METHOD FOR THE DEPOLYMERIZATION OF POLYSTYRENE

DE502020009706D1Active Publication Date: 2024-11-28INEOS STYROLUTION GRP GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502020009706
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-10
Filing Date
2020-09-17
Publication Date
2024-11-28
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Current processes for depolymerizing polystyrene to produce styrene monomers face challenges in achieving high yields while minimizing the formation of styrene oligomers and harmful by-products, which complicates subsequent purification and affects polymerization processes.

Method used

A process involving thermal splitting of polystyrene in a fluidized bed reactor with a silicon carbide fluidized bed at specific temperature and residence time conditions to maximize styrene monomer yield, followed by cooling and separation of styrene monomers from other components.

Benefits of technology

This process achieves high yields of styrene monomers with minimized oligomer formation, ensuring high product quality and efficient purification, thereby optimizing the use of polystyrene in new polymerization processes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a process for producing styrene monomers by depolymerization of polystyrene, a device for carrying out the process, and the use of a device for depolymerization (degradation) of polystyrene.

[0002] Polystyrene is preferably selected from the group consisting of: standard polystyrene (GPPS), high-impact polystyrene (HIPS), and styrene-butadiene copolymers. High-impact polystyrene (HIPS) and / or standard polystyrene are particularly preferred. High-impact polystyrene (HIPS) and standard polystyrene, as well as their production, structure, and properties, are described in detail in the review literature (A. Echte, F. Haaf, J. Hambrecht in Angew. Chem. (Int. Ed. Engl.) 20, 344-361 (1981); and also in the Plastics Handbook, edited by R. Vieweg and G. Daumiller, Volume 4 "Polystyrene", Carl Hanser Verlag Munich (1996).

[0003] The transition from a linear to a circular economy is both ecologically and economically necessary in light of climate change, environmental pollution, population growth, and resource dependence. Intensive efforts were already undertaken in the 1980s and 1990s to develop processes for the raw material recycling of plastic waste, but large-scale applications have not yet been achieved due to unresolved process engineering problems and economic reasons. However, due to growing environmental awareness and an increasing demand for sustainable solutions, interest in chemical recycling is also growing.

[0004] Not all thermoplastic polymers are equally suitable for chemical recycling. The thermal decomposition of polyolefins or polyesters produces mixtures of, among other things, waxes, light oil, and gases. The degradation of polyethylene terephthalate (PET) leads to organic acids, mainly benzoic acid and terephthalic acid, which are corrosive and can also cause reactor clogging (G. Grause et al., Rohstoffrecycling von polymerem Abfallmaterial, in: Journal of Material Cycles and Waste Management, 13(4), 2011, 265-282).

[0005] In the case of polystyrene and other styrene-containing polymers, it is possible to depolymerize these polymers into their basic components, especially styrene monomers, making polystyrene and other styrene-monomer-containing polymers an excellent choice for chemical recycling.

[0006] However, the resulting product mixture from a depolymerization process must be purified in order to use the components as raw material for new purposes, such as polymerization processes.

[0007] When polystyrene is sufficiently thermally treated, it decomposes into styrene monomers, but incomplete decomposition also leads to the formation of, for example, styrene dimers, trimers, and other oligomers. If the decomposition conditions are too harsh, byproducts such as benzene, toluene, ethylbenzene, cumene, and alpha-methylstyrene can be formed. The amounts of these reaction products vary and depend on the reaction conditions and the raw materials used (see C. Bouster et al., Study of the pyrolysis of polystyrenes: Kinetics of thermal decomposition, Journal of Analytical and Applied Pyrolysis, 1 (1980) 297-313 and C. Bouster, Evolution of the product yield with temperature and molecular weight in the pyrolysis of polystyrene, in: Journal of Analytical and Applied Pyrolysis 15 (1989) 249-259).

[0008] The recovered styrene monomers can be used for a new polymerization process. Styrene oligomers can potentially disrupt the polymerization process, as even small amounts can affect important properties of the polymer. This also applies to other byproducts. Therefore, the styrene monomers should be separated from other components of the product mixture to ensure high product quality.

[0009] In particular, aromatic compounds other than styrene monomers can act as chain transfer agents in radical polymerization processes, lowering the average molecular weight of the polymers produced and contributing to polymers with a lower glass transition temperature (Tg) (see DS Achilias et al., Chemical recycling of polystyrene by pyrolysis: Potential use of the liquid product for the reproduction of polymer, in: Macromolecular Materials and Engineering, 292(8) (2007), 923-934). Protons from, for example, carboxylic acids, alcohols, aldehydes, or ketones act as termination agents in anionic polymerization processes of styrene (see D. Baskaran, Anionic Vinyl Polymerization, in: Controlled and Living Polymerizations: From Mechanisms to Applications, John Wiley & Sons, 2009, 1-56).

[0010] In the present process, polystyrene, preferably selected from the group consisting of standard polystyrene (GPPS), high-impact polystyrene (HIPS), and styrene-butadiene copolymers, is used. Furthermore, the high-impact polystyrenes used may have been structurally modified compared to conventional rubbers by the use of special polybutadiene rubbers with, for example, a modified 1,4-cis and / or 1,4-trans fraction or 1,2- and 1,4-bond.

