing out the side or being squeezed out by the winding pressure.

[0092] In this document, thermal vulcanization refers exclusively to sulfur vulcanization, i.e. the crosslinking of unsaturated compounds using sulfur, activated and completed by increasing the temperature.

[0093] To activate the sulfur vulcanization process, vulcanization accelerators and vulcanization aids and additives can be added. These substances lower the activation temperature and / or accelerate curing and crosslinking.

[0094] In this document, a meltable polybutadiene polyurethane is understood to mean a meltable reaction product produced by a polyaddition reaction from at least one at least two-hydroxyl-functionalized polybutadiene or polybutadiene derivative and at least one diisocyanate, which is sufficiently solid and dimensionally stable at room temperature that it can be wound up into a roll on a release liner or on a carrier material at room temperature without flowing out at the side or being squeezed out by the winding pressure.At least doubly hydroxyl-functionalized polybutadiene derivatives are understood to be substances derived from polybutadiene diols or polyols which have several C4 units, each containing a carbon / carbon double bond, and at the same time carry either additional functional groups such as epoxy groups or additional side chains such as vinyl groups or other additional structural elements.

[0095] A meltable reaction product within the meaning of this document has a complex viscosity of at least 3,000 Pa*s, preferably at least 6,000 Pa*s, ideally at least 10,000 Pa*s, measured with a rheometer in an oscillation test under a sinusoidal oscillating shear stress in a plate-on-plate arrangement, a temperature of 23 °C, and an oscillation frequency of 10.0 rad / s. At temperatures in the range between 40 °C and 100 °C and an oscillation frequency of 10.0 rad / s, the complex viscosity decreases to less than 1,000 Pa*s, preferably to less than 500 Pa*s, ideally to less than 200 Pa*s. The oscillation frequency corresponds to the angular frequency.

[0096] The complex viscosity η* is defined as follows: η* = G* / ω (G* = complex shear modulus, ω = angular frequency).

[0097] The further definitions are: (G" = viscosity modulus (loss modulus), G' = elastic modulus (storage modulus)). G" = τ / γ •sin(δ) (τ = shear stress, γ = deformation, δ = phase angle = phase shift between shear stress and deformation vector). G' = τ / γ •cos(δ) (τ = shear stress, γ = deformation, δ = phase angle = phase shift between shear stress and deformation vector). ω = 2π • f (f = frequency).

[0098] Pressure-sensitive adhesiveness is the ability of a material to form a permanent bond with a substrate even under relatively light pressure. Materials that possess this property are called pressure-sensitive adhesives. Pressure-sensitive adhesives have been around for a long time. They can often be removed from the substrate after use, leaving essentially no residue. Pressure-sensitive adhesives are generally permanently tacky at room temperature, meaning they exhibit a certain viscosity and tackiness, allowing them to wet the surface of the substrate even under light pressure. The ability of a pressure-sensitive adhesive to adhere to materials and transfer forces is based on its adhesive strength and cohesion.

[0099] Pressure-sensitive adhesives can be considered extremely viscous liquids with an elastic component. Pressure-sensitive adhesives therefore have special, characteristic viscoelastic properties that lead to their permanent inherent tack and adhesive strength.

[0100] They are characterized by the fact that when they are mechanically deformed, both viscous flow processes and the buildup of elastic restoring forces occur. The respective contribution of both processes is proportional to each other, depending on the precise composition, structure, and degree of crosslinking of the respective pressure-sensitive adhesive, as well as the speed and duration of the deformation and the temperature.

[0101] The viscous flow component is necessary to achieve adhesion. Only the viscous components, caused by macromolecules with relatively high mobility, enable good wetting and flow onto the substrate to be bonded. A high proportion of viscous flow leads to high pressure-sensitive adhesion (also referred to as tack or surface adhesion) and thus often also to high adhesive strength. Highly cross-linked systems, crystalline, or glass-like polymers, are generally not or at least only slightly tacky due to the lack of flowable components.

[0102] The proportional elastic restoring forces are necessary to achieve cohesion. They are caused, for example, by very long-chain and highly entangled macromolecules, as well as by physically or chemically cross-linked macromolecules, and enable the transfer of forces acting on an adhesive bond. They ensure that an adhesive bond can sufficiently withstand continuous loading, for example, in the form of permanent shear stress, over an extended period of time.

[0103] For a more precise description and quantification of the degree of elastic and viscous components as well as the relationship between the components, the storage modulus (G') and loss modulus (G"), which can be determined using Dynamic Mechanical Analysis (DMA), can be used. G' is a measure of the elastic component, G" a measure of the viscous component of a material. Both parameters depend on the deformation frequency and the temperature.

[0104] These parameters can be determined using a rheometer. The material under test is subjected to sinusoidal oscillating shear stress, for example, in the form of a plane-parallel layer in a plate-on-plate arrangement. Shear stress-controlled devices measure the deformation as a function of time and the temporal offset of this deformation relative to the application of the shear stress. This temporal offset is referred to as the phase angle δ.

[0105] The storage modulus G' is defined as follows: G' = (τ / γ) * cos(δ) (τ = shear stress, γ = deformation, δ = phase angle = phase shift between shear stress and deformation vector). The definition of the loss modulus G" is: G" = (τ / γ) * sin(δ) (τ = shear stress, γ = deformation, δ = phase angle = phase shift between shear stress and deformation vector).

[0106] A material and the layer made from it are generally considered to be pressure-sensitive adhesive and are defined as pressure-sensitive adhesive in the sense of this document if, at room temperature, here by definition at 23 °C, in the deformation frequency range from 10 0< to 10 1< rad / sec, G` lies at least partly in the range from 10 3< to 10 7< Pa and if G" also lies at least partly in this range. Partly means that at least a section of the G' curve lies within the window spanned by the deformation frequency range from 10 0< to 10 1< rad / sec (abscissa) and the range of G' values ​​from 10 3< to 10 7< Pa (ordinate), and if at least a section of the G" curve also lies within this window.

[0107] Within this range, which can also be described as a viscoelastic window for pressure-sensitive adhesive applications or as a pressure-sensitive adhesive window according to viscoelastic criteria in a matrix plot of G' and G" (G' plotted as a function of G"), there are in turn different sectors and quadrants that further characterize the expected pressure-sensitive adhesive properties of the respective materials.

[0108] For example, fabrics with high G" and low G' within this window are generally characterized by high adhesive strength and low shear strength, while fabrics with high G" and high G` are characterized by both high adhesive strength and high shear strength.

[0109] In general, the knowledge about the relationship between rheology and pressure-sensitive adhesiveness is state of the art and is described, for example, in the "Handbook of Pressure Sensitive Adhesive Technology", by Donatas Satas, Third Edition, (1999), pages 153 to 203.

