AI Technical Summary
Existing mosquito net screens made from polymer-coated wires tend to accumulate dust and dirt, requiring frequent cleaning due to their hydrophobic nature, which limits their dirt resistance.
A glass thread coated with a polymer-based layer containing a specific silane, such as 3-glycidoxypropyltrimethoxysilane, is used to create screens with improved dirt resistance, incorporating a thermoplastic polymer like polyvinyl chloride and optional additives like photocatalytic or hydrophilic layers, which reduces dust accumulation.
The coated glass thread screens exhibit reduced dust accumulation and improved dirt resistance, as demonstrated by lower contact angles and lower loss of transparency in dirt tests, indicating a more hydrophilic surface that requires less frequent cleaning.
Description
[0001] The invention relates to a glass yarn provided with a polymer-based coating, intended for the manufacture of a screen, in particular in the form of a grid, fabric or knit, usable in particular as a mosquito net.
[0002] Screens made of a network of wires are generally placed at windows and doors to prevent insects from entering homes. The mesh size of the network is adapted to retain insects, especially mosquitoes, without blocking the passage of air and light.
[0003] Such screens are generally made from a wire with a coating based on a polymer, for example polyvinyl chloride (PVC): the wire is assembled in the appropriate form (grid, fabric or knit), then the assembly is treated in an enclosure heated to a temperature allowing the polymer to melt, and cooled to room temperature causing the polymer to solidify and the wires to bond at their crossing points.
[0004] Screens can also be obtained by making an assembly of wires (grid, fabric or knit), then treating it with a polymer-based coating composition, and finally subjecting it to a heat treatment as described above in order to bond the wires at the crossing points.
[0005] However, dust and dirt from the surrounding environment tend to stick to these screens, blocking all or part of the mesh, which requires regular cleaning of the screen.
[0006] There are known solutions to limit the clogging of mosquito nets and thus reduce the number of cleanings over a given period.
[0007] One solution described in CN-Y-2237104 is to integrate the screen into a frame and to associate it with mechanical cleaning means such as brushes.
[0008] In US-A1-2004 / 0224147, a self-cleaning screen was proposed in the form of a mesh of wires having a coating including either titanium oxide particles with photocatalytic activity or nanoparticles which give the screen a low surface energy (the surface is said to be "super-hydrophobic").
[0009] In EP 0 170 981 A1, a sizing composition for glass fibers has been proposed which may comprise a fiber protector chosen from a long list of polymers capable of forming a film and / or a lubricant, and possibly a coupling agent chosen from a long list of compounds which would only be present if the hydrophilic nature of the fibers limits their compatibility with the polymers.
[0010] From FR-A1-2 908 137, there is also known a method for treating an organic surface, for example PVC, aimed at forming a barrier layer above which is a photocatalytic layer based on titanium oxide. The method operates at atmospheric pressure, in the presence of an ionized gas which allows the formation of a layer, in particular SiO 2 , having better adhesion to the layer based on titanium oxide.
[0011] In US 3,922,466 A, sulfur-containing organosilane compounds are described which are used as coupling agents and flame retardants to effectively bond glass yarns and elastomeric materials.
[0012] The aim of the present invention is to obtain a glass yarn coated with a polymer-based layer which in particular allows the manufacture of screens having improved resistance to soiling.
[0013] This goal is achieved by adding, into the polymer forming the coating layer, a silane of the following formula (I): in which R 1 , R 2 , R 3 , which may be identical or different, represent a C 1 -C 6 alkyl group, a C 2 -C 6 alkenyl group, a C 2 -C 6 alkynyl group, a C 6 -C 10 aryl group, a hydroxyl group, a C 1 -C 6 alkoxy group, a C 6 -C 10 aryloxy group, a C 1 -C 6 acyloxy group, a C 2 -C 7 alkylcarbonyl group, at least two of the groups R 1 , R 2 , R 3 representing a hydroxyl group or an alkoxy group, and R 4 represents a group containing at least one epoxy function, an aryl group, optionally substituted, a halogen atom or a group bearing at least one atom of halogen, in particular fluorine, a group containing at least one aldehyde function, a group carrying at least one function containing a phosphorus atom, an acryloxy or methacryloxy group, said group carrying the aforementioned functions being a C carbon group 1 -C 18 , preferably C 1 -C 8 , which may contain at least one oxygen heteroatom.
