METHOD FOR PRODUCING A HARDENED GLASS SUBSTRATE WITH REDUCED IRISE
Patent Information
- Application Number
- DE602017085662
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-09-19
- Filing Date
- 2017-09-14
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2037-09-14
AI Technical Summary
Thermally reinforced glass substrates treated by air blowing nozzles often exhibit unwanted iridescence due to anisotropic stress distribution, which affects their optical properties and is undesirable in applications like automotive and building glass.
A temporary polymer layer, specifically a (meth)acrylate polymer, is applied to the glass substrate before thermal reinforcement, which improves heating homogeneity and reduces anisotropy by depolymerizing during the heating process, thereby minimizing iridescence.
The temporary polymer layer significantly reduces iridescence in thermally reinforced glass substrates by enhancing emissivity and reducing optical delays measured with circular polarized light, resulting in a more uniform stress distribution and improved optical performance.
Description
[0001] The invention relates to the field of thermally strengthened, semi-tempered or tempered glass and proposes a solution for reducing the phenomenon of unwanted iridescence affecting this type of glass substrate when the thermal strengthening cooling is administered by nozzles blowing air.
[0002] Rapid cooling of a glass substrate above its glass transition temperature gives it specific mechanical properties that are well known to those skilled in the art. In particular, glass has improved mechanical properties and characteristic breakage behavior since it fractures spontaneously and completely into a multitude of small, blunt pieces.
[0003] Different tempering processes have been described, such as chemical tempering (see in particular US8166778), thermal tempering by contact, in which the glass is cooled by contact with a cold mold (see in particular EP667320), thermal tempering in a fluidized bed of solid particles (see US4113458), “La Bastie” thermal tempering, in which the glass is immersed in greases or oils, or thermal tempering by blowing air (see in particular US2013255319). To implement the latter process, nozzles can be used to blow air directly onto the surface of the hot glass, generally onto the two main surfaces of the glass substrate. This latter process is relatively simple to implement, but the final glass may possibly exhibit more or less strong iridescence depending on the viewing angle, the layers deposited on the glass, the degree of tempering, the equipment used, etc.These iridescences are colorations affecting reflected light and are probably caused by the structure of the glass, in particular an anisotropic distribution of stresses. They are generally unwanted, whether in automotive glass or in building glass. These iridescences appear to represent a ghost of the network of blowing nozzles used.
[0004] WO2015019022 teaches a substrate bearing a functional coating and a temporary protective layer obtained from a liquid composition comprising (meth)acrylate compounds. Tempering of this substrate is envisaged but the cooling technique is not discussed.
[0005] A process has now been found to significantly reduce the iridescence of thermally strengthened glass substrates, the cooling of which was carried out by blowing air through nozzles. The concept of thermal strengthening covers those of semi-tempering and tempering.
[0006] According to the invention in claim 1, a layer comprising a polymer, in particular a polymer of a (meth)acrylate, is applied to the surface of the glass substrate before heating it and then cooling it to thermally strengthen it. The layer comprising the polymer disappears during the heating of the thermal strengthening treatment, in particular by depolymerization and / or oxidation and this is why it is called a temporary layer. Surprisingly, while the temporary layer disappears during heating, and therefore before the blowing of cooling air, the presence of the temporary layer produces a strong reduction in the iridescence observed after cooling. It is believed that the polymer layer improves the homogeneity of the heating of the glass, thereby reducing the final anisotropy of the glass substrate.
[0007] A transparent material with inhomogeneous residual stresses (this is the case for tempered or hardened glass of the prior art) does not transmit light identically at all points on its surface. This is called birefringence. This can be measured by the optical delay, which corresponds to the phase shift of a light wave between its entry and its exit from the transparent material. A high optical delay reflects a strong anisotropy. The reduction of iridescence can thus be evaluated by measuring the optical delay. These measurements can be carried out using the method described in the article by Ilguth, M., Schuler, M., Bucak, O., 2015, “The effect of optical anisotropies on building glass facades and its measurement method”, Frontiers of Architectural Research 4, pp. 119-126. One measurement per mm 2< of glass substrate is carried out, then the arithmetic mean of all these measurements is calculated. Optical delays are measured with circularly polarized light.