[0011] Furthermore, instead of polybutadiene rubber, other diene rubbers as well as ethylene-propylene-diene copolymer (EPDM rubber) and hydrogenated diene rubbers or silicone rubbers can be used.

[0012] In the impact-resistant polystyrene used as polystyrene, the diene monomer content, in particular the polybutadiene monomer content, is generally 5 to 12 wt.%, preferably 6 to 10 wt.%, particularly preferably 7 to 9 wt.%, and the polystyrene content is generally 88 to 95 wt.%, preferably 90 to 94 wt.%, more preferably 91 to 93 wt.%, wherein the sum of the polystyrene content and the diene monomer content is 100 wt.%.

[0013] Suitable standard polystyrene is produced by anionic or radical polymerization. The molecular weight inconsistency of the polymer, which can be influenced by the polymerization process, is of minor importance. Standard polystyrene and impact-resistant polystyrene are preferred, the toluene-soluble fraction of which has a mean molecular weight (Mw) of 150,000 to 300,000 g / mol, particularly preferably 150,000 to 270,000 g / mol, and which may optionally be further modified with additives such as mineral oil (e.g., white oil), stabilizers, antistatic agents, flame retardants, or waxes.

[0014] Styrene copolymers used as polystyrene may contain methyl(meth)acrylate, α-methylstyrene and / or maleic anhydride, as well as other copolymerizable monomers.

[0015] In JP 2005132802 and JPH 11100875 (Toshiba Plant Systems) a process for recovering styrene from polystyrene waste is described, but no solution for separating light boilings, styrene and heavy boilings is provided.

[0016] There is a high demand for a process for the production of styrene monomers by depolymerization of polystyrene that provides styrene in very high yield while keeping the formation of styrene oligomers as low as possible in order to minimize the subsequent purification process.

[0017] It is known that the fluidized bed process is suitable for the depolymerization of polymers such as polystyrene. Liu et al. ("Pyrolysis of polystyrene waste in a fluidizedbed reactor to obtain styrene monomer and gasoline fraction", Fuel Processing Technology, 63, 45-55 (2000)) and Williams et al. ("Product composition from the fast pyrolysis of polystyrene", Environmental Technology, 20, 1109-1118 (1999)) investigated the pyrolysis of PS waste using a fluidized bed reactor and observed the depolymerization of polystyrene into styrene mono- and oligomers.

[0018] US 5 672 794 A, Gabriela de la Puente et al.: "Recycled Plastics in FCC Feedstocks: Specific Contributions" (Industrial & Engineering Chemistry Research 1997, 36, 4530-4534), Dement'ev Konstantin et al: "Thermal depolymerization of polystyrene in highly aromatic hydrocarbon medium" (Journal of Analytical and Applied Pyrolysis 2019, 142), Samih Said et al.: "From complex feedstocks to new processes: The role of the newly developed micro-reactors" (Chemical Engineering and Processing: Process Intensification 2018, 131, 92-105), and WO 2018 / 018153 A1 also describe various processes for the depolymerization of polystyrene in fluidized bed reactors and other reactors under different conditions.

[0019] One object of the invention is to provide a process for the production of styrene monomers by depolymerization of polystyrene with optimized process conditions in order to maximize the yield of styrene monomers. Harmful byproducts should also be avoided.

[0020] It was found that certain combinations of depolymerization temperature and residence time in the reactor lead to particularly high styrene monomer yields.

[0021] The invention relates to a process for the production of styrene monomers by depolymerization of polystyrene, comprising the steps of: a) Feeding a polymer composition (A) containing 60 to 99.9 wt% polystyrene, based on the total weight of the polymer composition (A), into the reaction zone (R) of a pyrolysis reactor (P); b) thermally cracking the polystyrene contained in the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) at a temperature of 450 °C to 1000 °C to obtain a product mixture (G) containing styrene monomers and other components; c) removing the product mixture (G) obtained in step b) from the reaction zone (R) of the pyrolysis reactor (P); d) cooling the product mixture (G) removed in step c) to obtain a condensed product mixture (K) containing styrene monomers and other components; and e) separating the styrene monomers from the other components of the condensed product mixture (K) obtained in step d), wherein the mean residence time (Z) of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is from 0.01 s to 10 s;

[0022] In this case, the pyrolysis reactor (P) is a fluidized bed reactor whose reaction zone (R) comprises a silicon carbide fluidized bed, and / or the temperature in the reaction zone (R) of the pyrolysis reactor (P) is 580 °C to 630 °C with a mean residence time (Z) of the polymer composition (A) in the reaction zone of the pyrolysis reactor of 0.4 s to 0.6 s.

[0023] The polymer composition (A), which is fed into the reaction zone (R) of the pyrolysis reactor (P) in step a) of the process according to the invention, contains 60 to 99.9 wt.%, preferably 80 to 99.9 wt.%, particularly preferably 90 to 99.9 wt.%, most preferably 95 to 99.9 wt.% polystyrene, based on the total weight of the polymer composition (A).

[0024] The remaining 0.1 to 40 wt.%, preferably 0.1 to 20 wt.%, particularly preferably 0.1 to 10 wt.%, most preferably 0.1 to 5 wt.%, based on the total weight of the polymer composition (A), may consist of polymeric components other than polystyrene and / or additives and / or other foreign substances.

