COLOR REGISTER SETTING METHOD FOR ALUMINUM ALLOY HUB

DE602018075446T2Active Publication Date: 2024-10-16CITIC DICASTAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602018075446
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-11-30
Filing Date
2018-11-13
Publication Date
2024-10-16
Estimated Expiration
2038-11-13

AI Technical Summary

Technical Problem

The existing methods for color register edging on aluminum alloy hubs face challenges such as low production efficiency, high labor intensity, unclear boundaries, and poor fastness of the edged paint surface, making it difficult to achieve a uniform and durable finish.

Method used

A method involving sequential pretreatment and drying steps, including electrostatic and air gun spraying with specific parameters, and the use of an injection needle for precise paint application, along with optional ultrasonic treatment to enhance the finish, results in a uniform and durable edge.

Benefits of technology

The method significantly reduces edge defects and improves the fastness of the edged paint surface, achieving a high-quality, uniform finish with reduced labor intensity and increased production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The present invention relates to the technical field of automobile parts, specifically to a color register edging method for an aluminum alloy hub.Background of the Invention

[0002] Aluminum wheel hubs are important exterior parts of automobiles, and their external beauty and color match directly attract the attention of consumers. With people's demand for the use of automobiles, the personalization and differentiation of wheel appearance have become the focus of everyone's attention. The fashion and dynamics of wheel hubs have become a mainstream of the times.

[0003] However, when edging is performed on other paint of a wheel, the sprayed area of the edged paint is narrow and the condition is complicated, so it is difficult to obtain an edged paint surface with high fastness. The existing shielded color register spraying process has the problems of low production efficiency, low qualification rate, unclear boundary of the color register part, high labor intensity and the like. US 2017 / 016106 A1 relates to a method for color register spraying of a hub.Summary of the Invention

[0004] Accordingly, the object of the present invention is to provide a uniform color register edging method for an aluminum alloy hub as specified in any one of claims 1 to 7.Detailed Description of the Embodiments Embodiment 1

[0005] In a preferred aspect of the present invention, in steps I, III and V, the first, second and third pretreatment and drying steps sequentially include 11 processes: washing, pre-degreasing, degreasing, washing, acid pickling, washing, passivation, washing, closing, washing and drying; an electrostatic gun is adopted for spraying body powder in step II, the distance between the electrostatic gun and the surface of a wheel is 200 mm, the throughput of the powder gun is 2.5 m 3< / h, the atomizing pressure is 3.0 bar, the electrostatic pressure is controlled at 50 KV, the front spray thickness is 120 µm, the body powder curing temperature is 175°C, and the holding time is 25 min; an air gun is adopted for spraying a paint in step II, the distance between the air gun and the surface of the wheel is 180 mm, the throughput of the spray gun is 60 cc / min, the atomizing pressure is 2.0 bar, the sector pressure is 2.0 bar, the paint spray thickness is 10 µm, the temperature of the wheel workpiece is 40-50°C, the paint curing temperature is 145°C, and the holding time is 25 min; in edging color register spraying of step IV, the injection needle has a caliber of 1.5 mm, the hub is horizontally placed on an automatic rotary table, the needle is fixed on an adjustable bracket, a paint supply system is closed, the distance between the needle and the sprayed surface of the wheel is 4 mm, the flow rate of the injected paint is 10 cc / min, the power of the automatic rotary table is 56.6 Hz, and the air pressure of the closed paint supply system is 2.0 bar; electrostatic spraying is adopted in the high-gloss transparent powder spraying process of step VI, the distance between the electrostatic gun and the surface of the wheel is 200 mm, the throughput of the powder gun is 2.5 m 3< / h, the atomizing pressure is 1.5 bar, the electrostatic pressure is 40 KV, the front spray thickness is about 80 µm, the transparent powder curing temperature is 177°C, and the holding time is 22 min.Embodiment 2

