Printing substance for coating glass surfaces

DE502020009390D1Active Publication Date: 2024-10-31ANMELDERANGABEN UNKLAR UNVOLLSTANDIG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009390
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-27
Filing Date
2020-08-24
Publication Date
2024-10-31
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Existing printing inks for glass surfaces require a primer for adequate adhesion and are not sufficiently scratch and solvent resistant, necessitating additional protective coatings, which increases costs and complexity in the printing process.

Method used

A printing substance comprising monomers with C-C double bonds, cationically curable monomers with epoxy and oxetane groups, and an adhesion promoter, allowing for high adhesion and resistance without a primer, with the ability to cure quickly and maintain image sharpness.

Benefits of technology

The printing substance achieves high adhesion and resistance to solvents and scratches without a primer, enabling efficient and cost-effective printing with minimal maintenance and high throughput, while maintaining image sharpness and allowing for immediate use of printed glass surfaces.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to printing substances for coating glass surfaces, a process for producing these printing substances and a use of these printing substances.

[0002] Recently, UV-curing organic inks have increasingly been used for printing on glass, replacing the previously used ceramic (inorganic) inks. This opens up the possibility of avoiding heavy metals, offering a wider range of colors (standard and mixed shades), and achieving greater brilliance and a higher degree of gloss. Another advantage is the ability to assess the color directly after UV curing. In contrast, with inorganic inks, assessment is only possible after baking. They also offer process advantages. For example, a tempering process can be omitted, which reduces process costs compared to processes using inorganic printing inks. Inorganic printing inks undergo a tempering process that generally lasts approximately 90 minutes and is carried out at a tempering temperature in the range of 500-700°C.

[0003] Printing inks and printing processes with which decorations can be produced on various substrates are known, for example, from the publications DE 10 349 394 A1, WO 2014 / 123706 A1, WO 01 / 32789 A1, US 2017 / 298241 A1, KR 20180014115, WO 2016 / 048117, CN 106147381 A, JP 2007270089 A, US 2010 / 035003 A1, US 2014 / 031446 A1, and WO 98 / 43134 A1. WO2018070654 describes an ink composition for inkjet printing, which contains an epoxy component, an oxetane component, a vinyl ether component, an adhesion promoter, and an initiator.

[0004] Printing inks that are applied to glass bottles using inkjet printing to create a decorative effect are also known. These are commercially available from manufacturers such as Mankiewicz and Marabu. However, these systems require a primer layer and a protective varnish (top coat) to meet the usual requirements for adhesion, scratch resistance, image accuracy, and durability, especially water or solvent resistance.

[0005] Known printing inks can be used for printing on glass according to the previously described processes. However, in many cases, the application of a primer to the glass is necessary to achieve sufficient adhesion. Without this pretreatment, sufficient adhesion will not be achieved. Some of the previously described documents claim that pretreatment with an adhesion promoter is not necessary. However, these printing inks demonstrate adhesion that is in need of improvement. Furthermore, designs obtained with known printing inks are not very scratch-resistant and exhibit relatively low solvent resistance, so conventional topcoats are applied over the resulting designs.

[0006] In view of the state of the art, it is an object of the present invention to provide a printing substance for coating glass surfaces using an inkjet printing process, which exhibits high adhesion to a glass substrate without the need for a primer. Furthermore, the printing substance should be curable after application within a very short time, allowing the printed glass substrate to be used for its intended purpose.

[0007] In addition, the decoration obtained by the printing substance should be as solvent and scratch resistant as possible, especially alcohol and scratch resistant. In particular, the decoration should be able to withstand normal stresses without a protective varnish. Furthermore, the printing substance should be able to be maintained as easily and inexpensively as possible. Furthermore, the printing process based on it should be able to be carried out at low cost and with high efficiency. In particular, the printing process should be able to be carried out with the highest possible throughput rates, with particular emphasis on short curing times. Furthermore, the printing substance should require as little maintenance as possible on the printing machines. In particular, the printing substance should not lead to the printing nozzles of an inkjet printer becoming easily clogged. Furthermore, the decoration that can be obtained by the process should have a high level of image sharpness.In addition, the printing substance should be suitable for use in an inkjet printer.

[0008] These and other objects not explicitly mentioned, which can nevertheless be readily deduced or inferred from the contexts discussed in the introduction, are achieved by a printing substance having all the features of patent claim 1. Appropriate modifications of the printing substance according to the invention are protected in the subclaims. With regard to the methods for producing and using the printing substance, the subject matter of claims 15 to 20 provides a solution to the underlying problem.

[0009] The present invention relates to a printing substance for coating surfaces, preferably plastic surfaces or glass surfaces, particularly preferably glass surfaces, using an inkjet printing process, comprising A) at least one monomer having at least one CC double bond; B) at least one cationically curable monomer comprising epoxy groups; C) at least one cationically curable monomer comprising oxetane groups; D) at least one adhesion promoter, wherein components A) and D) are as defined in claim 1.

[0010] This design allows plastic or glass surfaces, preferably glass surfaces, to be printed using an inkjet printing process. The resulting decoration exhibits high adhesion to a plastic or glass substrate, preferably a glass substrate, without the plastic or glass substrate, preferably a glass substrate, requiring a primer. Furthermore, after application, the printing substance can be cured within a very short time in such a way that several colors can be printed consecutively, these colors side by side, and on top of one another, and that the printed glass substrate can be used for its intended purpose.

[0011] In addition, the decoration obtained by the printing substance exhibits very high solvent and scratch resistance, particularly alcohol and scratch resistance. In particular, the decoration withstands normal stresses without a protective varnish. Surprisingly, the surface hardness achievable after a very short time meets the usual requirements that must be met in a mechanical filling system. Thus, a plastic or glass container, preferably a glass container, can be printed with a printing substance according to the invention in a filling system and then filled with a liquid without the print being scratched. Full curing of the coating, for example a print, is generally achieved within 24 hours to 5 days, so that maximum solvent, especially alcohol, resistance is only achieved at a later time.This is not critical, as the filled containers are only handed over to the end customer at a later date.

[0012] Furthermore, the printing substance can be obtained easily and cost-effectively, and the printing process based thereon can be carried out very easily using known equipment. Furthermore, the printing process can be carried out at very high throughput rates, particularly with short curing times. Furthermore, the printing substance enables very low maintenance requirements for the printing machines. In particular, the printing substance does not lead to the printing nozzles of an inkjet printer becoming easily clogged. Furthermore, the decoration that can be obtained by the process exhibits high image sharpness. Furthermore, the printing substance can be designed for use in an inkjet printer.

[0013] The printing substance for coating glass surfaces using an inkjet printing process comprises at least one monomer with CC double bonds as component A). Monomers with at least one CC double bond are known from the prior art. These monomers can be polymerized via a radical mechanism and / or a cationic mechanism. These monomers can comprise one, two, or more CC double bonds. These monomers include, for example, olefins, vinyl monomers such as vinyl chloride, styrene, vinyl ether monomers, (meth)acrylates, and itaconates.