[0014] Preferably, the groups R 1 , R 2 and R 3 are chosen from methyl, ethyl, methoxy and ethoxy groups.
[0015] More preferably, the R 4 group is: a group carrying at least one epoxy function in the terminal position, in particular a glycidoxyalkyl group in which the alkylene radical contains 1 to 8 carbon atoms, advantageously glycidoxypropyl, an aryl group, in particular phenyl, a halogen atom or an aliphatic chain containing 1 to 9 carbon atoms carrying at least one halogen atom, in particular fluorine.
[0016] Particularly preferred silane is 3-glycidoxypropyl-methyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, phenyltriethoxysilane and triethoxyfluorosilane.
[0017] The polymer used in the composition of the coating is a thermoplastic polymer, possibly of an elastomeric nature. Examples include polyolefins such as polyethylene and polypropylene, vinyl polymers such as polyvinyl acetate, vinyl acetate-vinyl chloride copolymers, polyvinyl chloride, polyvinylidene chloride and (meth)acrylic polymers. Polyvinyl chloride is preferred.
[0018] Where appropriate, a plasticizer may be used to give greater flexibility to the aforementioned polymer. The plasticizer is generally chosen from organic acid esters, preferably containing at least two carboxylic groups, for example alkyl and / or aryl phthalates and alkyl adipates, phosphates and vegetable oils, in particular soybean or castor, or derived from petroleum cuts, in particular paraffinic, aromatic or naphthenic.
[0019] Preferred plasticizers for use with PVC are alkyl and / or aryl phthalates, e.g., di(2-ethylhexyl)phthalate, dibutylphthalate, dioctylphthalate, diphenylphthalate, and butyl and benzyl phthalate, alkyl adipates, e.g., di(2-ethylhexyl)adipate, dibutyladipate, and dioctyladipate, and phosphates.
[0020] The mixture of polymer and plasticizer is in the form of a plastisol or paste.
[0021] The mixture of polymer, silane and optionally plasticizer may further contain conventional additives, for example heat stabilizers, lubricants, flame retardants, organic and / or inorganic pigments, slip agents such as silicones, and anti-UV agents which protect the polymer from light radiation.
[0022] The yarn provided with a polymer-based coating according to the invention can be used as such to manufacture screens, for example in the form of grids, fabrics or knits.
[0023] The yarn may further comprise at least one additional layer which is superimposed on the aforementioned polymer layer, which additional layer makes it possible to give the yarn specific properties.
[0024] Examples of such layers include: photocatalytic layers that contain TiO 2 particles in anatase form, generally in a mesoporous silica matrix. Most often, a barrier sub-layer, in particular made of silica, is associated with the photocatalytic layer arranged between the PVC layer and said photocatalytic layer in order to avoid degradation of the PVC by the TiO 2 particles, antistatic layers, in particular obtained by sol-gel, for example ITO (indium - tin oxide) layers, SnO 2 layers doped with a metal, in particular Sb, Nb, Ta or W, and ZnO layers doped or not with Sn, Al, In, Y, Zr or B, as well as layers based on a UV-crosslinkable or thermocrosslinkable polymer matrix containing ITO nanoparticles, hydrophilic layers, in particular based on silica, deposited by sol-gel or atmospheric plasma as described for example in FR 2 908 137 A1, hydrophobic and / or oleophobic layers,in particular consisting of a matrix (in the form of a layer or beads) of silica grafted with fluorinated compounds, in particular trialkoxyfluoroalkylsilanes, alkylsilanes, arylsilanes or hexaalkyldisilazanes.