[0110] Ground sulfur is soluble or insoluble ground elemental sulfur. The purity should be at least 95%, preferably at least 99%. The sulfur should be ground so finely that the sieve residue at a mesh size of 100 µm is no more than 2%. Coarser grades will work in principle, but this can result in a visually noticeable roughness in the adhesive and the achievable bond strengths will be somewhat lower.

[0111] Vulcanization accelerators, which may optionally be included in the adhesive, are understood in this document to mean all substances known to accelerate vulcanization. These can also be sulfur donors. The inventive concept also includes known sulfur donors that are not explicitly classified as accelerators in the technical literature.

[0112] The most important vulcanization accelerators can be classified into the following well-known substance classes: mercapto accelerators, sulfenamide accelerators, sulfenimide accelerators, thiuram accelerators, dithiocarbamate accelerators, dithiocarbamyl sulfenamide accelerators, xanthate accelerators, guanidine accelerators, amine accelerators, thiourea accelerators, dithiophosphate accelerators and sulfur donors.

[0113] Examples of mercapto accelerators are 2-mercaptobenzothiazole (MBT), zinc 2-mercaptobenzothiazole (ZMBT), and dibenzothiazyl disulfide (MBTS). Typical sulfenamide accelerators are N-cyclohexyl-2-benzothiazolesulfenamide (CBS), N-tert-butyl-2-benzothiazolesulfenamide (TBBS), N-oxydiethylene-2-benzothiazolesulfenamide (MBS), and N,N'-dicyclohexyl-2-benzothiazolesulfenamide (DCBS). An example of a sulfenimide accelerator is N-tert-butyl-2-benzothiazolesulfenimide. Examples of thiuram accelerators are tetramethylthiuram monosulfide (TMTM), tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetrabenzylthiuram disulfide (TBzTD), tetraisopropylthiuram disulfide (TiPTD), dimethyldiphenylthiuram disulfide (MPTD), and dipentamethylenethiuram tetrasulfide (TPTT).Zinc dimethyldithiocarbamate (ZDMC), zinc diethyldithiocarbamate (ZDEC), zinc dibutyldithiocarbamate (ZDBC), zinc pentamethylenedithiocarbamate (Z5MC), zinc ethylphenyldithiocarbamate (ZEPC), zinc dibenzyldithiocarbamate (ZBEC), zinc diisopropyldithiocarbamate (ZDIPC), piperidine pentamethylenedithiocarbamate (PPC), tellurium dimethyldithiocarbamate (TDMC), tellurium diethyldithiocarbamate (ZDEC), lead dimethyldithiocarbamate (PbDMC), copper dimethyldithiocarbamate (CuDMC), copper dibutyldithiocarbamate (CuDBC), bismuth dimethyldithiocarbamate (BiDMC) and sodium dimethyldithiocarbamate (NaDMC) represent a selection of known dithiocarbamate accelerators. Typical Dithiocarbamyl sulfenamide accelerators are N-oxydiethylenedithiocarbamyl-N'-oxydiethylenesulfenamide (OTOS) and N-oxydiethylenedithiocarbamyl-N'-tert-butylsulfenamide (OTTBS). Well-known examples of xanthate accelerators are zinc isopropyl xanthate (ZIX), zinc butyl xanthate (ZBX), sodium isopropyl xanthate (NaIX), and polyxanthate.Typical guanidine accelerators are diphenylguanidine (DPG), di-o-tolylguanidine (DOTG), and o-tolylbiguanide (OTBG). Amine accelerators include butyraldehyde aniline (BAA), tricrotonylidenetetramine (TCT), hexamethylenetetramine (HEXA), polyethylenepolyamines (PEP), and cyclohexylethylamine (CEA). N,N'-ethylenethiourea (ETU), N,N'-dibutylthiourea (DBTU), N,N'-diethylthiourea (DETU), and N,N'-diphenylthiourea (DPTU) are examples of thiourea accelerators. Well-known dithiophosphate accelerators include zinc dibutyldithiophosphate (ZBPD), zinc diisooctyldithiophosphate (ZOPD), dodecylammonium diisooctyldithiophosphate (AOPD), and copper diisopropyldithiophosphate (CuPPD). Sulfur donors include 2-morpholinodithiobenzothiazole (MBSS), N,N'-dithiodimorpholine (DTDM), and caprolactam disulfide (CLD).

[0114] In general, knowledge about vulcanization accelerators is state of the art and is presented, for example, in the "Handbook of Rubber Technology (2001)" by Werner Hoffmann and Heinz Gupta.

[0115] Preferred substance classes are mercapto accelerators, thiuram accelerators, and dithiocarbamate accelerators. Mercapto accelerators are considered "all-purpose" accelerators, ensuring rapid vulcanization in the temperature range from 160 °C to 180 °C without negatively affecting the stability of the unvulcanized adhesive. Thiuram accelerators and dithiocarbamate accelerators, either individually or in combination with mercapto accelerators, are considered "ultra-accelerators," ensuring rapid vulcanization at temperatures as low as 130 °C while still maintaining sufficient stability during adhesive production, even at compounding temperatures up to approximately 90 °C, and during subsequent storage at temperatures between room temperature and 30 °C. A preferred "all-purpose" vulcanization accelerator is MBTS. Preferred "ultra accelerators" are TBzTD and ZBEC.In addition to technical and functional considerations, safety considerations also play a role in the selection process, particularly with regard to the potential release of dangerous, carcinogenic degradation products, particularly carcinogenic N-nirosamines. MBTS, TBzTD, and ZBEC are considered non-critical in this regard.

[0116] Preferred concentrations of the vulcanization accelerators in the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive are together between at least 0.1 wt.% and a maximum of 15.0 wt.%, preferably between at least 0.5 and a maximum of 12.5 wt.%, particularly preferably between at least 1.0 and a maximum of 10.0 wt.%.

[0117] High concentrations of vulcanization accelerators lower the curing temperature but increase the risk of curing (vulcanization) initiating during processing. If the curing temperature of the adhesive is below 130 °C, it is preferable to use a planetary roller extruder for compounding in the extruder, as this allows compounding temperatures to be kept below 90 °C, particularly preferably below 80 °C.

[0118] To further accelerate vulcanization, vulcanization aids and additives such as metal oxides, especially zinc oxide, fatty acids such as stearic acid, or their salts can be added if necessary. With regard to the stability of the unvulcanized adhesive and the adhesion properties after vulcanization, especially on oiled metal sheets, the use of vulcanization aids and additives has proven to be rather critical, so preferred embodiments are free of these substances.