[0014] Monomers with at least one carbon-carbon double bond to be used are (meth)acrylates. (Meth)acrylates are widely known in the art and commercially available. Cyclic (meth)acrylates are used; particularly preferred are cyclic (meth)acrylates selected from isobornyl acrylate, t-butylcyclohexyl acrylate, 2-phenoxyethyl acrylate, (5-ethyl-1,3-dioxan-5-yl)methyl acrylate (cyclotrimethylolpropane formal acrylate). The use of cyclic (meth)acrylates can achieve surprising advantages in terms of durability, curability, and printing properties of the printing substance.

[0015] The itaconates can be itacone polyester polyols, itacone polyester acrylates or itacone polyester glycidyl methacrylates. Further information on this can be found, among other things, in the master's thesis by Arjete Hasanaj: Development of a UV-curing printing ink for glass made from renewable raw materials, RheinMain University of Applied Sciences Wiesbaden Rüsselsheim, Frankfurt am Main University of Applied Sciences, 2013. The publication Arjete Hasanaj: Development of a UV-curing printing ink for glass made from renewable raw materials, RheinMain University of Applied Sciences Wiesbaden Rüsselsheim, Frankfurt am Main University of Applied Sciences, 2013 is incorporated into the present application by reference for disclosure purposes.

[0016] Vinyl ether monomers with at least one carbon-carbon double bond are also among the monomers to be used. Vinyl ether monomers are widely known in the art and commercially available. Particularly preferred are triethylene glycol divinyl ether, diethylene glycol divinyl ether, 1,4-cyclohexanedimethanol divinyl ether, 1,4-butanediol monovinyl ether, 1,4-butanediol divinyl ether, and ethylene glycol monovinyl ether. The use of vinyl ether monomers can achieve surprising advantages in terms of durability, curability, and printing properties of the printing substance.

[0017] The monomers with at least one CC double bond according to component A) are used as a mixture.

[0018] The mixtures comprise at least one cyclic (meth)acrylate and one vinyl ether monomer.

[0019] Preferably, the monomer having at least one CC double bond can be a monomer mixture comprising at least one (meth)acrylate and at least one vinyl ether monomer, and the molar ratio of (meth)acrylate to vinyl ether monomer is in the range from 20:1 to 1:20, preferably in the range from 6:1 to 1:6, particularly preferably in the range from 2:1 to 1:2. Monomers that have both a (meth)acrylate group and a vinyl ether group are counted as both monomer types, regardless of the number of the respective groups.

[0020] Furthermore, the monomer having at least one CC double bond according to component A) can comprise at least one crosslinking monomer. Free-radically and / or cationically curable monomers according to component A) that effect crosslinking comprise at least two CC double bonds that are polymerizable via a free-radical and / or cationic mechanism. The at least two CC double bonds can have identical reactivity, such as 1,4-butanediol divinyl ether, or different reactivity, such as vinyl (meth)acrylate. Preferred crosslinking monomers include (meth)acrylates having at least two (meth)acrylate groups and vinyl monomers, preferably vinyl ether monomers having at least two vinyl groups. Preferred crosslinking monomers include triethylene glycol divinyl ether, diethylene glycol divinyl ether, 1,4-cyclohexanedimethanol divinyl ether, and 1,4-butanediol divinyl ether.Especially preferred are mixtures which comprise at least one vinyl monomer, preferably vinyl ether monomer having at least two vinyl groups and at least one non-crosslinking (meth)acrylate.

[0021] Furthermore, it can be provided that the monomer having at least one CC double bond represents a monomer mixture comprising at least one radically curable monomer and at least one cationically curable monomer. Preferred radically curable monomers having at least one CC double bond are (meth)acrylates; preferred cationically curable monomers having at least one CC double bond are vinyl ether monomers. It is known to those skilled in the art that vinyl ether monomers are also curable via a radical mechanism. Therefore, a monomer mixture comprising at least one radically curable monomer and at least one cationically curable monomer represents a mixture with different monomers whose curability differs with regard to the type of mechanism, i.e. the reaction rate under corresponding conditions (cationic or radical).

[0022] Preferably, it can be provided that the monomer having at least one CC double bond represents a monomer mixture which comprises at least one crosslinking monomer and at least one non-crosslinking monomer and the molar ratio of crosslinking monomer to non-crosslinking monomer is in the range from 20:1 to 1:20, preferably in the range from 4:1 to 1:6, particularly preferably in the range from 3:2 to 1:2.

[0023] The printing substance for coating glass surfaces using an inkjet printing process comprises at least one cationically curable monomer containing epoxy groups as component B). Cationically curable monomers containing epoxy groups are widely known in the art and commercially available. Epoxy groups are oxirane residues that represent a three-membered ring containing an oxygen atom. Cationically curable monomers containing epoxy groups can be obtained by oxidation of corresponding alkenes with oxygen (epoxidation).

[0024] Aliphatic epoxides are preferred as cationically curable monomers containing epoxy groups. Cycloaliphatic epoxides are also preferred as cationically curable monomers containing epoxy groups. Aliphatic and / or cycloaliphatic epoxides preferably do not contain heteroaromatic or aromatic groups, such as bisphenol A.

[0025] The cationically curable monomer comprising epoxy groups may contain one, two, three, or more epoxy groups. Cationically curable monomers comprising epoxy groups to be used in accordance with component B) can be used individually or as a mixture, with mixtures being preferred. These include mixtures of different monomers having exactly one epoxy group, mixtures of different monomers having at least two epoxy groups, and mixtures having at least one monomer having exactly one epoxy group and at least one monomer having at least two epoxy groups.

[0026] In particular, it can be provided that cationically curable monomers with epoxy groups or component B) contains at least one monomer which has exactly one epoxy group.

[0027] Preferably, it can be provided that the cationically curable monomer with epoxy groups or component B) contains at least one monomer which has at least two epoxy groups.

[0028] Particularly preferably, the cationically curable monomer comprising epoxy groups can be a monomer mixture comprising at least one crosslinking monomer and at least one non-crosslinking monomer, wherein the molar ratio of crosslinking monomer to non-crosslinking monomer is preferably in the range from 100:1 to 1:5, preferably 10:1 to 1:2. Crosslinking monomers according to component B) have at least two epoxy groups, while non-crosslinking monomers comprise exactly one epoxy group.

[0029] Furthermore, it can be provided that the cationically curable monomer comprising epoxy groups has at least three epoxy groups. In a particular embodiment, a mixture of cationically curable monomers comprising epoxy groups is used, which comprises at least one monomer with exactly two epoxy groups and at least one monomer with at least three epoxy groups. The molar ratio of monomer with exactly two epoxy groups to monomer with at least three epoxy groups is preferably in the range from 100:1 to 1:4, particularly preferably 10:1 to 1:2.

