Structural polyurethane adhesive with good adhesion after brief heating

DE502019012312D1Active Publication Date: 2024-10-31SIKA TECH AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502019012312
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-17
Filing Date
2019-07-02
Publication Date
2024-10-31
Estimated Expiration
2039-07-02

AI Technical Summary

Technical Problem

Two-component polyurethane adhesives face challenges in achieving sufficient adhesion and early strength, especially on KTL-coated substrates, during IR pre-curing, and require improvements in heat resistance and storage stability.

Method used

A polyurethane adhesive composition comprising a polyol component with a diol, a triol, a polyester polyol based on dimer fatty acids, and an aliphatic polyol, combined with a polyisocyanate component, which enhances early strength, adhesion, and storage stability, allowing for effective bonding on KTL-coated substrates even after IR pre-curing.

Benefits of technology

The adhesive demonstrates improved early strength, adhesion, and storage stability, with cohesive fracture patterns and high tensile shear strength immediately after IR pre-curing, maintaining mechanical properties over time, including heat resistance and extended pot life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The invention relates to the field of two-component polyurethane adhesives, in particular tough-elastic structural polyurethane adhesives. State of the art

[0002] Two-component polyurethane adhesives based on polyols and polyisocyanates have been in use for a long time. Two-component polyurethane adhesives have the advantage that they cure quickly after mixing and can therefore absorb and transfer higher forces within a short period of time. For use as structural adhesives, such adhesives must meet high demands in terms of strength and adhesion strength, as they represent elements of load-bearing structures. Document EP 2 700 666 A1 discloses two-component polyurethane adhesives that exhibit high strength and high extensibility with only a slight dependence of their mechanical properties on temperature, making them suitable for use as structural adhesives.

[0003] There is a particular demand for adhesives that develop a certain degree of adhesion as quickly as possible, i.e., that are resilient even before they are fully cured, allowing bonded parts to be moved early, or devices securing the bond to be removed early. This property is also referred to as "high early strength."

[0004] Particularly in automotive engineering, components coated with cathodic dip coatings (CDPs) can be bonded by briefly heating the applied adhesive shortly after application, particularly using IR radiation, to a temperature of approximately 40-60 seconds at a temperature of 150°C. Adequate adhesion to such substrates with the aforementioned IR pre-curing is difficult to achieve. This pre-curing typically affects only a portion (e.g., 10-20 percent) of the applied and joined adhesive bead; this process is also called "stitching." It increases the "handling strength," allowing the bonded components to be processed more quickly without detaching. Ensuring adequate adhesion immediately after IR pre-curing is particularly challenging, especially when the adhesive is still in a heated state.

[0005] The adhesives should also be able to cure to final strength both at ambient temperature and in a heat-accelerated curing process, and exhibit good adhesion to metallic and non-metallic substrates. Furthermore, these adhesives should possess high strength and high elongation. Description of the invention

[0006] The object of the present invention is therefore to provide a two-component polyurethane adhesive that exhibits high early strength after brief heating after application, particularly on cathodic dip-coated substrates. Preferably, the heated adhesive should exhibit sufficient adhesion immediately after IR pre-curing, especially while the adhesive is still in a heated state. Furthermore, these adhesives should exhibit high strength and high extensibility.

[0007] Surprisingly, this object is achieved with the polyurethane adhesive according to the invention. It was surprisingly found that the polyurethane adhesive according to the invention, by using a polyester polyol A3 as a component of the polyol component, it has increased early strength and particularly good adhesion, especially on cathodic dip-coated substrates.

[0008] In addition, the composition undergoes additional use of an aliphatic polyol A4 a faster adhesion build-up and an improvement in the storage stability of the polyol component.

[0009] Further aspects of the invention are the subject of further independent claims. Particularly preferred embodiments of the invention are the subject of the dependent claims. Ways to implement the invention

[0010] The present invention relates to a polyurethane adhesive consisting of a polyol component K1and a polyisocyanate component K2; where the polyol component K1 at least one diol A1 with two primary hydroxyl groups and a molecular weight in the range of 60 to 150 g / mol, at least one triol A2 with an average molecular weight in the range of 1,000 to 10,000 g / mol, at least one polyester polyol A3 based on dimer fatty acids and / or dimer fatty alcohols, in particular based on dimer fatty acids; and the polyisocyanate component K2 at least one polyisocyanate B1 and / or at least one polyurethane polymer containing isocyanate groups B2 includes.

[0011] In this document, the prefix "poly" in substance names such as "polyol", "polyisocyanate", "polyether" or "polyamine" indicates that the respective substance formally contains more than one of the functional groups mentioned in its name per molecule.

[0012] In this document, "molecular weight" refers to the molar mass (in grams per mole) of a molecule. "Mean molecular weight" refers to the number-average molecular weight Mn of an oligomeric or polymeric mixture of molecules, which is usually determined by GPC against polystyrene as a standard.

[0013] A "primary hydroxyl group" is an OH group that is bonded to a C atom with two hydrogens.

[0014] In this document, the term "strength" refers to the strength of the cured adhesive, whereby strength refers in particular to the tensile strength and the modulus of elasticity (E-modulus), especially in the elongation range 0.05 to 0.25%.

[0015] In this document, "room temperature" is defined as 23 °C.

[0016] In this document, the term "fatty acids" refers in particular to fatty acids as described in the Rompp Chemie Lexikon, 10th edition, Thieme Verlag.

[0017] The term "soybean oil" (also called soybean oil) in this document refers in particular to soybean oil as described in the Rompp Chemie Lexikon, 10th edition, Thieme Verlag.

[0018] The term "castor oil" (also called castor oil or castor oil) in this document refers in particular to castor oil as described in the Rompp Chemie Lexikon, 10th edition, Thieme Verlag.

[0019] The term "open time", also called "open time" or "open waiting time", is primarily understood in this document to mean the open time as described in Römpp Chemie Lexikon, online version, Georg Thieme Verlag, accessed on 16 July 2018.

[0020] In this document, the term "cathodic dip coating (KTL)" refers primarily to cationic electrocoatings, as described in Römpp Chemie Lexikon, online version, Georg Thieme Verlag, accessed on 16 July 2018.

[0021] The polyol component K1 comprises at least one diol A1 with two primary hydroxyl groups and a molecular weight in the range of 60 to 150 g / mol. Diols with a molecular weight of more than 150 g / mol result in significantly lower strengths in the cured state.

[0022] As diol A1 Particularly suitable are 1,2-ethanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, and diethylene glycol. These diols have primary, sterically almost unhindered hydroxyl groups, which are particularly reactive with isocyanate groups.