[0119] Fillers that can also be included optionally include both reinforcing ones, such as carbon black, and non-reinforcing ones, such as carbonates, particularly chalk, or sulfates such as barium sulfate. Other examples of suitable fillers are silicates, such as talc, kaolin, calcined or partially calcined kaolin, wollastonite or mica, hydroxides or oxides, such as quartz powder, aluminum hydroxide, zinc oxide, or calcium oxide. Microspheres can also be used as fillers. Microspheres can be solid glass microspheres, hollow glass microspheres, and / or microplastic beads of all kinds. The microplastic beads can be pre-expanded or unexpanded. The particle size in the expanded state is usually in the range between 20 and 150 µm. Mixtures of the aforementioned substances can also be used.In particular, mixtures of calcium carbonate and calcium oxide have proven particularly advantageous in achieving high bond strengths and minimizing occasional blistering during thermal vulcanization. Advantageous weight proportions of calcium carbonate and calcium oxide in the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive are between 10.0 and 70.0 wt.%. Talc has also proven advantageous for the same reasons. Advantageous weight proportions of talc in the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive are between 10.0 and 50.0 wt.%.

[0120] Optionally, the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive can contain epoxy resins. An epoxy resin refers to synthetic resins that carry epoxy groups. Bisphenol-based epoxy resins are advantageous, especially bisphenol A-based, but also bisphenol F-based. A room-temperature liquid epoxy resin is particularly advantageous, especially the reaction product of bisphenol A and epichlorohydrin with a number-average molecular weight of less than or equal to 700 g / mol (CAS No. 25068-38-6). Corresponding solid reaction products with higher number-average molecular weights are also optional epoxy resins.Other advantageous epoxy resins include epoxyphenol novolac resins, epoxydicyclopentadienephenol novolac resins, epoxycresol novolac resins, glycidylamine-based epoxy resins, especially triglycidyl ethers of para-aminophenol, triglycidyl ethers of meta-aminophenol, tetraglycidyl ethers of methylenedianiline, hydroxyphenyl-based epoxy resins, and aliphatic epoxy resins, especially cycloaliphatic ones. Of particular note here is 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate (CAS No. 2386-87-0).

[0121] An advantageous concentration of the epoxy resin in the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive is between 1.0 wt.% and 20 wt.% inclusive. A concentration between 5.0 wt.% and 15.0 wt.% inclusive is particularly advantageous. The addition of epoxy resins has proven particularly advantageous with regard to the adhesion properties of the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive on oiled metal sheets after the thermal vulcanization reaction. Furthermore, the viscosity of the compound is advantageously reduced during adhesive production, allowing for lower process temperatures.

[0122] Advantageously, the chemical conversion to the meltable polybutadiene polyurethane already takes place in the presence of the optional at least one epoxy resin. The advantage of this process is that the at least one epoxy resin can be incorporated at room temperature in an energy-saving manner. If, on the other hand, the polybutadiene polyurethane were first produced and then the at least one epoxy resin were added, the polybutadiene polyurethane would first have to be heated to a high temperature until it exists as a melt. This would have the disadvantage that a higher energy input would be necessary. A further advantage is that the softening or melting temperature of the mixture of prepolymer and epoxy resin is significantly lower than the softening or melting temperature of the pure prepolymer, while the hotmelt character is still retained.Subsequent compounding with sulfur and other substances, such as vulcanization accelerators, can thus be carried out in an energy-saving and gentle manner at lower temperatures than without the epoxy resin already incorporated during polybutadiene polyurethane production. This also allows compounding with so-called ultra-accelerators, which can sometimes initiate vulcanization within just a few minutes at approximately 120°C, without causing undesirable curing or gelling during the compounding process.If the subsequent compounding of the polybutadiene polyurethane with sulfur, vulcanization accelerators and vulcanization aids and additives takes place in a continuously operating mixing unit, in particular a compounding extruder, a further advantage is that none of the generally limited dosing points on the compounding extruder would be blocked by the at least one epoxy resin.

[0123] The fact that it is technically possible to carry out the isocyanate-based chemical conversion to polybutadiene polyurethane in the presence of one or more epoxy resins is surprising to the person skilled in the art, because isocyanates are described in the specialist literature as reactive towards epoxides, for example in Ullmann's Encyclopedia of Industrial Chemistry, 6th Edition, Vol. 12, page 271 (table) and in Encyclopedia of Polymer Science and Engineering, Vol. 6, p. 345.

[0124] Surprisingly, it was also discovered that mixtures of epoxy resin and polybutadiene-polyurethane hotmelt tend to phase separate if the at least one epoxy resin is added after the polybutadiene-polyurethane has been produced. However, if the chemical conversion to polybutadiene-polyurethane occurs in the presence of the epoxy resin(s), depending on the mixing ratio, the resulting mixtures are generally cloudy but non-separating. These mixtures have the advantage of vulcanizing (curing) homogeneously, thus achieving greater strength and improved adhesion than when using an inhomogeneous mixture of polybutadiene-polyurethane and epoxy resin. In a similar manner, other substances, such as plasticizers, tackifier resins, bitumen, or even fillers or rheological additives, can be added to the polybutadiene-polyurethane before or during the chemical conversion.

[0125] Optionally, the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive can also contain tackifier resins. The term "tackifier resin" refers to a resin-based substance that increases tackiness. Tackifier resins can be divided into natural resins and synthetic resins.

[0126] Typical natural resins are rosin-based resins and their derivatives. Rosin resins include, for example, natural rosin, polymerized rosin, partially hydrogenated rosin, fully hydrogenated rosin, esterified products of these rosins (such as glycerol esters, pentaerythritol esters, ethylene glycol esters, and methyl esters), and rosin derivatives (such as disproportionation rosin, fumaric acid-modified rosin, and lime-modified rosin).

[0127] Typical synthetic resins are polyterpene resins (although the raw materials here come from natural sources), hydrocarbon resins, and terpene-phenolic resins. These are low-molecular-weight polymers. The weight-average molecular weight is usually less than 25,000 g / mol.

[0128] Polyterpene resins are based on α-pinene and / or β-pinene and / or δ-limonene. These can be hydrogenated, non-hydrogenated, or partially hydrogenated.

[0129] Raw materials for most hydrocarbon resins are byproducts resulting from the cracking of naphtha or gasoil. Hydrocarbon resins can be classified according to whether they are based primarily on aromatic, aliphatic, or diene monomers. Aromatic resins are often referred to as C-9 resins, aliphatic resins as C-5 resins, and diene resins as (C-5)2 resins. Mixed aromatic-aliphatic hydrocarbon resins ((C-5 / C-9) resins) are also encompassed by the invention. Hydrocarbon resins can also be hydrogenated, non-hydrogenated, or partially hydrogenated.

[0130] The invention also encompasses monomer resins of the styrene / α-methylstyrene type (CAS No.: 9011-11-4). According to DIN 16916-1 1981-06 and ISO / TR 8244:1988, terpene-phenolic resins are resins produced by the acid-catalyzed addition of phenols to terpenes or rosin.

[0131] Tackifier resins preferred according to the invention are polyterpene resins based on α-pinene and / or β-pinene and / or δ-limonene. Particularly preferred are β-pinene resins (CAS No.: 25719-60-2), for example the resin Dercolyte S-115 from DRT.