[0030] The printing substance for coating glass surfaces using an inkjet printing process comprises at least one cationically curable monomer containing oxetane groups as component C). Cationically curable monomers containing oxetane groups are widely known in the art and commercially available. Oxetane groups are radicals with a four-membered ring containing an oxygen atom. Cationically curable monomers containing oxetane groups can be obtained from alkenes and carbonyls by a Paternö-Büchi reaction.

[0031] These include, among others, monomers such as bis[1-ethyl(3-oxetanyl)]methyl ether, 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetanyl)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-cyclohexyloxymethyloxetane. As component C), for example, ARON OXETAN OXT-101, ARON OXETAN OXT-121, ARON OXETAN OXT-211, ARON OXETAN OXT-221 or ARON OXETAN OXT-212 manufactured by Toagosei Co., Ltd. and the like can be used. The cationically curable monomer having oxetane groups can be used either alone or in combination of two or more.

[0032] Preferably, the cationically curable monomer comprising oxetane groups may have at least two oxetane groups.

[0033] Particularly preferably, it can be provided that the molar ratio of monomer comprising epoxy groups to monomer comprising oxetane groups is in the range from 40:1 to 1:15, preferably 30:1 to 1:10, preferably 25:1 to 1:8, particularly preferably 20:1 to 1:5, especially preferably 10:1 to 1:1, especially preferably 6:1 to 2:1 and very preferably 4:1 to 9:4.

[0034] Furthermore, it can be provided that the molar ratio of monomer having at least one CC double bond to cationically curable monomer having an epoxy and / or oxetane group is in the range from 20:1 to 1:5, preferably 10:1 to 1:3, particularly preferably 5:1 to 1:2 and especially preferably 2:1 to 1:1.

[0035] Preferably, the molar ratio of monomer having at least one CC double bond to monomer comprising epoxy groups can be in the range from 20:1 to 1:4, preferably 10:1 to 1:2, particularly preferably 5:1 to 1:1 and especially preferably 3:1 to 3:2.

[0036] Preferably, it can further be provided that the molar ratio of monomer having at least one CC double bond to monomer comprising oxetane groups is in the range from 40:1 to 1:2, preferably 20:1 to 1:1, particularly preferably 10:1 to 2:1 and especially preferably 8:1 to 3:1.

[0037] As component D), the printing substance for coating glass surfaces using an inkjet printing process comprises at least one adhesion promoter comprising at least one silane compound. Adhesion promoters are substances that improve the adhesion of coatings to the substrate. Accordingly, adhesion promoters comprise groups and / or residues that promote a good bond with the substrate and groups and / or residues that promote a bond with the coating.

[0038] These can be isocyanate adhesion promoters, e.g., aliphatic isocyanates and polyisocyanates, preferably polyisocyanates based on hexamethylene diisocyanate (HDI), trimethylhexane diisocyanate (TMHDI), cycloaliphatic polyisocyanates such as isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate (HXDI), or diisocyanatodicyclohexylmethane (HMDI), as well as aromatic isocyanates and polyisocyanates, preferably polyisocyanates based on tolylene diisocyanate (TDI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), or diisocyanatodiphenylmethane (MDI). Commercially available products include Desmodur E41 or Desmodur N 75 (Covestro). Vinyl phosphates or organometallic compounds such as titanates or zirconates can also be used.

[0039] Preferred groups that achieve strong adhesion to a glass substrate include silane groups. The adhesion promoter according to the application comprises at least one silane compound and consists of one or more silane compounds.

[0040] To ensure a good bond with the coating, preferred adhesion promoters can be polymerized into the coating. The adhesion promoter can preferably comprise a curable group. Curable groups are residues that react during a polymerization reaction. These include radically polymerizable groups and / or cationically polymerizable groups. The adhesion promoter can preferably be a silane compound with a cationically or radically curable group. The preferred adhesion promoters are silane adhesion promoters, such as vinylsilanes, methacryloxysilanes, epoxysilanes, chlorosilanes, and isocyanatosilanes, preferably epoxysilanes.

[0041] Preferred silane coupling agents contain, in addition to a curable group, at least one, preferably at least two hydrolyzable groups, such as, for example, halogen radicals, such as chlorine or bromine radicals and / or alkoxy groups, preferably methoxy, ethoxy, propoxy and / or butoxy groups, with methoxy and / or ethoxy groups being preferred.

[0042] Preferred epoxysilanes include, among others, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 4-(methyldiethoxysilyl)-1,2-epoxycyclohexane and 3-(3,4-epoxycyclohexyl)propyltri(isobutoxy)silane, (3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-glycidoxypropyldiethoxymethylsilane, 3-glycidoxypropyltri-(isobutoxy)silane, (3,4-epoxycyclohexyl)ethyltri-(isobutoxy)silane, 3-glycidoxypropyltrimethoxysilane and / or 3-glycidoxypropyltriethoxysilane.

[0043] Preferably, it can be provided that the printing substance comprises at least 5 wt.%, preferably at least 6 wt.% and particularly preferably at least 7 wt.% adhesion promoter.

[0044] Furthermore, it can be provided that the molar ratio of monomer with at least one CC double bond to adhesion promoter is in the range from 40:1 to 1:2, preferably 20:1 to 1:1, particularly preferably 10:1 to 2:1 and especially preferably 8:1 to 3:1.

[0045] Preferably, the molar ratio of cationically curable monomer to adhesion promoter can be in the range from 20:1 to 1:2, preferably 15:1 to 1:1, particularly preferably 10:1 to 2:1.

[0046] Preferably, the molar ratio of monomer comprising epoxy groups to adhesion promoter can be in the range from 15:1 to 1:2, preferably 10:1 to 1:1, particularly preferably 8:1 to 3:2 and especially preferably 4:1 to 2:1.

[0047] Preferably, it can further be provided that the molar ratio of monomer comprising oxetane groups to adhesion promoter is in the range from 15:1 to 1:15, preferably 10:1 to 1:10, particularly preferably 5:1 to 1:5 and especially preferably 2:1 to 1:2.

[0048] The printing substance comprises curable monomers and is cured after application to the substrate. The printing substance is preferably curable by irradiation with electromagnetic waves, particularly preferably by UV radiation, without this being intended to impose any restriction. Accordingly, the printing substance preferably comprises an initiator, preferably for cationic curing, and / or a radical initiator. Furthermore, it can be provided that the printing substance comprises at least one photoinitiator, which preferably effects curing upon exposure to UV radiation. Furthermore, it can be provided that the printing substance comprises at least one sensitizer.

[0049] The printing substance preferably contains at least one photoinitiator, usually two and possibly three or more, to initiate the surface and depth curing (crosslinking) of the ink for printing on glass under UV light. They can be selected from the photoinitiators commonly used in UV-curing inks and varnishes, etc.