[0025] If polymers other than polystyrene are included in the polymer composition (A), these are selected, for example, from the group consisting of polyolefins, polyesters, (co-)polymers of acrylonitrile, (co-)polymers of vinylaromatic monomers other than styrene, (co-)polymers of alkyl(meth)acrylates and copolymers of styrene with other monomers that do not belong to the other (co-)polymers listed here.

[0026] Suitable polymers other than polystyrene include, for example, copolymers of vinylaromatic monomers with further comonomers such as butadiene, (meth)acrylate, acrylonitrile, alpha-methylstyrene and phenylmaleimide. In particular, these are vinyl aromatic copolymers selected from the group consisting of: styrene-acrylonitrile copolymers (SAN), α-methylstyrene-acrylonitrile copolymers (AMSAN), styrene-maleic anhydride copolymers, styrene-phenyl maleimide copolymers, styrene-methyl methacrylate copolymers (SMMA), styrene-acrylonitrile-maleic anhydride copolymers, styrene-acrylonitrile-phenyl maleimide copolymers, α-methylstyrene-acrylonitrile-methyl methacrylate copolymers, α-methylstyrene-acrylonitrile-t-butyl methacrylate copolymers, styrene-acrylonitrile-t-butyl methacrylate copolymers.

[0027] Other suitable polymers include, for example, diene rubbers such as homopolymers of conjugated dienes and copolymers of such dienes with each other, copolymers of such dienes with acrylates, in particular n-butyl acrylate, and copolymers of such dienes with the comonomers selected from styrene, α-methylstyrene, acrylonitrile, methacrylonitrile, methyl methacrylate (MMA), maleic anhydride (MSA), and N-phenylmaleimide (N-PMI). The diene rubbers may also contain crosslinking, polyfunctional monomers.

[0028] Also suitable are polyolefins such as PE-LD (low-density polyethylene), PE-LLD (linear low-density polyethylene), PE-HD (high-density polyethylene), metallocene polyethylenes, ethylene copolymers such as poly(ethylene-co-vinyl acetate), ethylene-butene, ethylene-hexene, ethylene-octene copolymers, as well as cycloolefin copolymers, individually or as mixtures. Furthermore, polypropylenes, such as homo- or copolymers of propylene, metallocene-catalyzed polypropylenes, and copolymers of propylene with other comonomers known to those skilled in the art, are also suitable.

[0029] Polycarbonates, polyamides, poly(meth)acrylates, polyvinyl chlorides, polyesters, halogenated polymers, vinyl aromatic diene copolymers (SBC), polyethers, polysulfones, polyethersulfones, polyimidazoles and related polymers may also be included in the polymer composition (A).

[0030] Preferably, the polymer composition (A) contains less than 30 wt.%, particularly preferably less than 15 wt.%, most preferably less than 5 wt.%, based on the total weight of the polymer composition (A), of polyolefins, less than 5 wt.%, particularly preferably less than 2 wt.%, most preferably less than 1 wt.%, based on the total weight of the polymer composition (A), of (co-)polymers of acrylonitrile, and less than 5 wt.%, particularly preferably less than 2 wt.%, most preferably less than 1 wt.%, based on the total weight of the polymer composition (A), of polyesters.

[0031] Preferably the polymer composition (A) contains no polymeric components other than polystyrene.

[0032] The polymer composition (A) may contain 0 to 20 wt.% of common plastic additives and auxiliaries, based on the total weight of the polymer composition (A). For example, an additive or auxiliary may be selected from the group consisting of antioxidants, UV stabilizers, peroxide destructors, antistatic agents, lubricants, mold release agents, flame retardants, fillers or reinforcing agents (glass fibers, carbon fibers, etc.), colorants, and combinations of two or more thereof. Examples of oxidation retarders and heat stabilizers include halides of Group I metals of the periodic table, e.g., sodium, potassium, and / or lithium halides, possibly in combination with copper(I) halides, e.g., chlorides, bromides, iodides, sterically hindered phenols, hydroquinones, various substituted members of these groups, and their mixtures in concentrations up to 1 wt.-%, based on the total weight of the polymer composition (A).

[0033] Examples of UV stabilizers, which are generally present in amounts up to 2 wt% based on the total weight of the polymer composition (A), include various substituted resorcinols, salicylates, benzotriazoles and benzophenones.

[0034] Furthermore, organic dyes such as nigrosine, pigments such as titanium dioxide, phthalocyanines, ultramarine blue, and carbon black may be included as colorants in the polymer composition (A), as well as fibrous and powdered fillers and reinforcing agents. Examples of the latter are carbon fibers, glass fibers, amorphous silica, calcium silicate (wollastonite), aluminum silicate, magnesium carbonate, kaolin, chalk, powdered quartz, mica, and feldspar.

[0035] Examples of germination agents that may be included are talc, calcium fluoride, sodium phenylphosphinate, aluminum oxide, silicon dioxide and nylon 22.

[0036] Lubricants and demolding agents, which can generally be used in quantities up to 1 wt% based on the total weight of the polymer composition (A), include, for example, long-chain fatty acids such as stearic acid or behenic acid, their salts (e.g., Ca or Zn stearate) or esters (e.g., stearyl stearate or pentaerythritol tetrastearate) as well as amide derivatives (e.g., ethylene bisstearylamide).