[0008] Thermal strengthening is applied to glass substrates by a technique well known to those skilled in the art involving heating followed by blowing air through nozzles. This may be semi-tempering (generating a glass surface stress in the range of 40 to 90 MPa, in absolute value) or tempering (generating a glass surface stress greater than 90 MPa in absolute value). Thermal strengthening is applied by rapid cooling and by blowing air through nozzles onto the previously heated glass substrate. The heating brings the glass substrate above the glass transition temperature Tg of the glass as measured by dilatometry. Generally, this heating brings the glass substrate to more than 550°C, and generally to more than 590°C. Generally, the heating is carried out below 720°C and more generally below 700°C.In most cases, heating is carried out around 620°C, depending on the glass composition and the desired degree of reinforcement. The stronger the thermal reinforcement, the higher the surface stress caused. The surface stress can be determined by a device operating on the principle of polariscopy such as the Scalp-04 polariscope, the determined value being an average of 5 measurements on a main surface of the glass substrate and at least 20 cm from the edge. The surface stress values mentioned above are absolute values, since the skilled person can also express them with a negative sign.
[0009] In the context of the present application, a glass substrate is defined as a glass sheet or a glass sheet coated with at least one thin layer such as a functional coating, in particular of the low-emissivity or solar control type. The term sheet covers the notion of plate. The term "thermally reinforced glass substrate" refers to glass substrates after application of the method according to the invention, i.e. after application of thermal reinforcement (heating then cooling). The glass substrate used at the start of the method according to the invention is generally not thermally reinforced. It can be thermally reinforced, but this is unnecessary since its quality of being thermally reinforced disappears as soon as the strengthening treatment according to the invention is heated.
[0010] Thus, the invention according to claim 1 relates to a method of manufacturing a thermally reinforced glass substrate, comprising the application of a layer comprising a polymer, in particular a polymer of a (meth)acrylate, called a temporary layer, on a glass substrate comprising a glass sheet, then the application to the glass substrate coated with the temporary layer of a thermal glass strengthening treatment comprising heating leading to the elimination of the temporary layer, then cooling by blowing air through nozzles.
[0011] Heating is generally carried out at a temperature above 550°C, or even above 590°C. It is generally carried out at a temperature below 720°C and more generally below 700°C.
[0012] Generally, the starting glass substrate comprises a functional coating between the glass and the temporary layer, the functional coating being able to be of the low-emissivity type or of the solar control type. This type of coating can cause difficulty in heating the glass, which reinforces the anisotropic nature of the stresses inside the final glass. It is observed that the glass substrates coated with such a functional coating exhibit, after thermal reinforcement, more marked iridescence than in the absence of a functional coating. The method according to the invention drastically reduces the iridescence of such thermally reinforced glass substrates. Without this explanation being able to provide a limitation of the present application, it seems that the temporary layer according to the invention helps in the homogeneous heating of the glass substrate thanks to its high emissivity.In the presence of a functional coating, it counteracts the effect of the latter during the heating step of the thermal strengthening treatment, thereby reducing the anisotropy of the stress distribution and consequently the importance of iridescence. The temporary layer would thus increase the emissivity of the glass surface already coated with the functional coating, the latter having by nature a low emissivity. Thus, the glass substrate coated with the temporary layer has a higher emissivity than the same glass substrate without a temporary layer. In particular, the glass substrate has, before application of the temporary layer, a normal emissivity of less than 10%, or even less than 5%.