[0006] In steps I, III and V, the first, second and third pretreatment and drying steps sequentially include 11 processes: washing, pre-degreasing, degreasing, washing, acid pickling, washing, passivation, washing, closing, washing and drying; an electrostatic gun is adopted for spraying body powder in step II, the distance between the electrostatic gun and the surface of a wheel is 300 mm, the throughput of the powder gun is 4.5 m 3< / h, the atomizing pressure is 4.0 bar, the electrostatic pressure is controlled at 70 KV, the front spray thickness is 160 µm, the body powder curing temperature is 185°C, and the holding time is 20 min; an air gun is adopted for spraying a paint in step II, the distance between the air gun and the surface of the wheel is 250 mm, the throughput of the spray gun is 100 cc / min, the atomizing pressure is 3.0 bar, the sector pressure is 3.0 bar, the paint spray thickness is 20 µm, the temperature of the wheel workpiece is 40-50°C, the paint curing temperature is 150°C, and the holding time is 15 min; in edging color register spraying of step IV, the injection needle has a caliber of 1.5 mm, the hub is horizontally placed on an automatic rotary table, the needle is fixed on an adjustable bracket, a paint supply system is closed, the distance between the needle and the sprayed surface of the wheel is 6 mm, the flow rate of the injected paint is 20 cc / min, the power of the automatic rotary table is 56.6 Hz, and the air pressure of the closed paint supply system is 3.0 bar; electrostatic spraying is adopted in the high-gloss transparent powder spraying process of step VI, the distance between the electrostatic gun and the surface of the wheel is 300 mm, the throughput of the powder gun is 3.5 m 3< / h, the atomizing pressure is 2.5 bar, the electrostatic pressure is 60 KV, the front spray thickness is about 120 µm, the transparent powder curing temperature is 180°C, and the holding time is 15 min.Embodiment 3

[0007] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that step VI further includes the step of ultrasonic treatment, ultrasonic waves are applied to the wheel in a pulsed manner, each pulse lasts for 0.7 s, and the energy density is 400W / cm 2< .Embodiment 4

[0008] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that step VI further includes the step of ultrasonic treatment, ultrasonic waves are applied to the wheel in a pulsed manner, each pulse lasts for 0.7 s, and the energy density is 120W / cm 2< .Embodiment 5

[0009] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that step VI further includes the step of ultrasonic treatment, ultrasonic waves are applied to the wheel in a pulsed manner, each pulse lasts for 0.7 s, and the energy density is 240 W / cm 2< .Comparative Example 1

[0010] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that a spray gun is used for spraying a paint at a small flow rate and a low angle in step IV, the distance between the spray head and the sprayed surface of the wheel is 6 mm, the flow rate of the injected paint is 20 cc / min, the power of the automatic rotary table is 56.6 Hz, and the air pressure of a closed paint supply system is 3.0 bar.Embodiment 6

[0011] Edged products having bright color and sprayed uniformly are obtained from Embodiments 1-5 and Comparative Example 1.

[0012] First, the edge of the edged area of the product of each embodiment or the comparative example is observed with a magnifying glass. The edged area of the product of each embodiment or the comparative example is observed under an 8x magnifying glass, and the numbers of edge splashing points and edge protruding points within 5 cm are calculated. The edge splashing points are calculated as 3 scores, and the edge protruding points are calculated as 1 score. Five samples of the edged area of each product are counted and averaged. The results are shown in Table 1. Table 1: Edge characteristic test of Embodiments 1-5 and Comparative Example 1Group No.Edging defect integralEmbodiment 11.6Embodiment 21.2Embodiment 30.6Embodiment 40.6Embodiment 50.4Comparative example 15.8

[0013] It can be seen from the above statistical results that the edge defects are greatly reduced by replacing the nozzle with a syringe. In addition, the applicant also pleasantly surprised to find that the edge defects were further reduced by ultrasonic treatment.Embodiment 7

[0014] Fastness test is performed on the edged product of Embodiments 1-5 and Comparative Example 1. The specific method is to scribe 11 parallel lines every 2 mm using a paper knife on a sample of each edged product, and then scribe 11 lines in the vertical direction to reach a metal layer. Then, a transparent tape is adhered to the drawn area firmly by light pressing. After 5 min, the transparent tape is torn, and the damaged or peeled part in 10*10 grids is calculated. The test is carried out five times in parallel and the average value is taken, and the test results are shown in Table 2. Table 2: Scribe test results of Embodiments 1-5 and Comparative Example 1Group No.Average number of edging defectsEmbodiment 12.4Embodiment 21.8Embodiment 30.8Embodiment 40.6Embodiment 51.0Comparative example 17.6