[0132] Advantageous concentrations of the tackifier resins in the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive are between 1.0 wt.% and 30.0 wt.% inclusive. Concentrations between 5.0 wt.% and 20.0 wt.% inclusive are particularly advantageous. The addition of tackifier resins has proven particularly advantageous with regard to the adhesion properties of the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive on oiled metal sheets prior to the thermal vulcanization reaction. The adhesive strength of the as yet unvulcanized adhesive on oiled metal sheets can thus be significantly increased.

[0133] Optionally, the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive can also contain bitumen. Bitumen is a dark-colored, semi-solid to spring-hard, high-molecular hydrocarbon mixture that arises as a residue from the distillation of suitable petroleum and still contains chemically bound sulfur, oxygen, nitrogen, and some traces of metals. Physically, bitumen is a thermoplastic material, meaning its properties are temperature-dependent. Upon cooling, it becomes brittle; upon heating, it continuously transitions through all states from solid to viscous to fluid. A distinction is made between the following types of bitumen and derived products: road construction bitumen, especially soft bitumen; modified bitumen, especially polymer-modified bitumen; industrial bitumen, especially oxidation bitumen or hard bitumen; flux bitumen; and bitumen emulsion.

[0134] According to the invention, road construction bitumen is preferred. The 50 / 70 grade is particularly preferred, with the numbers indicating the minimum and maximum penetration at 25 °C in the unit mm / 10 according to DIN EN 1426. Advantageous bitumen concentrations in the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive are between 1.0 wt.% and 30.0 wt.%, inclusive. Concentrations between 5.0 wt.% and 20.0 wt.%, inclusive, are particularly advantageous. The addition of bitumen can improve oil absorption when bonding to oiled metal sheets.

[0135] Optionally, the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive can also contain plasticizers. Plasticizers are liquid or solid, inert organic substances with low vapor pressure, predominantly ester-like substances, which, without chemical reaction, preferably through their dissolving and swelling properties, but under certain circumstances also without such, can physically interact with high-polymer materials and form a homogeneous system with them. The abbreviations for plasticizers are regulated in DIN EN ISO 1043-3: 2000-01. The most important plasticizers can be divided into larger groups, which are listed below, with the abbreviations according to DIN EN ISO 1043-3: 2000-01 in parentheses.

[0136] Phthalic acid esters, also called phthalates for short, include dioctyl phthalate (DOP; di(2-ethylhexyl)phthalate), diisononyl phthalate (DINP), diisodecyl phthalate (DIDP), phthalic acid esters with predominantly linear C6 to C11 alcohols, dibutyl phthalate (DBP), diisobutyl phthalate (DIBP), dicyclohexyl phthalate (DCHP), dimethyl phthalate (DMP) and diethyl phthalate (DEP) as well as mixed esters of benzyl(butyl)- (BBP), butyl(octyl), butyl(decyl) and dipentyl phthalate, bis(2-methoxyethyl)phthalate and dicapryl phthalate (DCP).

[0137] An example of trimellitic acid esters with (predominantly) linear C 6 to C 11 alcohols is tris(2-ethylhexyl) trimellitate (TOTM).

[0138] Acyclic aliphatic dicarboxylic acid esters include, for example, esters of adipic acid such as bis(2-ethylhexyl)adipate (dioctyl adipate, DOA), bis(8-methylnonyl)adipate (diisodecyl adipate, DIDA), dibutyl decanedioate (dibutyl sebacate, DBS), and bis(2-ethylhexyl)decanedioate (dioctyl sebacate, DOS). An example of a cyclic aliphatic dicarboxylic acid ester is diisononyl 1,2-cyclohexanedicarboxylate (DINCH).

[0139] Examples of polymer plasticizers are polyesters made from adipic, decanedic, nonanedic and phthalic acid with diols such as butane-1,3-diol, propane-1,2-diol, butane-1,4-diol, hexane-1,6-diol and others (M r approx. 1800 to 13000 g / mol).

[0140] Phosphoric acid esters, also known as phosphates, constitute another group. Examples include tricresyl phosphate (TCF), triphenyl phosphate (TPP), diphenyl cresyl phosphate (DPCF), (2-ethylhexyl)diphenyl phosphate (diphenyloctyl phosphate, DPOF), tris(2-ethylhexyl)phosphate (TOF), and tris(2-butoxyethyl)phosphate.

[0141] Butyl oleate and butyl stearate are examples of fatty acid esters, which represent a further group. Further examples of this group are methyl and butyl esters of acetylated ricinoleic fatty acid and fatty acid glycol esters, as well as triethylene glycol bis(2-ethylbutyrate).

[0142] Citric acid esters are examples of the group of hydroxycarboxylic acid esters. Other examples are tartaric acid esters and lactic acid esters.

[0143] Another group of plasticizers are epoxy plasticizers, for example, epoxidized fatty acid derivatives, especially triacylglycerols and monoesters. Some of the previously mentioned epoxy resins can also be classified as plasticizers. Polyamide plasticizers, such as benzenesulfonamides or methylbenzenesulfonamides, should also be mentioned. Another group of plasticizers are alkylsulfonic acid esters of phenol (ASE). Mineral oils are also considered plasticizers for the purposes of this document. Naphthenic mineral oils are preferred. Bitumen, already listed separately, could also be classified as plasticizers.

[0144] In an optional embodiment, the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive contains further auxiliaries and additives such as rheological additives, anti-aging agents (antioxidants), light stabilizers, or UV absorbers. Examples of rheological additives include pyrogenic, hydrophobic, or non-hydrophobic silicas, phyllosilicates (bentonites), high-molecular-weight polyamide powders, or castor oil derivative powders. These rheological additives can also be classified as fillers. Suitable antioxidants include, for example, sterically hindered phenols, hydroquinone derivatives, amines, organic sulfur compounds, or organic phosphorus compounds.

[0145] Light stabilizers used include those described in Gaechter and Müller, Taschenbuch der Kunststoff-Additive, Munich 1979, and in Kirk-Othmer (3.) 23, 615 to 627, in Encycl. Polym. Sci. Technol. 14, 125 to 148 and in Ullmann (4.) 8, 21; 15 , 529, 676 disclosed compounds.

[0146] In an advantageous embodiment, the meltable polybutadiene polyurethane is a reaction product produced by a polyaddition reaction of at least one polybutadiene diol, at least one chain extender having a hydroxyl functionality of two and a molecular weight of less than or equal to 300 g / mol and optionally at least one polybutadiene polyol having a number-average functionality between greater than 2.0 and less than or equal to 3.0 with at least one aliphatic or alicyclic diisocyanate.