[0013] The functional coating comprises at least one metallic layer, in particular comprising silver. The functional coating may comprise a stack of thin layers comprising an alternation of x metallic layers, and (x+1) anti-reflective coatings, each metallic layer being arranged between two anti-reflective coatings. An anti-reflective coating comprises at least one dielectric layer. Thus, a dielectric layer of the anti-reflective coating of the functional coating may be in direct contact with the glass. The value of x is greater than or equal to 1 and generally goes up to 4. A metallic layer may be silver or silver-based (more than 50% by weight of silver) or be a metallic alloy containing silver. A dielectric layer within the meaning of the present invention is made of an electrically insulating and “non-metallic” material, and is therefore not a metal.A dielectric material is a material containing oxygen and / or nitrogen, introduced deliberately. This material has an n / k ratio over the entire visible wavelength range (from 380 nm to 780 nm) equal to or greater than 5, n designating the real refractive index of the material at a given wavelength and k representing the imaginary part of the refractive index at a given wavelength, the n / k ratio being calculated at a given wavelength identical for n and for k.
[0014] The dielectric layers of the anti-reflective coatings can be chosen from oxides, nitrides or oxynitrides of one or more elements chosen from titanium, silicon, aluminum, zirconium, hafnium, tin and zinc.
[0015] In particular, the upper layer of the functional coating preferably comprises a nitride or oxide or oxynitride of titanium and / or zirconium and / or hafnium, the expression "upper layer" designating the layer furthest from the glass if the functional coating comprises several layers. In particular, the upper layer may be chosen from a layer from the following list: titanium nitride, zirconium nitride, hafnium nitride, titanium and zirconium nitride, titanium and zirconium and hafnium nitride, titanium oxide, zirconium oxide, hafnium oxide, titanium and zirconium oxide, titanium and zirconium and hafnium oxide.
[0016] The functional coating can be deposited by any known means such as magnetic field assisted sputtering, thermal evaporation, CVD or PECVD, pyrolysis, chemical deposition, sol-gel deposition or wet deposition of inorganic layers.
[0017] All layers of the functional coating can be deposited by magnetic field-assisted sputtering. The temporary protective layer is advantageously in direct contact with the functional coating. Generally, the thickness of the functional coating is: greater than 100 nm, preferably greater than 150 nm, less than 300 nm, preferably less than 250 nm.
[0018] Thermal strengthening of glass involves heating followed by cooling by blowing air through nozzles, the blowing generally being carried out simultaneously towards the two main faces of the glass substrate. Cooling may cause semi-tempering or tempering. Preferably, the thermal strengthening is sufficient so that the absolute value of the surface stress of the sheet is greater than 40 MPa, in particular greater than 90 MPa, in particular greater than 110 MPa, in particular greater than 120 MPa (in absolute value). Generally, the absolute value of the surface stress of the sheet is less than 250 MPa.
[0019] The temporary layer may be deposited on a single main face or on each of the main faces of the glass substrate. It may be deposited on at least one edge of the glass substrate. The temporary layer is preferably deposited at each location already coated with a functional coating already described above. Thus, the temporary layer is generally in direct contact with the functional coating. Generally, the glass substrate comprises a functional coating on only one of its main faces and the temporary layer is applied to only one of the main faces, the one already comprising the functional coating.
[0020] The temporary layer is essentially organic in nature. It is made by applying a liquid composition to a thickness greater than 1 micrometer on the glass substrate, followed by its solidification by polymerization and / or crosslinking. Generally, the liquid composition has a viscosity between 0.05 and 5 Pa.s when applied.
[0021] The polymer, in particular a polymer of a (meth)acrylate, may represent at least 90% of the mass of the temporary layer. The temporary layer may comprise an organic material distinct from the polymer which may disappear during heating of the thermal strengthening treatment.
[0022] A polymer of a (meth)acrylate is formed from the reaction between them of (meth)acrylate compounds contained in the liquid composition. The (meth)acrylate compounds are chosen from monomers, oligomers, prepolymers or polymers comprising at least one (meth)acrylate function.