[0037] Furthermore, mineral-based antiblocking agents may be present in amounts up to 0.1 wt%, based on the total weight of the polymer composition (A). Examples include amorphous or crystalline silica, calcium carbonate, or aluminum silicate.

[0038] For example, mineral oil, preferably medical white oil, may be included as a processing aid in amounts up to 5 wt.%, preferably up to 2 wt.%, based on the total weight of the polymer composition (A).

[0039] Examples of plasticizers include phthalic dioctyl esters, phthalic dibenzyl esters, phthalic butylbenzyl esters, hydrocarbon oils, N-(n-butyl)benzenesulfonamide and o- and p-tolylethylsulfonamide.

[0040] Furthermore, all flame retardants known for the respective thermoplastics may be included, in particular those based on phosphorus compounds or red phosphorus itself.

[0041] Furthermore, it may still contain moisture and / or other inorganic and / or organic foreign components, such as food residues.

[0042] In a particularly preferred embodiment, the polymer composition (A) consists of 90 to 99.9 wt.%, based on the total weight of the polymer composition (A), of polystyrene and 0.1 to 10 wt.%, based on the total weight of the polymer composition (A), of additive(s). In a very particularly preferred embodiment, the polymer composition (A) consists of 95 to 99.9 wt.%, based on the total weight of the polymer composition (A), of polystyrene and 0.1 to 5 wt.%, based on the total weight of the polymer composition (A), of additive(s).

[0043] Preferably, the polystyrene component contained in the polymer composition (A) consists substantially, preferably entirely, of GPPS (general purpose polystyrene). In this context, "substantially" means that the polystyrene component does not contain any components that significantly alter the properties of the GPPS.

[0044] The polymer composition (A) used according to the invention can optionally be pretreated in a suitable manner to remove, for example, adhering contaminants such as food residues or dirt, moisture and foreign substances such as metals or other substances and composite materials.

[0045] This is advantageously achieved in a pretreatment that may include one or more of the following steps, the order of which is not fixed and which may also be repeated several times: manual sorting of contaminants, washing, comminution, automatic sorting in suitable equipment. If necessary, polymer compositions that do not correspond to polymer composition (A) can also be converted into a polymer composition (A) used according to the invention by such a process.

[0046] A preferred embodiment of the inventive method is therefore one in which a polymer composition that does not correspond to polymer composition (A) is subjected to a pretreatment comprising one or more of the following steps, the order of which is not fixed and steps can also be repeated several times: manual sorting of contaminants, washing, comminution, automatic sorting in suitable equipment in order to obtain polymer composition (A).

[0047] The thermal decomposition of polystyrene is carried out in a fluidized bed reactor with a silicon carbide fluidized bed in the reaction zone (R). Alternatively, the decomposition of polystyrene can take place at a temperature of 580 °C to 630 °C and a mean residence time (Z) of the polymer composition of 0.4 s to 0.6 s in any suitable reactor where the temperature required for decomposition can be reached. For example, thermal decomposition can be carried out in a rotary kiln. Rotary kilns are described, for example, in EP-A 1481957. Thermal decomposition can also take place in extruders, which are described, for example, in EP-A 1966291. Such reactors can be operated with or without a gas flow, such as a carrier gas or gas as the reaction medium.

[0048] The pyrolysis reactor (P) can therefore, in principle, be any known type of pyrolysis reactor, provided that the design of the pyrolysis reactor allows for precise temperature control in the reaction zone (R) of the pyrolysis reactor (P) and precise control of the mean residence time (Z) of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P).

[0049] In this context, "precise setting" means that the deviation of the actual temperature in the reaction zone (R) of the pyrolysis reactor (P) from the set temperature is at most 10 °C, preferably at most 5 °C, particularly preferably at most 1 °C, or that the deviation of the actual mean residence time (Z) from the set mean residence time (Z) is at most 0.2 s, preferably at most 0.1 s, particularly preferably at most 0.05 s, most preferably at most 0.01 s.

[0050] The pyrolysis reactor (P) is preferably a fluidized bed reactor, as described, for example, in Schildhauer et al., "Reactors for Fluid-Solid Reactions: Fluidized Bed Reactors" in: Reschetilowski W. (ed.): Handbook of Chemical Reactors, Springer Spektrum, Berlin, Heidelberg (2019). A gas or gas mixture is typically used as the fluidization medium. The gas or gas mixture is usually non-reactive under the conditions prevailing in the pyrolysis reactor (P). Preferably, the gas is selected from water vapor, nitrogen, noble gases (Xe, Ar, Ne, He), or a mixture thereof.

[0051] The gas or gas mixture can be introduced into the pyrolysis reactor (P) as a separate gas stream. The optimal flow rate of the gas or gas mixture depends on the reactor configuration as well as the reaction or process conditions.

[0052] The process can be optimized by adjusting the parameters of temperature, residence time of the reaction mixture in the reaction zone (R) of the pyrolysis reactor (P), and concentration of the starting materials. The area of ​​the reactor where the reaction mixture is subjected to conditions conducive to depolymerization reactions is referred to here as the reaction zone (R).