[0050] Examples of cationic UV initiators include aryldiazonium salts, diaryliodonium salts, triarylsulfonium salts, triarylselenonium salts, dialkylphenacylsulfonium salts, aryloxydiarylsulfoxonium salts, and diarylphenacylsulfoxonium salts. Preferred examples of cationic UV initiators include diphenyl(4-phenylthio)phenylsulfonium hexafloroantimonate, (thiodi-4,1-phenylene)bis(diphenylsulfonium) dihexafluoroantimonate (a mixture of these substances is sold under the name CHIVACURE®<1176 by Chitec Technology Co. Ltd., Phoenix, Arizona), diphenyl(4-phenylthio)phenylsulfonium hexafluorophosphate, (thiodi-4,1-phenylene)bis(diphenylsulfonium)dihexafluorophosphate (a mixture of these substances is sold under the name CHIVACURE®<1190 by Chitec Technology Co.Ltd), triarylsulfonium hexafluorophosphate salt (CYRACURE®< UVI-6990) and triarylsulfonium hexafluoroantimonate salt (CYRACURE®< UVI-6974) (both available from Union Carbide Chemicals and Plastics Co. Inc., Danbury, Conn.), triphenylselenonium hexafluoroantimonate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium hexafluorophosphate, bis(4-dodecylphenyl)iodonium hexafluoroantimonate and η-5-2,4-cyclopentadien-1-yl)[(1,2,3,4,5,6-η)-(1-methylethyl)benzene] iron(1+) hexafluorophosphate(1-) (CYRACURE®< 261 from Ciba-Geigy Corporation, McIntosh Ala.) and combinations or two or more of the foregoing.

[0051] Examples of radical UV initiators include 1-hydroxycyclohexyl phenyl ketone, benzophenone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 1,2-methyl-1-(4-methylthio)phenyl-2-(4-morpholinyl)-1-propanone, 2,4,6-trimethylbenzoylphenylphosphinic acid ethyl ester, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzyl dimethyl ketal, and isopropylthioxanthone. 2-Methyl-1-[4-(methylthiophenyl)-2-morpholinopropan]-1-one (Irgacure ®< 907 from BASF Corporation or OMNIRAD ®< 4817 from IGM Resins, Bartlett III.), 1-Hydroxycyclohexylacetophenone (Irgacure ®< 184 from BASF Corporation), 2-Benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one (Irgacure ®< 369 from BASF Corporation), Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Irgacure ®< 819 from BASF Corporation), 2-Hydroxy-2-methyl-1-phenyl-1-propanone (Darocur ®< 1173 from Ciba), 2-Chlorothioxanthone (CTX from Lambson), Benzophenone, 2,4,6-Trimethylbenzenediphenylphosphine oxide (TPO from BASF or OMNIRAD ®< TPO from IGM Resins), Ethyl 2,4,6-trimethylbenzoylphenylphosphinate (TPO-L from BASF) and Methylbenzoylformate (MBF from Lambson) and combinations of two or more of the above.

[0052] The total amount of photoinitiators is preferably 1 to 12 wt.%, preferably 3 to 9 wt.%, based on the weight of the printing substance.

[0053] Furthermore, it can be provided that the printing substance comprises at least one colorant, preferably a pigment and / or a dye, preferably at least one pigment.

[0054] The pigments preferably contained in the printing substance according to the invention can be any desired pigment, e.g., titanium dioxide, zinc sulfide, carbon black, azodiaryl yellow, isoindole yellow, diarylide orange, quinacridone magenta, diketopyrrolo red, copper phthalocyanine blue, copper phthalocyanine green, dioxazine violet, and diketometal oxide. A fairly comprehensive list of other usable pigments can be found in the Colour Index International, Fourth Edition Online, 2001, published by the Society of Dyers and Colourists in conjunction with the American Association of Textile Chemists and Colorists. Effect pigments, such as metal oxide-coated micas and metallic pigments, can also be used.Precious metal powders or matting agents, such as silicates and / or natural and / or synthetically produced fillers such as calcium carbonate, barium sulfate, talc, can also be used to influence the physical and chemical properties such as gloss, hardness, refractive index, chemical resistance, etc.

[0055] The amount of color pigment is usually 1 to 40 wt.%, preferably 2 to 35 wt.%, based on the weight of the printing substance, depending on the type of pigment and the desired opacity. White pigment is usually used in an amount of 5 to 40 wt.%, preferably 10 to 30 wt.%.

[0056] Surprising advantages can be achieved by dispersing the pigment in a curable monomer or oligomer, preferably in a radically or cationically curable monomer or oligomer, particularly preferably a (meth)acrylate.

[0057] In general, a printing substance according to the invention can contain other conventional additives. These include, among others, defoamers, flow control agents, wetting agents, rheology additives, and / or stabilizers, preferably in an amount of 0.1 to 10 wt. %, particularly preferably 0.2 to 5 wt. %, and especially preferably 0.3 to 2.5 wt. %, based on the total mass of the printing substance. Defoamers can be selected, for example, from modified acrylates or modified acrylate copolymers, but also, and preferably, from silicone-containing compounds. Flow control agents include, for example, modified polyacrylates and polysiloxanes.

[0058] Rheological additives include, for example, compounds based on castor oils, urea, polyurethanes or polyamides.

[0059] The preferred stabilizers are Genorad 16 from Rahn and Fluorstab UV2 from Kromachem, 10, Park Industrial Centre, Tolpits Lane, Watford, Hertfordshire WD1 8SP, UK.

[0060] The printing substance can also contain organic solvents and / or water. This can improve processability. On the other hand, organic solvents and / or water have disadvantages. For example, the use of water in the printing substance impairs curing. Organic solvents are compounds containing carbon and hydrogen atoms that evaporate from the coating after the printing substance has been applied. Reactive thinners, such as components A) to C), which are liquid, are therefore not considered organic solvents. Accordingly, organic solvents do not react with other components of the printing substance during curing. The water content of the printing substance is preferably at most 4% by weight, preferably at most 2% by weight, and particularly preferably at most 1% by weight. The printing substance particularly preferably does not contain any significant amounts of water.The proportion of organic solvent in the printing substance is preferably at most 4 wt.%, preferably at most 2 wt.%, and particularly preferably at most 1 wt.%. Particularly preferably, the printing substance does not contain any significant proportions of organic solvent.

[0061] In a preferred embodiment, the printing substance is suitable for inkjet printing processes. Therefore, the printing substance, preferably the ink, can have a viscosity in the range of 3 mPas to 100 mPas at a shear rate of 600 s -1 and 23°C, measured using a cone / plate on a rotational viscometer.

[0062] In a further embodiment, the printing substance is suitable for screen printing processes. Therefore, the printing substance, preferably the paste, can have a viscosity in the range of 1 Pas to 15 Pas at a shear rate of 200 s -1< and 23°C, measured using a cone / plate on a rotational viscometer.

[0063] In a further embodiment, the printing substance is suitable for spraying processes. Therefore, the printing substance, preferably the paste, can have a viscosity in the range of 1 mPas to 350 mPas at a shear rate of 200 s -1< and 23°C, measured using a cone / plate on a rotational viscometer.