[0015] It can also be seen from the results of this embodiment that the edge defects are greatly reduced by replacing the nozzle with a syringe. In addition, the applicant also pleasantly surprised to find that the edge defects were further reduced by ultrasonic treatment. holding time is 25 min; in edging color register spraying of step IV, the injection needle has a caliber of 1.5 mm, the hub is horizontally placed on an automatic rotary table, the needle is fixed on an adjustable bracket, a paint supply system is closed, the distance between the needle and the sprayed surface of the wheel is 4 mm, the flow rate of the injected paint is 10 cc / min, the power of the automatic rotary table is 56.6 Hz, and the air pressure of the closed paint supply system is 2.0 bar; electrostatic spraying is adopted in the high-gloss transparent powder spraying process of step VI, the distance between the electrostatic gun and the surface of the wheel is 200 mm, the throughput of the powder gun is 2.5 m 3< / h, the atomizing pressure is 1.5 bar, the electrostatic pressure is 40 KV, the front spray thickness is about 80 µm, the transparent powder curing temperature is 177°C, and the holding time is 22 min.Embodiment 2

[0016] In steps I, III and V, the first, second and third pretreatment and drying steps sequentially include 11 processes: washing, pre-degreasing, degreasing, washing, acid pickling, washing, passivation, washing, closing, washing and drying; an electrostatic gun is adopted for spraying body powder in step II, the distance between the electrostatic gun and the surface of a wheel is 300 mm, the throughput of the powder gun is 4.5 m 3< / h, the atomizing pressure is 4.0 bar, the electrostatic pressure is controlled at 70 KV, the front spray thickness is 160 µm, the body powder curing temperature is 185°C, and the holding time is 20 min; an air gun is adopted for spraying a paint in step II, the distance between the air gun and the surface of the wheel is 250 mm, the throughput of the spray gun is 100 cc / min, the atomizing pressure is 3.0 bar, the sector pressure is 3.0 bar, the paint spray thickness is 20 µm, the temperature of the wheel workpiece is 40-50°C, the paint curing temperature is 150°C, and the holding time is 15 min; in edging color register spraying of step IV, the injection needle has a caliber of 1.5 mm, the hub is horizontally placed on an automatic rotary table, the needle is fixed on an adjustable bracket, a paint supply system is closed, the distance between the needle and the sprayed surface of the wheel is 6 mm, the flow rate of the injected paint is 20 cc / min, the power of the automatic rotary table is 56.6 Hz, and the air pressure of the closed paint supply system is 3.0 bar; electrostatic spraying is adopted in the high-gloss transparent powder spraying process of step VI, the distance between the electrostatic gun and the surface of the wheel is 300 mm, the throughput of the powder gun is 3.5 m 3< / h, the atomizing pressure is 2.5 bar, the electrostatic pressure is 60 KV, the front spray thickness is about 120 µm, the transparent powder curing temperature is 180°C, and the holding time is 15 min.Embodiment 3

[0017] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that step VI further includes the step of ultrasonic treatment, ultrasonic waves are applied to the wheel in a pulsed manner, each pulse lasts for 0.7 s, and the energy density is 400W / cm 2< .Embodiment 4

[0018] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that step VI further includes the step of ultrasonic treatment, ultrasonic waves are applied to the wheel in a pulsed manner, each pulse lasts for 0.7 s, and the energy density is 120W / cm 2< .Embodiment 5

[0019] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that step VI further includes the step of ultrasonic treatment, ultrasonic waves are applied to the wheel in a pulsed manner, each pulse lasts for 0.7 s, and the energy density is 240 W / cm 2< .Comparative Example 1

[0020] The condition of each step in this embodiment is substantially the same as that in Embodiment 1, except that a spray gun is used for spraying a paint at a small flow rate and a low angle in step IV, the distance between the spray head and the sprayed surface of the wheel is 6 mm, the flow rate of the injected paint is 20 cc / min, the power of the automatic rotary table is 56.6 Hz, and the air pressure of a closed paint supply system is 3.0 bar.Embodiment 6

[0021] Edged products having bright color and sprayed uniformly are obtained from Embodiments 1-5 and Comparative Example 1.