[0053] The pyrolysis reactor (P) can contain a solid medium, e.g., SiO₂ (quartz sand) or SiC. In a preferred embodiment, the pyrolysis reactor (P) is a fluidized bed reactor comprising a fluidized bed of silicon carbide (SiC) in the reaction zone (R). SiC, in addition to high chemical and mechanical stability, possesses good thermal conductivity and heat capacity. This combination is advantageous for carrying out endothermic processes.

[0054] SiC with a weight-average particle size of 20 to 1000 µm, and particularly preferably 40 to 500 µm, is preferably used. At such particle sizes, particularly good fluidization of the fluidized bed is achieved and particularly effective heat transfer to the polymer composition (A) is enabled.

[0055] It has been found that the yield of styrene monomers is particularly high when the residence time of the polystyrene in the depolymerization zone is kept short. This can be achieved in fluidized bed reactors or other reactors that utilize a gas stream to transport the introduced polymer composition (A) through the reactor. The mean residence times of the reactant in a fluidized bed reactor with a silicon carbide fluidized bed in the reaction zone (R) range from 0.1 seconds to 10 seconds. Short residence times can be achieved by using high gas flow velocities. Depolymerization can be carried out at pressures from 0.01 bar to 5 bar or at atmospheric pressure (1 bar). Preferably, the gas stream is preheated before being introduced into the reaction zone (R). Preheating is preferably performed at a temperature that is at most 200 °C lower than the temperature in the reaction zone (R) of the pyrolysis reactor (P).

[0056] In the process according to the invention, the temperature in the reaction zone (R) of the pyrolysis reactor (P) is set to 400 to 1000 °C, often 450 to 1000 °C, preferably 500 to 800 °C, particularly preferably 550 to 650 °C, and most preferably 580 to 630 °C in a fluidized bed reactor with a silicon carbide fluidized bed in the reaction zone (R). The mean residence time of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is set to 0.1 to 10 s, preferably 0.2 to 2 s, particularly preferably 0.3 to 1 s, and most preferably 0.4 to 0.6 s. In a preferred embodiment, the temperature in the reaction zone (R) is 500 to 800 °C and the mean residence time of the polymer composition (A) therein is 0.2 to 2 s. In a particularly preferred embodiment, the temperature in the reaction zone (R) is 550 to 650 °C and the mean residence time of the polymer composition (A) therein is 0.3 to 1 s.In a particularly preferred embodiment, the temperature in the reaction zone (R) is 580 to 630 °C and the mean residence time of the polymer composition (A) therein is 0.4 to 0.6 s.

[0057] The temperature can be set in any known way, for example by microwave radiation, with the aid of heat exchangers, gas burners, resistive heating elements (resistance heating), or by introducing superheated gas, in particular steam, either alone or in combination. In one embodiment, the temperature is set using resistive heating elements in contact with the wall of the reaction zone (R) of the pyrolysis reactor (P). Alternatively, the temperature can be set using steam, which is provided by evaporating water and heated to the desired temperature by a steam superheater. In another embodiment, a combination of resistive heating elements in contact with the wall of the reaction zone (R) of the pyrolysis reactor (P) and steam is used to set the temperature in the reaction zone (R) of the pyrolysis reactor (P).

[0058] In a preferred embodiment, the pyrolysis reactor (P) is a fluidized bed reactor, preferably comprising a SiC fluidized bed in its reaction zone (R), wherein the temperature in the reaction zone (R) is adjusted by introducing steam of the desired temperature. In this embodiment, the steam is supplied by an evaporator and heated to the desired temperature by a steam superheater. Also in this embodiment, the steam is used both for adjusting the temperature in the reaction zone (R) and for generating the fluidized bed. Optionally, in this embodiment, the heating energy in the reaction zone (R) can additionally be supplied by resistive heating elements that are in contact with the wall of the reaction zone (R) of the pyrolysis reactor (P).

[0059] The particle size and concentration of the polymer composition (A) in the reaction zone (R) can be adapted to the specific characteristics of the reactor and its configuration, the reaction conditions, and the composition of the polymer composition (A). Typically, the polymer composition (A) has a particle size between 100 µm and 50 mm, preferably between 250 µm and 5 mm, and particularly preferably between 500 µm and 2 mm. The particles can have a spherical or non-spherical shape. In the case of a spherical shape, the particle size is determined by measuring the volume-mean diameter. In the case of non-spherical particles, for example, needle-shaped particles, the longest dimension is used to determine the particle size.

[0060] The concentration of the reactant in the reactor depends on the reactor type, reactor size, and reactor configuration. Typically, the concentration of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is between 1 and 50 wt.%, preferably between 1 and 25 wt.%, particularly preferably between 1 and 10 wt.%, and most preferably between 2 and 7 wt.%.

[0061] Preferably, the polymer composition (A) is pneumatically fed into the reaction zone (R) of the pyrolysis reactor (P) in step a), mixed with the silicon carbide fluidized bed, and finally depolymerized in step b). Particularly preferably, the polymer composition (A) is fed continuously in step a).

[0062] During the residence time (Z) in the reaction zone (R) of the pyrolysis reactor (P), the polystyrene component and, if applicable, other polymers of the polymer composition (A) are at least partially depolymerized to yield a product mixture (G) containing styrene monomers and other components.