[0064] Preferably, it can be provided that the printing substance comprises at least 60 wt.%, preferably at least 70 wt.%, particularly preferably at least 80 wt.% of components A), B), C) and D).

[0065] Preferably, it can be provided that the printing substance comprises at least 70 wt.%, preferably at least 80 wt.%, particularly preferably at least 90 wt.% of solids and components A), B), C) and D).

[0066] Another object of the present invention is a UV ink for coating surfaces, preferably plastic surfaces or glass surfaces, particularly preferably glass surfaces, using an inkjet printing process, comprising A) at least one monomer having at least one CC double bond; B) at least one cationically curable monomer comprising epoxy groups; C) at least one cationically curable monomer comprising oxetane groups; D) at least one adhesion promoter; E) at least one pigment and / or dye, preferably at least one pigment; F) at least one photoinitiator, preferably a UV initiator. UV initiator, wherein components A) and D) are as defined in claim 1.

[0067] Preferably, it can be provided that the UV ink comprises at least 75 wt.%, preferably at least 85 wt.%, particularly preferably at least 95 wt.% of components A), B), C), D), E) and F).

[0068] Another object of the present invention is a UV ink for coating surfaces, preferably plastic surfaces or glass surfaces, particularly preferably glass surfaces, using an inkjet printing process, comprising A) at least one monomer having at least one CC double bond; B) at least one cationically curable monomer comprising epoxy groups; C) at least one cationically curable monomer comprising oxetane groups; D) at least one adhesion promoter; F) at least one photoinitiator, preferably a UV initiator, wherein components A) and D) are as defined in claim 1.

[0069] Preferably, it can be provided that the UV ink comprises at least 75 wt.%, preferably at least 85 wt.%, particularly preferably at least 95 wt.% of components A), B), C), D) and F).

[0070] The UV ink particularly preferably contains a sensitizer. The use of sensitizers can surprisingly achieve curing with a UV LED lamp. LED lamps are very energy-efficient compared to other lamps, such as mercury lamps.

[0071] A preferred subject of the present invention is a UV ink for coating surfaces, preferably plastic surfaces or glass surfaces, particularly preferably glass surfaces, using an inkjet printing process, comprising A) at least one monomer having at least one CC double bond; B) at least one cationically curable monomer comprising epoxy groups; C) at least one cationically curable monomer comprising oxetane groups; D) at least one adhesion promoter; E) at least one pigment and / or dye, preferably at least one pigment; F) at least one photoinitiator, preferably a UV initiator; G) at least one sensitizer, wherein components A) and D) are as defined in claim 1.

[0072] Preferably, it can be provided that the UV ink comprises at least 80 wt.%, preferably at least 90 wt.%, particularly preferably at least 95 wt.% of components A), B), C), D), E), F) and G).

[0073] A preferred subject of the present invention is a UV ink for coating surfaces, preferably plastic surfaces or glass surfaces, particularly preferably glass surfaces, using an inkjet printing process, comprising A) at least one monomer having at least one CC double bond; B) at least one cationically curable monomer comprising epoxy groups; C) at least one cationically curable monomer comprising oxetane groups; D) at least one adhesion promoter; F) at least one photoinitiator, preferably a UV initiator; G) at least one sensitizer, wherein components A) and D) are as defined in claim 1.

[0074] Preferably, it can be provided that the UV ink comprises at least 80 wt.%, preferably at least 90 wt.%, particularly preferably at least 95 wt.% of components A), B), C), D), F) and G).

[0075] UV inks for coating glass surfaces using an inkjet printing process that do not contain any pigment and / or dye are particularly suitable for creating reliefs (colorless elevations) on a substrate.

[0076] The above-mentioned components A) to F) and A) to G) are described in detail above, so that reference is made thereto, wherein the mentioned preferences and preferred embodiments of these components also apply to a UV ink.

[0077] The present invention further provides a process for producing a printing substance for coating glass surfaces using an inkjet printing process. This process is characterized in that components A), B), C) and D) are mixed, preferably components A), B), C), D), E) and F) or A), B), C), D) and F) and particularly preferably components A), B), C), D), E), F) and G) or A), B), C), D), F) and G). In a preferred embodiment of the process according to the invention, a pigment is preferably added in the form of a dispersion and / or suspension which comprises a monomer, preferably a monomer having at least one CC double bond.

[0078] Furthermore, it can be provided that the printing substance, preferably the UV ink, comprises only small amounts of one or more modifiers. The printing substance, preferably the UV ink, preferably comprises at most 1 wt. %, particularly preferably at most 0.8 wt. % of one or more modifiers. Modifiers are, in particular, polyols with a hydroxyl value of 40 to 330 mg KOH / g; polyols with a hydroxyl value of 40 to 330 mg KOH / g and an acid value of 2 to 20 mg KOH / g; modified rubbers and / or compounds with an epoxy equivalent of 150 to 700 g / mol. Modified rubbers are, in particular, carboxylated polyisoprenes and / or carboxylated polybutadienes. Particularly preferably, the printing substance, preferably the UV ink, does not comprise significant amounts of one or more modifiers.

[0079] Furthermore, it can be provided that the printing substance, preferably the UV ink, comprises only small amounts of one or more base generators. The printing substance, preferably the UV ink, preferably comprises at most 1 wt.%, particularly preferably at most 0.8 wt.% of one or more base generators. A base generator is a compound that generates a base when exposed to active rays, radicals, or a base. In particular, base generators are known compounds such as base generators that generate a base upon irradiation, base generators that generate a base when exposed to radicals, and base generators that generate a base when brought into contact with a base.For example, oxime derivatives, quaternary ammonium salts, and quaternary amidine salts each generate a base when exposed to either active radiation or radicals. Therefore, each of these derivatives can be used both as a base generator, generating a base when irradiated, and as a base generator, generating a base when exposed to radicals. Carbamate derivatives generate a base when exposed to a base. More preferably, the printing substance, preferably the UV ink, does not comprise significant amounts of one or more modifiers.

[0080] Furthermore, it can be provided that the printing substance, preferably the UV ink, contains only small amounts of one or more alkylene carbonates or butyrolactone. Examples of alkylene carbonates include glycerol carbonates, ethylene carbonate, propylene carbonate, butylene carbonate, and combinations containing at least one of the aforementioned substances. Preferably, the printing substance, preferably the UV ink, comprises at most 1 wt.%, particularly preferably at most 0.8 wt.%, of one or more alkylene carbonates or butyrolactone. Particularly preferably, the printing substance, preferably the UV ink, does not comprise any significant amounts of one or more alkylene carbonates or butyrolactone.

[0081] Furthermore, it can be provided that the printing substance, preferably the UV ink, comprises only small amounts of one or more acrylate esters of a carboxylic acid ester. Preferably, the printing substance, preferably the UV ink, comprises at most 1 wt. %, particularly preferably at most 0.4 wt. % of one or more acrylate esters of a carboxylic acid ester. Acrylate esters of a carboxylic acid ester are compounds which, in addition to an acrylate group, additionally comprise an ester group, so that the alcohol group of the acrylate additionally comprises an ester group. Particularly preferably, the printing substance, preferably the UV ink, does not comprise any significant amounts of one or more acrylate esters of a carboxylic acid ester.