[0023] By (meth)acrylate is meant an acrylate or a methacrylate. By "(meth)acrylate compounds" is meant the esters of acrylic or methacrylic acid containing at least one acryl (CH2=CH-CO-) or methacryl (CH2=CH(CH3)-CO-) function. These esters can be monomers, oligomers, pre-polymers or polymers. These (meth)acrylate compounds, when subjected to polymerization conditions, give a polymer network with a solid structure.
[0024] The (meth)acrylate compounds used may be chosen from monofunctional and polyfunctional (meth)acrylates such as mono-, di-, tri-, poly-functional (meth)acrylates. Examples of such monomers are: monofunctional (meth)acrylates such as methyl(meth)acrylate, ethyl(meth)acrylate, n- or tert-butyl(meth)acrylate, hexyl(meth)acrylate, cyclohexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, benzyl(meth)acrylate, 2-ethoxyethyl(meth)acrylate, phenyloxyethyl(meth)acrylate, hydroxyethylacrylate, hydroxypropyl(meth)acrylate, vinyl(meth)acrylate caprolactone acrylate, isobornyl methacrylate, lauryl methacrylate, polypropylene glycol monomethacrylate, difunctional (meth)acrylates such as 1,4-butanediol di(meth)acrylate, ethylene dimethacrylate, 1,6-hexandiol di(meth)acrylate, bisphenol A di(meth)acrylate, trimethylolpropane diacrylate, triethylene glycol diacrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tricyclodecane dimethanol diacrylate, trifunctional (meth)acrylates such as trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, ethoxylated trimethylolpropane triacrylate,trimethylolpropane trimethacrylate, tripropylene glycol triacrylate, higher functionality (meth)acrylates such as pentaerythritol tetra(meth)acrylate, ditrimethylpropane tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate or hexa(meth)acrylate.
[0025] Preferably, the temporary layer does not include any mineral material such as a filler or a pigment. The temporary layer also does not include any additive that cannot be removed during heating as part of the thermal strengthening, such as, for example, an organic compound comprising silicon of the siloxane type. The temporary layer has the property of disappearing completely at the heating temperature as part of the thermal strengthening treatment and must therefore not contain anything that cannot disappear during this heating.
[0026] The temporary layer generally has a thickness greater than 1 micrometer and preferably greater than 5 micrometers. It generally has a thickness less than 100 micrometers, preferably less than 50 micrometers. Its thickness is generally between 2 and 100 micrometers, and even between 5 and 50 micrometers, in particular between 10 and 30 micrometers. The temporary layer generally has a weight between 5 and 50 g / m 2< , preferably between 10 and 30 g / m 2< . The thicker the temporary layer, the more it increases the emissivity of the glass substrate. It is therefore made thick enough so that the emissivity of the glass substrate is greater than that of the same glass substrate without a temporary layer.
[0027] For its application, the liquid composition advantageously comprises less than 20%, and preferably less than 10% by mass of solvent relative to the total mass of the liquid composition, or is even free of solvent. It preferably has a viscosity measured at 25°C of at least 0.05 Pa.s, or even at least 0.08 Pa.s, or even at least 0.1 Pa.s, or even at least 0.50 Pa.s. Its viscosity measured at 25°C is generally at most 5 Pa.s, or even at most 2 Pa.s.
[0028] The liquid composition generally comprises at least one polymerization initiator, preferably a photoinitiator, said initiator generally representing 0.1 to 20%, or even 1 to 15%, preferably 5 to 15% and better still 8 to 12% of the total mass of the (meth)acrylate compounds. The nature of the initiator depends on the type of curing chosen. For example, in the case of thermal curing, initiators of the benzoyl peroxide type are used. In the case of curing by UV radiation, initiators known as photoinitiators are used. The liquid composition may further comprise at least one additive chosen from plasticizers, absorbers, separating agents, heat and / or light stabilizers, thickening agents or surface modifiers, the sum of all the additives generally being between 0 and 5% of the mass of the liquid composition. The polymerization initiators are not considered to be additives.