[0025] The amount of polymer-based coating deposited on the glass yarn generally represents 15 to 80% of the total weight of the coated yarn, preferably 50 to 70% and advantageously 55 to 65%.
[0026] The quantity of silane deposited on the glass wire represents 0.5 to 15% of the total weight of the coating, preferably 1 to 10% and advantageously 3 to 7%.
[0027] The yarn according to the invention is obtained by applying a composition containing the polymer and the silane to a glass yarn containing a plurality of glass filaments.
[0028] The glass yarn according to the invention is a yarn composed of a multitude of glass filaments (or base yarn) or a yarn obtained by assembling several base yarns into rovings (roving in English), a co-mingled yarn composed of intimately mixed glass filaments and thermoplastic filaments or a mixed yarn consisting of assembled glass yarns and thermoplastic yarns. The base yarn and the yarns composed of glass and polyester filaments are preferred. In the aforementioned yarns, the glass filaments are conventionally coated with a size applied to them during their drawing and before they are gathered in the form of one or more yarns. The size makes it possible in particular to protect the filaments from the risks of abrasion when they are in contact with the various members necessary to manufacture the yarn, and also to bind the filaments together.
[0029] The above-mentioned yarn can be an untwisted yarn or a twisted yarn, for example with a twist of 0.4 to 1 turn per centimeter.
[0030] The glass used in the construction of the wires can be of any type, for example E, C, R, AR (alkali-resistant). E glass is preferred.
[0031] The diameter of the glass filaments constituting the yarns can vary widely, for example from 3 to 30 µm and preferably from 5 to 20 µm. Similarly, wide variations can occur in the linear density of the yarn which can range from 10 to 100 tex and preferably from 20 to 50 tex.
[0032] The glass yarn may be bare or provided with a layer based on a polymer, preferably of the same chemical nature as the polymer of the coating layer containing the silane of formula (I) in accordance with the invention.
[0033] The glass yarn of the invention is obtained by applying said coating composition to the aforementioned glass yarn by any means known to those skilled in the art, for example by impregnation (“dip coating” in English), in particular by passing through a die or in a bath, or extrusion. Preferably, the application is carried out by passing through a die, by passing the yarn through a loop supplied with the coating composition, then into a heated enclosure, the yarn finally being collected in the form of a winding. The temperature of the enclosure varies according to the nature of the polymer used: it is higher than the softening temperature of the polymer and in any case is much lower than the degradation temperature of the polymer. In the case of polyvinyl chloride, the temperature varies from 100 to 250°C.
[0034] The glass yarn obtained is used to make screens in the form of grids, fabrics or knits which can be used in particular as mosquito nets.
[0035] Conventionally, the grids are formed by superimposing a first layer of parallel glass threads oriented in one direction and a second layer of parallel glass threads oriented in another direction, preferably in directions forming an angle generally of the order of 90°.
[0036] Glass yarn fabrics and knits can be obtained by any method known to those skilled in the art.
[0037] The grids, fabrics and knits are then subjected to a heat treatment which aims to bond the threads at their points of contact or intersection and therefore to consolidate the grid. The treatment temperature varies depending on the nature of the polymer, above the softening temperature and below the polymer degradation temperature. For polyvinyl chloride, the temperature varies from 100 to 250°C.
[0038] If necessary, an additional layer can be applied to the grid, fabric or knit, from a sol-gel as mentioned above. The sol-gel can be applied by impregnation, spraying, roller or curtain, followed by a heat treatment step, for example in a hot air chamber or under one or more infrared radiation lamps.
[0039] The grids, fabrics and knits incorporating the glass yarns according to the invention have a surface mass which varies to a wide extent, for example from 50 to 300 g / m 2< , preferably 70 to 200 g / m 2< .
[0040] The screen according to the invention can be used as a mosquito net but also as a blind or sunshade, placed indoors or outdoors.
