METHOD FOR PRODUCING AN INSULATION PRODUCT BASED ON ROCK WOOL
Patent Information
- Application Number
- DE602020041601
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-11
- Filing Date
- 2020-01-08
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-01-08
AI Technical Summary
Mineral wool insulation products using carbohydrate-based binders face issues with mechanical property retention over time, especially at high humidity, leading to increased binder proportions and costs, and instability of phenolic resins in acidic environments.
A binder composition with a pH between 1.0 and 6.5, containing hydrogenated sugars, monomeric polycarboxylic acids, and aminated phenolic resins, which are stable in acidic conditions and improve mechanical properties without the need for high phenolic resin quantities.
The solution enhances the mechanical properties and resistance to aging of mineral wool insulation products, maintaining performance under humid conditions without increasing costs or altering fire reaction properties.
Description
[0001] The present invention relates to a method for manufacturing a fiber-based insulation product, in particular based on mineral wool, using a binder composition containing a carbohydrate component, at least one monomeric polycarboxylic acid or anhydride and an amino phenolic resin, water-soluble and stable in an acid medium.
[0002] The manufacture of mineral wool insulation products generally involves a step in which the glass or rock fibres are produced using a centrifugation process. On their way from the centrifugation device to the fibre collection belt, an aqueous sizing compound, also known as a binder, is sprayed onto the still-hot fibres, which then undergo a thermosetting reaction at temperatures of around 200°C.
[0003] Phenolic resins, used for decades as binders, are increasingly being replaced by products from renewable sources that emit little or no formaldehyde, a compound considered harmful to human health.
[0004] It is thus known, for example from WO2009 / 0809038, to bind mineral fibres with formaldehyde-free aqueous sizing compositions containing, as heat-crosslinkable reagents, carbohydrates and polycarboxylic acids.
[0005] Application WO2007 / 014236 discloses aqueous, formaldehyde-free binders comprising Maillard reagents, namely reducing sugars and amino compounds.
[0006] These sizing compositions based on reducing sugars have the disadvantage of giving rise to coloring reactions (caramelization, Maillard reaction) which make it difficult, if not impossible, to obtain light-colored products.
[0007] The Applicant proposed in its applications WO2010 / 029266 and WO2013 / 014399 binders not based on reducing sugars, but based on hydrogenated sugars, also called sugar alcohols. These reagents have considerably higher thermal stability than reducing sugars and do not give rise to Maillard and / or caramelization reactions.
[0008] Formaldehyde-free binders containing both hydrogenated sugars and reducing or non-reducing sugars have been disclosed in applications WO2013 / 021112 and WO2015 / 159012 in the name of the Applicant, respectively.
[0009] Insulation products based on mineral wool and carbohydrate-based binders (reducing sugars, non-reducing sugars, hydrogenated sugars), however, are relatively hygroscopic and retain their mechanical properties less well over time than products made with phenolic binders (resols), especially at high humidity. To compensate for the loss of mechanical properties after a certain period of aging of these insulation products, it is generally necessary to increase the proportion of binder by approximately 10 to 20%, which not only increases the cost of the final product but also alters its reaction to fire.
[0010] The Applicant proposed in application WO2015 / 132518 to improve the resistance to aging of mineral wool insulation products bound by binders based on hydrogenated sugars, possibly mixed with reducing sugars, by incorporating fairly large quantities of epoxysilanes into the binder composition.
[0011] It has also successfully used both hydrophobic and water-soluble monohydric alcohols, such as phenoxyethanol, to reduce the moisture sensitivity of such insulation products (see WO2015 / 181458).
[0012] However, the hydrophobic epoxysilanes and monoalcohols used in these binder compositions undesirably increase their cost.
[0013] In the course of its research aimed at finding further solutions, in particular more economical solutions, to improve the mechanical properties and resistance to aging of insulation products based on fibers bound by carbohydrate-based binders, the Applicant tested binder compositions containing small amounts of phenolic resins (resols). These tests were, however, unsuccessful because the usual phenolic resins, consisting of phenol / formaldehyde condensates (PF resins), or phenol / formaldehyde and urea / formaldehyde condensates (PFU resins), proved to be unstable. They react and precipitate rapidly, even at room temperature, when brought into contact with the aqueous binder compositions based on sugars and polycarboxylic acids described in the introduction (WO2009 / 0809038, WO2010 / 029266, WO2013 / 014399, WO2013 / 021112, WO2015 / 159012, WO2015 / 132518, WO2015 / 181458).The Applicant attributed this instability of the PF and PFU resins to the acidic pH of the binder compositions.