[0082] Furthermore, it can be provided that the printing substance, preferably the UV ink, comprises only small amounts of one or more purely thermal initiators, whereby these thermal initiators can initiate both radical and cationic polymerization. Preferably, the printing substance, preferably the UV ink, comprises at most 1 wt.%, particularly preferably at most 0.4 wt.%, of one or more purely thermal initiators. Purely thermal initiators are compounds that can initiate both radical and cationic polymerization upon heating, but do not initiate either radical or cationic polymerization upon irradiation with UV light. The term "purely thermal initiators" represents a distinction in particular from the preferred UV initiators, so that UV initiators that trigger polymerization upon heating are not purely thermal initiators.Particularly preferably, the printing substance, preferably the UV ink, does not comprise significant amounts of one or more purely thermal initiators.

[0083] The present invention further relates to the use of a printing substance according to the invention, which is characterized in that the printing substance is applied to glass, ceramic, metal, wood, or plastic, preferably to glass or plastic, particularly preferably to glass. The term "glass," as used in the claims and the description, is intended to mean glass, ceramic, tile glazes, and similarly glassy materials.

[0084] The objects to be printed can be in any shape or form, such as a container, a plate, a tile, a figure, etc. A preferred embodiment of the invention is packaging (beverage bottles, cosmetic containers) and household glass (e.g. juice glass).

[0085] In a preferred embodiment of the present use, it can be provided that the printing substance is applied to a substrate, preferably to glass, using an inkjet printing process.

[0086] In a further preferred embodiment of the present use, it can be provided that after the application of the printing substances (both next to and on top of each other) to a substrate, preferably to glass, no further layer, for example in the form of a clear topcoat, is applied to protect the underlying ink.

[0087] Furthermore, it can be provided that no layer is applied before applying the printing substance to a substrate, preferably glass, and preferably untreated glass is printed. Furthermore, it can be provided that the substrate, preferably glass, is subjected to a pretreatment (flame treatment and / or silane flame treatment). However, pretreatment is not absolutely necessary, as the example data show.

[0088] Furthermore, it can be provided that the printing substance is applied in an atmosphere having a relative humidity in the range of 25% to 50%.

[0089] Furthermore, it can be provided that the printing substance is applied at a temperature in the range of 10 to 60°C, preferably 15 to 55°C and particularly preferably 20 to 50°C.

[0090] The printing substance is preferably cured with UV light in a wavelength range of 160 to 420 nm for a period of time sufficient to achieve complete curing. Alternatively, the printing substance can be cured without photoinitiators using electron beams. Furthermore, the printing substance can also be provided with thermal initiators and cured accordingly. Conventional UV light sources such as mercury vapor lamps (also iron- or gallium-doped), metal halide lamps, quartz lamps, excimer lasers, or UV light-emitting diodes (UV LEDs) can be used for UV curing.

[0091] Here, curing can occur via a purely cationic mechanism, so that only initiators, preferably photoinitiators for a cationic reaction, are used. In a preferred embodiment, curing is achieved via a radical and a cationic mechanism, so that both an initiator for a cationic polymerization and an initiator for a radical polymerization are used.

[0092] The present invention is explained in more detail below using examples, without this being intended to limit the invention. Test procedures Thumb twist test

[0093] After UV curing, the coated glass plate is removed directly from the printing press. Using a cloth, a rotating thumb motion is applied to the freshly cured ink while applying firm pressure. The resulting print is assessed according to the scheme below. 5 = detachment of the coating down to the glass 4 = strong imprint (partially down to the glass) 3 = clearly visible imprint 2 = slight imprint 1 = barely visible imprint, only visible by reflecting the surface 0 = no imprint Cross-cut experiment

[0094] Using the cross-cut tester (blade spacing 1 mm), a cross is scratched into the cured surface down to the substrate. An adhesive tape is then applied to the cross-cut, pressed firmly, and quickly removed. The rating is based on the scale below, from 0 (no loss of adhesion) to 5 (complete detachment). 5 = Complete detachment beyond the cross-cut. 4 = Detachment within the cross-cut. 3 = Detachment 30-50%. 2 = Detachment 10-30%. 1 = Detachment at the cut <10%. 0 = No detachment. Double Rub Ethanol Experiment

[0095] A cloth is secured with a cable tie over a 0.5 kg hammer. The cloth is then moistened with ethanol until it is completely saturated. The hammer is moved over the surface without applying pressure (using only its own weight). If the cloth becomes dry, it should be moistened again after 20 to 50 double strokes. The number of double strokes required until the coating is attacked is recorded. Cold water test

[0096] A can is filled with deionized water. The painted glass plates are placed in the can so that the painted surface is in open contact with the water. The can is then sealed and placed in the refrigerator at a temperature between 4 and 10°C for a specified period of time. Pasteurization

[0097] A pot is filled with deionized water. The water is heated to 70°C. The painted glass plates are placed in the pot so that the painted surface is in open contact with the water. After 30 minutes, the glass plates are removed and examined. Embodiments 1 and 2 and Comparative Examples 1 and 2

[0098] The printing substances shown in the table below are produced by mixing, Pretreatment of the flat glass (both air and bath sides): First, clean with ethanol, then with ethyl acetate. Application with a doctor blade: 8µm spiral doctor blade from BYK. Wet film thickness per layer: 8-12µm. Measured with an Erichsen wet film thickness gauge. Model: 234 R / I. Lamp: Höhnle UV Technology (LED-Powerline PLD), water-cooled, wavelength: 385nm.

[0099] The dose is 380 - 420 mJ / cm 2< , measured with PUK (Kühnast Strahlentechnik) UV integrator. Example 1 Comparison example 1 Example 2 Comparison example 2 Color White White Cyan Cyan Components % by weight % by weight % by weight % by weight Cycloaliphatic epoxide 6,87 7,77 8,80 9,96 Aliphatic epoxy, glycidyl ether with two epoxy groups 6,38 7,19 5,28 5,99 Aliphatic epoxy, glycidyl ether with three epoxy groups 7,56 8,34 6,65 7,53 Oxetane with two oxetane groups 6,87 7,78 8,81 10,01 Vinyl ethers with a vinyl group 3,93 4,47 5,28 6,02 Vinyl ethers with two vinyl groups 14,48 15,56 18,59 21,06 Cyclic acrylate (non-crosslinking) 14,74 16,65 19,56 22,34 Polyvinyl butyral 1,96 3,37 Cationic initiator; diaryliodonium salt 5,89 6,66 3,67 4,14 sensitizer; UV radical initiator thioxanthone 1,97 2,22 1,22 1,39 Silicone-based flow agents 0,39 0,46 0,39 0,44 Rheology additive 1,0 1,15 Epoxysilanes; 9,84 9,79 White pigment dispersed in acrylates 20,07 21,76 Cyan pigment dispersed in acrylates 10,00 7,75 sum 100,00 100,00 100,00 100,00

[0100] The coatings obtained on a glass plate are tested by the cross-cut test and the double rub ethanol test, obtaining the results presented in the table below: Example 1 Example 1 Comparison example 1 Comparison example 1 Example 2 Comparison example 2 Side of the flat glass Airside bathroom side Airside bathroom side Airside Airside Cross-cut after hardening 0 0 2-3 5 0-1 3 Double Rub Ethanol 24 h after curing >50 >50 30 22 >50 25

[0101] The examples show that surprising increases in solvent resistance can be achieved by adding adhesion promoters.