[0147] Chain extenders within the meaning of this document are all hydroxyl-containing compounds with a hydroxyl functionality of two and a molar mass of less than or equal to 300 g / mol. They do not carry any other isocyanate-reactive groups. They are therefore diols with a molar mass of less than or equal to 300 g / mol. It is known that many chain extenders used to produce polyurethanes based on polyester or polyether polyols are incompatible with polybutadiene diols and polyols. This leads to demixing. Chain extenders compatible with polybutadiene diols and polyols are preferred according to the invention. These include, for example, N,N-diisopropanol aniline (CAS No. 003077-13-2), 2,2,4-trimethyl-1,3-pentanediol (CAS No. 144-19-4), and 2-butyl-2-ethyl-1,3-propanediol (CAS No. 115-84-4). 2-ethyl-1,3-hexanediol (CAS No. 94-96-2) is particularly preferred.The findings on chain extenders compatible with polybutadiene diols and polyols are state of the art. They are published, for example, in Herbert Chao, Nan Tian, ​​Cray Valley, USA, LLC, Exton, PA, PCI, April 2010.

[0148] To achieve high pressure-sensitive adhesion (high tack) while simultaneously avoiding excessive softness of the polybutadiene polyurethane, which would lead to reduced shear strength, it is advantageous if the numerical fraction of the hydroxyl groups introduced to form the polybutadiene polyurethane, which originate from the at least one chain extender, is between greater than or equal to 20.0% and less than or equal to 80.0%, preferably between greater than or equal to 30.0% and less than or equal to 70.0%. The numerical fraction always corresponds to the molar fraction.

[0149] In this document, a polybutadiene diol is understood to mean all hydroxyl-functionalized polybutadienes or their derivatives whose number-average hydroxyl functionality is two or slightly less than two, but at least 1.5, preferably at least 1.8. In no case is the number-average hydroxyl functionality of a polybutadiene diol greater than two.

[0150] In this document, a polybutadiene polyol is understood to mean all hydroxyl-functionalized polybutadienes or their derivatives with a number-average functionality between greater than 2.0 and less than or equal to 3.0.

[0151] The number-average hydroxyl functionality is the average number of hydroxyl groups per molecule of a polyol. In this document, it is related to the number-average molecular weight of the respective polyol and calculated using the following formula: f = M n g / mol × OHZ mmol OH / kg / 10 6 f is the number-average hydroxyl functionality. M n is the number-average molecular weight of the respective polyol in [g / mol], and OH number is the hydroxyl number of the polyol in [mmol OH / kg].

[0152] The hydroxyl number is a measure of the content of hydroxyl groups in a polyol.

[0153] The hydroxyl number is determined according to DIN 53240. According to this method, the hydroxyl number (OHN) is expressed in [mg KOH / g]. It corresponds to the amount of KOH in [mg] that is equivalent to the amount of acetic acid bound during the acetylation of 1 g of polyol. To simplify formulation calculations, the hydroxyl number is converted to the unit [mmol OH / kg] in this document.

[0154] This is done according to the following formula: OHZ mmol OH / kg = OHZ mg KOH / g × 1000 / 56,1 . 56.1 is the molar mass of KOH.

[0155] The hydroxyl groups of polybutadiene diols and polyols can be bonded to the polybutadiene chain in a primary or secondarily bonded manner. The butadiene units of the polybutadiene chain can be linked in a 1,4-cis or -trans form, or in a 1,2-form with vinyl groups in the side chain, or in a mixed manner. Polybutadiene diols are produced by anionic polymerization, while polybutadiene polyols with a number-average functionality between greater than 2.0 and less than or equal to 3.0 are produced by free-radical polymerization. Polybutadiene diols are commercially available under the trade name Krasol®, and polybutadiene polyols with a number-average functionality between greater than 2.0 and less than or equal to 3.0 are available under the trade name Poly bd®; both grades are available from Cray Valley.

[0156] To achieve high pressure-sensitive adhesiveness (high tack), it is advantageous to use polybutadiene diols with a number-average molecular weight between greater than 1000 g / mol and less than 5000 g / mol, preferably between greater than or equal to 2000 g / mol and less than or equal to 3000 g / mol.

[0157] For the same reason, the optional polybutadiene polyols with a number-average functionality between greater than 2.0 and less than or equal to 3.0 should also advantageously have a number-average molecular weight between greater than 1000 g / mol and less than 5000 g / mol, preferably between greater than or equal to 2000 g / mol and less than or equal to 3000 g / mol.

[0158] Polybutadiene polyols with a number-average functionality between greater than 2.0 and less than or equal to 3.0 can optionally be used in the production of the polybutadiene polyurethane to incorporate branching points into the polyurethane. A certain degree of branching would have the advantage that the coated polyurethane would soften less during thermal vulcanization during the temperature application but before the vulcanization reaction begins, and would thus possess higher shear strength in this phase immediately before the curing induced by vulcanization.

[0159] When using optional polybutadiene polyols with a number-average functionality between greater than 2.0 and less than or equal to 3.0 to produce the polybutadiene polyurethane, care must be taken to prevent gelation. This means that the degree of branching relative to the length of the prepolymer chains produced is not so high that crosslinking occurs during the polyaddition reaction. The degree of branching is adjusted to ensure the meltability of the polybutadiene polyurethane, thus preventing the formation of crosslinked structures. To prevent crosslinked structures, the so-called gel point must not be exceeded. The theoretical gel point can be calculated using PJFlory's gel point equation. A formula derived from the Flory equation for estimating the gelation NCO / OH ratio in polyurethane formation reactions from diols and triols with diisocyanates in deficit is: NCO OH Gelierung = 1 1 + 1 Diol − OH Triol − OH + 1

[0160] In this formula, "diol-OH" refers to the total number of hydroxyl groups involved in the polyurethane formation reaction that originate from polyols whose hydroxyl functionality is less than or equal to two. This also includes the chain extenders. "triol-OH" refers to the total number of hydroxyl groups involved in the polyurethane formation reaction that are bound to polyols whose functionality is greater than two and less than or equal to three.

[0161] If the gelation NCO / OH ratio is reached or exceeded, the formation of cross-linked structures, i.e., the onset of gelation, must be expected. The formula provides only an approximate, but generally sufficient, indication of the NCO / OH ratio at which actual gelation occurs.

[0162] If an excess of diisocyanates is used, i.e. the NCO / OH ratio is greater than 1.0, the above formula must be applied reciprocally.

[0163] The numerical proportion of the hydroxyl groups introduced to form the polybutadiene polyurethane, which originate from the optional at least one polybutadiene polyol with a number-average functionality between greater than 2.0 and less than or equal to 3.0, is advantageously a maximum of 50.0%, preferably a maximum of 30.0%, particularly preferably a maximum of 10%. Higher proportions require an unfavorably low NCO / OH ratio in the case of an NCO deficiency or an unfavorably high NCO / OH ratio in the case of an NCO excess, which would result in an unfavorably low softening temperature of the hydroxyl-functionalized polybutadiene polyurethane hotmelt prepolymer.

[0164] In terms of process reliability, the proportion of 0.0% is particularly advantageous. At a proportion of 0.0%, the risk of premature formation of cross-linked structures, i.e., the onset of gelation during polyurethane production, is lowest.