[0014] The present invention is based on the discovery that a particular group of phenolic resins containing basic (protonable) amine functions was stable in acidic media and therefore usable with the aqueous binder compositions based on polycarboxylic acids and sugars and / or hydrogenated sugars of the state of the art. These phenolic resins with amine functions are known and their preparation is described in detail in the Applicant's applications WO2008 / 043960 and WO2008 / 043961.
[0015] The use of these amino phenolic resins in acid binder compositions based on sugars and polycarboxylic acids has made it possible to improve the mechanical properties of the insulation products obtained, including after aging in humid conditions, provided that certain quantities of phenolic resin are not exceeded.
[0016] The present application therefore has as its first object a method of manufacturing an insulating product based on mineral or organic fibers, comprising applying an aqueous binder composition to mineral or organic fibers, heating the fibers sized by the aqueous binder composition so as to evaporate the volatile phase of the aqueous binder composition and to achieve thermal curing of the non-volatile residue, or packaging the mineral or organic fibers glued with the aqueous binder composition for storage and / or transport, the aqueous binder composition having a pH between 1.0 and 6.5, preferably between 1.5 and 5.0, and comprising: (a) at least one carbohydrate selected from hydrogenated sugars, reducing sugars, non-reducing sugars and mixtures thereof, (b) at least one monomeric polycarboxylic acid or an anhydride of such an acid, (c) from 1 to 35% by weight, based on the total weight of components (a), (b), and (c), of a water-soluble amino phenolic resin consisting essentially of phenol-formaldehyde condensates and phenol-formaldehyde-amine condensates.
[0017] The present application also relates to an insulating product based on mineral or organic fibers obtained by such a process.
[0018] Finally, it relates to an aqueous binder composition for the preparation of insulation products based on mineral or organic fibers, having a pH of between 1.0 and 6.5, preferably between 1.5 and 5.0, and comprising: (a) at least one carbohydrate selected from hydrogenated sugars, reducing sugars, non-reducing sugars and mixtures thereof, (b) at least one monomeric polycarboxylic acid or an anhydride of such an acid, (c) from 1 to 35% by weight, based on the total weight of components (a), (b), and (c), of a water-soluble amino phenolic resin consisting essentially of phenol-formaldehyde condensates and phenol-formaldehyde-amine condensates.
[0019] In the present application the terms "carbohydrate" and "carbohydrate" have a broader meaning than usual, because they include oses and osides having at least one aldehyde or ketone group (reducing group), non-reducing sugars consisting of several carbohydrate units whose carbons carrying the hemiacetalic hydroxyl are involved in the osidic bonds linking the units together, as well as hydrogenated sugars (also called alditols or sugar alcohols) which are the products of hydrogenation of oses or osides where the aldehyde or ketone group has been reduced to an alcohol function.
[0020] Component (a) may in principle contain any carbohydrate selected from reducing sugars, non-reducing sugars and hydrogenated sugars and mixtures thereof.
[0021] Component (a) of the binder composition of the present invention advantageously comprises a certain fraction of hydrogenated sugars. This hydrogenated sugar content of the carbohydrate (component (a)) is advantageously between 25 and 100% by weight, preferably at least equal to 30% by weight, in particular at least equal to 50% by weight, and ideally at least equal to 70% by weight, relative to the total weight of the carbohydrate component.
[0022] In a preferred embodiment, component (a) consists solely of hydrogenated sugars and is free of reducing and non-reducing sugars. This embodiment is advantageous because it leads to particularly low-color insulating products.
[0023] The term "hydrogenated sugar" means all the products resulting from the reduction of a saccharide chosen from monosaccharides, disaccharides, oligosaccharides and polysaccharides and mixtures of these products. Hydrogenated sugars are also called sugar alcohols, alditols or polyols. They can be obtained by catalytic hydrogenation of saccharides. The hydrogenation can be carried out by known methods operating under conditions of high hydrogen pressure and temperature, in the presence of a catalyst chosen from the elements of groups IB, IIB, IVB, VI, VII and VIII of the periodic table of elements, preferably from the group comprising nickel, platinum, palladium, cobalt, molybdenum and mixtures thereof. The preferred catalyst is Raney nickel.