[0023] Particularly preferred is the diol A1 a linear diol, in particular selected from the group consisting of 1,3-propanediol, 1,4-butanediol, and 1,5-pentanediol. These diols are particularly easy to handle because they are barely hydrophilic and liquid at room temperature. They form rich chain segments at urethane bonds during the curing of the adhesive, which promotes high strength with good extensibility over a wide temperature range. Of these, 1,4-butanediol and 1,5-pentanediol are particularly preferred, with 1,4-butanediol being the most preferred.

[0024] As a triplet A2A polyoxyalkylene triol, also called a polyether triol, is particularly suitable. These are polymerization products of ethylene oxide, 1,2-propylene oxide, 1,2- or 2,3-butylene oxide, or mixtures thereof. They are typically polymerized using a starter molecule with three active hydrogen atoms, such as glycerol, 1,1,1-trimethylolethane, 1,1,1-trimethylolpropane, or mixtures thereof.

[0025] Preferably as a triplet A2 are polyoxypropylene triols, polyoxyethylene triols and polyoxypropylene-polyoxyethylene triols.

[0026] The triol is particularly preferred A2 primary hydroxyl groups, most preferably exclusively primary hydroxyl groups.

[0027] Particularly preferred as a triol A2are so-called "EO-endcapped" (ethylene oxide-endcapped) polyoxypropylene triols. These are special polyoxypropylene polyoxyethylene triols obtained, for example, by further alkoxylating pure polyoxypropylene triols with ethylene oxide after polypropoxylation, thus possessing primary hydroxyl groups. Compared to pure polyoxyethylene triols, they have the advantage of being less hydrophilic and liquid at room temperature.

[0028] The triplet A2 preferably has an average OH functionality in the range of 2.2 to 3. With such triols A2 adhesives with good mechanical properties are obtained.

[0029] The triplet A2Preferably, the average molecular weight is in the range of 3,000 to 8,000 g / mol, particularly preferably 4,000 to 6,000 g / mol, and most preferably 4,500 to 5,000 g / mol. Such a triol exhibits a good combination of high functionality and chain length, resulting in an adhesive with good mechanical properties.

[0030] The polyol component K1 further comprises at least one polyester polyol A3 based on dimer fatty acids and / or dimer fatty alcohols.

[0031] Preferably, the at least one polyester polyol is A3 a polyester polyol A3 based on dimer fatty acids.

[0032] Preferably, the at least one polyester polyol is A3 a polyester polyol A3 based on dimer fatty acids from C10 - C30 fatty acids, preferably C12 - C25 fatty acids, especially C14 - C22 fatty acids.

[0033] Preferably, the at least one polyester polyol is A3 a polyester polyol A3 based on dimer fatty acids selected from the list consisting of dimerization products of fatty acids selected from the list consisting of oleic acid, linoleic acid, linolenic acid, palmitoleic acid and elaidic acid.

[0034] The dimerization products of unsaturated fatty acid mixtures obtained during the hydrolysis of natural fats and oils, e.g., sunflower oil, soybean oil, olive oil, rapeseed oil, cottonseed oil, and tall oil, can also be used. In addition to the dimer fatty acids, dimerization typically results in the presence of varying amounts of oligomeric fatty acids (so-called "trimers") and residues of monomeric fatty acids (so-called "monomers") or esters thereof. Suitable dimer fatty acids have a dimer acid content of more than 60%, preferably more than 75%, more preferably in the range of 90 to 99.5%, especially 95 to 99%, and especially 97 to 99%.

[0035] Commercially available suitable polyester polyols A3include amorphous materials, preferably materials that are liquid at room temperature, available materials are, for example, Dynacoll ®< 7360, 7380, 7330, 7231, 7250 (Evonik), Rucoflex ®< S-105-10 (Bayer), Stepanpol ®< PN110 (Stepan), Priplast ®< 1838, 3196 (Croda).

[0036] Preferably, the polyester polyol has A3 an average molecular weight in the range of 500 to 10,000 g / mol, 500 to 7,000 g / mol, 500 to 5,000 g / mol, in particular 1,000 to 3,000 g / mol.

[0037] Preferably, the at least one polyester polyol is A3 a diol.

[0038] Such polyester polyols A3are advantageous in that the adhesive exhibits better adhesion to e-coated substrates after pre-curing, especially after IR pre-curing at 150 °C for 40 seconds. This is particularly true when the tensile shear strength is determined immediately after pre-curing, when the adhesive is still in a heated state. Furthermore, such polyester polyols A3 to an improvement in pot life.

[0039] Preferably, the polyol component comprises K1 furthermore at least one aliphatic polyol A4, which is a hydroxylation product of a triglyceride based on fatty acids.

[0040] The fatty acids are preferably hydroxyfunctional fatty acids. The preferred hydroxyl groups are aliphatically bound primary and / or secondary hydroxyl groups, especially aliphatically bound secondary hydroxyl groups.

[0041] The fatty acids are preferably fatty acids which individually contain between 10 and 30 carbon atoms, in particular between 16 and 20 carbon atoms, and are free of aromatic groups.

[0042] Preferred aliphatic polyols A4 have an average OH functionality in the range of 2 to 8, more preferably from 2 to 4 and most preferably from 2 to 3.

[0043] The aliphatic polyols A4 are preferably liquid at 25°C and have hydroxyl values ​​between 20 and 300 mg KOH / g (corresponding to a hydroxyl equivalent weight range of 2800 to 190). An even more preferred range of hydroxyl values ​​is from 50 to 200 mg KOH / g (corresponding to a hydroxyl equivalent weight range of 1100 to 280).

[0044] Preferably, the aliphatic polyol is A4a hydroxylation product based on soybean oil, also called soybean oil, or a hydroxylation product based on castor oil, particularly preferably a hydroxylation product based on castor oil.

[0045] Particularly preferably, the aliphatic polyol is A4 a hydroxylation product of soybean oil, also called soybean oil, or a hydroxylation product of castor oil, most preferably a hydroxylation product of castor oil.

[0046] Such aliphatic polyols A4 are advantageous in that the adhesive has a faster adhesion build-up, especially after 1 h or after 24 h, at room temperature.

[0047] Furthermore, the presence of the aliphatic polyol A4to an improvement in pot life as well as higher values ​​of the Young's modulus, tensile strength and elongation at break. Furthermore, it was surprisingly found that the addition of aliphatic polyol A4 to improve the storage stability of the component K1 leads.

[0048] Preferably the diol A1, the triplet A2, the polyester polyol A3 and optionally the aliphatic polyol A4 present in the adhesive in such an amount that the weight ratio (A1+A2) / (A3+A4) in the range of 0.3 to 1.3, 0.35 to 1.1, 0.4 to 0.9, in particular 0.5 to 0.8.

[0049] A weight ratio of less than 0.3 is disadvantageous in that it leads to lower values ​​for strength and elastic modulus. A weight ratio of more than 1.3 is disadvantageous in that it leads to lower values ​​for adhesion after pre-curing.