[0029] Preferably, the (meth)acrylate compounds are chosen from esters of acrylic or methacrylic acid comprising at least two acryl (CH2=CH-CO-) or methacryl (CH2=CH(CH3)-CO-) functions. Preferably, the liquid composition comprises by mass relative to the total mass of the (meth)acrylate compounds, in increasing order of preference, at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, 100% of (meth)acrylate compounds chosen from esters of acrylic or methacrylic acid comprising at least two acryl (CH2=CH-CO-) or methacryl (CH2=CH(CH3)-CO-) functions,
[0030] Preferably, the liquid composition comprises by mass relative to the total mass of the (meth)acrylate compounds: 30 to 80% by mass of at least one aliphatic urethane-acrylic oligomer, 20 to 70% by mass of at least one (meth)acrylate monomer chosen from a mono, bi, tri functional (meth)acrylate.
[0031] The liquid composition may include: at least one aliphatic urethane-acrylic oligomer, at least one (meth)acrylate monomer chosen from mono-, bi-, tri-functional (meth)acrylate monomers, at least one polymerization initiator.
[0032] The liquid composition may include: at least one aliphatic urethane-acrylic oligomer, at least one difunctional (meth)acrylate monomer, at least one trifunctional (meth)acrylate monomer, at least one polymerization initiator, preferably a photoinitiator.
[0033] The liquid composition may be applied at room temperature by any known means, including roller coating, spraying, dipping, curtain coating, or spraying. The liquid composition is preferably applied by roller coating. The deposition speed of the liquid composition may be between 1 and 90 m / min.
[0034] The temporary layer can be hardened: by drying at a temperature below 200°C for a period ranging, for example, from 10 s to 180 s, by UV crosslinking (different wavelengths) preferably in the open air and at room temperature or by electron beam.
[0035] The starting glass substrate, as well as the final glass substrate (thermally reinforced) can have a thickness in the range from 1 to 20 mm, and more particularly in the range from 2 to 10 mm.
[0036] The temporary layer may be deposited on the glass substrate before or after a cutting step, i.e. in the latter case on a glass substrate at or close to the final size of the thermally strengthened glass substrate.
[0037] In addition to its beneficial effect in reducing the anisotropy of the thermally reinforced glass substrate, the polymer layer protects any functional coating from oxidation and mechanical stresses that may occur during its conveyance.
[0038] The invention also relates to a line for manufacturing thermally reinforced glass substrates from glass substrates comprising a glass sheet, comprising in the following order: a device for applying a temporary layer comprising a polymer to the glass substrates, a device for heating the glass substrates coated with the temporary layer, a device for blowing air through nozzles onto the heated glass substrates, means for conveying the glass substrates from the first to the last device in the line.
[0039] In the case where the temporary layer comprises a polymer of a (meth)acrylate, the device for depositing a temporary layer comprises a device for depositing a layer of a liquid composition comprising (meth)acrylate compounds on the glass substrates, a device for solidification by polymerization and / or crosslinking of the (meth)acrylate compounds leading to the temporary layer on the glass substrates.
[0040] Generally, the means for conveying glass substrates comprise a bed of rollers on which the glass substrates pass one behind the other. This bed of rollers passes through the heating furnace and the air blowing device by nozzles. Nozzles blow air through the bed of rollers towards the downward-facing face of the glass substrates and towards the upward-facing face of the glass substrates. The air blowing device by nozzles comprises nozzles arranged above and below the bed of rollers in order to blow air towards the two main faces of the glass substrates.
[0041] The manufacturing line may include a device for depositing a functional coating before the device for depositing a layer of a liquid composition. This may be a magnetic field-assisted cathode sputtering device.
[0042] In particular, the device for depositing a liquid composition may comprise a roller coating device. In particular, the crosslinking device may comprise a UV lamp. In particular, the manufacturing line may comprise a device for cutting the glass substrates between the crosslinking device and the heating device.