[0024] The hydrogenated sugar(s) are advantageously chosen from the hydrogenation products of monosaccharides, disaccharides, oligosaccharides and their mixtures, preferably from the group consisting of erythritol, arabitol, xylitol, sorbitol, mannitol, iditol, maltitol, isomaltitol, lactitol, cellobitol, palatinitol, maltotritol, and the hydrogenation products of starch hydrolysates or hydrolysates of lignocellulosic materials, in particular hemicellulose, in particular xylans and xyloglucans.
[0025] Particular preference will be given to using a hydrogenated sugar chosen from the group formed by maltitol, xylitol, sorbitol and the hydrogenation products of starch hydrolysates or lignocellulosic materials.
[0026] The reducing sugars are preferably selected from monosaccharides such as glucose, galactose, mannose and fructose, disaccharides such as lactose, maltose, isomaltose, cellobiose and mixtures thereof, as well as the starch or lignocellulosic material hydrolysates described above. Glucose and fructose and mixtures thereof, in particular glucose, will preferably be used.
[0027] The non-reducing sugars are preferably disaccharides such as trehalose, isotrehaloses, sucrose, isosucroses and mixtures thereof. Sucrose is particularly preferred.
[0028] The polycarboxylic acid(s) used in the present invention are monomeric polycarboxylic acids. In other words, in the present invention this term does not include polymers obtained by polymerization of monomeric carboxylic acids, such as homopolymers or copolymers of acrylic acid or methacrylic acid.
[0029] Polycarboxylic acids chosen from the group consisting of dicarboxylic acids, tricarboxylic acids and tetracarboxylic acids will preferably be used.
[0030] The dicarboxylic acids are for example chosen from the group formed by oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, malic acid, tartaric acid, tartronic acid, aspartic acid, glutamic acid, fumaric acid, itaconic acid, maleic acid, traumatic acid, camphoric acid, phthalic acid and its derivatives, in particular containing at least one boron or chlorine atom, tetrahydrophthalic acid and its derivatives, in particular containing at least one chlorine atom such as chlorendic acid, isophthalic acid, terephthalic acid, mesaconic acid and citraconic acid. Tricarboxylic acids are for example chosen from the group formed by citric acid, tricarballylic acid, 1,2,4-butanetricarboxylic acid, aconitic acid, hemimellitic acid, trimellitic acid and trimesic acid.Examples of tetracarboxylic acids are 1,2,3,4-butanetetracarboxylic acid and pyromellitic acid.
[0031] The particularly preferred polycarboxylic acid is citric acid.
[0032] The Applicant has carried out numerous tests to determine the respective proportions of components (a) and (b) which result in binders which, in the crosslinked state, give the final product the best mechanical properties, in particular after accelerated aging in humid conditions.
[0033] These tests have shown that the carbohydrate / polycarboxylic acid weight ratio is advantageously between 25 / 75 and 75 / 25.
[0034] When the polycarboxylic acid is citric acid, this ratio is preferably between 25 / 75 and 55 / 45, in particular between 30 / 70 and 50 / 50.
[0035] In the technical field of phenol-formaldehyde resins, two main families are distinguished, namely: novolak resins prepared in an acid medium and resols obtained by basic catalysis.
[0036] The phenolic resins of the present invention are part of this second family.
[0037] Resol resins are obtained in a basic medium by reacting phenol with an excess of formaldehyde, the formaldehyde / phenol molar ratio typically being between 2 and 4, each phenol molecule potentially being able to react with three formaldehyde molecules.
[0038] Resol resins contain numerous methylol functions carried by an aromatic nucleus, which constitute the crosslinking sites by dehydration / release of formalin. These resins are essentially composed of phenol / formaldehyde (PF) condensates, residual phenol and residual formaldehyde. In an acidic environment they react, i.e. polymerize, very quickly at room temperature and precipitate.
[0039] These resol resins, consisting essentially of phenol / formaldehyde (PF) condensates and residual phenol and formaldehyde, can, after neutralization of the catalyst, be mixed with urea, which serves mainly as a cosolvent improving the dilutability of the resin and as a trapping agent for residual formaldehyde. Such resols and their preparation are described in detail in application WO 01 / 96254. The addition of urea described in this application, however, does not significantly improve the stability of the resols at acidic pH, and the resins described in this application cannot be used in the present application.