[0041] The following examples illustrate the invention without, however, limiting it. EXAMPLES 1 TO 4
[0042] In a container, pour 95 parts by weight of a PVC plastisol and 5 parts by weight of the following silane: 3-glycidoxypropyltrimethoxysilane: example 1 phenyltriethoxysilane: example 2 triethoxyfluorosilane: example 3.
[0043] The PVC plastisol used consists of 66.5% by weight of PVC and 33.5% by weight of a butyl or benzyl phthalate.
[0044] The resulting composition is deposited on a glass plate using a film puller (thickness: 200 µm), then the plate is placed in an oven at 160°C for 5 minutes.
[0045] Under the same conditions, a PVC composition not containing silane is deposited on a glass plate (Reference).
[0046] The glass plate is placed in a climatic chamber (40°C; relative humidity: 95%). 3 µl of water is placed on the plate, which is kept at room temperature, and the contact angle is measured using a tensiometer at different intervals. The measurements are shown in Table 1 below. Table 1 Ex. 1 Ex. 2 Ex. 3 Ref. 0 days 83,5 90,8 92,8 79,7 1 day 55,0 72,5 58,1 75,0 4 days 36,0 72,4 47,5 71,2 6 days 24,7 66,3 43,8 68,0 11 days - 53,6 39,1 67,9 14 days 19,6 - - 67,7 34 days 23,3 - - 66,5
[0047] It is noted that examples 1 to 3 according to the invention make it possible to reduce the contact angle, i.e. to have a more hydrophilic surface than the Reference. EXAMPLES 5 AND 6 (COMPARATIVE) a) manufacture of the glass yarn screen
[0048] A glass yarn is continuously manufactured by passing an E-glass yarn, with a linear density of between 30 and 35 tex, through an impregnation bath containing 95 parts by weight of PVC plastisol and 5 parts by weight of 3-glycidoxypropyltrimethoxysilane in accordance with Example 1. The glass yarn obtained has a linear density of between 85 and 90 tex and the average thickness of the PVC coating is 305 µm.
[0049] A glass thread is manufactured in the same way using a PVC plastisol without the aforementioned silane (comparative example 6).
[0050] With the above-mentioned yarn, a fabric is produced with an average mesh opening of dimension equal to 1000 µm x 1500 µm. The fabric is treated in an oven at 165°C for a time sufficient to melt the PVC and after cooling fix the yarns at the crossing points. b) screen soiling test
[0051] A square sample (11 cm on each side) of the screen obtained in a) is placed in the center of an easel inclined backwards at an angle of 10° to the vertical. 30 cm from the sample, a spray nozzle is placed which dispenses a perpendicular jet (100 ml in total) to the surface of the sample and over the entire surface.
[0052] The sprayed solution is representative of the most commonly encountered soiling. The solution is a hydroalcoholic solution (volume ratio water:ethanol:isopropan-2-ol 51:26.5:22.5) which contains the following compounds in the following concentrations, expressed in g / l: - stearic acid 0,735 - adipic acid 2,940 - graphite (d 50 = 2.5 µm) 0,147 - calcium nitrate 0,235 - copper nitrate 0,044 - zinc nitrate 0,044 - potassium sulfate 0,117 - sodium sulfate 0,088 - calcium sulfate 0,088 - sodium chloride 0,088
[0053] On each screen sample, 6 measurement zones are defined (4 cm square each) on which the surface corresponding to the opening of the meshes is measured before and after the soiling test. The measurement is carried out using Fourier transform image processing which proceeds by counting white pixels (clean surface) and black pixels (dirty surface). The test is carried out on 5 samples.