[0043] The invention leads to glass substrates that can exhibit reduced iridescence. The invention allows in particular the production of a thermally reinforced glass sheet comprising a surface stress greater than 40 MPa, or even greater than 90 MPa, and comprising iridescence visible to the naked eye and whose arithmetic mean of the optical retardation measured with circularly polarized light is less than 50 nm. In particular, this sheet can comprise on one of its main faces a functional coating, in particular a solar control coating, and comprising at least one metal layer, said coating having a thickness of between 100 and 300 nm. In particular, the thermally reinforced glass sheet has a high proportion of its surface exhibiting an optical retardation of less than 50 nm. This proportion is greater than 60% or even greater than 70%. Examples 1 and 2
[0044] We take two sheets of glass 6 mm thick and 800 mm x 600 mm from Saint Gobain Glass CoolLite154 II. These two sheets had on one of their main faces a functional coating of the solar control type made of a stack of thin layers successively comprising, starting from the glass, an alternation of two layers of silver and three anti-reflective coatings, each anti-reflective coating comprising several dielectric layers including one in Si 3 N 4 and one in ZnO, so that each layer of silver is placed between two anti-reflective coatings. The total thickness of this functional coating is between 150 and 200 nm.
[0045] On one of the sheets, a temporary layer is applied directly onto the functional coating as follows: A liquid composition was produced with mixtures of oligomers and monomers comprising at least one acrylate function marketed by the company Sartomer: CN9276: Tetra-functional aliphatic urethane-acrylate oligomer, SR351: Trimethylolpropane triacrylate, tri-functional acrylate monomer, SR833S: Tricyclodecane dimethanol diacrylate, di-functional acrylate monomer.
[0046] The presence of the urethane-acrylate oligomer allows the hardness and flexibility properties of the temporary protective layer to be modulated. The temporary protective layer is then cured by UV crosslinking. Irgacure 500, marketed by BASF, as a polymerization initiator is added to the liquid composition. The acrylates and the initiator were present in the liquid composition in the following proportions, given in parts by mass: Table 1 acrylate oligomer CN9276 60 tri-functional acrylate SR351 20 di-functional acrylate SR833S 20 Irgacure 500 Initiator 5
[0047] The liquid composition had a viscosity at 25 °C of 1.08 Pa.s and was applied to the glass substrate by roller coating. A thickness between 10 and 20 µm was obtained using speeds for the applicator roller between 15 and 25 m / min. The temporary layer was cured by UV radiation provided by a 120 W mercury lamp. Under these conditions, polymerization of the mixture of monomers and oligomers was obtained in the thickness range of 10 to 20 µm.
[0048] The emissivity of the glass substrate without polymer layer (example 1, comparative) was 2.52%. The emissivity of the glass substrate with the polymer layer (example 2, according to the invention) was 56.9%. The emissivity is the normal emissivity (in the sense of perpendicular) measured by the EN12898 standard of January 2001.
[0049] These two sheets are thermally strengthened by heating them to 600°C followed by rapid cooling by blowing air through nozzles on the two main faces of the two sheets. The surface compression is then measured at 60 MPa.
[0050] These substrates are then observed with a circular polariscope (the substrates are placed between two polarizing filters). figure 1 shows these two substrates. In a), the substrate that had not received the temporary layer (example 1) has a strong white mark in the central area.
[0051] The arithmetic mean of the optical delays of these two sheets was measured by the method described in the article by Ilguth, M., Schuler, M., Bucak, O., 2015, “The effect of optical anisotropies on building glass facades and its measurement method”, Frontiers of Architectural Research 4, pp. 119-126. One measurement per mm 2< was made, then the arithmetic mean was calculated. The optical delays were measured with circularly polarized light. The results are summarized in Table 2. Table 2 Average optical delay % of area with optical retardation < 50 nm Ex 1 (without polymer layer) 56,6 50% Ex 2 (with polymer layer) 33,2 80% Examples 3 and 4
[0052] The procedure is the same as for examples 1 and 2 except that the thermal reinforcement is more intense due to faster cooling and leads to a surface compression of 110 MPa and that the observation is simply carried out in reflection with the naked eye. figure 2shows these two substrates. In a), the substrate had not received the temporary layer and in b) the substrate had received the temporary layer. The substrate that had not received the temporary layer shows much more marked iridescence.