[0063] The product mixture (G), containing styrene monomers and other components, is withdrawn from the reaction zone (R) of the pyrolysis reactor (P) in step c). Preferably, the withdrawal takes place continuously. Particularly preferably, the product mixture (G) is withdrawn continuously in a gaseous state from the upper region of the reaction zone (R) of the pyrolysis reactor (P). In this case, the withdrawal of the product mixture (G) can be carried out automatically, for example, by conveying the product mixture (G) out of the reaction zone (R) due to the reaction-induced increase in pressure in the reaction zone (R).

[0064] The pyrolysis reactor may contain or be connected to a quench. In this context, a quench is understood to be a region of the pyrolysis reactor in which the depolymerization reaction is rapidly stopped, preferably by cooling the hot gas consisting of the product mixture (G) and an inert gas stream, for example, steam. The quench serves, among other things, to stabilize the reaction products and to prevent or reduce unwanted repolymerization. Typical quenchers cool the product mixture (G) from a temperature of more than 400 °C to a temperature of less than 350 °C within a very short period of time, preferably within less than 10 seconds, particularly preferably within less than 5 seconds, and most preferably within less than 1 second. Quenches are described, for example, in EP 1966291.

[0065] After being removed from the reaction zone (R) of the pyrolysis reactor (P), the product mixture (G) is cooled, causing condensation of the styrene monomers and other components, resulting in a condensed product mixture (K) containing styrene monomers and other components. The product mixture (G) is cooled to a temperature below the condensation point of styrene monomers. Preferably, the product mixture (G) is cooled to a temperature below 70 °C, particularly preferably below 50 °C, and most preferably below 40 °C. In a preferred embodiment, the product mixture (G) is cooled to a temperature between 0 °C and 70 °C. In a particularly preferred embodiment, the product mixture (G) is cooled to a temperature between 0 °C and 50 °C. In a most particularly preferred embodiment, the product mixture (G) is cooled to a temperature between 15 °C and 40 °C.

[0066] Cooling can be achieved in any known way. For example, cooling is possible on a solid surface cooled by water or air. Cooling is also possible using a water mist that is brought into direct contact with the product mixture (G). Preferably, cooling takes place in a water mist.

[0067] The condensable components of the product mixture (G) are condensed according to their vapor pressures and collected along with the water. Condensation yields a condensed product mixture (K) containing styrene monomers and other components. When cooled in a water mist, the condensed product mixture (K) is obtained as a two-phase system with the cooling water. In this case, the condensed product mixture (K) is separated from the aqueous phase as a floating organic phase. The aqueous phase can be cooled again and used as a water mist to cool the product mixture (G).

[0068] The condensed product mixture (K) typically contains more than 50 wt%, based on the total weight of the condensed product mixture (K), styrene monomers and less than 50 wt%, based on the total weight of the condensed product mixture (K), of the other components. Preferably, the condensed product mixture (K) contains 50 to 99 wt.%, based on the total weight of the condensed product mixture (K), styrene monomers and 1 to 50 wt.%, based on the total weight of the condensed product mixture (K), of the other components, particularly preferably 60 to 99 wt.%, based on the total weight of the condensed product mixture (K), of styrene monomers and 1 to 40 wt.%, based on the total weight of the condensed product mixture (K), of the other components, most preferably 75 to 99 wt.%, based on the total weight of the condensed product mixture (K), of styrene monomers and 1 to 25 wt.-%, based on the total weight of the condensed product mixture (K) and the other components.

[0069] In the further course of the process, the condensed product mixture (K) is separated into styrene monomers and other components. This separation can be carried out by any known method suitable for separating mixtures of liquid products and, optionally, solids into their components. Depending on the other components besides styrene monomers, suitable methods for separating the condensed product mixture (K) into styrene monomers and other components may include, for example, sedimentation, centrifugation, filtration, decantation, distillation, chromatography, crystallization, and sublimation.

[0070] If the condensed product mixture (K) contains solids, it is advantageous to separate the solids before separating the liquid components. In this case, it is preferred to separate the solids from the liquid components by sedimentation, centrifugation, filtration, distillation, sublimation and / or decantation, particularly preferably by filtration, and most preferably by filtration using a solid-liquid filter.

[0071] The further separation of the liquid components into styrene monomers and other components preferably comprises at least one distillation step, such as fractional distillation, at least one chromatography step, such as column chromatography, HPLC, or flash chromatography, and / or at least one crystallization step, such as fractional crystallization. Particularly preferably, the separation of the liquid components comprises at least one distillation step, and most preferably, at least one fractional distillation step. In a particularly preferred embodiment, the separation of the liquid components into styrene monomers and other components comprises at least one fractional distillation step in one or more rectification columns.

[0072] It is often advantageous to recycle at least some of the other components into the reaction zone (R) of the pyrolysis reactor (P). This is particularly advantageous if some of the other components contain styrene oligomers, such as styrene dimers and styrene trimers. This allows for an overall better yield of styrene monomers, as it also enables the depolymerization of the remaining oligomers. For this reason, preferably at least some of the other components of the condensed product mixture (K) that have been separated from styrene monomers are recycled into the reaction zone (R) of the pyrolysis reactor (P). Continuous recycling of the other components is especially preferred.