[0102] Reference Example 3, Working Example 4 and Comparative Example 3

[0103] The printing substances shown in the table below are prepared by mixing, applied to a glass substrate (flat glass) by inkjet printing and cured as previously described (Example 3 is a reference example): Example 3 Example 4 Comparison example 3 Color White White White Components % by weight % by weight % by weight Cycloaliphatic epoxide 9,50 7,03 9,35 Aliphatic epoxy, glycidyl ether with two epoxy groups 5,50 6,58 8,75 Aliphatic epoxy, glycidyl ether with three epoxy groups 7,23 7,72 10,26 Oxetane with two oxetane groups 9,49 7,03 0,00 Vinyl ethers with a vinyl group 5,51 4,08 4,08 Vinyl ethers with two vinyl groups 20,37 14,72 14,72 Cyclic acrylate (non-crosslinking) 15,36 15,36 Cationic initiator; diaryliodonium salt 5,99 5,70 5,70 sensitizer; UV radical initiator thioxanthone 2,00 1,90 1,90 Silicone-based flow agents 0,41 0,38 0,38 Epoxysilanes; 10,02 9,5 9,5 White pigment dispersed in acrylates 20,00 20,00 White pigment dispersed in cycloaliphatic epoxy and vinyl ether 23,97 sum 100,00 100,00 100,00

[0104] The coatings obtained on a glass plate were tested by the cross-cut test and the double rub ethanol test, obtaining the results presented in the table below: Example 3 Example 3 Example 4 Example 4 Comparison example 3 Comparison example 3 Side of the flat glass Airside bathroom side Airside bathroom side Airside bathroom side Cross-cut after hardening 2-3 4 0-1 2-3 3-4 5 Cross-cut after 30 minutes in water at 70°C 2-3 5 0 0-1 5 5 Double Rub Ethanol 24 h after curing 50 40

[0105] The examples and the comparative example demonstrate that significantly higher bond strengths can be achieved by using cationically curable monomers with oxetane groups. Furthermore, printing substrates containing acrylates exhibit better bond strengths than printing substrates without acrylates. Examples 5 to 9

[0106] The printing substances shown in the following table are prepared by mixing, applied to a glass substrate (flat glass) by inkjet printing and cured as previously described: Example 5 Example 6 Example 7 Example 8 Example 9 Ratio of epoxy to oxetane groups based on wt.% 1:0,33 1:1,79 1:0,6 1:0,14 1:2,13 Components % by weight % by weight % by weight % by weight % by weight Cycloaliphatic epoxide 6,23 1,33 4,67 7,79 0,85 Aliphatic epoxy, glycidyl ether with two epoxy groups 5,83 1,25 4,37 7,29 0,80 Aliphatic epoxy, glycidyl ether with three epoxy groups 6,84 1,47 5,13 8,55 0,93 Oxetane with two oxetane groups 9,46 24,31 14,19 4,73 25,78 Vinyl ethers with a vinyl group 4,08 4,08 4,08 4,08 4,08 Vinyl ethers with two vinyl groups 14,72 14,72 14,72 14,72 14,72 Cyclic acrylate (non-crosslinking) 15,36 15,36 15,36 15,36 15,36 Cationic initiator; diaryliodonium salt 5,7 5,7 5,7 5,7 5,7 sensitizer; UV radical initiator thioxanthone 1,9 1,9 1,9 1,9 1,9 Silicone-based flow agents 0,38 0,38 0,38 0,38 0,38 Epoxysilanes; 9,5 9,5 9,5 9,5 9,5 White pigment dispersed in acrylates 20,00 20,00 20,00 20,00 20,00 sum 100,00 100,00 100,00 100,00 100,00

[0107] The coatings obtained on a glass plate are tested by the cross-cut test, obtaining the results shown in the table below: Example 5 Example 6 Example 7 Example 8 Example 9 Side of the flat glass bathroom side bathroom side bathroom side bathroom side bathroom side Cross-cut after hardening 5 5 5 5 5 Cross-cut 24 hours after curing 0 1,5 0 0,5 0,5 Cross-section after 3 days in cold water (7°C) 2 5 4 3 5 Examples 10 to 15

[0108] The printing substances shown in the following table are prepared by mixing, applied to a glass substrate (flat glass) by inkjet printing and cured as previously described: Example 10 Example 11 Example 12 Ratio of epoxy to oxetane groups based on wt.% 1:0,29 1:0,33 1:1,81 Components % by weight % by weight % by weight Cycloaliphatic epoxide 9,0 8,55 1,83 Aliphatic epoxy, glycidyl ether with two epoxy groups 5,4 5,13 1,10 Aliphatic epoxy, glycidyl ether with three epoxy groups 6,8 6,45 1,38 Oxetane with two oxetane groups 9,0 10,07 25,89 Vinyl ethers with a vinyl group 5,4 5,4 5,4 Vinyl ethers with two vinyl groups 19,0 19,0 19,0 Cyclic acrylate (non-crosslinking) 20,0 20,0 20,0 Polyvinyl butyral 3,0 3,0 3,0 Cationic initiator; diaryliodonium salt 3,8 3,8 3,8 sensitizer; UV radical initiator thioxanthone 1,3 1,3 1,3 Silicone-based flow agents 0,4 0,4 0,4 Epoxysilanes; 10,0 10,0 10,0 Cyan pigment dispersed in acrylates 7,0 7,0 7,0 sum 100,00 100,00 100,00 Example 13 Example 14 Example 15 Ratio of epoxy to oxetane groups based on wt.% 1:0,60 1:0,14 1:2,15 Components % by weight % by weight % by weight Cycloaliphatic epoxide 6,41 10,69 1,17 Aliphatic epoxy, glycidyl ether with two epoxy groups 3,85 6,41 0,70 Aliphatic epoxy, glycidyl ether with three epoxy groups 4,84 8,07 0,88 Oxetane with two oxetane groups 15,1 5,03 27,45 Vinyl ethers with a vinyl group 5,4 5,4 5,4 Vinyl ethers with two vinyl groups 19,0 19,0 19,0 Cyclic acrylate (non-crosslinking) 20,0 20,0 20,0 Polyvinyl butyral 3,0 3,0 3,0 Cationic initiator; diaryliodonium salt 3,8 3,8 3,8 sensitizer; UV radical initiator thioxanthone 1,3 1,3 1,3 Silicone-based flow agents 0,4 0,4 0,4 Epoxysilanes; 10,0 10,0 10,0 Cyan pigment dispersed in acrylates 7,0 7,0 7,0 sum 100,00 100,00 100,00