Claims
1. A process for the manufacture of a heat strengthened glass substrate, comprising: - the application of a layer comprising a polymer, a "temporary layer", on a glass substrate comprising a glass sheet, the glass substrate comprising a functional coating comprising at least one metallic layer, the temporary layer being applied on the functional coating, the temporary layer having a thickness of between 1 and 100 micrometers, then - the application to the glass substrate coated with the temporary layer of a treatment for the heat strengthening of the glass comprising heating, leading to the removal of the temporary layer, and then cooling by blowing of air through nozzles. the normal emissivity of the substrate coated with the temporary layer is greater than the normal emissivity of the substrate before application of the temporary layer, the percentage of the glass substrate surface area exhibiting a retardation of less than 50 nm is greater than 60%.
2. The process as claimed in the preceding claim, characterized in that the heating is carried out at a temperature of greater than 550°C, indeed even of greater than 590ºC.
3. The process as claimed in either of the preceding claims, characterized in that the glass substrate exhibits, before application of the temporary layer, a normal emissivity of less than 10%, indeed even of less than 5%.
4. The process as claimed in one of the preceding claims, characterized that the temporary layer has a thickness of between 5 and 50 micrometers.
5. The process as claimed in the preceding claim, characterized in that the functional coating is of the low-e type or of the solar control type.
6. The process as claimed in either of the two preceding claims, characterized in that the functional coating is deposited by cathode sputtering assisted by a magnetic field and in that the temporary layer is directly in contact with the functional coating.
7. The process as claimed in one of the three preceding claims, characterized in that the functional coating comprises at least one metal layer, in particular comprising silver.
8. The process as claimed in the preceding claim, characterized in that the functional coating comprises a stack of thin layers comprising an alternation of x metal layers based on silver or on a metal alloy containing silver and of (x+1) antireflective coatings, each antireflective coating comprising at least one dielectric layer, each metal layer being positioned between two antireflective coatings, x being greater than or equal to 1.
9. The process as claimed in one of claims 1 to 8, characterized in that the functional coating comprises an upper layer chosen from nitrides, oxides or oxinitrides of titanium and / or of zirconium and / or of hafnium, in particular chosen from: titanium nitride, zirconium nitride, hafnium nitride, titanium zirconium nitride, titanium zirconium hafnium nitride, titanium oxide, zirconium oxide, hafnium oxide, titanium zirconium oxide or titanium zirconium hafnium oxide.
10. The process as claimed in one of the preceding claims, characterized in that the cooling produces a surface stress of the glass of greater than 40 MPa.
11. The process as claimed in the preceding claim, characterized in that the cooling is a heat tempering producing a surface stress of greater than 90 MPa.
12. The process as claimed in one of the preceding claims, characterized in that the polymer is a polymer of a (meth)acrylate.
13. The process as claimed in the preceding claim, characterized in that it comprises: the preparation of a liquid composition comprising (meth)acrylate compounds chosen from monomers, oligomers, prepolymers or polymers comprising at least one (meth)acrylate functional group, the application of the liquid composition on the glass substrate, then the solidification, by polymerization and / or crosslinking, of the composition, so as to form the temporary layer.
14. The process as claimed in the preceding claim, characterized in that the liquid composition comprises less than 20% by weight of solvent and has a viscosity of between 0.05 and 5 Pa.s at its application.
15. The process as claimed in one of the preceding claims, characterized in that it comprises a stage of cutting up the glass substrate between the application of the temporary layer and the heating.
16. The process as claimed in one of the preceding claims, characterized in that the percentage of its surface area exhibiting a retardation of less than 50 nm is greater than 70%.
17. The process as claimed in one of the preceding claims, characterized in that the coating has a thickness of between 100 and 300 nm.