[0165] The polybutadiene polyurethane is obtained by reacting the mentioned diols / polyols with at least one aliphatic or alicyclic diisocyanate.

[0166] In this document, aliphatic or alicyclic diisocyanates are understood to mean all organic polyisocyanates with an isocyanate functionality of two in which the isocyanate groups are not directly bonded to an aromatic ring system according to the Hückel rule. Examples of aliphatic or alicyclic diisocyanates are butane-1,4-diisocyanate, tetramethoxybutane-1,4-diisocyanate, hexane-1,6-diisocyanate, ethylene diisocyanate, 2,2,4-trimethyl-hexamethylene diisocyanate, ethylethylene diisocyanate, dicyclohexylmethane-4,4'-diisocyanate (H12MDI), 1,4-diisocyanatocyclohexane, 1,3-diisocyanatocyclohexane, 1,2-diisocyanatocyclohexane, 1,3-diisocyanatocyclopentane, 1,2-diisocyanatocyclopentane, 1,2-diisocyanatocyclobutane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane (isophorone diisocyanate, IPDI), 1-methyl-2,4-diisocyanatocyclohexane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1,6-Diisocyanato-2,4,4-trimethylhexane, 5-Isocyanato-1-(2-isocyanatoeth-1-yl)-1,3,3-trimethylcyclohexane,5-Isocyanato-1-(3-isocyanatoprop-1-yl)-1,3,3-trimethylcyclohexane, 5-Isocyanato-1-(4-isocyanatobut-1-yl)-1,3,3-trimethylcyclohexane, 1-Isocyanato-2-(3-isocyanatoprop-1-yl)cyclohexane, 1-Isocyanato-2-(2-isocyanatoeth-1-yl)cyclohexane, 2-heptyl-3,4-bis(9-isocyanatononyl)-1-pentylcyclohexane, norbonane diisocyanatomethyl, and m-tetramethylxylene diisocyanate (TMXDI). Particularly preferred are isophorone diisocyanate (CAS No. 4098-71-9) and dicyclohexylmethane 4,4'-diisocyanate (CAS No. 5124-30-1).

[0167] In an advantageous embodiment, the ratio of the total number of isocyanate groups to the total number of hydroxyl groups of the substances involved in the chemical conversion to polybutadiene polyurethane is between greater than or equal to 0.3 and less than or equal to 1.3, preferably between greater than or equal to 0.4 and less than or equal to 1.2, particularly preferably between greater than or equal to 0.5 and less than or equal to 1.1, and most particularly preferably between greater than or equal to 0.6 and less than or equal to 1.0. The preferred ratios lead to hotmelt polyurethanes with a particularly solid consistency at room temperature and, at the same time, high pressure-sensitive adhesiveness (high tack).

[0168] The polybutadiene polyurethane according to the invention preferably comprises the chemical reaction product of exclusively one or more polybutadiene diols, optionally one or more polybutadiene polyols with a number-average functionality between greater than 2.0 and less than or equal to 3.0, and one or more chain extenders with a hydroxyl functionality of two and a molar mass of less than or equal to 300 g / mol, with one or more aliphatic or alicyclic diisocyanates. Therefore, no additional, other polyols or isocyanates are preferably involved in the chemical reaction to form the polybutadiene polyurethane, in particular no polyether polyols, no polyester polyols, and no aromatic diisocyanates.It is assumed that when using the polybutadiene polyurethane of the invention as a base elastomer for producing a thermally vulcanizable, meltable, preferably pressure-sensitive adhesive, polyether and polyester polyols have an adverse effect on the adhesion properties after the vulcanization reaction, particularly on the adhesion properties on oiled metal sheets. Furthermore, it is assumed that aromatic diisocyanates have an adverse effect on the tack.

[0169] To accelerate the reaction, the chemical conversion to polybutadiene polyurethane is preferably carried out with the addition of a catalyst. One or more catalysts known to those skilled in the art can be used, such as tertiary amines, organobismuth or organotin compounds, to name just a few. Bismuth and carbon-containing catalysts can be used very advantageously, preferably a bismuth carboxylate or a bismuth carboxylate derivative. Bismuth trisneodecanoate (CAS No. 34364-26-6) is particularly advantageous.

[0170] The concentration of the catalysts is adjusted to the desired reaction rate and is typically between 0.01 wt% and 0.5 wt% of the polybutadiene polyurethane to be produced.

[0171] Polybutadiene polyurethane is preferably manufactured without the use of solvents. While the inclusion of solvents in the manufacturing process is technically feasible, it typically offers no advantages.

[0172] The present invention further relates to an adhesive tape that is at least partially coated with the pressure-sensitive adhesive on one or both sides. The adhesive tape can also be a transfer adhesive tape. An adhesive tape enables particularly simple and precise bonding and is therefore particularly suitable.

[0173] The general term "adhesive tape" encompasses a carrier material that is at least partially coated on one or both sides with a (pressure-sensitive) adhesive. The carrier material includes all flat structures, for example, films or film sections extended in two dimensions, tapes with extended length and limited width, tape sections, die-cuts (for example, in the form of borders or boundaries of an assembly to be bonded), other molded bodies, multilayer assemblies, and the like. A wide variety of carriers, such as films, fabrics, nonwovens, and papers, can be combined with the adhesives for various applications. Furthermore, the term "adhesive tape" also encompasses so-called "transfer adhesive tapes," i.e., adhesive tapes without a carrier. Rather, with a transfer adhesive tape, the adhesive is applied between flexible liners provided with a release layer and / or having anti-adhesive properties prior to application.For application, one liner is usually removed first, the adhesive is applied, and then the second liner is removed. The adhesive can then be used directly to bond two surfaces.

[0174] However, adhesive tapes are also possible that use a single, double-sided separating liner instead of two. The adhesive tape strip is then covered on its upper side with one side of a double-sided separating liner, and its underside with the back of the double-sided separating liner, particularly on an adjacent wrap on a bale or roll.

[0175] In the present case, polymer films, film composites, or films or film composites provided with organic and / or inorganic layers are preferably used as the carrier material for an adhesive tape, with films, in particular dimensionally stable plastic or metal films, being preferred. Such films / film composites can consist of all common plastics used for film production, including, by way of example but not limitation: polyethylene, polypropylene - in particular oriented polypropylene produced by mono- or biaxial stretching (OPP), cyclic olefin copolymers (COC), polyvinyl chloride (PVC), polyester - in particular polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), ethylene vinyl alcohol (EVOH), polyvinylidene chloride (PVDC), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polycarbonate (PC), polyamide (PA), polyethersulfone (PES), or polyimide (PI).

[0176] Polyester films have the advantage of providing temperature stability and increased mechanical stability. Therefore, a carrier layer in a liner according to the invention particularly preferably consists of a polyester film, for example, biaxially oriented polyethylene terephthalate.