[0073] In a preferred embodiment, the further components that are recycled to the reaction zone (R) of the pyrolysis reactor (P) consist essentially of styrene oligomers, preferably styrene dimers and styrene trimers. In this context, "essentially" means that the further components recycled to the reaction zone (R) of the pyrolysis reactor (P) contain no other components besides styrene oligomers that would interfere with the depolymerization process in the reaction zone (R) of the pyrolysis reactor (P).

[0074] A further aspect of the invention is the use of a fluidized bed reactor for the depolymerization of polystyrene at a temperature in the reaction zone (R) of 400 °C to 1000 °C and a mean residence time of the polystyrene in the reaction zone (R) of 0.01 s to 10 s, wherein the fluidized bed reactor comprises a fluidized bed of silicon carbide (SiC) in the reaction zone (R). The silicon carbide, the temperature in the reaction zone (R), and the mean residence time of the polystyrene in the reaction zone (R) are particularly preferably selected as described for the process according to the invention.

[0075] Furthermore, the invention also relates to an apparatus for carrying out the inventive process for the production of styrene monomers, in which the reaction zone (R) and the pyrolysis reactor (P) are designed in such a way that gentle depolymerization of polystyrene can take place, wherein the apparatus as pyrolysis reactor (P) comprises a fluidized bed reactor comprising a fluidized bed of silicon carbide (SiC) in the reaction zone (R), wherein the silicon carbide preferably has a weight-average particle size of 20 to 1000 µm, particularly preferably 40 to 500 µm, optionally resistive heating conductors on the outer walls of the reaction zone (R), an evaporator for generating steam, a steam superheater for setting the desired steam temperature, a line for introducing the steam into the reaction zone (R) and a quench for cooling the product mixture (G).

[0076] The invention is illustrated by the following examples, figures and claims. Examples

[0077] From an inerted feed hopper (B101), the polymer is metered via volumetric dosing into a gas jet, which pneumatically conveys the particles into the reaction zone of a fluidized bed reactor (R101) containing SiC particles. Heating energy is transferred to the reaction zone via resistive heating conductors through the metallic reactor wall. The steam for generating the fluidized bed is supplied by an evaporator (D101) and heated to the desired temperature by a steam superheater (E102).

[0078] In the reaction zone, the SiC fluidized bed is created with the steam, and the pneumatically introduced polymer particles are mixed in the fluidized bed and finally depolymerized.

[0079] The product mixture from the depolymerization process (R101) is cooled to below 50 °C in column (K101) using a water mist. Condensable components condense according to their vapor pressures and are collected with the water in the cooled sump. Solid particles are also precipitated by the mist according to their coalescence tendency. Floating, water-insoluble components are transferred to a buffer vessel via a skimmer system. Samples are taken from the concentrated organic fraction of the condensed product mixture and analyzed by gas chromatography.

[0080] The water from the condensation process is cooled via a heat exchanger and then pumped back into the cooling column (K101). Any solids are removed using a solid-liquid filter. Examples 1.1 to 1.6

[0081] An amorphous polystyrene (GPPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200°C / 5 kg load, ISO 1133) of approximately 28 cm³ / 10 min was depolymerized in the apparatus described above under various conditions. The temperature in the reaction zone of the fluidized bed reactor (R101) was varied between 550 °C and 650 °C, and the residence time between 0.46 and 1 s. Unless otherwise specified, the concentration of the polymer composition in the reaction zone was maintained at 5 wt% based on the total reactor filling, consisting of SiC and polymer particles. The yields of pyrolysis oil (condensate oil) and styrene monomers as a function of the reaction conditions are shown in Table 1. The compositions of the pyrolysis oil are shown in Table 2. Example 2

[0082] Example 1.2 was repeated with a high-impact amorphous polystyrene (HIPS) (INEOS Styrolution, Frankfurt) with a melt volume flow rate (Melt Volume Rate 200 °C / 5 kg load, ISO 1133) of approximately 4 cm³ / 10 min. The styrene monomer yield is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Example 3

[0083] Example 1.1 was repeated using a polymer composition consisting of 50 wt% of the polymer composition from Example 1 and 50 wt% of the polymer composition from Example 2. The yield of styrene monomers is shown in Table 1. The composition of the pyrolysis oil is shown in Table 2. Table 1: Results of the pyrolysis experiments Example polymer Temperature in the reaction zone [°C] Average residence time in reaction zone [s] Mass fraction of condensate oil relative to mass used [wt.%] Styrene concentration in condensate oil [wt%] 1.1 GPPS 550 0,54 70,6 74,8 1.2 GPPS 600 0,51 65,9 83,2 1.3 GPPS 550 0,46 64,8 68,2 1.4 GPPS 650 0,48 69,0 76,8 1.5 GPPS 550 0,66 72,3 76,3 1.6 GPPS, 8 wt% in reaction zone 550 0,54 72,5 73,4 2 HIPS 600 0,51 45,7 70,9 3 50% by weight GPPS / 50% by weight HIPS 550 0,54 91,9 70,1 Table 2: Composition of the pyrolysis oil Example Styrene concentration in condensate oil [wt%] Dimer concentration in condensate oil [wt%] Trimer concentration in condensate oil [wt.%] Concentration of other compounds in the condensate oil [wt.%] 1.1 74,8 8,4 8,3 8,6 1.2 83,2 6,0 0,6 10,3 1.3 68,2 10,7 9,8 11,2 1.4 76,8 4,5 0,7 17,9 1.5 76,3 7,0 5,3 11,3 1.6 73,4 8,2 1,1 17,3 2 70,9 7,3 3,3 18,6 3 70,1 6,6 7,5 15,7