[0050] Furthermore, it is advantageous if the diol A1 and the triplet A2 are present in the adhesive in such an amount that the weight ratio A1 / A2 in the range of 0.1 to 0.5, 0.15 to 0.4, 0.2 to 0.4, in particular 0.25 to 0.35.

[0051] Such a weight ratio is advantageous in that it provides particularly advantageous values ​​for strength and modulus of elasticity for a structural adhesive.

[0052] It may also be advantageous if the polyester polyol A3 and the aliphatic polyol, if present A4 are present in the adhesive in such an amount that the weight ratio A3 / A4 in the range of 1.0 to 3.0, 1.2 to 2.5, 1.3 to 2.0, 1.3 to 1.8, in particular 1.35 to 1.6.

[0053] A weight ratio of less than 1.0 is disadvantageous in that it leads to lower adhesion values ​​after pre-curing. A weight ratio of more than 3.0 is disadvantageous in that it leads to lower storage stability and reduced heat resistance.

[0054] The polyisocyanate component K2 comprises at least one polyisocyanate B1 and / or at least one polyurethane polymer containing isocyanate groups B2. Preferably, the polyisocyanate component comprises K2 at least one polyurethane polymer containing isocyanate groups B2.

[0055] As polyisocyanate B1 Particularly suitable are monomeric di- or triisocyanates, as well as oligomers, polymers and derivatives of monomeric di- or triisocyanates, as well as any mixtures thereof.

[0056] Suitable aromatic monomeric di- or triisocyanates are in particular 2,4- and 2,6-tolylene diisocyanate and any mixtures of these isomers (TDI), 4,4'-, 2,4'- and 2,2'-diphenylmethane diisocyanate and any mixtures of these isomers (MDI), 1,3- and 1,4-phenylene diisocyanate, 2,3,5,6-tetramethyl-1,4-diisocyanatobenzene, naphthalene-1,5-diisocyanate (NDI), 3,3'-dimethyl-4,4'-diisocyanatodiphenyl (TODI), dianisiside diisocyanate (DADI), 1,3,5-tris-(isocyanatomethyl)benzene, tris-(4-isocyanatophenyl)methane and tris-(4-isocyanatophenyl)thiophosphate.

[0057] Suitable aliphatic monomeric di- or triisocyanates are in particular 1,4-tetramethylene diisocyanate, 2-methylpentamethylene-1,5-diisocyanate, 1,6-hexamethylene diisocyanate (HDI), 2,2,4- and 2,4,4-trimethyl-1,6-hexamethylene diisocyanate (TMDI), 1,10-decamethylene diisocyanate, 1,12-dodecamethylene diisocyanate, lysine and lysine ester diisocyanate, cyclohexane-1,3- and -1,4-diisocyanate, 1-methyl-2,4- and -2,6-diisocyanatocyclohexane and any mixtures of these isomers (HTDI or H 6 TDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethyl-cyclohexane (=isophorone diisocyanate or IPDI), perhydro-2,4'- and -4,4'-diphenylmethane diisocyanate (HMDI or H 12 MDI), 1,4-diisocyanato-2,2,6-trimethylcyclohexane (TMCDI), 1,3- and 1,4-bis-(isocyanatomethyl)cyclohexane, m- and p-xylylene diisocyanate (m- and p-XDI), m- and p-tetramethyl-1,3- and -1,4-xylylene diisocyanate (m- and p-TMXDI), bis-(1-isocyanato-1-methyl-ethyl)naphthalene, dimer and trimer fatty acid isocyanates such as 3,6-bis-(9-isocyanatononyl)-4,5-di-(1-heptenyl)cyclohexene (dimeryl diisocyanate) and α,α,α',α',α",α"-hexamethyl-1,3,5-mesitylene triisocyanate.

[0058] Suitable oligomers, polymers and derivatives of the above-mentioned monomeric di- and triisocyanates are in particular derived from MDI, TDI, HDI and IPDI.Of these, commercially available types are particularly suitable, in particular HDI biurets such as Desmodur ®< N 100 and N 3200 (from Bayer), Tolonate ®< HDB and HDB-LV (from Rhodia) and Duranate ®< 24A-100 (from Asahi Kasei); HDI isocyanurates such as Desmodur ®< N 3300, N 3600 and N 3790 BA (all from Bayer), Tolonate ®< HDT, HDT-LV and HDT-LV2 (from Rhodia), Duranate ®< TPA-100 and THA-100 (from Asahi Kasei) and Coronate ®< HX (from Nippon Polyurethane); HDI uretdiones such as Desmodur ®< N 3400 (from Bayer); HDI iminooxadiazinediones such as Desmodur ®< XP 2410 (from Bayer); HDI allophanates such as Desmodur ®< VP LS 2102 (from Bayer); IPDI isocyanurates, such as in solution as Desmodur ®< Z 4470 (from Bayer) or in solid form as Vestanat ®< T1890 / 100 (from Degussa); TDI oligomers such as Desmodur ®< IL (from Bayer); and mixed isocyanurates based on TDI / HDI, for example as Desmodur ®< HL (from Bayer).Also particularly suitable are forms of MDI which are liquid at room temperature (so-called "modified MDI"), which are mixtures of MDI with MDI derivatives, such as in particular MDI carbodiimides or MDI uretonimines or MDI urethanes, known under trade names such as Desmodur ®< CD, Desmodur ®< PF, Desmodur ®< PC (all from Bayer) or Isonate ®< M 143 (from Dow), as well as mixtures of MDI and MDI homologues (polymeric MDI or PMDI), available under trade names such as Desmodur ®< VL, Desmodur ®< VL50, Desmodur ®< VL R10, Desmodur ®< VL R20, Desmodur ®< VH 20 N and Desmodur ®< VKS 20F (all from Bayer), Isonate ®< M 309, Voranate ®< M 229 and Voranate®< M 580 (all from Dow) or Lupranat®< M 10 R (from BASF). In practice, the aforementioned oligomeric polyisocyanates typically represent mixtures of substances with different degrees of oligomerization and / or chemical structures. They preferably have an average NCO functionality of 2.1 to 4.0.

[0059] Preferred as polyisocyanate B1 are forms of MDI that are liquid at room temperature. These include, in particular, so-called polymeric MDI and MDI containing oligomers or derivatives thereof. The MDI content (=4,4'-, 2,4'-, or 2,2'-diphenylmethane diisocyanate and any mixtures of these isomers) of such liquid forms of MDI is in particular 50 to 95% by weight, especially 60 to 90% by weight.

[0060] Particularly preferred as polyisocyanate B1 are polymeric MDI and in particular MDI types that are liquid at room temperature and contain proportions of MDI carbodiimides or their adducts.