[0040] The amine resols (component (c)) used in the present application are water-soluble resins stable at acid pH, even at very acid pH between 1 and 2. This good stability is obtained by means of an additional reaction step which consists of reacting resol resins containing essentially phenol / formaldehyde condensates, phenol and formaldehyde with an amine, preferably a monoalkanolamine, and in particular monoethanolamine.
[0041] This alkanolamine reacts according to the Mannich reaction with phenol / formaldehyde (PF) condensates, phenol and formaldehyde to form phenol / formaldehyde / amine (PFA) condensates. At the end of the reaction the reaction mixture can be acidified without this causing polymerization at room temperature. These resol resins are therefore considered to be stable in acidic media. Their synthesis is described in the Applicant's applications WO2008 / 043960 and WO2008 / 043961. They are also distinguished by the fact that they are almost free of urea-formaldehyde condensates which are present only in trace amounts. These urea-formaldehyde condensates are present in significant quantities in many prior art phenolic resins and have insufficient thermal stability, releasing formaldehyde by thermal decomposition.
[0042] In a known manner, up to 25% by weight, preferably between 10% and 20% by weight of urea, can be added to the amino resol resin after reaction with the monoalkanolamine, cooling of the reaction mixture and acidification, these quantities being expressed relative to the total dry weight of amino resol resin and urea. Urea serves mainly as a cosolvent in this type of resin.
[0043] During the tests aimed at developing insulation products based on predominantly bio-sourced ingredients, which are more resistant to aging, the Applicant noted that it was important to use a relatively low fraction of amino phenolic resin. Optimum mechanical properties were observed for amino phenolic resin fractions of around 5 to 20% by weight relative to the total weight of components (a), (b) and (c).
[0044] The aqueous binder composition of the present invention therefore contains between 1 and 35% by weight, preferably from 2 to 30%, in particular from 5 to 27% by weight, and more preferably from 7 to 20% by weight, based on the total weight of components (a), (b) and (c), of water-soluble phenolic amino resin consisting essentially of phenol-formaldehyde condensates and phenol-formaldehyde-amine condensates. These amounts are understood to be expressed as dry matter. Furthermore, they do not include the weight of urea or other additives possibly added to the mixture of the phenolic amino resin and (a) and (b).
[0045] The aqueous binder composition has, at the time of its application to the mineral wool fibres, a pH between 1.0 and 6.5, preferably between 1.5 and 5.0. This pH is more preferably between 1.5 and 4.0, or even between 1.7 and 3.0.
[0046] The aqueous binder composition of the present invention further advantageously contains between 0.5% and 10% by weight, preferably between 1.0% and 5% by weight, based on the total weight of solids of the binder composition, of an esterification catalyst, preferably selected from the group consisting of sodium hypophosphite and hypophosphorous acid.
[0047] The binder composition may further comprise known additives in the following proportions calculated on the basis of 100 parts by weight of component (a) + (b) + (c): from 0 to 5 parts of silane, in particular of an epoxysilane or aminosilane (coupling agent), from 0 to 40 parts, preferably from 4 to 25 parts, of an oil or an oil emulsion (anti-dust agent), from 0 to 5 parts of a silicone.
[0048] The preparation of the binder composition is carried out by simply mixing the constituents (components (a), (b), (c), catalyst, urea and additives) with water.
[0049] At the time of application to the fibers, the binder composition has a dry matter content of between 2 and 15% by weight, preferably between 3 and 10% by weight.
[0050] It is applied in an amount such that the content of insoluble and infusible binder in the final product obtained after thermal hardening is between 2% and 20% by weight, preferably between 3% and 15% by weight, in particular between 4 and 12% by weight.
[0051] When the insulation product is a mineral wool-based product, the binder composition is sprayed onto the mineral fibers at the outlet of the centrifugal device and before the mineral fibers are collected on the receiving member in the form of a sheet of fibers which is then treated in an oven at a temperature allowing the crosslinking of reactive ingredients and the formation of an infusible binder. This crosslinking / thermal curing step is carried out by heating to a temperature greater than or equal to 180°C, preferably between 190°C and 220°C, for a period of between 20 seconds and 300 seconds, preferably between 30 and 250 seconds.