[0054] The loss of transparency, in percent, is calculated as follows: nombre de pixels noirs / nombre total de pixels × 100
[0055] The results are as follows: Ex. 5 Ex. 6 (comp.) Loss of transparency (%) 4,8 23,8
Claims
1. A glass strand comprising a coating layer, characterized in that said layer comprises: - a polymer chosen from the group consisting of vinyl acetate / vinyl chloride copolymers, polyvinyl chloride and polyvinylidene chloride, and - a silane of following formula (I): in which: • R1, R2 and R3, which are identical or different, represent: - a C1-C6 alkyl group, - a C2-C6 alkenyl group, - a C2-C6 alkynyl group, - a C6-C10 aryl group, - a hydroxyl group, - a C1-C6 alkoxy group, - a C6-C10 aryloxy group, - a C1-C6 acyloxy group, - a C2-C7 alkylcarbonyl group, at least two of the R1, R2 and R3 groups representing a hydroxyl group or an alkoxy group, and • R4 represents: - a group including at least one epoxy functional group, - an optionally substituted aryl group, - a halogen atom or a group carrying at least one halogen atom, in particular a fluorine atom, - a group including at least one aldehyde functional group, - a group carrying at least one functional group including a phosphorus atom, - an acryloyloxy or methacryloyloxy group, said group carrying the abovementioned functional groups being a C1-C18, preferably C1-C8, carbon-based group which can comprise at least one oxygen heteroatom.
2. The strand as claimed in claim 1, characterized in that the R1, R2 and R3 groups are chosen from the methyl, ethyl, methoxy and ethoxy groups.
3. The strand as claimed in claim 1 or 2, characterized in that the R4 group is: - a group carrying at least one epoxy functional group in the end position, in particular a glycidoxyalkyl group in which the alkylene radical includes from 1 to 8 carbon atoms, advantageously glycidoxypropyl, - an aryl group, in particular a phenyl group, - a halogen atom or an aliphatic chain including from 1 to 9 carbon atoms carrying at least one halogen atom, in particular a fluorine atom.
4. The strand as claimed in one of claims 1 to 3, characterized in that the silane is 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, phenyltriethoxysilane and triethoxyfluorosilane.
5. The strand as claimed in one of claims 1 to 4, characterized in that the polymer is a thermoplastic polymer optionally having an elastomeric nature.
6. The strand as claimed in one of claims 1 to 5, characterized in that the coating layer additionally comprises a plasticizer chosen from organic acid esters, phosphates and oils resulting from petroleum fractions.
7. The strand as claimed in one of claims 1 to 6, characterized in that it additionally comprises an additional layer which is superimposed on the polymer layer chosen from photocatalytic layers, antistatic layers, hydrophilic layers and hydrophobic and / or oleophobic layers.
8. The strand as claimed in claim 7, characterized in that the photocatalytic layer comprises TiO2 particles in anatase form, preferably in a matrix of mesoporous silica.
9. The strand as claimed in claim 7, characterized in that the antistatic layer is an ITO layer, an SnO2 layer doped with a metal, in particular Sb, Nb, Ta or W, a ZnO layer which is or is not doped with Sn, Al, In, Y, Zr or B, or a layer based on a UV-crosslinkable or heat-crosslinkable polymer matrix comprising ITO nanoparticles.
10. The strand as claimed in claim 7, characterized in that the hydrophilic layer is based on silica.
11. The strand as claimed in claim 7, characterized in that the hydrophobic and / or oleophobic layer is composed of a matrix (in the form of a layer or of beads) of silica grafted with fluorinated compounds, alkylsilanes, arylsilanes or hexaalkyldisilazanes.
12. The strand as claimed in one of claims 1 to 11, characterized in that the amount of polymer-based coating deposited on the glass strand represents from 15 to 80% of the total weight of the coated strand, preferably from 50 to 70% and advantageously from 55 to 65%.
13. The strand as claimed in one of claims 1 to 12, characterized in that the amount of silane deposited on the glass strand represents from 0.5 to 15% of the total weight of the coated strand, preferably from 1 to 10% and advantageously from 3 to 7%.
14. A screen in the form of a grid, woven fabric or knitted fabric, characterized in that it is composed of glass strands as claimed in one of claims 1 to 13.
15. The screen as claimed in claim 14, characterized in that it exhibits a weight per unit area which varies from 50 to 300 g / m2 and preferably from 70 to 200 g / m2.
16. The use of the screen as claimed in claim 14 or 15 as mosquito net, blind or sun screen.