[0061] With these polyisocyanates B1 Particularly good processing properties and particularly high strength are achieved.

[0062] The polyisocyanate component K2 preferably comprises at least one polyurethane polymer containing isocyanate groups B2.

[0063] The polyurethane polymer B2 Preferably, it contains 50 to 95 mass percent, in particular 70 to 90 mass percent, of polyoxyalkylene units, particularly preferably polyoxyethylene and / or polyoxypropylene units, in particular polyoxypropylene units. Such a polyurethane polymer has a low viscosity and allows for good extensibility.

[0064] The polyurethane polymer B2 preferably has an average molecular weight in the range of 1,000 to 20,000 g / mol, particularly preferably 2,000 to 10,000 g / mol.

[0065] The polyurethane polymer B2 Preferably, the polyurethane polymer has an average NCO functionality in the range of 1.7 to 3, particularly 1.8 to 2.5. Such a polyurethane polymer enables good processing properties and good mechanical properties in the cured state.

[0066] Particularly preferably, the polyurethane polymer B2a medium NCO functionality in the range of 2.05 to 2.5. Such a polyurethane polymer enables particularly good extensibility with high strength.

[0067] The polyurethane polymer B2 preferably has a content of free isocyanate groups of 1 to 10% by weight, particularly preferably 1 to 5% by weight.

[0068] A suitable polyurethane polymer containing isocyanate groups B2is obtainable from the reaction of at least one polyisocyanate with at least one polyol. This reaction can be carried out by reacting the polyol and the polyisocyanate using conventional methods, for example at temperatures of 50°C to 100°C, optionally with the use of suitable catalysts. The polyisocyanate is dosed such that its isocyanate groups are present in a stoichiometric excess relative to the hydroxyl groups of the polyol. The polyisocyanate is advantageously dosed such that an NCO / OH ratio of 1.3 to 5, in particular one of 1.5 to 3, is maintained. The "NCO / OH ratio" is understood to mean the ratio of the number of isocyanate groups used to the number of hydroxyl groups used. As a polyol for the production of a polyurethane polymer B2The following commercially available polyols or mixtures thereof are particularly suitable: polyoxyalkylene polyols, also called polyether polyols or oligoetherols, which are polymerization products of ethylene oxide, 1,2-propylene oxide, 1,2- or 2,3-butylene oxide, oxetane, tetrahydrofuran or mixtures thereof, possibly polymerized with the aid of a starter molecule with two or more active hydrogen atoms such as water, ammonia or compounds with several OH or NH groups such as 1,2-ethanediol, 1,2- and 1,3-propanediol, neopentyl glycol, diethylene glycol, triethylene glycol, the isomeric dipropylene glycols and tripropylene glycols, the isomeric butanediols, pentanediols, hexanediols, heptanediols, octanediols, nonanediols, decanediols, undecanediols, 1,3- and 1,4-Cyclohexanedimethanol, bisphenol A, hydrogenated bisphenol A, 1,1,1-trimethylolethane, 1,1,1-trimethylolpropane, glycerin, aniline,as well as mixtures of the aforementioned compounds. Both polyoxyalkylene polyols with a low degree of unsaturation (measured according to ASTM D-2849-69 and expressed in milliequivalents of unsaturation per gram of polyol (mEq / g)), produced, for example, using so-called double metal cyanide complex catalysts (DMC catalysts), and polyoxyalkylene polyols with a higher degree of unsaturation, produced, for example, using anionic catalysts such as NaOH, KOH, CsOH, or alkali metal alkoxides, can be used. Polyoxyalkylene diols or polyoxyalkylene triols, in particular polyoxyethylene and polyoxypropylene diols and triols, are particularly suitable. Polyoxyalkylene diols and triols with a degree of unsaturation lower than 0.02 mEq / g and with a molecular weight in the range of 1,000 - 30,000 g / mol, are particularly suitable.as well as polyoxypropylene diols and triols with a molecular weight of 400–8,000 g / mol. Particularly suitable are so-called ethylene oxide-terminated ("EO-endcapped") polyoxypropylene polyols. Styrene-acrylonitrile or acrylonitrile-methyl methacrylate-grafted polyether polyols. Polyester polyols, also called oligoesterols, produced by known processes, in particular the polycondensation of hydroxycarboxylic acids or the polycondensation of aliphatic and / or aromatic polycarboxylic acids with di- or polyhydric alcohols. Particularly suitable polyester polyols are those which are prepared from di- to trihydric, in particular dihydric, alcohols, such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-hexanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, 1,12-dodecanediol, 1,12-hydroxystearyl alcohol, 1,4-cyclohexanedimethanol,Dimer fatty acid diol (dimerdiol), neopentyl glycol hydroxypivalate, glycerol, 1,1,1-trimethylolpropane, or mixtures of the aforementioned alcohols, with organic di- or tricarboxylic acids, especially dicarboxylic acids, or their anhydrides or esters, such as succinic acid, glutaric acid, adipic acid, trimethyladipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, maleic acid, fumaric acid, dimer fatty acid, phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, dimethyl terephthalate, hexahydrophthalic acid, trimellitic acid, and trimellitic anhydride, or mixtures of the aforementioned acids, as well as polyester polyols made from lactones, such as ε-caprolactone, and starters such as the aforementioned di- or trihydric alcohols. Particularly suitable polyester polyols are polyester diols. Polycarbonate polyols, such as those obtained by reacting, for example, the above-mentioned alcohols used to construct the polyester polyols with dialkyl carbonates,Diaryl carbonates or phosgene are accessible. Block copolymers bearing at least two hydroxyl groups, which have at least two different blocks with a polyether, polyester and / or polycarbonate structure of the type described above, in particular polyetherpolyester polyols. Polyacrylate and polymethacrylate polyols. Polyhydroxy-functional fats and oils, for example natural fats and oils, in particular castor oil; or polyols obtained by chemical modification of natural fats and oils - so-called oleochemical polyols, for example the epoxy polyesters or epoxy polyethers obtained by epoxidation of unsaturated oils and subsequent ring opening with carboxylic acids or alcohols, or polyols obtained by hydroformylation and hydrogenation of unsaturated oils; or from natural fats and oils by degradation processes such as alcoholysis or ozonolysis and subsequent chemical linkage, for example by transesterification or dimerization.polyols obtained from the degradation products thus obtained or derivatives thereof. Suitable degradation products of natural fats and oils are, in particular, fatty acids and fatty alcohols, as well as fatty acid esters, in particular the methyl esters (FAME), which can be derivatized to hydroxy fatty acid esters, for example, by hydroformylation and hydrogenation. Polyhydrocarbon polyols, also called oligohydrocarbonols, such as, for example, polyhydroxy-functional polyolefins, polyisobutylenes, polyisoprenes; polyhydroxy-functional ethylene-propylene, ethylene-butylene, or ethylene-propylene-diene copolymers, such as those produced, for example, by Kraton Polymers; polyhydroxy-functional polymers of dienes, in particular of 1,3-butadiene, which can also be produced, in particular, from anionic polymerization; polyhydroxy-functional copolymers of dienes such as 1,3-butadiene or diene mixtures and vinyl monomers such as styrene, acrylonitrile, vinyl chloride, vinyl acetate, vinyl alcohol,Isobutylene and isoprene, for example polyhydroxy-functional acrylonitrile / butadiene copolymers, such as those produced from epoxides or amino alcohols and carboxyl-terminated acrylonitrile / butadiene copolymers (for example commercially available under the name Hypro ®< (formerly Hycar ®< ) CTBN and CTBNX and ETBN from Nanoresins AG, Germany, or Emerald Performance Materials LLC); as well as hydrogenated polyhydroxy-functional polymers or copolymers of dienes.