[0052] When the insulation product is a product made from organic fibers, such as fibers of plant origin, for example cellulose fibers, or animal fibers, for example wool, the cooking temperature is generally lower than that used for cooking products made from mineral fibers in order to protect the organic fibers from possible thermal degradation. Cooking temperatures are, for example, between 150 and 200 °C. The cooking time is generally between several minutes and several tens of minutes, for example between 5 and 50 minutes, preferably between 10 and 30 minutes.
[0053] In the process of the present invention, the cooking of the mineral or organic fibers can be carried out immediately after application of the binder composition to the fibers and collection of the glued fibers on a conveyor belt, for example by passing through a thermostatically controlled oven at the desired cooking temperature.
[0054] The method of the present application also covers an embodiment where the sized fiber mat is not immediately cooked but is packaged, for example partially dried, cut, compressed, shaped and packaged, for a cooking step separate from the step of manufacturing the sized fiber mat. The packaging material must be chosen so as to allow the storage and / or transport of these intermediate products (fibers sized with an uncured binder) for a further process step, carried out later or in a different location, and comprising the thermal curing of the binder, possibly after forming the intermediate product, for example in a mold. Example
[0055] A Composition 1 is prepared at 30% dry extract containing 48 parts by weight of maltitol (component (a)), 52 parts by weight of citric acid (component (b)), and 5 parts by weight of sodium hypophosphite (catalyst).
[0056] A 2 to 30% dry extract composition is prepared containing 80 parts of amino phenolic resin (component (c)), 20 parts of urea (cosolvent) and 3 parts of ammonium sulfate (catalyst)
[0057] Compositions 1 and 2 are mixed in varying proportions so as to obtain different weight ratios of component (c) to the sum of components (a)+(b)+(c). [Table 1] Test solution Component parts (c) Urea parts Parts of component (a) + component (b) (c) / (a)+(b)+(c) Test 1 according to the invention 8 2 90 8,2 % Test 2 according to the invention 16 4 80 16,7 % Test 3 according to the invention 24 6 70 25,5 % Comparative test 4 40 10 50 44,4 % Comparative Test 5 0 0 100 0 %
[0058] The solutions from tests 1 - 5 are used to determine the curing onset temperature (TR) of the binder by dynamic mechanical analysis (DMA). In addition, the Young's modulus and tensile strength of glass fiber wovens bonded by the different cured binders are determined before and after accelerated aging in humid conditions. Dynamic mechanical analysis :
[0059] Using a pipette, 0.4 g of test solutions 1 - 5 are deposited onto strips of Whatman glass fiber filters (grade GF / C; reference 1822-915) measuring 60 x 12 mm, stacked two by two. The dynamic mechanical analysis is carried out on a TA Instruments Q800 DMA apparatus equipped with a double-ended jaw. During each cooking test, a temperature ramp is applied with the following parameters: stress: 0.1% temperature gradient: 25°C to 250°C (4°C per minute) frequency: 1 Hz
[0060] The curing start temperature is defined as the temperature at the maximum of the tan delta loss factor. The measurement accuracy is ±5°C. Determination of Young's modulus and tensile strength
[0061] Glass fibre fabrics are impregnated in a bath of test solutions 1 - 5, previously diluted to 20% dry extract, so as to deposit approximately 6% of binder on the fibres. The impregnated fabrics are baked for 120 seconds in a fan-assisted oven at 215°C.
[0062] For each test, the cooked woven fabrics were cut into ten rectangular strips. Half of the strips were subjected to an accelerated aging protocol under humid conditions (3 days at 35°C and 95% relative humidity).
[0063] An Instron Series 5960 tensile tester is used, with the tensile direction at a 45° angle to the warp and weft direction.
[0064] The Young's modulus before aging and the tensile strength of the binder joints were measured before and after accelerated aging. The results, averaged over 5 tests, are presented in Table 2 below. [Table 2] Essay pH TR (°C) Young's modulus (MPa) Tensile strength (N) before aging Tensile strength (N) after aging 1 (invention) 1,8 140±5 5200±315 125 ± 4 73 ± 3 2 (invention) 1,9 138±5 5280±250 122 ± 4 72 ± 2 3 (invention) 2,0 nd 5000±900 113 ± 5 68 ± 2 4 (comparative) 2,1 130±5 5220±130 95 ± 3 63 ± 2 5 (comparative) 1,7 144±5 5190±190 116 ± 5 63 ± 4
[0065] It is found that the three tests according to the invention (tests 1 - 3) using a mixed binder based on maltitol (component (a)), citric acid (component (b)) and amino phenolic resin (component (c)) in proportions such that component (c) represents from approximately 8% to 25% by weight of the sum of components (a), (b) and (c) have a better tensile strength after accelerated aging than a binder based on maltitol and citric acid only (test 5) and than a binder containing more than 40% by weight of amino phenolic resin (component (c)) (test 4).