[0177] Double-sided (self-)adhesive tapes can use adhesives of the same or different types and / or of the same or different thicknesses as the top and bottom layers. The carrier can be pretreated on one or both sides according to the state of the art, for example, to improve adhesive anchorage. The pressure-sensitive adhesive layers can optionally be covered with release papers or release films. Alternatively, only one adhesive layer can be covered with a double-sided release liner.

[0178] In one variant, the double-sided (self-)adhesive tape contains an adhesive as well as any other adhesive, for example one that adheres particularly well to a covering substrate or has particularly good repositionability.

[0179] The thickness of the pressure-sensitive adhesive layer, which is present either as a transfer adhesive tape or coated on a flat structure, is preferably between 10 µm and 5000 µm, more preferably between 100 µm and 4000 µm and particularly preferably between about 200 µm and 3000 µm.

[0180] For double-sided adhesive tapes, the thickness of the individual pressure-sensitive adhesive layer(s) is also preferably between 10 µm and 5000 µm, more preferably between 100 µm and 4000 µm and particularly preferably between about 200 µm and 3000 µm.

[0181] Adhesive tapes coated with adhesive on one or both sides are usually wound into a roll in the shape of an Archimedean spiral or cross-wound at the end of the manufacturing process. To prevent the adhesives from coming into contact with each other in the case of double-sided adhesive tapes, or to prevent the adhesives from sticking to the carrier in the case of single-sided adhesive tapes, the adhesive tapes are covered with a release liner (also known as a release liner) before winding, which is wound up together with the adhesive tape. Such release liners are known to those skilled in the art as liners or release liners. In addition to covering single- or double-sided adhesive tapes, liners are also used to cover pure adhesives (transfer tape) and adhesive tape sections (e.g., labels).

[0182] The thermally vulcanizable, meltable, preferably pressure-sensitive adhesive of the present invention is preferably used as a layer for producing a thermally vulcanizable, preferably pressure-sensitive adhesive tape or sealing tape, as well as molded articles or diecuts produced therefrom, wherein the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive tape or sealing tape can contain additional pressure-sensitive and / or non-pressure-sensitive layers, carrier foils or films, adhesion-promoting layers, release layers or other functional layers as well as several thermally vulcanizable or otherwise curable or crosslinkable adhesive tape layers and can be provided with a release liner which can be siliconized on one or both sides.

[0183] The thermally vulcanizable, meltable, preferably pressure-sensitive adhesive according to the invention and pressure-sensitive adhesive tapes produced therefrom exhibit an excellent combination of product properties which could not have been foreseen in this way even by the person skilled in the art.

[0184] At room temperature up to approximately 30 °C, the adhesive is sufficiently solid or highly viscous so that it can be wound into a roll as a film coated on a release liner or on a carrier material without flowing out of the side or being squeezed out by the winding pressure.

[0185] The adhesive, or an adhesive tape made from it, has proven to be very stable in storage at temperatures ranging from room temperature to approximately 40°C. It does not require refrigeration, which is a major advantage. Its shelf life extends to at least one year.

[0186] Optional epoxy resins can offer particular advantages. The addition of one or more epoxy resins can improve adhesion properties, particularly on some oiled sheet metal types after the thermal vulcanization reaction.

[0187] The optional addition of bitumen can improve oil absorption, so that cohesive fracture patterns occur even when bonding heavily oiled sheets in the tensile shear test.

[0188] The optional addition of tackifier resins has proven particularly advantageous with regard to the adhesion properties of the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive on oiled metal sheets prior to the thermal vulcanization reaction. The bond strength of the unvulcanized adhesive on oiled metal sheets can thus be significantly increased. This is particularly advantageous with the addition of β-pinene resins.

[0189] Surprisingly, fillers can contribute positively to increasing bond strength. In particular, mixtures of calcium carbonate and calcium oxide have proven particularly advantageous in achieving high bond strengths and minimizing occasional blistering during thermal vulcanization. In this way, tensile shear strengths could be significantly increased while maintaining the same sulfur concentration. Talc has also proven advantageous in this regard.

[0190] Table 1 lists the base materials (raw materials) used to produce the polybutadiene polyurethane, each with its trade name, manufacturer, and the technical data relevant to this invention.

[0191] Table 2 lists the additional base materials (raw materials) used for the resulting adhesives and adhesive tape layers according to the invention. All of these raw materials are commercially available.

[0192] The weight-average molecular weight M w and the number-average molecular weight M n are determined by gel permeation chromatography (GPC). THF with 0.1 vol.% trifluoroacetic acid is used as the eluent. The measurement is carried out at 25 °C. The precolumn is PSS-SDV, 5 µ, 10 3 < Å, ID 8.0 mm x 50 mm. The columns PSS-SDV, 5 µ, 10 3 < Å, 10 5 < Å, and 10 6 < Å, each with ID 8.0 mm x 300 mm, are used for separation. The sample concentration is 4 g / L, and the flow rate is 1.0 ml per minute. The measurement is carried out against PMMA standards (µ = µm; 1 Å = 10 -10 < m).

[0193] The invention will be described in more detail using the following example. Example Production of the adhesive:

[0194] A PBD-PU 3 mixture (including epoxy resin) was used to produce the adhesive. For this purpose, PBD-PU 3 (including epoxy resin) was further blended in the first planetary roller extruder (PWE) according to the following recipe. The goal was to lower the process temperature to reduce the risk of premature crosslinking, especially with increased ultraaccelerator concentrations. Furthermore, lowering the process temperature can have a positive effect on the achievable throughput or the maximum possible extruder speed. Higher speeds increase the shear rate and can thus improve the dispersion of additives.

[0195] The chemical conversion to polybutadiene polyurethane took place in the presence of an epoxy resin. The polybutadiene polyurethane (PBD-PU 3), including the epoxy resin, is composed as follows: Composition of PBD-PU 3:

[0196] In the following table, the epoxy resin already mixed in during polybutadiene polyurethane production is listed separately.

[0197] Composition of the thermally vulcanizable adhesive tape layer based on PBD-PU 3:

[0198] In the planetary roller extruder, powdered solids such as talc, chalk, lime (calcium oxide), sulfur, and an ultra-accelerator premix were incorporated into the PU base according to the recipe. The carbon black component was introduced into the downstream vented planetary roller extruder, where degassing also took place.

[0199] The plasticized polymers were fed into the extruder (Entex PWE type, four-shot, diameter 70 mm, equipped with standard spindles: 7, 7, 6, 6 per shot) via a drum melt and forced feed (polymer melt temperature 85 °C). The throughput was 50 kg / h, the speed 110 rpm. It was shown that the reduced spindle loading in the last two shots was advantageous for a low process temperature.

[0200] To reduce dosing complexity, premixes were prepared for talc and lime (P1) and for the ultraaccelerators ZBEC and TBzTD (P2). Chalk and sulfur were fed separately into the first shot of the planetary roller extruder, as was P1. P2 was fed into the second shot. Figure 1 shows the structure.