[0069] As a polyol for the production of a polyurethane polymer B2 Preferred are polyoxyalkylene polyols, polyester polyols, polycarbonate polyols, and polyacrylate polyols. Particular preference is given to polyoxyalkylene polyols, especially polyoxypropylene polyols and polyoxyethylene-polyoxypropylene mixed polyols.

[0070] The polyol for producing a polyurethane polymer B2preferably has an average molecular weight in the range of 500 to 20,000 g / mol, in particular 1,000 to 8,000 g / mol.

[0071] The polyol for producing a polyurethane polymer B2 is preferably a diol or a mixture of at least one diol and at least one triol, in particular a mixture of at least one diol and at least one triol.

[0072] As a polyisocyanate for the production of a polyurethane polymer B2The following commercially available polyisocyanates or mixtures thereof are particularly suitable: 2,4- and 2,6-tolylene diisocyanate and any mixtures of these isomers (TDI), 4,4'-, 2,4'- and 2,2'-diphenylmethane diisocyanate and any mixtures of these isomers (MDI), 1,3- and 1,4-phenylene diisocyanate, 2,3,5,6-tetramethyl-1,4-diisocyanatobenzene, naphthalene-1,5-diisocyanate (NDI), 3,3'-dimethyl-4,4'-diisocyanatodiphenyl (TODI), 1,3,5-tris-(isocyanatomethyl)benzene, 2-methylpentamethylene-1,5-diisocyanate, 1,6-hexamethylene diisocyanate (HDI), 2,2,4- and 2,4,4-trimethyl-1,6-hexamethylene diisocyanate (TMDI), 1,10-decamethylene diisocyanate, 1,12-dodecamethylene diisocyanate, lysine and lysine ester diisocyanate, cyclohexane-1,3- and -1,4-diisocyanate, 1-methyl-2,4- and -2,6-diisocyanatocyclohexane and any mixtures of these isomers (HTDI or H 6 TDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethyl-cyclohexane (=isophorone diisocyanate or IPDI), perhydro-2,4'- and -4,4'-Diphenylmethane diisocyanate (HMDI or H 12 MDI), 1,4-diisocyanato-2,2,6-trimethylcyclohexane (TMCDI), 1,3- and 1,4-bis(isocyanatomethyl)cyclohexane, m- and p-xylylene diisocyanate (m- and p-XDI), and m- and p-tetramethyl-1,3- and -1,4-xylylene diisocyanate (m- and p-TMXDI). Preferred are MDI, TDI, IPDI, and HDI. MDI is particularly preferred.

[0073] Most preferred is 4,4'-diphenylmethane diisocyanate.

[0074] Preferably, the polyurethane polymer containing isocyanate groups is B2 Obtainable from the reaction of 4,4'-diphenylmethane diisocyanate with at least one polyol. This results in particularly effective hard segments and thus particularly high strengths during the curing of the adhesive.

[0075] Preferably, the polyisocyanate is B1 and the one used to produce the polyurethane prepolymer B2 used polyisocyanate is a different type of polyisocyanate.

[0076] The polyurethane polymer is preferably produced B2 not in the presence of the polyisocyanate B1.

[0077] A particularly preferred polyurethane adhesive contains a polyisocyanate component K2, comprehensive at least one polyurethane polymer containing isocyanate groups B2, wherein its urethane groups and free isocyanate groups are preferably derived from 4,4'-diphenylmethane diisocyanate.

[0078] The polyurethane adhesive can be used as a component of the polyol component K1 additionally contain other substances that react with isocyanate groups. In particular, the polyol component K1 at least one polyol and / or at least one low molecular weight di- or polyhydric alcohol, which are used to produce the polyurethane polymer B2 were mentioned.

[0079] Furthermore, the polyurethane adhesive may contain catalysts that accelerate the reaction of hydroxyl groups with isocyanate groups, in particular tin, zinc and bismuth organometallic catalysts, for example dibutyltin dilaurate, or tertiary amines, amidines or guanidines, for example 1,4-diazabicyclo[2.2.2]octane (DABCO) or 1,8-diazabicyclo[5.4.0]-undec-7-ene (DBU).

[0080] To achieve heat activation, tertiary amines, amidines, or guanidines, in particular, can reversibly form a salt with phenol or carboxylic acids, especially phenolic or other aromatic carboxylic acids, which decomposes upon increasing temperature. Therefore, the polyurethane adhesive preferably contains at least one catalyst selected from the list consisting of tertiary amines, amidines, and guanidines, which are present as salts with phenol or carboxylic acids. In particular, this salt is decomposed upon increasing temperature, especially at a temperature of 80–170°C.

[0081] Furthermore, the polyurethane adhesive may contain additional components, as known to those skilled in the art from two-component polyurethane chemistry. These may be present in only one component or in both. Such additional components may include, in particular, solvents, plasticizers and / or extenders, fillers such as carbon blacks, chalks, or phyllosilicates, as well as pigments, rheology modifiers such as amorphous silicas, drying agents such as zeolites, adhesion promoters such as trialkoxysilanes, stabilizers against oxidation, heat, light, and UV radiation, flame-retardant substances, and surface-active substances, particularly wetting agents.

[0082] The polyol component K1 and the polyisocyanate component K2are advantageously formulated such that their mixing ratio by volume is in the range of 1:3 and 3:1, in particular 1:2 and 2:1. It is particularly preferably in the range of 0.8:1.2.

[0083] The mixing ratio between the components K1 and K2 is preferably such that in the mixed polyurethane adhesive the ratio between the number of isocyanate groups and the number of groups reactive towards isocyanates, in particular the sum of OH and NH 2 groups, before curing is in the range from 1.3 to 0.8, 1.2 to 0.9, 1.2 to 0.95, 1.2 to 1, preferably 1.15 to 1.05.