[0022] First, the edge of the edged area of the product of each embodiment or the comparative example is observed with a magnifying glass. The edged area of the product of each embodiment or the comparative example is observed under an 8x magnifying glass, and the numbers of edge splashing points and edge protruding points within 5 cm are calculated. The edge splashing points are calculated as 3 scores, and the edge protruding points are calculated as 1 score. Five samples of the edged area of each product are counted and averaged. The results are shown in Table 1. Table 1: Edge characteristic test of Embodiments 1-5 and Comparative Example 1Group No.Edging defect integralEmbodiment 11.6Embodiment 21.2Embodiment 30.6Embodiment 40.6Embodiment 50.4Comparative example 15.8

[0023] It can be seen from the above statistical results that the edge defects are greatly reduced by replacing the nozzle with a syringe. In addition, the applicant also pleasantly surprised to find that the edge defects were further reduced by ultrasonic treatment.Embodiment 7

[0024] Fastness test is performed on the edged product of Embodiments 1-5 and Comparative Example 1. The specific method is to scribe 11 parallel lines every 2 mm using a paper knife on a sample of each edged product, and then scribe 11 lines in the vertical direction to reach a metal layer. Then, a transparent tape is adhered to the drawn area firmly by light pressing. After 5 min, the transparent tape is torn, and the damaged or peeled part in 10*10 grids is calculated. The test is carried out five times in parallel and the average value is taken, and the test results are shown in Table 2. Table 2: Scribe test results of Embodiments 1-5 and Comparative Example 1Group No.Average number of edging defectsEmbodiment 12.4Embodiment 21.8Embodiment 30.8Embodiment 40.6Embodiment 51.0Comparative example 17.6

[0025] It can also be seen from the results of this embodiment that the edge defects are greatly reduced by replacing the nozzle with a syringe. In addition, the applicant also pleasantly surprised to find that the edge defects were further reduced by ultrasonic treatment.

Claims

1. A color register edging method for an aluminum alloy hub, wherein including the following steps: (I) a first pretreatment and drying step, including washing, degreasing, acid pickling and passivation; (II) a body powder spraying and curing step, and a subsequent paint spraying and curing step; (III) a second pretreatment and drying step, including washing, degreasing, acid pickling and passivation; (IV) an edging color register applying and curing step, wherein a color register paint is squeezed onto a surface that needs color register by using an injection needle; (V) a third pretreatment and drying step, including washing, degreasing, acid pickling and passivation; and (VI) a high-gloss transparent powder spraying and curing step.

2. The method according to claim 1, wherein in step II, an electrostatic gun is adopted for spraying body powder, the distance between the electrostatic gun and the surface of a wheel is 200-300 mm, the throughput of the powder gun is 2.5-4.5 m3 / h, the atomizing pressure is 3.0-4.0 bar, the electrostatic pressure is controlled at 50-70 KV, the front spray thickness is 120-160 µm, the body powder curing temperature is 175-185°C, and the holding time is 20-25 min.

3. The method according to claim 1, wherein in step II, an air gun is adopted for spraying a paint, the distance between the air gun and the surface of the wheel is 180-250 mm, the throughput of the spray gun is 60-100 mL / min, the atomizing pressure is 2.0-3.0 bar, the sector pressure is 2.0-3.0 bar, the paint spray thickness is 10-20 µm, the temperature of the wheel workpiece is 40-50°C, the paint curing temperature is 145-150°C, and the holding time is 15-25 min.

4. The method according to claim 1, wherein in edging color register applying of step IV, the injection needle has a caliber of 1.5 mm, the hub is horizontally placed on an automatic rotary table, and the needle is fixed on an adjustable bracket.

5. The method according to claim 4, wherein the distance between the needle and the sprayed surface of the wheel is 4-6 mm, the flow rate of the injected paint is 10-20 mL / min, the rotational frequency of the automatic rotary table is 56.6 Hz, and the air pressure of a closed paint supply system is 2.0-3.0 bar.

6. The method according to claim 1, wherein electrostatic spraying is adopted in the high-gloss transparent powder spraying process, the distance between the electrostatic gun and the surface of the wheel is 200-300 mm, the throughput of the powder gun is 2.5-3.5 m3 / h, the atomizing pressure is 1.5-2.5 bar, the electrostatic pressure is controlled at 40-60KV, the front spray thickness is about 80-120 µm, the transparent powder curing temperature is 177-180°C, and the holding time is 15-22 min.