[0109] The coatings obtained on a glass plate are tested by the cross-cut test and the thumb-twist test, obtaining the results shown in the table below: Example 10 Example 11 Example 12 Example 13 Example 14 Example 15 Side of the flat glass bathroom side bathroom side bathroom side bathroom side bathroom side bathroom side Cross-cut after hardening 3 3 5 4 3,5 5 Cross-cut 24 hours after curing 0 0 0 0 0 0 Cross-section after 3 days in cold water (7°C) 2 3 5 5 0 5 Thumb twist test 1 1 0 0 2 0 Examples 16 and 17

[0110] The printing substances shown in the following table are produced by mixing, applied to a glass substrate (flat glass) using inkjet printing and cured: Example 16 Example 17 Components % by weight % by weight Cycloaliphatic epoxide 7,24 7,12 Aliphatic epoxy, glycidyl ether with two epoxy groups 6,73 6,61 Aliphatic epoxy, glycidyl ether with three epoxy groups 7,97 7,83 Oxetane with two oxetane groups 7,24 7,12 Vinyl ethers with a vinyl group 4,14 4,07 Vinyl ethers with two vinyl groups 14,90 14,65 Cyclic acrylate (non-crosslinking) 15,52 15,26 Cationic initiator; diaryliodonium salt 6,21 6,10 sensitizer; UV radical initiator thioxanthone 2,07 2,04 Silicone-based flow agents 0,41 0,41 Rheology additive 0,66 0,71 Epoxysilanes; 10,34 10,17 White pigment dispersed in acrylates 16,57 17,91 sum 100,00 100,00

[0111] The coating composition presented in Example 16 was cured at a relative humidity above approximately 60% (room temperature), curing over a relatively long period of time without achieving a suitable degree of cure. The essentially identical composition according to Example 17 was cured at a relative humidity of approximately 32% (room temperature), achieving good cure in a short time. Due to the poor cure, no tests were conducted with the coating obtained according to Example 16. Example 17 Example 17 Side of the flat glass Airside bathroom side Cross-cut after hardening 0 1 Cross-cut after 30 minutes in water at 70°C 0 0 Double Rub Ethanol 24 h after curing >100 >100

[0112] The examples show that the present invention achieves the objects set out above, in particular the adhesion and stability of a decoration obtained by the printing substance according to the invention can be surprisingly significantly increased without other properties of the printing substance or the decoration being adversely affected thereby.

Claims

1. Printing substance for coating surfaces, preferably glass surfaces with an inkjet printing process, comprising A) at least one monomer with at least one C-C double bond; B) at least one cationic hardenable monomer comprising epoxy groups; C) at least one cationic hardenable monomer comprising oxetane groups; D) at least an adhesion promoter, characterized in that the monomer with at least one C-C double bond is a mixture which comprises at least one (meth)acrylate and at least one vinyl ether monomer, wherein the monomer having at least one C-C double bond comprises at least one cyclic (meth)acrylate and the adhesion promoter comprises at least one silane compound.

2. Printing substance according to claim 1, characterized in that the monomer with at least one C-C double bond comprises at least one crosslinking monomer.

3. Printing substance according to claim 1 or 2, characterized in that the adhesion promoter consists of one or more silane compounds.

4. Printing substance according to at least one of the previous claims, characterized in that the printing substance contains at least 5% by weight, preferably at least 6 % by weight and particularly preferably at least 7 % by weight, of an adhesion promoter.

5. Printing substance according to at least one of the preceding claims, characterized in that the cationic hardenable monomer which comprises epoxy groups contains at least one monomer with two epoxy groups.

6. Printing substance according to at least one of the previous claims, characterized in that the cationic hardenable monomer, which comprises oxetane groups comprises at least one monomer having at least two oxetane groups.

7. Printing substance according to at least one of the previous claims, characterized in that the molar ratio of monomer comprising epoxy groups to monomer comprising oxetane groups is in the range from 40:1 to 1:15, preferably 30:1 to 1:10, more preferably from 25:1 to 1:8,particularly preferably 20:1 to 1:5, especially preferably 10:1 to 1:1, particularly preferably 6:1 to 2:1 and most preferably 4:1 to 9:4.

8. Printing substance according to at least one of the previous claims, characterized in that the molar ratio of monomer having at least one C-C double bond to cationic hardenable monomer with an epoxy and / or oxetane group is in the range from 20:1 to 1:5, preferably 10:1 to 1:3, particularly preferably 5:1 to 1:2 and especially preferably 2:1 to 1:1.

9. Printing substance according to at least one of the previous claims, characterized in that the water content of the printing substance is at most 4 % by weight, preferably at most 2 % by weight and particularly preferably at most 1% by weight, wherein the printing substance very particularly preferably does not contain any significant proportion of water.

10. Printing substance according to at least one of the previous claims, characterized in that the proportion of organic solvent in the printing substance is at most 4% by weight, preferably at most 2% by weight and particularly preferably at most 1% by weight, wherein the printing substance particularly preferably contains no substantial amounts of organic solvent.

11. Printing substance according to at least one of the previous claims, characterized in that the adhesion promoter comprises a hardenable group.

12. Printing substance according to at least one of the previous claims, characterized in that the printing substance contains at least 60 % by weight, preferably at least 70 % by weight, particularly preferably at least 80 % by weight of components A), B), C) and D).

13. Printing substance according to at least one of the previous claims, characterized in that the printing substance comprises at least one initiator, preferably a photoinitiator.

14. Printing substance according to at least one of the previous claims, characterized in that the molar ratio of (meth)acrylate to vinyl ether monomer is in the range from 20:1 to 1:20, preferably in the range from 6:1 to 1:6, particularly preferably in the range from 2:1 to 1:2.

15. Process for preparing a printing substance according to at least one of the previous claims, characterized in that the components A), B), C) and D) are mixed.

16. Use of a printing substance according to one of the previous claims 1 to 14, characterized in that the printing substance is applied to glass, ceramic, metal, wood or plastic, preferably on glass.

17. Use according to claim 16, characterized in that the printing substance is applied to a substrate using an inkjet printing process, preferably on glass.

18. Use according to claim 16 or 17, characterized in that the printing substance is applied in an atmosphere which has a relative humidity in the range from 25% to 50%.

19. Use according to one of claims 16 to 18, characterized in that after the printing substance has been applied to a substrate, preferably on glass, no further layer is applied.

20. Use according to one of claims 16 to 19, characterized in that, before the printing substance is applied to a substrate preferably on glass, no layer is applied, preferably untreated glass or flamed glass is being coated.