[0084] The production of the two components K1 and K2 is carried out separately and, at least for the polyisocyanate component K2, under exclusion of moisture. The components K1 and K2are typically stored in their own containers. The other components of the polyurethane adhesive can be used as part of the polyol component K1 or the polyisocyanate component K2 be present, with further components reactive towards isocyanate groups preferably being a component of the polyol component K1 A suitable container for storing the respective component is, in particular, a drum, a hobbock, a bag, a bucket, a can, a cartridge or a tube. The components K1 and K2 Both are storage-stable, which means that they can be stored for several months up to a year or longer before use without their respective properties changing to an extent relevant to their use.

[0085] The polyol component K1 and the polyisocyanate component K2are stored separately from each other before the adhesive is applied and are only mixed together during or immediately before use. They are preferably packaged in two separate compartments.

[0086] In a further aspect, the invention comprises a package consisting of a package with two separate chambers, each of which contains the polyol component K1 or the polyisocyanate component K2 of the polyurethane adhesive.

[0087] Preferred packaging of this type is, on the one hand, side-by-side double cartridges or coaxial cartridges, in which two tubular chambers are arranged next to each other or inside each other and are sealed airtight and moisture-tight with pistons. The components can be pressed out of the cartridge via the propulsion of these pistons. The sides of the tubes opposite the pistons are modified, if necessary via an adapter, such that the chamber openings are directly connected to each other via a partition. A thread is advantageously provided in the area of ​​the outlet opening of the chambers so that a static mixer or a dynamic mixer can be tightly attached. Such packaging is particularly preferred for small applications, especially for filling quantities up to 1 liter.

[0088] For applications involving larger quantities, especially in industrial manufacturing, the two components are best filled and stored in drums or hobbocks. During use, the components are extruded via feed pumps and metered via lines into a mixing device, as is typically used for two-component adhesives in industrial manufacturing.

[0089] Mixing is typically done using static mixers or dynamic mixers. During mixing, care must be taken to ensure that the polyol component K1 and the polyisocyanate component K2They should be mixed as homogeneously as possible. If the two components are poorly mixed, local deviations from the optimal mixing ratio will occur, which can result in a deterioration in the mechanical properties. To visually check the mixing quality, it can be advantageous if the two components have two different colors. Good mixing is achieved when the mixed adhesive has a homogeneous mixed color, without visible streaks or smears.

[0090] When the polyol component comes into contact K1 with isocyanate groups of the polyisocyanate component K2 Curing begins through a chemical reaction. The hydroxyl groups of the diol react A1, of the triplet A2 and the polyester polyol A3and any other substances that may be present that are reactive toward isocyanate groups. Excess isocyanate groups react with the moisture present. As a result of these reactions, the polyurethane adhesive cures into a solid material. This process is also known as crosslinking.

[0091] A further subject matter of the invention is therefore also a cured polyurethane adhesive obtained from the curing of a polyurethane adhesive as described in the present document.

[0092] A further aspect of the present invention relates to a method for bonding a first substrate to a second substrate, which comprises the steps: a) Mixing the previously described polyol component K1 and polyisocyanate component K2,b) Applying the mixed polyurethane adhesive to at least one of the substrate surfaces to be bonded, c) Joining the substrates to be bonded within the open time, d) Heating the polyurethane adhesive to a temperature of 80 - 170 °C, in particular for 30 seconds - 5 minutes, e) Curing the polyurethane adhesive.

[0093] The two substrates can be made of the same or different materials.

[0094] In this bonding process, suitable substrates are particularly Glass, glass ceramics, glass mineral fiber mats; metals and alloys, such as aluminum, iron, steel, and non-ferrous metals, as well as surface-treated metals and alloys, such as galvanized or chrome-plated metals, in particular cathodic dip-coated metals and alloys; coated and painted substrates, such as powder-coated metals or alloys and painted sheets; Plastics such as polyvinyl chloride (rigid and soft PVC), acrylonitrile-butadiene-styrene copolymers (ABS), polycarbonate (PC), polyamide (PA), poly(methyl methacrylate) (PMMA), polyester, epoxy resins, in particular epoxy-based thermosets, polyurethanes (PUR), polyoxymethylene (POM), polyolefins (PO), polyethylene (PE) or polypropylene (PP), ethylene / propylene copolymers (EPM) and ethylene / propylene / diene terpolymers (EPDM), whereby the plastics can preferably be surface-treated by means of plasma, corona or flames;Fiber-reinforced plastics, such as carbon fiber-reinforced plastics (CFRP), glass fiber-reinforced plastics (GRP), and sheet molding compounds (SMC); wood, wood materials bonded with resins, for example phenolic, melamine, or epoxy resins, resin-textile composites, and other so-called polymer composites; as well as concrete, mortar, brick, gypsum, and natural stone such as granite, limestone, cinderblock, or marble.

[0095] In this process, one or both substrates are preferably a metal or an alloy, in particular a cathodic dip-coated metal or a cathodic dip-coated alloy.

[0096] If necessary, the substrates can be pretreated before applying the adhesive. Such pretreatments include, in particular, physical and / or chemical cleaning processes, as well as the application of an adhesion promoter, adhesion promoter solution, or primer.

[0097] Furthermore, it may be advantageous if in step d) the polyurethane adhesive is heated to a temperature of 90 - 170 °C, preferably to a temperature of 100 - 160 °C, in particular to a temperature of 120 - 160 °C, particularly preferably to a temperature of 140 - 160 °C.

[0098] Preferably, the polyurethane adhesive is heated to the aforementioned temperature for 30 seconds - 5 minutes, 30 seconds - 4 minutes, 30 seconds - 3 minutes, 40 seconds - 2 minutes.

[0099] Furthermore, it may be advantageous if only a portion of the applied polyurethane adhesive, in particular 5-30%, preferably 10-20%, is heated in step d). Preferably, the polyurethane adhesive is applied in step b) in the form of an adhesive bead, and 5-30%, preferably 10-20%, of the length of the applied adhesive bead is heated in step d).

[0100] Preferably, the adhesive heated in step d) has a tensile shear strength of more than 1.5 MPa, more than 2.0 MPa, in particular more than 2.2 MPa, immediately after step d), in particular 10-100 seconds, preferably 15-30 seconds. Furthermore, the adhesive preferably exhibits a cohesive fracture pattern.

[0101] The heating in step d) takes place in particular by means of an infrared radiator, a hot air dryer, an induction heater or in an oven, particularly preferably by means of an infrared radiator.

[0102] This described bonding process results in an article in which the adhesive bonds two substrates together.

[0103] This article is in particular a sandwich element of a lightweight structure, a building, for example a bridge, an industrial good or a consumer good, in particular a window, a rotor blade of a wind turbine or a means of transport, in particular a vehicle, preferably an automobile, a bus, a lorry, a rail vehicle or a ship, as well as an aircraft or a helicopter; or an attachment of such an article.