[0084] Explanation of the characters Fig. 1shows a flow diagram of the pilot plant for carrying out the production of styrene monomers by depolymerization of polystyrene. Fig. 2 shows an overview of the styrene concentration in the condensate oil. Fig. 3 shows the dependence of the pyrolysis oil composition on the temperature. Fig. 4 shows the dependence of the pyrolysis oil composition on the residence time for pure GPPS. Fig. 5 shows the dependence of the pyrolysis oil composition on the concentration of the reactant in the reactor. Fig. 6 This shows the dependence of the pyrolysis oil composition on the composition of the reactant.

Claims

1. Process for the preparation of styrene monomers by depolymerization of polystyrene, comprising the steps of: (a) feeding a polymer composition (A) containing 60 to 99.9% by weight of polystyrene, based on the total weight of the polymer composition (A), into the reaction zone (R) of a pyrolysis reactor (P); b) thermally cracking the polystyrene contained in the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) at a temperature of 400°C to 1000°C to obtain a product mixture (G) containing styrene monomers and further components; c) removing the product mixture (G) obtained in step b) from the reaction zone (R) of the pyrolysis reactor (P); d) cooling the product mixture (G) removed in step c) to obtain a condensed product mixture (K) containing styrene monomers and further components; and e) separating the styrene monomers from the further components of the condensed product mixture (K) obtained in step d), wherein the average residence time (Z) of the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) is from 0.01 s to 10 s, and wherein the pyrolysis reactor (P) is a fluidized bed reactor, and wherein the reaction zone (R) of the fluidized bed reactor comprises a silicon carbide fluidized bed.

2. Process for the preparation of styrene monomers by depolymerization of polystyrene, comprising the steps of: (a) feeding a polymer composition (A) containing 60 to 99.9% by weight of polystyrene, based on the total weight of the polymer composition (A), into the reaction zone (R) of a pyrolysis reactor (P); b) thermally cracking the polystyrene contained in the polymer composition (A) in the reaction zone (R) of the pyrolysis reactor (P) at a temperature of 400°C to 1000°C to obtain a product mixture (G) containing styrene monomers and further components; c) removing the product mixture (G) obtained in step b) from the reaction zone (R) of the pyrolysis reactor (P); d) cooling the product mixture (G) removed in step c) to obtain a condensed product mixture (K) containing styrene monomers and further components; and e) separating the styrene monomers from the further components of the condensed product mixture (K) obtained in step d), the temperature in the reaction zone (R) of the pyrolysis reactor (P) being from 580°C to 630°C and the average residence time (Z) of the polymer composition (A) in the reaction zone of the pyrolysis reactor being from 0.4 s to 0.6 s.

3. Process according to claim 1 or 2, wherein the condensed product mixture (K) obtained in step d) contains from 75 to 99% by weight of styrene and from 1 to 25% by weight of the further components, in each case based on the total weight of the product mixture (K).

4. Process according to claim 2, wherein the pyrolysis reactor (P) is a fluidized bed reactor.

5. Process according to claim 4, wherein the reaction zone (R) of the fluidized bed reactor comprises a silicon carbide fluidized bed.

6. Process according to any one of claims 1 to 5, wherein at least a part of the further components obtained in step e) is recycled to the reaction zone (R) of the pyrolysis reactor (P).

7. Process according to claim 6, in which the further components obtained in step e), which are recycled into the reaction zone (R) of the pyrolysis reactor (P), consist essentially of styrene oligomers.

8. Process according to claim 6 or 7, in which the recycling of the further components obtained in step e) into the reaction zone (R) of the pyrolysis reactor (P) is carried out continuously.

9. Process according to any one of claims 1 to 8, wherein the polystyrene component in the polymer composition (A) fed into the reaction zone (R) of the pyrolysis reactor (R) in step a) consists essentially of GPPS (general purpose polystyrene).

10. Process according to any one of claims 1 to 9, in which in step d) the product mixture (G) removed in step c) is cooled to a temperature of 0 °C to 50 °C.

11. Process according to any one of claims 1 to 10, wherein the polymer composition (A) comprising polystyrene in step a) contains no further polymeric components.

12. Process according to any one of claims 1 to 11, wherein the separation of the styrene monomers in step e) comprises the step of fractional distillation.

13. Use of a fluidized bed reactor for the depolymerization of polystyrene at a temperature in the reaction zone (R) of from 400°C to 1000°C and an average residence time of the polystyrene in the reaction zone (R) of from 0.01 s to 10 s, wherein the fluidized bed reactor comprises a silicon carbide fluidized bed.

14. Apparatus for carrying out a process for the production of styrene monomers according to any one of claims 1 to 12, wherein the reaction zone (R) and the pyrolysis reactor (P) are designed such that a gentle depolymerization of polystyrene can take place, wherein the pyrolysis reactor (P) is a fluidized bed reactor, and wherein the reaction zone (R) of the fluidized bed reactor comprises a silicon carbide fluidized bed.