[0201] The four roller cylinders were tempered to 70 / 50 / 35 / 35 °C, respectively, and the central spindle was tempered to 20 °C. The melt temperature immediately behind the PWE was determined to be 76 °C.

[0202] The compound was transferred into the vented planetary roller extruder via a melt pump heated to 70 °C and a subsequent melt hose, also heated to 70 °C.

[0203] The three roller cylinders, as well as the central spindle, were tempered to 40 °C. The outlet temperature immediately downstream of the vented planetary roller extruder was determined to be 70 °C.

[0204] Figure 2 shows this part of the system schematically.

[0205] In the process known from WO 2018 / 059931 A1, a twin-screw extruder was used for venting instead of a vented planetary roller extruder. At a speed of 120 rpm, the individual zones were preselected to 50 °C. The hold-down device in the venting area ran at 250 rpm. The outlet temperature was approximately 85 °C.

[0206] The example shows that the preferred use of a vented planetary roller extruder allows for further reduction of process temperatures. Leaende to the Fiaures

[0207] Figure 1 : First planetary roller extruder 51) Input Polybutadiene Polyurethane 52) Inlet Sulphur, Chalk 53) Inlet Premix Ultra Accelerator (ZBEC / TBzTD) 54) Inlet Premix Talc & Lime 55): Inlet 56): Outlet Compound Figure 2 : Degassing planetary roller extruder1) Filling section with single screw 2) Roller cylinder 1 3) Roller cylinder 2 4) Roller cylinder 3 5) Melt pump for product discharge 6) Rear vacuum degassing via filling section 7) Feed opening for the plasticized polymers 8) Opening in the roller cylinder for vacuum degassing with product hold-down device (degassing (< 0.1 bar)) 9) Feed opening in the intermediate ring for liquids (supply of carbon black dispersion) 10) Feed opening in the roller cylinder for liquids 11) Vacuum pump 12) Product outlet 13) Temperature control circuit for central spindle 14) Temperature control circuit for roller cylinder 1 15) Temperature control circuit for roller cylinder 2 16) Temperature control circuit for roller cylinder 3 17) Intermediate ring

Claims

1. Method for producing a preferably pressure-sensitive adhesive using a first planetary roller extruder and a downstream second venting planetary roller extruder, where a) the first planetary roller extruder consists of a filling and dispersing zone operated atmospherically and comprising at least one roller cylinder, b) the polymers which form the thermally vulcanizable, meltable, preferably pressure-sensitive adhesive are supplied to the planetary roller extruder in a plastified state, c) the plastified polymers are fed into the at least one roller cylinder of the filling and dispersing zone, and specifically within the first third of the roller cylinder, d) solids such as thermal crosslinkers are added to the plastified polymers downstream of the addition of the plastified polymers in the filling and dispersing zone, in particular by means of a lateral screw feeder, via an opening of the at least one roller cylinder, e) the solids are dispersed in the plastified polymers in the filling and dispersing zone, f) the solids comprise at least thermal crosslinkers which are able to crosslink the plastified polymers for the purpose of increasing the molar mass of the polymers, g) the initial temperatures of the central spindle and of the at least one roller cylinder within the filling and dispersing zone are established such that there is no gelling of the plastified polymers blended with the thermal crosslinkers, h) the mixture of plastified polymers and solids, preferably thermal crosslinkers, is supplied, more preferably in-line, to a second venting planetary roller extruder, i) the second venting planetary roller extruder consists of a venting zone composed of at least one roller cylinder, j) the mixture of plastified polymers and solids, preferably thermal crosslinkers, is vented in the venting planetary roller extruder, k) the vented mixture of plastified polymers and solids, preferably thermal crosslinkers, is supplied, more preferably in-line, to a coating assembly.

2. Method according to Claim 1, characterized in that the filling and dispersing zone consists of preferably at least two, preferably four, coupled roller cylinders connected to one another via a geared intermediate ring.

3. Method according to Claim 1 or 2, characterized in that the planetary spindles of the first roller cylinder of the filling and dispersing zone and also the planetary spindles of the second venting planetary roller extruder are driven respectively via a common central spindle.

4. Method according to at least one of Claims 1 to 3, characterized in that the at least one roller cylinder and more particularly all the roller cylinders of the filling and dispersing zone of the first planetary roller extruder are fitted with a number of planetary spindles which is more than 70%, preferably more than 80%, of the maximum possible number of planetary spindles.

5. Method according to at least one of the preceding claims, characterized in that the at least one roller cylinder of the second planetary roller extruder, and more particularly all the roller cylinders of the venting zone, are fitted with a number of planetary spindles which is less than 75%, preferably less than 60%, of the maximum possible number of planetary spindles.

6. Method according to at least one of the preceding claims, characterized in that the at least one roller cylinder and more particularly all the roller cylinders of the filling and dispersing zone are fitted with a number of planetary spindles which is more than 70%, preferably more than 80%, of the maximum possible number of planetary spindles, and the at least one roller cylinder and more particularly all the roller cylinders of the venting zone are fitted with a number of planetary spindles which is less than 75%, preferably less than 60%, of the maximum possible number of planetary spindles.

7. Method according to at least one of the preceding claims, characterized in that the roller cylinder region of the venting zone consists of at least two, more preferably exactly three or four, coupled roller cylinders which are connected to one another via a geared intermediate ring and each possess at least one opening in the casing.

8. Method according to at least one of the preceding claims, characterized in that a single-screw conveying section is provided upstream of the first planetary roller extruder.

9. Method according to at least one of the preceding claims, characterized in that the plastified polymers are fed into the planetary roller extruder through an opening in the wall of the first roller cylinder casing or via an intermediate ring which is located between filling section and first roller cylinder and which possesses at least one radial hole for the purpose of feeding of the plastified polymers.

10. Method according to at least one of the preceding claims, characterized in that the plastified polymers are fed into the planetary roller extruder by means of a melt pump, by means of a single-screw or multi-screw extruder or by means of a drum or tank melting unit.

11. Method according to at least one of the preceding claims, characterized in that the thermally sensitive polymer mixture emerges from the planetary roller extruder by means of a melt pump coupled at the end of the last roller cylinder region.

12. Method according to at least one of the preceding claims, characterized in that the coating assembly is a calender or a die through which the mixture is applied to a carrier material.

13. Method according to at least one of the preceding claims, characterized in that the plastified polymers are polymers from the group of non-thermoplastic elastomers, thermoplastic synthetic rubbers, polyacrylates, polyurethanes, polyepoxides and mixtures in any ratios thereof.

14. Method according to at least one of the preceding claims, characterized in that the plastified polymers are blended with, for example, tackifying resins, fillers, plasticizers, oils, thixotropic agents and optionally further adjuvants.

15. Method according to at least one of the preceding claims, characterized in that the mixture emerging from the planetary roller extruder is a self-adhesive compound or is a curable structural adhesive compound.