[0104] The described polyurethane adhesive has very good properties as a structural adhesive.

[0105] A structural adhesive is an adhesive that, when cured, forms part of the supporting structure of the bonded components. The structural adhesive is therefore an important link in the construction, joining two components or substrates. Accordingly, high demands are placed on its mechanical properties. Examples substances used:

[0106] A1, Diol 1,4-Butanediol from LyondellBasell A2, Triplet EO-endcapped polyoxypropylene triol, OH number 35.0 mg KOH / g (Voranol ®< CP 4755 from Dow) A3, polyester polyol Polyesterdiol liquid at room temperature based on dimer fatty acids of C14-C22 fatty acids, dimer acid content of more than 95%, average molecular weight approx. 2000 g / mol. A4, aliphatic polyol Hydroxylated castor oil liquid at room temperature, OH number approx. 120 mg KOH / g, average OH functionality of approx. 2.2. Polyether diol EO-endcapped polyoxypropylene diol, OH number approx. 28 mg KOH / g (Voranol ®< EP 1900 from Dow) Cat Acid-blocked amine catalyst, tertiary amine based on 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) Soot Zeolite Sylosiv ®< A3 by Grace

[0107] The Polymer-1 was prepared by reacting 1300 g of polyoxypropylene diol (Acclaim ®< 4200 N from Bayer; OH number 28.5 mg KOH / g), 2600 g of polyoxypropylene polyoxyethylene triol (Caradol ®< MD34-02 from Shell; OH number 35.0 mg KOH / g), 600 g of 4,4`-methylenediphenyl diisocyanate (Desmodur ®< 44 MC L from Bayer) and 500 g of diisodecyl phthalate according to a known method at 80 °C to form an NCO-terminated polyurethane polymer with a content of free isocyanate groups of 2.1% by weight. Production of polyurethane adhesives

[0108] For each adhesive, the ingredients listed in Table 1 were added in the specified amounts (in parts by weight) of the polyol component K1using a vacuum dissolver under exclusion of moisture to form a homogeneous paste and stored. The ingredients of the polyisocyanate component listed in Table 1 were also K2 processed and stored. The two components were then mixed in the specified ratio K2 / K1 (in parts by weight, w / w) using a SpeedMixer ®< (DAC 150 FV, Hauschild) for 30 seconds to form a homogeneous paste and immediately tested as follows: To determine the mechanical properties, the adhesive was shaped into a dumbbell according to ISO 527, Part 2, 1B, and stored or cured for 24 hours at 25°C and then for 3 hours at 80°C.

[0109] After a conditioning time of 24h at 23 °C, the elastic modulus was measured in the range of 0.05 to 0.25% strain (" Young's modulus") the Tensile strength and the Elongation at breakThe test specimens thus produced were measured in accordance with ISO 527 on a Zwick Z020 tensile testing machine at the temperature specified in the table and a test speed of 50 mm / min.

[0110] To measure the Tensile shear strength Various test specimens were prepared, with the adhesive being applied 1 minute after the end of the mixing time between two KTL-painted steel sheets degreased with isopropanol in a layer thickness of 2 mm and on an overlapping adhesive surface measuring 15 x 45 mm. The tensile shear strength of these test specimens was determined according to DIN EN 1465, with the test specimens being stored in different conditions before the measurement: either, as a measure of early strength, for 1 h at 23 °C (" ZSF 1h RT") or for 24 h at 23 °C (" ZSF 24h RT") and measured at 23 °C; or, for measuring the tensile shear strength in the fully cured state, for 7 days at 23 °C and then measured at 23 °C (" ZSF 7d RT"),respectively for 7 days at 23 °C and then for 3 h at 80 °C and then measured at 80 °C. (Heat resistance, " ZSF 7d RT (80°C)"). For measuring the tensile shear strength after cataplasmic storage (" CSF 3d Cataplasm") The test specimens were stored for 3 days at 80 °C and 100 % humidity, then stored for 3 h at 23 °C and then measured at 23 °C.

[0111] To measure the tensile shear strength immediately after pre-curing (" ZSF pre-curing")Various test specimens were prepared. The adhesive was applied one minute after the end of the mixing time between two e-coated steel sheets degreased with isopropanol, in a layer thickness of 2 mm, and on an overlapping bonding surface measuring 15 x 45 mm. These test specimens were heated to a temperature of 150 °C using an IR lamp and held at this temperature for 40 seconds. Fifteen seconds later, the tensile shear strength was determined according to DIN EN 1465 on the still-hot test specimens (no active cooling of the test specimens).

[0112] The values ​​(af) and (cf) each indicate the fracture pattern, where "af" stands for an adhesive fracture pattern and "cf" for a cohesive fracture pattern.

[0113] To measure the Pot lifeApproximately 20 g of adhesive (components K1 and K2) were placed in a beaker. The timer was started, and the two components were thoroughly mixed with a spatula for approximately 30 seconds. After 30 seconds, the mixture was poured onto the lower plate of a rheometer. The plate was heated to 25°C. Then the measurement was started: a plate-to-plate rheometer from Anton Paar, spindle diameter 25 mm, gap 0.2 mm, temperature 25°C, shear rate 10 1 / s. The pot life is the time that elapses from the start of mixing until the mixture reaches a viscosity of 500 Pas.

[0114] To measure the viscosity of component K1, respectively K2 ("viscosity component K1 / K2"), these were determined using a rheometer as described above.

[0115] To determine the viscosity of the mixture of components K1 and K2 ("Viscosity Mixture K1+K2"), approximately 20 g of adhesive (components K1 and K2) were placed in a beaker and the two components were thoroughly mixed with a spatula for approximately 30 seconds. After 30 seconds, the mixture was measured using a rheometer as described above.

[0116] The results are shown in Table 2.

[0117] The information (A1+A2) / (A3+A4), A1 / A2 and A3 / A4 in Table 1 refer to the weight ratios of the diols present A1, Triplet A2, Polyester polyol A3 and optionally aliphatic polyols A4 in the respective adhesive.