Claims
1. A method for manufacturing an insulating product based on mineral or organic fibers, comprising - applying an aqueous binder composition to mineral or organic fibers, preferably mineral wool fibers, - heating the fibers coated with the aqueous binder composition so as to evaporate the volatile phase of the aqueous binder composition and to bring about the thermal curing of the non-volatile residue, or packaging the mineral or organic fibers coated with the aqueous binder composition for the purpose of storage and / or transport, the aqueous binder composition having a pH of between 1.0 and 6.5, preferably between 1.5 and 5.0, and comprising: (a) at least one carbohydrate selected from hydrogenated sugars, reducing sugars, non-reducing sugars and mixtures thereof, (b) at least one monomeric polycarboxylic acid or an anhydride of such an acid, (c) from 1 to 35% by weight, relative to the total weight of components (a), (b) and (c), of a water-soluble, amine-containing phenolic resin consisting essentially of phenol-formaldehyde condensates and phenol-formaldehyde-amine condensates.
2. The method according to claim 1, characterized in that the aqueous binder composition contains from 2 to 30%, preferably from 5 to 27% by weight, and in particular from 7 to 20% by weight, relative to the total weight of components (a), (b) and (c), of water-soluble amine-containing phenolic resin consisting substantially of phenol-formaldehyde condensates and of phenol-formaldehyde-amine condensates.
3. The method according to claim 1 or 2, characterized in that the phenol-formaldehyde-amine condensates are phenol-formaldehyde-monoalkanolamine condensates.
4. The method according to one of the preceding claims, characterized in that the polycarboxylic acid is citric acid.
5. The method according to one of the preceding claims, characterized in that the proportion of hydrogenated sugars in the carbohydrate (component (a)) is between 25 and 100% by weight.
6. The method according to claim 5, characterized in that the carbohydrate (component (a)) contains at least 30% by weight, preferably at least 50% by weight, and in particular at least 70% by weight of hydrogenated sugars.
7. The method according to one of the preceding claims, characterized in that the hydrogenated sugar is selected from the hydrogenation products of monosaccharides, disaccharides, oligosaccharides and mixtures thereof.
8. The method according to any one of the preceding claims, characterized in that the hydrogenated sugar is selected from the group consisting of maltitol, xylitol, sorbitol and the hydrogenation products of starch hydrolysates or lignocellulosic materials.
9. The method according to any one of the preceding claims, characterized in that the weight ratio of the carbohydrate(s) (component (a)) to the polycarboxylic acid ((component (b)) is between 25 / 75 and 75 / 25.
10. The method according to any one of the preceding claims, characterized in that the aqueous binder composition has a pH of between 1.5 and 4.0, preferably between 1.7 and 3.0.
11. The method according to any one of the preceding claims, characterized in that the aqueous binder composition further contains between 0.5 and 10% by weight, preferably between 1.0 and 5% by weight, relative to the total weight of solid materials of the binder composition, of an esterification catalyst, preferably selected from the group consisting of sodium hypophosphite and hypophosporous acid.
12. An aqueous binder composition for the preparation of insulating products based on mineral or organic fibers, having a pH of between 1.0 and 6.5, preferably between 1.5 and 5.0, and comprising: (a) at least one carbohydrate selected from hydrogenated sugars, reducing sugars, non-reducing sugars and mixtures thereof, (b) at least one monomeric polycarboxylic acid or an anhydride of such an acid, (c) from 1 to 35% by weight, relative to the total weight of the components (a), (b) and (c), of a water-soluble, amine-containing phenolic resin consisting essentially of phenol-formaldehyde condensates and phenol-formaldehyde-amine condensates.
13. An insulating product based on mineral or organic fibers, obtained by the method according to any one of claims 1 to 11.