[0118] At Rf.1 and Rf.2 These are comparative examples, Z-1 and Z-2 These are examples according to the invention. Table 1 Examples Rf.1 Z-1 Rf.2 Z-2 Polyol component K1 : A1 ,1,4-Butandiol 10 9 6 8 A2 , Polyether-Triol 24 24 24 24 Polyether diol 49 - - - A3 - 49 - 29 A4 - - 49 20 Zeolite 4 4 4 4 Soot 18 16 16 19 Cat 0.7 0.7 0.7 0.7 ( A1+A2 ) / ( A3+A4 ) - 0.67 0.61 0.65 A1 / A2 0.42 0.38 0.25 0.33 A3 / A4 - - - 1.45 Polyisocyanate component K2 : Prepolymer-1 85 85 85 85 Soot 13 13 13 13 K2 / K1 (in / out) 1 / 1 1 / 1 1 / 1 1 / 1 Table 2, nb not determined Examples Rf.1 Z-1 Rf.2 Z-2 Viscosity component K1 / K2 [Pas] 73.6 / 110.5 73.6 / 65.3 54.6 / 65.3 126.6 / 37.4 Pot life [min] 12 12,5 12,9 13,3 Viscosity of mixture K1+K2, [Pas] 40,1 77,3 47,5 67 ZSF, pre-curing [MPa] 2.4 (AF) 2.4 (CF) 1.8 (CF) 2.1 (CF) CSF, 1h RT [MPa] 0.56 CF 0.32 CF 0.53 CF 0.52 CF CSF, 24 h RT [MPa] 9.9 CF 4.0 CF 8.0 CF 5.5 CF ZSF, 7d RT [MPa] 11.5 CF 8.5 CF nb 8.1 CF ZSF, 7d RT (80°C) [MPa] 5.0 CF 5.3 CF 3.4 CF 4.9 CF CSF, 3d cataplasm 10.2 CF 10.2 CF 7.7 CF 9.5 CF Young's modulus [MPa] 40 36 40 40 Tensile strength [MPa] 11,3 11,1 10,4 14,4 Elongation at break [%] 260 230 230 270

[0119] The inventive example Z-1 shows opposite Rf.1 better adhesion after IR pre-curing at 150 °C for 40 seconds on a KTL-coated substrate. Instead of an adhesive fracture behavior of Rf.1 a cohesive fracture behavior is obtained.

[0120] Furthermore, the comparison of Z-1 opposite Rf.1 an improvement in pot life with otherwise comparable mechanical properties and the adhesion values ​​of the final strength (ZSF 7 d RT) as well as the adhesion values ​​after cataplasm storage.

[0121] The addition of A4 to the composition according to the invention Z-2 leads to Z-1to a faster adhesion build-up (ZSF 1 h RT and 24 h RT), an improvement in the pot life as well as higher values ​​of the Young's modulus, tensile strength and elongation at break. Furthermore, it was surprisingly found that the addition of A4 to the component K1 leads to an improvement in their storage stability. When storing the component K1 the Z-1 in a cartridge for 7 days at 40 °C, a slight demixing of the component K1 detected. When the component is stored in the same way K1 from Z-2 However, no demixing could be detected.

[0122] Furthermore, the comparison example Rf.2 It is clear that in the case of compositions which only A4 and no A3 The adhesion values ​​after IR pre-curing are significantly lower. The adhesion values ​​after cataplasmic storage and heat resistance are also significantly worse.

Claims

1. Polyurethane adhesive consisting of a polyol component K1 and a polyisocyanate component K2; wherein the polyol component K1 comprises - at least one diol A1 having two primary hydroxyl groups and a molecular weight in the range from 60 to 150 g / mol, - at least one triol A2 having an average molecular weight in the range from 1'000 to 10'000 g / mol, - at least one polyester polyol A3 based on dimer fatty acids and / or dimer fatty alcohols, especially based on dimer fatty acids; and the polyisocyanate component K2 comprises - at least one polyisocyanate B1 and / or - at least one polyurethane polymer B2 having isocyanate groups.

2. Polyurethane adhesive according to Claim 1, characterized in that the triol A2 is a polyether triol.

3. Polyurethane adhesive according to either of the preceding claims, characterized in that the triol A2 has exclusively primary hydroxyl groups.

4. Polyurethane adhesive according to any of the preceding claims, characterized in that the at least one polyester polyol A3 is a polyester polyol A3 based on dimer fatty acids formed from C10-C30 fatty acids, more preferably C12-C25 fatty acids, especially C14-C22 fatty acids.

5. Polyurethane adhesive according to any of the preceding claims, characterized in that the polyol component K1 additionally includes at least one aliphatic polyol A4 which is a hydroxylation product of a triglyceride based on fatty acids.

6. Polyurethane adhesive according to Claim 5, characterized in that the aliphatic polyol A4 has an average OH functionality in the range from 2 to 4, preferably from 2 to 3.

7. Polyurethane adhesive according to Claim 5 or 6, characterized in that the aliphatic polyol A4 is a hydroxylation product based on soya oil or a hydroxylation product based on castor oil, preferably a hydroxylation product based on castor oil.

8. Polyurethane adhesive according to any of the preceding claims, characterized in that the mixing ratio in volume between the polyol component K1 and the polyisocyanate component K2 is in the range from 1:3 to 3:1 and is preferably 0.8:1.2.

9. Polyurethane adhesive according to any of the preceding claims, characterized in that the diol A1, the triol A2, the polyester polyol A3 and optionally the aliphatic polyol A4 are present in the adhesive in such an amount that the weight ratio (A1+A2) / (A3+A4) is in the range from 0.3 to 1.3, 0.35 to 1.1, 0.4 to 0.9, especially 0.5 to 0.8.

10. Polyurethane adhesive according to any of the preceding claims, characterized in that the diol A1 and the triol A2 are present in the adhesive in such an amount that the weight ratio A1 / A2 is in the range from 0.1 to 0.5, 0.15 to 0.4, 0.2 to 0.4, especially 0.25 to 0.35.

11. Polyurethane adhesive according to any of the preceding claims, characterized in that the polyester polyol A3 and the optionally present aliphatic polyol A4 are present in the adhesive in such an amount that the weight ratio A3 / A4 is in the range from 1.0 to 3.0, 1.2 to 2.5, 1.3 to 2.0, 1.3 to 1.8, especially 1.35 to 1.6.

12. Method of adhesive bonding of a first substrate to a second substrate, comprising the steps of: - a) mixing the polyol component K1 and the polyisocyanate component K2 of a polyurethane adhesive according to any of Claims 1 to 11, - b) applying the mixed polyurethane adhesive to at least one of the substrate surfaces to be bonded, - c) joining the substrates to be bonded within the open time, - d) heating the polyurethane adhesive to a temperature of 80-170°C, especially for 30 seconds-5 minutes, - e) curing the polyurethane adhesive.

13. Method according to Claim 12, characterized in that one or both substrates is / are a metal or an alloy, especially a cathodically electrocoated metal or a cathodically electrocoated alloy.

14. Method according to Claim 12 or 13, characterized in that the polyurethane adhesive is applied in step b) in the form of an adhesive bead and, in step d), 5-30%, preferably 10-20%, of the length of the adhesive bead applied is heated in step d).

15. Article formed from the method of adhesive bonding according to any of Claims 12 to 14.